A spinning process and spinning equipment for 30D / 72F ultrafine denier cool-feeling low-elastic polyester fiber

By employing a process involving deep drying pretreatment, gradient low-temperature melting, low-temperature dynamic blending, gradient filtration, graded cooling, and constant tension winding, the production challenges of 30D/72F ultrafine denier cool-feeling low-elastic polyester fiber have been solved. This process achieves uniformity and washability of the cool-feeling fiber, improves spinnability and stability of the finished fiber, and makes it suitable for large-scale production.

CN123108754APending Publication Date: 2026-11-17TONGKUN GRP ZHEJIANG HENGCHAO CHEM FIBER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611309914.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies cannot simultaneously meet the requirements of high coolness, uniformity, water resistance, and high porosity spinning adaptability of 30D/72F ultrafine denier cool-feeling low-elasticity polyester fibers, and there are problems such as masterbatch agglomeration, melt hydrolysis, and monofilament adhesion.

Method used

The process involves deep drying pretreatment, gradient low-temperature melting, low-temperature dynamic blending, gradient filtration, staged cooling, uniform oiling, and constant tension winding. Combined with specialized spinning equipment, this ensures uniform dispersion of the cooling masterbatch, integrity of the polyester molecular chains, and uniform cooling of the monofilaments, thus avoiding high-temperature damage and adhesion.

Benefits of technology

It achieves uniformity and washability of cooling fibers throughout the entire range, improves spinnability and stability of finished fibers, reduces the use of chemical auxiliaries and wastewater discharge, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108754A_ABST
    Figure CN123108754A_ABST
Patent Text Reader

Abstract

This invention discloses a spinning process and equipment for 30D / 72F ultrafine denier cool-feeling low-elasticity polyester fiber. The process includes: air-powered dust removal and deep constant-temperature drying of the cool-feeling masterbatch, followed by gradient low-temperature melting to obtain masterbatch melt; quantitative injection of low-elasticity polyester melt, followed by static premixing and low-temperature dynamic mixing to obtain blended melt; extrusion through a 72-hole spinneret after three-stage gradient filtration, followed by windless slow cooling and double-sided ring blowing for curing, uniform oiling and two-stage low-pressure bundling, and finally constant-tension winding to obtain the finished product; the equipment is arranged sequentially along the material flow direction, including cool-feeling masterbatch pretreatment, online melt mixing, dedicated spinning components, graded cooling, oiling and bundling, and constant-tension winding units; this invention can achieve high-proportion homogeneous dispersion of cool-feeling masterbatch, solving problems such as melt degradation, component blockage, and uneven monofilament; the finished fiber has a long-lasting cool feel, mechanical stability, and excellent low-elasticity properties, making it suitable for large-scale mass production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of functional polyester fiber spinning technology, and discloses a spinning process and spinning equipment for 30D / 72F ultrafine denier cool-feeling low-elastic polyester fiber. Background Technology

[0002] 30D / 72F ultra-fine denier cooling low-elasticity polyester fiber monofilaments are fine in fineness, resulting in fabrics that are lightweight, breathable, and have a prominent cooling sensation upon contact. They also possess moderate resilience and excellent drape, making them widely applicable in summer cooling apparel, quick-drying sportswear, loungewear, sun-protective fabrics, and close-fitting knitwear. These products utilize a melt-spinning process with online addition of cooling masterbatch, eliminating the need for subsequent padding, dyeing, and functional finishing processes. This significantly reduces the use of chemical auxiliaries and wastewater discharge, offering substantial green and environmental advantages. Furthermore, the functional components are firmly bonded to the fiber body, ensuring wash resistance and long-lasting cooling sensation, resulting in high market added value. This represents the current mainstream research and development direction for functional differentiated synthetic fibers.

[0003] Currently, the industry generally uses a direct spinning process of blending cooling masterbatch with polyester melt to produce ultrafine denier cooling polyester fibers. The low elasticity is achieved through polyester matrix modification and the coordinated control of spinning tension, temperature, and cooling parameters. The masterbatch addition ratio for conventional cooling fibers is mostly controlled between 1.5% and 3.0%, and these are mostly products with conventional fineness and low porosity. However, the 30D / 72F ultrafine denier specification has a high number of monofilaments and extremely small monofilament diameters. To ensure long-lasting cooling and a satisfactory contact cooling coefficient, the cooling masterbatch addition ratio needs to be increased to over 3.8%. Furthermore, the rheological properties and molecular orientation of low-elasticity polyester melt differ significantly from those of conventional polyester melt, making it difficult for traditional equipment and processes to match the production of this specification. These technical shortcomings constitute a major bottleneck for industrialization.

[0004] High proportions of cooling masterbatch are prone to agglomeration and sedimentation in polyester melt, resulting in uneven cooling sensation in local fiber areas and cooling blind spots in fabric. Cooling functional fillers are prone to failure and precipitation under high temperature spinning conditions, resulting in poor water washability of finished fibers and rapid decay of cooling effect after long-term use.

[0005] Cooling masterbatch often contains inorganic cooling powder. If the masterbatch is not dried thoroughly and has a high moisture content, it will accelerate the hydrolysis and degradation of the polyester melt during high-temperature melt spinning. The melt viscosity will fluctuate greatly, which will not only reduce the spinnability, but also destroy the regularity of the polyester molecular chain, resulting in a decrease in fiber strength and unstable elongation.

[0006] 30D / 72F is a high-pore-count ultrafine denier fiber with a large number of monofilaments and a large bundle spreading area. Traditional cooling air, oiling, and bundling processes cannot achieve uniform treatment over the entire area, which can easily lead to problems such as monofilament adhesion, filament drift, and uneven filament strands. The orientation and elasticity indicators of low-elasticity fibers are difficult to consistently meet the standards.

[0007] In summary, conventional processes are limited by the amount of masterbatch added, equipment structure, and process parameters, and cannot simultaneously meet the four major production requirements of high coolness, ultra-fine denier, high porosity, and low elasticity. Summary of the Invention

[0008] In view of this, the embodiments of this specification provide a spinning process and spinning equipment for 30D / 72F ultrafine denier cool-feeling low-elasticity polyester fiber, which solves the problems of uneven dispersion of high proportion of cool-feeling masterbatch, easy hydrolysis and degradation of melt, and poor adaptability of high-pore-count ultrafine denier spinning in existing production.

[0009] To achieve the above-mentioned technical effects, the technical solution adopted by this invention is: a spinning process for 30D / 72F ultrafine denier cool-feeling low-elastic polyester fiber, comprising:

[0010] S101: The cooling masterbatch is subjected to wind dust removal and deep constant temperature drying to obtain pretreated masterbatch; wind dust removal removes fine powder and impurities from the surface of the masterbatch to prevent impurities from entering the melt and causing spinning defects; deep constant temperature drying controls the moisture content of the masterbatch to an extremely low level, preventing melt hydrolysis and degradation from the source, while the low temperature drying environment can protect the cooling functional components from premature thermal deactivation.

[0011] S102: The pretreated masterbatch is melted at a gradient low temperature to obtain a cool-feeling masterbatch melt. The gradient heating low-temperature melting method avoids the deactivation of the cool-feeling filler caused by sudden high temperatures, while ensuring that the masterbatch is fully plasticized and melted, and outputting a masterbatch melt with stable viscosity.

[0012] S103: The cooling masterbatch melt is quantitatively injected into the low-elasticity polyester melt, and a homogeneous blended melt is obtained through static premixing and low-temperature dynamic mixing. The initial mixing of the two-phase melt is completed through static mixing, and then the homogeneous dispersion of the whole domain is achieved through low-temperature dynamic mixing. This ensures that the cooling powder does not agglomerate, and avoids high-temperature shearing damage to the polyester molecular chain and cooling functional components.

[0013] S104: The blended melt is subjected to three-stage gradient filtration and quantitatively extruded through a 72-hole spinneret to obtain a fine melt stream; the three-stage gradient filtration can intercept agglomerated particles and impurities of different sizes in layers, reducing melt flow resistance while ensuring filtration accuracy and extending the service life of the spinning assembly; the customized 72-hole spinneret is adapted to the requirements of ultra-fine denier high-hole number extrusion, ensuring uniform extrusion of monofilaments and regular cross-section.

[0014] S105: The melt stream is first slowly cooled in a windless slow cooling zone, and then solidified by double-sided ring blowing to obtain the nascent filament bundle. The windless slow cooling zone can slow down the cooling rate, eliminate the extrusion swelling effect, and allow the polyester macromolecular chains to slowly and regularly arrange themselves, stabilizing the low-elasticity orientation structure of the fiber. Double-sided ring blowing can achieve all-round uniform cooling of the wide filament bundle, avoid uneven stress and adhesion of single filaments, and accurately control the degree of molecular orientation.

[0015] S106: The nascent filament bundle is uniformly oiled and then bundled through a two-stage low-pressure network to obtain a stable finished filament bundle. Uniform oiling can reduce the friction coefficient between monofilaments and improve the smoothness of subsequent processing. The two-stage low-pressure network gradually gathers and disperses the monofilaments, improves the cohesion of the filament bundle, and avoids damage to the monofilaments and the cooling components on the surface of the fiber by high-pressure airflow.

[0016] S107: The finished yarn bundle is wound under constant tension to obtain 30D / 72F ultra-fine denier cool-feel low-elasticity polyester fiber; constant tension winding can avoid fiber deformation and solidification caused by tension fluctuations, ensure stable low-elasticity rebound index, and at the same time make the finished yarn cake form regular and unwind smoothly.

[0017] As a preferred embodiment, in step S101, the cooling masterbatch is dusted by a low wind speed of 2.8 m / s; then dried for 18 hours at a constant temperature of 75±5℃ using hot air at 142℃, combined with low-speed stirring at 4-7 rpm, to obtain a pretreated masterbatch with a moisture content ≤40 PPM. Low-speed dust removal prevents the masterbatch particles from breaking down and generating new fine powder; constant-temperature drying combined with low-speed stirring ensures uniform heating of the masterbatch without clumping, strictly controlling the moisture content to below 40 PPM, and preventing melt hydrolysis during subsequent spinning.

[0018] As a preferred embodiment, in step S102, the pretreated masterbatch is melted by a four-zone gradient temperature-controlled screw extruder, with the extrusion pressure controlled at 42-52 bar and the screw speed at 22-32 rpm, to obtain a cooling masterbatch melt. The four-zone gradient temperature control enables gradual heating and melting, matching the melting characteristics of the cooling masterbatch. The low-temperature extrusion conditions can minimize the heat loss of the cooling functional components.

[0019] As a preferred embodiment, in step S103, the cooling masterbatch melt is injected into the low-elasticity polyester melt at a mass ratio of 3.8% to 5.0%, and a polyester compatibilizer at a mass ratio of 0.08% to 0.11% is added simultaneously; a homogeneous blend melt is obtained by low-temperature dynamic mixing at 268±3℃ and a rotation speed of 28 to 33 rpm; this addition ratio can ensure that the cooling performance of the finished fiber meets the standard, and the polyester compatibilizer can improve the interfacial compatibility of the two-phase melt and inhibit the agglomeration of inorganic powder; the low-temperature dynamic mixing conditions take into account both the mixing uniformity and the thermal stability of the functional components.

[0020] As a preferred embodiment, in step S104, the blended melt is filtered through a three-stage gradient metal sand filter of 70-90-110 mesh; the initial pressure of the spinning assembly is controlled at 14.0-15.0 MPa, and the melt is extruded through a 72-hole spinneret with an aspect ratio of 7:1 to obtain a fine melt stream; the three-stage gradient filtration with increasing mesh size can intercept impurities and agglomerated particles step by step, reducing pressure loss while ensuring filtration accuracy; the spinneret micro-holes with an aspect ratio of 7:1 can optimize the rheological state of the melt extrusion and improve the uniformity of the monofilament cross section.

[0021] As a preferred embodiment, in step S105, the melt stream is first slowly cooled through a 55-65mm windless slow cooling zone; then it is cooled by double-sided ring blowing with a wind pressure of 20-26Pa, a wind temperature of 20-23℃, and a relative humidity of 60%-66% to obtain the nascent filament bundle. The height of the windless zone can match the extrusion expansion law of the 30D / 72F filament bundle, and the double-sided ring blowing parameters can achieve synchronous and uniform cooling of 72 monofilaments, ensuring consistent fiber orientation and stable low elasticity performance.

[0022] As a preferred embodiment, in step S106, the nascent filament bundle is oiled through a micro-aperture oil nozzle, and the oil content is controlled to a set value of ±0.03%; the bundle is then bundled under low pressure through a two-stage network device to obtain a stable and cohesive finished filament bundle; the micro-aperture oil nozzle with a large coverage area can ensure uniform oiling of the high-pore-count filament bundle, and the precise control of the oil content can take into account both the smoothness of the filament bundle and its adaptability to subsequent processing.

[0023] As a preferred embodiment, in step S106, the aperture of the two-stage network device is 1.0 to 1.2 mm, the air pressure of the first stage is 0.04 to 0.05 MPa, and the air pressure of the second stage is 0.06 to 0.07 MPa; the gradually increasing network air pressure can realize the gradual gathering of the filament bundle, which not only ensures the cohesion effect, but also avoids the formation of fuzz by the impact of airflow on the single filament.

[0024] As a preferred embodiment, in step S107, the winding tension is controlled to be 25-30 cN and the winding angle is 5.0°-7.0°, and constant tension winding is maintained by a tension compensation mechanism. The tension and winding angle parameters match the characteristics of low elastic fiber, which can avoid irreversible deformation of fiber, ensure stable elastic recovery rate, and at the same time make the yarn cake well formed and unwind smoothly.

[0025] On the other hand, the present invention provides a spinning device for 30D / 72F ultra-fine denier cool-feeling low-elastic polyester fiber, which is arranged in sequence along the material flow direction as a cool-feeling masterbatch pretreatment unit, a melt online mixing unit, a special spinning assembly, a graded cooling unit, an oiling and bundling unit and a constant tension winding unit.

[0026] The cooling masterbatch pretreatment unit removes dust and dries the input cooling masterbatch, and outputs low moisture content masterbatch, which is used to control the moisture content of the masterbatch from the source, remove impurities and fine powder, and protect the activity of the cooling functional components.

[0027] The online melt mixing unit performs low-temperature blending of the input cool-feeling masterbatch melt and low-elasticity polyester melt, and outputs a homogeneous blended melt to achieve uniform dispersion of a high proportion of masterbatch and matrix melt, avoiding high-temperature damage to functional components and molecular structure.

[0028] The dedicated spinning assembly filters and extrudes the input blended melt, outputting a fine melt stream to adapt to the extrusion characteristics of high-pore-count ultrafine denier melts, intercepting agglomerated impurities and extending the assembly's service life.

[0029] The graded cooling unit performs graded cooling on the input melt stream and outputs nascent filament bundles to precisely control the fiber cooling rate and molecular orientation, ensuring low elasticity and monofilament uniformity.

[0030] The oiling and bundling unit applies oil to the input nascent filament bundles and outputs cohesive filament bundles. This is used to achieve uniform oiling and low-pressure bundling of filament bundles with a high number of holes, thereby improving the cohesion and processing performance of the filament bundles.

[0031] The constant tension winding unit winds the input cohesive filament bundle with constant tension and outputs a finished filament cake to maintain stable winding tension, ensuring stable fiber elasticity and filament cake forming quality.

[0032] Compared with existing technologies, this invention effectively protects the cooling functional components from thermal deactivation and precipitation through full-process low-temperature control, including deep drying pretreatment, gradient low-temperature melting, and low-temperature dynamic blending. Combined with the homogeneous blending process of static premixing and dynamic mixing, the cooling powder is evenly dispersed in the fiber matrix without agglomeration, resulting in consistent cooling sensation throughout the finished fiber with no cooling blind spots, and minimal cooling sensation attenuation after multiple washes.

[0033] By strictly controlling the moisture content of the cooling masterbatch to within 40 PPM, the hydrolytic degradation of polyester during the high-temperature spinning process is eliminated from the source. Combined with gradient melting and low-temperature mixing processes, the melt viscosity fluctuates little, the polyester molecular chain structure is intact, and the mechanical properties of the finished fiber, such as breaking strength and elongation, are stable, thus improving the spinnability.

[0034] Employing a staged cooling method combining windless slow cooling and double-sided ring blowing, along with specialized microporous oiling and a two-stage low-pressure network bundling process, it can achieve uniform treatment of the entire area of ​​a wide bundle composed of 72 monofilaments. This effectively solves the problems of monofilament adhesion, filament drift, and unevenness, resulting in high fiber evenness, controllable low-elasticity orientation, and stable elastic recovery rate.

[0035] The three-stage gradient metal sand filter structure can intercept agglomerated powder and impurity particles of different sizes in layers. While ensuring filtration accuracy, it reduces melt flow resistance, effectively alleviates the problem of micropore blockage in the spinneret, significantly extends the service life of the spinning components, reduces fuzz and breakage, and improves production efficiency and product qualification rate.

[0036] The melt spinning process, which uses online masterbatch addition, eliminates the need for subsequent functional finishing processes, significantly reducing the discharge of chemical auxiliaries and wastewater. The equipment can be modified from a traditional melt spinning unit, resulting in low modification costs. The process parameters are adjustable over a wide range, making it suitable for customized production needs with different cooling sensation levels and elasticity indices, and suitable for large-scale mass production. Attached Figure Description

[0037] Figure 1 A flowchart illustrating the spinning process of 30D / 72F ultrafine denier cool-feeling low-elasticity polyester fiber in a specific implementation method.

[0038] Figure 2 The diagram shows the connection of each unit in the 30D / 72F ultra-fine denier cool-feel low-elastic polyester fiber spinning equipment, which is a specific implementation method. Detailed Implementation

[0039] The present invention will now be described in further detail with reference to the embodiments and accompanying drawings. However, this should not be construed as limiting the scope of the above-described subject matter of the present invention to the following embodiments; all technologies implemented based on the content of the present invention fall within the scope of the present invention.

[0040] Example 1

[0041] refer to Figure 1 This embodiment provides a spinning process for 30D / 72F ultrafine denier cool-feeling low-elasticity polyester fiber, and the specific implementation process is as follows:

[0042] Step S101: Cooling masterbatch air-powered dust removal and deep constant temperature drying

[0043] The cool-feeling masterbatch is subjected to wind-powered dust removal and deep constant-temperature drying to obtain pretreated masterbatch.

[0044] This embodiment employs a centrifugal fan combined with a cyclone separator to perform wind-powered dust removal on the cooling masterbatch at a low wind speed of 2.8 m / s. This removes fine powder, agglomerated particles, and foreign impurities adhering to the masterbatch surface, preventing impurities from entering the subsequent melt preparation stage and causing spinning defects. The dust-removed masterbatch is then fed into a large-capacity constant-temperature silo, where it is circulated with drying hot air at 142°C and continuously dried at a constant temperature of 75±5°C for 18 hours. During the drying process, the stirring mechanism within the silo operates at a low speed of 4–7 rpm to prevent the masterbatch from clumping due to heat and to ensure uniform heating of the entire masterbatch. Testing showed that the moisture content of the dried masterbatch was ≤40 PPM, meeting the low moisture content requirements for subsequent spinning.

[0045] Step S102: Pre-treated masterbatch gradient low-temperature melting

[0046] The pretreated masterbatch was melted at a gradient low temperature to obtain a cool-feeling masterbatch melt.

[0047] The dried pretreated masterbatch is fed into a four-zone gradient temperature-controlled screw extruder. The four-zone temperature control structure, which gradually increases the temperature along the material flow direction, achieves gradient low-temperature melting, avoiding the deactivation of the cooling functional components caused by sudden high temperatures. During the production process, the extrusion pressure of the screw extruder is controlled at 42-52 bar and the screw speed is controlled at 22-32 rpm to ensure that the masterbatch is fully plasticized while maintaining stable melt viscosity. Finally, a uniformly plasticized cooling masterbatch melt is obtained and transported to the subsequent mixing process through a constant temperature pipeline.

[0048] Step S103: Static premixing and low-temperature dynamic mixing of melt

[0049] A quantity of cooling masterbatch melt is injected into low-elasticity polyester melt, and a homogeneous blend melt is obtained through static premixing and low-temperature dynamic mixing.

[0050] At a mass ratio of 3.8% to 5.0%, the cooling masterbatch melt is quantitatively injected into the low-elasticity polyester melt. Simultaneously, a polyester compatibilizer at a mass ratio of 0.08% to 0.11% is added to the matrix melt to improve the interfacial compatibility of the two-phase melts. The two-phase melts first enter a static mixer for preliminary premixing to achieve initial dispersion of components. Then, they enter a low-temperature dynamic mixing device, where dynamic mixing is carried out at a temperature control of 268±3℃ and a stirring speed of 28 to 33 rpm. Through gentle shearing action, the cooling functional powder is uniformly dispersed in the low-elasticity polyester matrix, ultimately obtaining a homogeneous blend melt without agglomeration and with uniform components.

[0051] Step S104: Three-stage gradient filtration and spinneret extrusion of blended melt

[0052] The blended melt was subjected to three-stage gradient filtration and quantitatively extruded through a 72-hole spinneret to obtain a fine melt stream.

[0053] The blended melt is quantitatively delivered to a dedicated spinning assembly by a metering pump. It first flows through a three-stage gradient metal sand filter layer of 70-90-110 mesh, with the filtration precision increasing step by step along the melt flow direction. This layered interception of agglomerated particles and impurities in the melt prevents clogging of the spinneret micropores. The initial pressure of the spinning assembly is controlled at 14.0-15.0 MPa. The filtered melt is then quantitatively extruded through a 72-hole spinneret with a length-to-diameter ratio of 7:1, forming a uniformly shaped fine stream of melt.

[0054] Step S105: Melt stream staged cooling and solidification

[0055] The molten stream is first slowly cooled in a windless cooling zone, and then solidified by double-sided ring blowing to obtain nascent filament bundles.

[0056] The molten stream extruded from the spinneret first enters a windless slow cooling zone at a height of 55–65 mm. Under windless conditions, it cools naturally and slowly, slowing the cooling rate and eliminating the melt extrusion swelling effect. This allows the polyester macromolecular chains to slowly and regularly align, stabilizing the fiber's orientation structure. The slowly cooled filament then enters a double-sided annular cooling zone, where cooling air at a pressure of 20–26 Pa, a temperature of 20–23 °C, and a relative humidity of 60%–66% is simultaneously and uniformly blown from both sides of the filament, causing the 72 monofilaments to solidify and form a uniformly even nascent filament bundle.

[0057] Step S106: Oiling the nascent filament bundle and bundling with a two-stage low-pressure network

[0058] The nascent filament bundles are uniformly oiled and then bundled through a two-stage low-pressure network to obtain a stable and cohesive finished filament bundle.

[0059] The nascent fiber bundle moves downwards to a micro-aperture oil nozzle for uniform oiling. The nozzle features a large coverage area design to accommodate the oiling needs of high-pore-count fiber bundles, controlling the oil content of the finished fiber to a set value ±0.03%, reducing the coefficient of friction between monofilaments, and improving the smoothness of subsequent processing. The oiled fiber bundle then passes through a two-stage network device for low-pressure bundling. The aperture of the two network devices is 1.0–1.2 mm, with the first-stage network pressure controlled at 0.04–0.05 MPa and the second-stage network pressure controlled at 0.06–0.07 MPa. The progressively increasing low-pressure airflow gradually gathers the dispersed monofilaments, improving the overall cohesion of the fiber bundle and preventing problems such as monofilament drift and spiderweb-like strands, ultimately resulting in a stable and cohesive finished fiber bundle.

[0060] Step S107: Finished filament bundle is wound under constant tension to form a shape.

[0061] The finished filament bundles are wound under constant tension to obtain 30D / 72F ultrafine denier cool-feeling low-elasticity polyester fibers.

[0062] After being bundled, the finished filament bundles are guided by a yarn guiding mechanism and then fed into a winding device. During production, the winding tension is controlled at 25–30 cN and the winding angle at 5.0°–7.0°. Tension fluctuations are corrected in real time by a tension compensation mechanism to maintain constant tension throughout the winding process, preventing irreversible fiber deformation caused by tension fluctuations and ensuring the stability of the fiber's low elasticity properties. After winding, a well-formed 30D / 72F ultra-fine denier cool-feeling low-elasticity polyester fiber finished filament cake is obtained.

[0063] Example 2

[0064] refer to Figure 1 In this embodiment, within the process framework of Embodiment 1, a set of specific preferred parameters are selected for mass production verification. The specific parameters are as follows:

[0065] Masterbatch pretreatment: dust removal wind speed 2.8m / s, drying hot air temperature 142℃, silo constant temperature 75℃, drying time 18h, stirring speed 5rpm, final masterbatch moisture content 36PPM.

[0066] Gradient melting: The screw extrusion pressure is 48 bar, the screw speed is 28 rpm, and low-temperature melting is achieved by using four-zone gradient temperature control;

[0067] Melt mixing: Cooling masterbatch added at a mass ratio of 4.0%, polyester compatibilizer added at a mass ratio of 0.09%, dynamic mixing temperature at 268℃, stirring speed at 30 rpm;

[0068] Filtration and extrusion: 70-90-110 mesh three-stage gradient metal sand filtration is adopted, the initial pressure of the spinning assembly is 14.5MPa, the spinneret has 72 holes and the length-to-diameter ratio is 7:1;

[0069] Staged cooling: No-wind slow cooling zone height 60mm, annular air pressure 23Pa, air temperature 21℃, relative humidity 63%;

[0070] Oiling and bundling: The fiber oil content is controlled at ±0.03% of the set value, the mesh device aperture is 1.1mm, the pre-stage mesh air pressure is 0.045MPa, and the post-stage mesh air pressure is 0.065MPa;

[0071] Winding and forming: winding tension 28cN, winding angle 6.0°, constant tension winding is maintained by tension compensation mechanism.

[0072] Through continuous production testing, the finished fiber prepared in this embodiment has stable performance indicators. Core indicators such as breaking strength, breaking elongation, contact cold sensitivity coefficient, evenness, and elastic recovery rate all meet the product quality requirements. The spinning process runs smoothly, the component has a long service life, and the incidence of fuzz and breakage is low. Continuous and stable production can be achieved, verifying the reliability and practicality of the process parameter range.

[0073] Example 3

[0074] refer to Figure 2 The 30D / 72F ultrafine denier cool-feeling low-elasticity polyester fiber spinning equipment, in this embodiment, is a dedicated spinning equipment for realizing the above-mentioned spinning process. Along the material flow direction, it is sequentially arranged with a cool-feeling masterbatch pretreatment unit 10, an online melt mixing unit 20, a dedicated spinning assembly 30, a constant tension winding unit 40, an oiling and bundling unit 50, and a constant tension winding unit 60. The specific structure and function of each unit are as follows:

[0075] Cooling Masterbatch Pretreatment Unit 10: The cooling masterbatch pretreatment unit 10 performs dust removal and drying on the input cooling masterbatch, outputting masterbatch with low moisture content. This unit mainly consists of a centrifugal fan, a cyclone separator, a dehumidification and drying component, a constant temperature silo, and a low-speed stirring mechanism. It can complete the wind-driven dust removal, deep dehumidification and drying, and constant temperature storage of the cooling masterbatch, controlling the moisture content of the masterbatch at an extremely low level, while avoiding premature deactivation of the cooling functional components.

[0076] Online melt mixing unit 20: The online melt mixing unit 20 performs low-temperature blending of the input cooling masterbatch melt and low-elasticity polyester melt, outputting a homogeneous blended melt. This unit adopts a combination of a masterbatch quantitative injection structure, a static mixer, and a low-temperature dynamic mixer, which can achieve homogeneous dispersion of a high proportion of cooling masterbatch and low-elasticity polyester melt, while completing the mixing under low-temperature conditions, protecting the functional components and polyester molecular structure from damage.

[0077] Dedicated spinning assembly 30: The dedicated spinning assembly 30 filters and extrudes the input blended melt, outputting a fine melt stream. The assembly is internally equipped with a three-stage gradient metal sand filter layer and a 72-hole spinneret, which can filter impurities while adapting to the extrusion requirements of high-pore-count, ultra-fine denier melts, ensuring uniform monofilament extrusion and extending the assembly's service life.

[0078] Constant tension winding unit 40: The constant tension winding unit 40 performs staged cooling of the input melt stream and outputs nascent filament bundles. This unit consists of a windless slow cooling zone and a double-sided ring blowing device. It can precisely control the fiber cooling rate and molecular orientation by first slow cooling and then uniform ring blowing, ensuring the uniformity of monofilaments and the stability of low elasticity properties.

[0079] Oiling and bundling unit 50: The oiling and bundling unit 50 applies oil to the input nascent filament bundle and outputs a cohesive filament bundle. This unit includes a micro-aperture oil nozzle and a two-stage low-pressure network device, which can achieve uniform oiling and gradual bundling of high-pore-count filament bundles, improve filament cohesion, and avoid damage to the surface of individual filaments.

[0080] Constant tension winding unit 60: The constant tension winding unit 60 winds the input cohesive filament bundle under constant tension, outputting a finished filament cake. This unit is equipped with a winding head and a tension compensation mechanism, which can maintain a stable winding tension throughout the process, avoid irreversible deformation of the fibers, and ensure the stability of the low elasticity index and the quality of the filament cake formation.

[0081] The above are merely preferred embodiments of the present invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A spinning process for 30D / 72F ultrafine denier cool-feeling low-elasticity polyester fiber, characterized in that, include: S101: The cool-feeling masterbatch is subjected to wind-powered dust removal and deep constant-temperature drying to obtain pretreated masterbatch; S102: The pretreated masterbatch is melted at a gradient low temperature to obtain a cool-feeling masterbatch melt; S103: The cool-feeling masterbatch melt is quantitatively injected into the low-elasticity polyester melt, and a homogeneous blend melt is obtained through static premixing and low-temperature dynamic mixing; S104: The blended melt is subjected to three-stage gradient filtration and quantitatively extruded through a 72-hole spinneret to obtain a fine melt stream; S105: The melt stream is first slowly cooled in a windless cooling zone, and then solidified by double-sided ring blowing to obtain the nascent filament bundle; S106: The nascent filament bundle is uniformly oiled and then bundled through a two-stage low-pressure network to obtain a stable and cohesive finished filament bundle. S107: The finished filament bundle is wound under constant tension to obtain 30D / 72F ultra-fine denier cool-feeling low-elastic polyester fiber.

2. The spinning process for 30D / 72F ultrafine denier cool-feeling low-elastic polyester fiber according to claim 1, characterized in that, In step S101, the cool-feeling masterbatch is dusted by a low wind speed of 2.8 m / s; it is then dried for 18 hours in a constant temperature environment of 75±5℃ by hot air at 142℃, with low-speed stirring at 4~7 rpm, to obtain a pretreated masterbatch with a moisture content ≤40PPM.

3. The spinning process for 30D / 72F ultrafine denier cool-feeling low-elastic polyester fiber according to claim 1, characterized in that, In step S102, the pretreated masterbatch is melted using a four-zone gradient temperature-controlled screw extruder, with the extrusion pressure controlled at 42–52 bar and the screw speed at 22–32 rpm, to obtain a cool-feeling masterbatch melt.

4. The spinning process for 30D / 72F ultrafine denier cool-feeling low-elastic polyester fiber according to claim 1, characterized in that, In step S103, the cool-feeling masterbatch melt is injected into the low-elasticity polyester melt at a mass ratio of 3.8% to 5.0%, and a polyester compatibilizer at a mass ratio of 0.08% to 0.11% is added simultaneously; a homogeneous blend melt is obtained by low-temperature dynamic mixing at 268±3℃ and a rotation speed of 28 to 33 rpm.

5. The spinning process for 30D / 72F ultrafine denier cool-feeling low-elastic polyester fiber according to claim 1, characterized in that, In step 104, the blended melt is filtered through a three-stage gradient of 70-90-110 mesh metal sand; the initial pressure of the spinning assembly is controlled at 14.0-15.0 MPa, and the melt is extruded through a 72-hole spinneret with an aspect ratio of 7:1 to obtain a fine melt stream.

6. The spinning process for 30D / 72F ultrafine denier cool-feeling low-elastic polyester fiber according to claim 1, characterized in that, In step S105, the melt stream is first slowly cooled through a 55-65mm windless slow cooling zone; then it is cooled by double-sided ring blowing with a wind pressure of 20-26Pa, a wind temperature of 20-23℃, and a relative humidity of 60%-66% to obtain the nascent filament bundle.

7. The spinning process for 30D / 72F ultrafine denier cool-feeling low-elastic polyester fiber according to claim 1, characterized in that, In step S106, the nascent filament bundle is oiled through a micro-aperture oil nozzle, and the oil content is controlled to a set value of ±0.03%; the bundle is then bundled under low pressure through a two-stage network device to obtain a stable and cohesive finished filament bundle.

8. The spinning process for 30D / 72F ultrafine denier cool-feeling low-elastic polyester fiber according to claim 1, characterized in that, In step S106, the aperture of the two-stage network device is 1.0 to 1.2 mm, the air pressure of the front stage is 0.04 to 0.05 MPa, and the air pressure of the rear stage is 0.06 to 0.07 MPa.

9. The spinning process for 30D / 72F ultrafine denier cool-feeling low-elastic polyester fiber according to claim 1, characterized in that, In step S107, the winding tension is controlled to be 25-30 cN and the winding angle is 5.0°-7.0°, and constant tension winding is maintained by the tension compensation mechanism.

10. A spinning device for 30D / 72F ultrafine denier cool-feeling low-elasticity polyester fibers, characterized in that, Along the material flow direction, a cooling masterbatch pretreatment unit, an online melt mixing unit, a dedicated spinning assembly, a graded cooling unit, an oiling and bundling unit, and a constant tension winding unit are set in sequence. Cooling masterbatch pretreatment unit, which removes dust and dries the input cooling masterbatch and outputs masterbatch with low moisture content; An online melt mixing unit performs low-temperature blending of two input melts and outputs a homogeneous blended melt. A dedicated spinning assembly filters and extrudes the input blended melt, outputting a fine stream of melt. A staged cooling unit cools the input melt stream in stages and outputs nascent filament bundles. The oiling and bundling unit applies oil to the input nascent filament bundles and bundles them together, outputting cohesive filament bundles. A constant tension winding unit winds the input cohesive filament bundle at a constant tension and outputs a finished filament cake.