A process for processing soybean protein isolate into protein velvet for spinning
By preparing hydroxylated porous graphene and enzymatically modified soy protein isolate, the problem of insufficient performance of soy protein fiber under high humidity and heat conditions was solved, the mechanical and antibacterial properties of protein fluff for spinning were improved, and an environmentally friendly spinning process was realized.
Patent Information
- Application Number
- CN202611254171.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-18
- Publication Date
- 2026-11-17
AI Technical Summary
Soy protein fiber has poor breaking strength and moisture absorption under high humidity and heat conditions, and its friction is low when blended with other fibers, which affects the durability and mechanical properties of the fabric. In addition, the effect of existing antibacterial treatment is not durable.
Hydroxylated porous graphene was prepared using graphite. Soy protein isolate was enzymatically hydrolyzed and modified, and sodium tripolyphosphate and chitosan were added. The mixture was then wet-spun to prepare a spinning solution.
It improves the stability and antibacterial properties of soy protein isolate, enhances the mechanical properties and antibacterial durability of protein wool for spinning, reduces the use of chemical reagents, and avoids formaldehyde residue.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to a process for processing soybean protein isolate into protein fluff for spinning. It belongs to the field of soybean processing technology. Background Technology
[0002] Protein fleece fabric is made from protein fibers, or a combination of protein and chemical fibers, woven using a special process. It is characterized by its comfort, skin-friendliness, high luster, durability, wrinkle resistance, and washability. Protein fleece fabric is widely applicable and can be used to make coats, jackets, skirts, trousers, bedding, sofa covers, etc., offering a high-end feel and being environmentally friendly and healthy.
[0003] The spinning raw material for protein fleece fabric is protein fiber, which can be obtained from soybeans, animal cheese, silkworm pupae, animal connective tissue, etc., specifically including soybean protein fiber and milk protein fiber. Soybean protein fiber has abundant raw material sources and low cost, especially soybean meal, the residue left after soybean oil extraction, which contains rich soy protein isolate, making it more valuable for promotion and application in the production of protein fleece fabric.
[0004] However, soybean protein fiber also has many drawbacks, such as: generally low tensile strength and poor high-temperature resistance, especially under high temperature and humidity conditions, resulting in poor tensile strength and moisture absorption. Furthermore, the low friction between soybean protein fiber and other fibers affects the fabric's durability and mechanical properties. Additionally, soybean protein fiber itself has virtually no antibacterial properties. To impart antibacterial properties to protein fleece fabrics, finishing agents containing antibacterial agents are usually required, but the durability of the antibacterial effect cannot be guaranteed; the antibacterial effect gradually weakens and eventually disappears after repeated washing.
[0005] Patent CN103388195B discloses a method for producing antibacterial soybean protein fiber and its product. The method involves dissolving soybean protein powder in water, adding sodium phosphate, sodium hydroxide, and acetamide, and heating and stirring to prepare a soybean protein solution. The soybean protein solution is then mixed with soaked polyvinyl alcohol, and formaldehyde, glutaraldehyde, benzoyl peroxide, silver nanoparticles (no larger than 100 nm), reactive dyes, boric acid, and sodium tetraborate are added at different temperatures, followed by stirring to obtain a spinnable solution. The spinnable solution is then filtered and degassed under vacuum. Spinning is performed using a conventional wet spinning process. This patented technology uses a large number of chemical reagents, resulting in soybean protein fibers containing excessive amounts of free formaldehyde and other harmful substances, which seriously affect human health. Summary of the Invention
[0006] The purpose of this invention is to overcome the shortcomings of the prior art and provide a process for processing soybean protein isolate into protein fluff for spinning.
[0007] To achieve the above objectives, the present invention adopts the following technical solution: A process for processing soy protein isolate into protein fluff for spinning, the specific steps of which are as follows: (1) First, hydroxylated porous graphene is prepared using graphite as raw material; (2) Then the soy protein isolate is enzymatically hydrolyzed to obtain enzymatically hydrolyzed protein, and then the enzymatically hydrolyzed protein is modified by transglutaminase and chitosan to obtain modified protein. (3) Then, the hydroxylated porous graphene and modified protein are ultrasonically dispersed in water, and sodium tripolyphosphate is added and mixed evenly to obtain a spinning solution. The solution is pre-crosslinked and wet-spun to obtain the final product.
[0008] Preferably, in step (1), the preparation method of hydroxylated porous graphene is as follows: first, graphite is ultrasonically dispersed in an ethanol aqueous solution, transferred to a reaction vessel, and subjected to a solvothermal reaction to obtain porous graphene; then, under stirring conditions, porous graphene is added to a mixed acid solution, potassium permanganate is added slowly, and the reaction is heated to obtain a suspension; finally, the suspension is poured into cold water, hydrogen peroxide solution is added, and after the reaction stops, it is washed and dried to obtain the hydroxylated porous graphene.
[0009] More preferably, the mass ratio of graphite, aqueous ethanol solution, mixed acid solution, and potassium permanganate is 1:12-15:7-9:0.0003-0.0005, wherein the volume concentration of the aqueous ethanol solution is 50-60%, and the mixed acid solution is obtained by mixing 98% concentrated sulfuric acid and 85% concentrated phosphoric acid at a volume ratio of 9:1.
[0010] Further preferred, the solvothermal reaction conditions are: 140-160℃ for 15-17 hours; the heating reaction conditions are: 45-50℃ for 12-15 hours.
[0011] More preferably, the volume ratio of the suspension, cold water, and hydrogen peroxide solution is 1:1:0.3, the temperature of the cold water is 4°C, and the mass concentration of the hydrogen peroxide solution is 30%.
[0012] More preferably, the washing process includes: sequentially washing with distilled water, 30% hydrochloric acid solution, and anhydrous ethanol; the drying conditions are: drying at 80°C for 12 hours.
[0013] Preferably, in step (2), the enzymatic hydrolysis method is as follows: the soy protein isolate is ultrasonically dispersed in water, the pH is adjusted to 8 using 0.1 mol / L sodium hydroxide solution, alkaline protease is added, and the enzyme is hydrolyzed at 50-60°C for 3-4 hours. The enzyme is then inactivated, filtered, concentrated, and dried to obtain the hydrolyzed protein.
[0014] A further preferred embodiment has a mass ratio of soy protein isolate, water, and alkaline protease of 10:80-100:0.1-0.2.
[0015] Preferably, in step (2), the modification treatment method is as follows: the enzymatically hydrolyzed protein is stirred and dispersed in water, transglutaminase and chitosan are added, the reaction is carried out at 40-45°C for 1-2 hours, the enzyme is inactivated, and then the modified protein is obtained.
[0016] Further preferably, the mass ratio of enzymatically hydrolyzed protein, water, transglutaminase, and chitosan is 1:8-10:0.01-0.02:0.06-0.08.
[0017] Further preferred post-processing includes: dialysis using a dialysis bag with a molecular weight cutoff of 100–200 kDa, filtration through a 0.45 μm filter membrane, concentration, and drying.
[0018] Preferably, in step (3), the mass ratio of hydroxylated porous graphene, modified protein, water, and sodium tripolyphosphate is 0.03-0.05:1:15-20:0.02-0.03.
[0019] Preferably, in step (3), the pre-crosslinking process conditions are as follows: first, adjust the pH to 6.5 using 0.1 mol / L acetic acid solution, stir at room temperature for 25 to 35 minutes, and then adjust the pH to 9 using 0.1 mol sodium hydroxide solution.
[0020] Preferably, in step (3), the wet spinning conditions are as follows: the spinning plate has 6 holes with a hole diameter of 150 μm, the spinning speed is 20 m / min, and the spinning temperature is 80 °C; the coagulation bath temperature is 45 °C, and the coagulation bath is a mixed aqueous solution including: 300 g / L sodium sulfate, 70 g / L sulfuric acid, and 15 g / L zinc sulfate.
[0021] Preferably, in step (3), after wet spinning, the yarn is washed with water until neutral and then subjected to secondary hot stretching. The specific conditions are: 150℃, stretching ratio 1.5 times; 200℃, stretching ratio 3 times.
[0022] A method for processing soy protein isolate into a protein wool for spinning is obtained through the aforementioned process.
[0023] The beneficial effects of this invention are: This invention provides a process for processing soybean protein isolate into protein fleece for spinning. First, hydroxylated porous graphene is prepared using graphite as a raw material. Then, the soybean protein isolate is enzymatically hydrolyzed to obtain hydrolyzed protein. Next, the hydrolyzed protein is modified using transglutaminase and chitosan to obtain modified protein. The hydroxylated porous graphene and modified protein are then ultrasonically dispersed in water, and sodium tripolyphosphate is added and mixed thoroughly to obtain a spinning solution. This solution is pre-crosslinked and then wet-spun to obtain the final product. This invention processes soybean protein isolate into protein fleece for spinning, resulting in high-performance fabrics with broad application prospects.
[0024] This invention involves enzymatically hydrolyzing soybean protein isolate, followed by modification with transglutaminase and chitosan to improve the stability and antibacterial properties of the modified protein. Furthermore, this invention introduces hydroxylated porous graphene, which, under the action of sodium tripolyphosphate, is compounded with the modified protein to further improve antibacterial properties and mechanical properties.
[0025] This invention reduces the use of chemical reagents and eliminates problems such as formaldehyde residue. Detailed Implementation
[0026] The present invention will be further described below with reference to embodiments. It should be noted that the following description is only for explaining the present invention and does not limit its content.
[0027] The soy protein isolate of this invention was purchased from Hefei Nuoerda Biotechnology Co., Ltd., under the brand name Shansong. Example
[0028] A process for processing soy protein isolate into protein fluff for spinning, the specific steps of which are as follows: (1) First, hydroxylated porous graphene is prepared using graphite as raw material; (2) Then the soy protein isolate is enzymatically hydrolyzed to obtain enzymatically hydrolyzed protein, and then the enzymatically hydrolyzed protein is modified by transglutaminase and chitosan to obtain modified protein. (3) Then, the hydroxylated porous graphene and modified protein are ultrasonically dispersed in water, and sodium tripolyphosphate is added and mixed evenly to obtain a spinning solution. The solution is pre-crosslinked and wet-spun to obtain the final product.
[0029] In step (1), the preparation method of hydroxylated porous graphene is as follows: first, graphite is ultrasonically dispersed in an ethanol aqueous solution, transferred to a reaction vessel, and subjected to a solvothermal reaction to obtain porous graphene; then, the porous graphene is added to a mixed acid solution under stirring conditions, potassium permanganate is added slowly, and the reaction is heated to obtain a suspension; finally, the suspension is poured into cold water, hydrogen peroxide solution is added, and after the reaction stops, it is washed and dried to obtain the hydroxylated porous graphene.
[0030] The mass ratio of graphite, aqueous ethanol solution, mixed acid solution, and potassium permanganate is 1:12:7:0.0003. The volume concentration of the aqueous ethanol solution is 50%, and the mixed acid solution is obtained by mixing 98% concentrated sulfuric acid and 85% concentrated phosphoric acid in a volume ratio of 9:1.
[0031] The solvothermal reaction conditions were: 140℃ for 15 hours; the heating reaction conditions were: 45℃ for 12 hours.
[0032] The volume ratio of the suspension, cold water, and hydrogen peroxide solution is 1:1:0.3, the temperature of the cold water is 4℃, and the mass concentration of the hydrogen peroxide solution is 30%.
[0033] The washing process includes sequentially washing with distilled water, 30% hydrochloric acid solution, and anhydrous ethanol; the drying conditions are: drying at 80℃ for 12 hours.
[0034] In step (2), the enzymatic hydrolysis method is as follows: the soy protein isolate is ultrasonically dispersed in water, the pH is adjusted to 8 using 0.1 mol / L sodium hydroxide solution, alkaline protease is added, and the enzyme is hydrolyzed at 50°C for 3 hours. The enzyme is then inactivated, filtered, concentrated, and dried to obtain the hydrolyzed protein.
[0035] The mass ratio of soy protein isolate, water, and alkaline protease was 10:80:0.1.
[0036] In step (2), the modification treatment method is as follows: the enzymatically hydrolyzed protein is stirred and dispersed in water, transglutaminase and chitosan are added, the reaction is carried out at 40°C for 1 hour, the enzyme is inactivated, and then the modified protein is obtained.
[0037] The mass ratio of enzymatically hydrolyzed protein, water, transglutaminase, and chitosan was 1:8:0.01:0.06.
[0038] Post-processing included: dialysis using a dialysis bag with a molecular weight cutoff of 100 kDa, filtration through a 0.45 μm filter membrane, concentration, and drying.
[0039] In step (3), the mass ratio of hydroxylated porous graphene, modified protein, water, and sodium tripolyphosphate is 0.03:1:15:0.02.
[0040] In step (3), the pre-crosslinking process conditions are as follows: first, adjust the pH to 6.5 using 0.1 mol / L acetic acid solution, stir at room temperature for 25 minutes, and then adjust the pH to 9 using 0.1 mol sodium hydroxide solution.
[0041] In step (3), the wet spinning conditions are as follows: the spinning plate has 6 holes with a hole diameter of 150 μm, the spinning speed is 20 m / min, and the spinning temperature is 80℃; the coagulation bath temperature is 45℃, and the coagulation bath is a mixed aqueous solution including: 300 g / L sodium sulfate, 70 g / L sulfuric acid, and 15 g / L zinc sulfate.
[0042] In step (3), after wet spinning, the yarn is washed with water until neutral and then subjected to secondary hot stretching. The specific conditions are: 150℃, stretching ratio 1.5 times; 200℃, stretching ratio 3 times. Example
[0043] A process for processing soy protein isolate into protein fluff for spinning, the specific steps of which are as follows: (1) First, hydroxylated porous graphene is prepared using graphite as raw material; (2) Then the soy protein isolate is enzymatically hydrolyzed to obtain enzymatically hydrolyzed protein, and then the enzymatically hydrolyzed protein is modified by transglutaminase and chitosan to obtain modified protein. (3) Then, the hydroxylated porous graphene and modified protein are ultrasonically dispersed in water, and sodium tripolyphosphate is added and mixed evenly to obtain a spinning solution. The solution is pre-crosslinked and wet-spun to obtain the final product.
[0044] In step (1), the preparation method of hydroxylated porous graphene is as follows: first, graphite is ultrasonically dispersed in an ethanol aqueous solution, transferred to a reaction vessel, and subjected to a solvothermal reaction to obtain porous graphene; then, the porous graphene is added to a mixed acid solution under stirring conditions, potassium permanganate is added slowly, and the reaction is heated to obtain a suspension; finally, the suspension is poured into cold water, hydrogen peroxide solution is added, and after the reaction stops, it is washed and dried to obtain the hydroxylated porous graphene.
[0045] The mass ratio of graphite, aqueous ethanol solution, mixed acid solution, and potassium permanganate is 1:15:9:0.0005. The volume concentration of the aqueous ethanol solution is 60%, and the mixed acid solution is obtained by mixing 98% concentrated sulfuric acid and 85% concentrated phosphoric acid in a volume ratio of 9:1.
[0046] The solvothermal reaction conditions were: 160℃ for 17 hours; the heating reaction conditions were: 50℃ for 15 hours.
[0047] The volume ratio of the suspension, cold water, and hydrogen peroxide solution is 1:1:0.3, the temperature of the cold water is 4℃, and the mass concentration of the hydrogen peroxide solution is 30%.
[0048] The washing process includes sequentially washing with distilled water, 30% hydrochloric acid solution, and anhydrous ethanol; the drying conditions are: drying at 80℃ for 12 hours.
[0049] In step (2), the enzymatic hydrolysis method is as follows: the soy protein isolate is ultrasonically dispersed in water, the pH is adjusted to 8 using 0.1 mol / L sodium hydroxide solution, alkaline protease is added, and the enzyme is hydrolyzed at 60°C for 4 hours. The enzyme is then inactivated, filtered, concentrated, and dried to obtain the hydrolyzed protein.
[0050] The mass ratio of soy protein isolate, water, and alkaline protease was 10:100:0.2.
[0051] In step (2), the modification treatment method is as follows: the enzymatically hydrolyzed protein is stirred and dispersed in water, transglutaminase and chitosan are added, the reaction is carried out at 45°C for 2 hours, the enzyme is inactivated, and then the modified protein is obtained.
[0052] The mass ratio of enzymatically hydrolyzed protein, water, transglutaminase, and chitosan was 1:10:0.02:0.08.
[0053] Post-processing included: dialysis using a dialysis bag with a molecular weight cutoff of 200 kDa, filtration through a 0.45 μm filter membrane, concentration, and drying.
[0054] In step (3), the mass ratio of hydroxylated porous graphene, modified protein, water, and sodium tripolyphosphate is 0.05:1:20:0.03.
[0055] In step (3), the pre-crosslinking process conditions are as follows: first, adjust the pH to 6.5 using 0.1 mol / L acetic acid solution, stir at room temperature for 35 minutes, and then adjust the pH to 9 using 0.1 mol sodium hydroxide solution.
[0056] In step (3), the wet spinning conditions are as follows: the spinning plate has 6 holes with a hole diameter of 150 μm, the spinning speed is 20 m / min, and the spinning temperature is 80℃; the coagulation bath temperature is 45℃, and the coagulation bath is a mixed aqueous solution including: 300 g / L sodium sulfate, 70 g / L sulfuric acid, and 15 g / L zinc sulfate.
[0057] In step (3), after wet spinning, the yarn is washed with water until neutral and then subjected to secondary hot stretching. The specific conditions are: 150℃, stretching ratio 1.5 times; 200℃, stretching ratio 3 times. Example
[0058] A process for processing soy protein isolate into protein fluff for spinning, the specific steps of which are as follows: (1) First, hydroxylated porous graphene is prepared using graphite as raw material; (2) Then the soy protein isolate is enzymatically hydrolyzed to obtain enzymatically hydrolyzed protein, and then the enzymatically hydrolyzed protein is modified by transglutaminase and chitosan to obtain modified protein. (3) Then, the hydroxylated porous graphene and modified protein are ultrasonically dispersed in water, and sodium tripolyphosphate is added and mixed evenly to obtain a spinning solution. The solution is pre-crosslinked and wet-spun to obtain the final product.
[0059] In step (1), the preparation method of hydroxylated porous graphene is as follows: first, graphite is ultrasonically dispersed in an ethanol aqueous solution, transferred to a reaction vessel, and subjected to a solvothermal reaction to obtain porous graphene; then, the porous graphene is added to a mixed acid solution under stirring conditions, potassium permanganate is added slowly, and the reaction is heated to obtain a suspension; finally, the suspension is poured into cold water, hydrogen peroxide solution is added, and after the reaction stops, it is washed and dried to obtain the hydroxylated porous graphene.
[0060] The mass ratio of graphite, aqueous ethanol solution, mixed acid solution, and potassium permanganate is 1:13:8:0.0004. The volume concentration of the aqueous ethanol solution is 55%, and the mixed acid solution is obtained by mixing 98% concentrated sulfuric acid and 85% concentrated phosphoric acid in a volume ratio of 9:1.
[0061] The solvothermal reaction conditions were: 150℃ for 16 hours; the heating reaction conditions were: 48℃ for 13 hours.
[0062] The volume ratio of the suspension, cold water, and hydrogen peroxide solution is 1:1:0.3, the temperature of the cold water is 4℃, and the mass concentration of the hydrogen peroxide solution is 30%.
[0063] The washing process includes sequentially washing with distilled water, 30% hydrochloric acid solution, and anhydrous ethanol; the drying conditions are: drying at 80℃ for 12 hours.
[0064] In step (2), the enzymatic hydrolysis method is as follows: the soy protein isolate is ultrasonically dispersed in water, the pH is adjusted to 8 using 0.1 mol / L sodium hydroxide solution, alkaline protease is added, and the enzyme is hydrolyzed at 55°C for 3 hours. The enzyme is then inactivated, filtered, concentrated, and dried to obtain the hydrolyzed protein.
[0065] The mass ratio of soy protein isolate, water, and alkaline protease was 10:90:0.15.
[0066] In step (2), the modification treatment method is as follows: the enzymatically hydrolyzed protein is stirred and dispersed in water, transglutaminase and chitosan are added, the reaction is carried out at 42°C for 2 hours, the enzyme is inactivated, and then the modified protein is obtained.
[0067] The mass ratio of enzymatically hydrolyzed protein, water, transglutaminase, and chitosan was 1:9:0.01:0.07.
[0068] Post-processing included: dialysis using a dialysis bag with a molecular weight cutoff of 200 kDa, filtration through a 0.45 μm filter membrane, concentration, and drying.
[0069] In step (3), the mass ratio of hydroxylated porous graphene, modified protein, water, and sodium tripolyphosphate is 0.04:1:18:0.02.
[0070] In step (3), the pre-crosslinking process conditions are as follows: first, adjust the pH to 6.5 using 0.1 mol / L acetic acid solution, stir at room temperature for 30 minutes, and then adjust the pH to 9 using 0.1 mol sodium hydroxide solution.
[0071] In step (3), the wet spinning conditions are as follows: the spinning plate has 6 holes with a hole diameter of 150 μm, the spinning speed is 20 m / min, and the spinning temperature is 80℃; the coagulation bath temperature is 45℃, and the coagulation bath is a mixed aqueous solution including: 300 g / L sodium sulfate, 70 g / L sulfuric acid, and 15 g / L zinc sulfate.
[0072] In step (3), after wet spinning, the yarn is washed with water until neutral and then subjected to secondary hot stretching. The specific conditions are: 150℃, stretching ratio 1.5 times; 200℃, stretching ratio 3 times.
[0073] A process for processing soy protein isolate into protein fluff for spinning, the specific steps of which are as follows: (1) Soy protein isolate is enzymatically hydrolyzed to obtain enzymatically hydrolyzed protein, and then the enzymatically hydrolyzed protein is modified by transglutaminase and chitosan to obtain modified protein; (2) Disperse the modified protein in water by ultrasonication, add sodium tripolyphosphate, mix evenly to obtain a spinning solution, and then perform wet spinning to obtain the product.
[0074] In step (1), the enzymatic hydrolysis method is as follows: the soy protein isolate is ultrasonically dispersed in water, the pH is adjusted to 8 using 0.1 mol / L sodium hydroxide solution, alkaline protease is added, and the enzyme is hydrolyzed at 50°C for 3 hours. The enzyme is then inactivated, filtered, concentrated, and dried to obtain the hydrolyzed protein.
[0075] The mass ratio of soy protein isolate, water, and alkaline protease was 10:80:0.1.
[0076] In step (1), the modification treatment method is as follows: the enzymatically hydrolyzed protein is stirred and dispersed in water, transglutaminase and chitosan are added, the reaction is carried out at 40°C for 1 hour, the enzyme is inactivated, and then the modified protein is obtained.
[0077] The mass ratio of enzymatically hydrolyzed protein, water, transglutaminase, and chitosan was 1:8:0.01:0.06.
[0078] Post-processing included: dialysis using a dialysis bag with a molecular weight cutoff of 100 kDa, filtration through a 0.45 μm filter membrane, concentration, and drying.
[0079] In step (2), the mass ratio of modified protein to water is 1:15.
[0080] In step (2), the wet spinning conditions are as follows: the spinning plate has 6 holes with a hole diameter of 150 μm, the spinning speed is 20 m / min, and the spinning temperature is 80℃; the coagulation bath temperature is 45℃, and the coagulation bath is a mixed aqueous solution including: 300 g / L sodium sulfate, 70 g / L sulfuric acid, and 15 g / L zinc sulfate.
[0081] In step (2), after wet spinning, the yarn is washed with water until neutral and then subjected to secondary hot stretching. The specific conditions are: 150℃, stretching ratio 1.5 times; 200℃, stretching ratio 3 times.
[0082] A process for processing soy protein isolate into protein fluff for spinning, the specific steps of which are as follows: (1) First, hydroxylated porous graphene is prepared using graphite as raw material; (2) Then the soy protein isolate is enzymatically hydrolyzed to obtain hydrolyzed protein; (3) Then, the hydroxylated porous graphene and enzymatically hydrolyzed protein are ultrasonically dispersed in water, and sodium tripolyphosphate is added and mixed evenly to obtain a spinning solution. The solution is pre-crosslinked and wet-spun to obtain the final product.
[0083] In step (1), the preparation method of hydroxylated porous graphene is as follows: first, graphite is ultrasonically dispersed in an ethanol aqueous solution, transferred to a reaction vessel, and subjected to a solvothermal reaction to obtain porous graphene; then, the porous graphene is added to a mixed acid solution under stirring conditions, potassium permanganate is added slowly, and the reaction is heated to obtain a suspension; finally, the suspension is poured into cold water, hydrogen peroxide solution is added, and after the reaction stops, it is washed and dried to obtain the hydroxylated porous graphene.
[0084] The mass ratio of graphite, aqueous ethanol solution, mixed acid solution, and potassium permanganate is 1:12:7:0.0003. The volume concentration of the aqueous ethanol solution is 50%, and the mixed acid solution is obtained by mixing 98% concentrated sulfuric acid and 85% concentrated phosphoric acid in a volume ratio of 9:1.
[0085] The solvothermal reaction conditions were: 140℃ for 15 hours; the heating reaction conditions were: 45℃ for 12 hours.
[0086] The volume ratio of the suspension, cold water, and hydrogen peroxide solution is 1:1:0.3, the temperature of the cold water is 4℃, and the mass concentration of the hydrogen peroxide solution is 30%.
[0087] The washing process includes sequentially washing with distilled water, 30% hydrochloric acid solution, and anhydrous ethanol; the drying conditions are: drying at 80℃ for 12 hours.
[0088] In step (2), the enzymatic hydrolysis method is as follows: the soy protein isolate is ultrasonically dispersed in water, the pH is adjusted to 8 using 0.1 mol / L sodium hydroxide solution, alkaline protease is added, and the enzyme is hydrolyzed at 50°C for 3 hours. The enzyme is then inactivated, filtered, concentrated, and dried to obtain the hydrolyzed protein.
[0089] The mass ratio of soy protein isolate, water, and alkaline protease was 10:80:0.1.
[0090] In step (3), the mass ratio of hydroxylated porous graphene, enzymatically hydrolyzed protein, water, and sodium tripolyphosphate is 0.03:1:15:0.02.
[0091] In step (3), the pre-crosslinking process conditions are as follows: first, adjust the pH to 6.5 using 0.1 mol / L acetic acid solution, stir at room temperature for 25 minutes, and then adjust the pH to 9 using 0.1 mol sodium hydroxide solution.
[0092] In step (3), the wet spinning conditions are as follows: the spinning plate has 6 holes with a hole diameter of 150 μm, the spinning speed is 20 m / min, and the spinning temperature is 80℃; the coagulation bath temperature is 45℃, and the coagulation bath is a mixed aqueous solution including: 300 g / L sodium sulfate, 70 g / L sulfuric acid, and 15 g / L zinc sulfate.
[0093] In step (3), after wet spinning, the yarn is washed with water until neutral and then subjected to secondary hot stretching. The specific conditions are: 150℃, stretching ratio 1.5 times; 200℃, stretching ratio 3 times.
[0094] The mechanical properties and antibacterial properties of the protein fibers obtained in Examples 1-3 and Comparative Examples 1 and 2 were tested respectively, as follows: 1. Mechanical property testing: The strength properties were determined using the FAVIMAT fully automatic single fiber universal tester. Forty test samples were used, and the average value was taken.
[0095] 2. Antibacterial properties: Referring to GB / T 15979-2024 "Hygienic requirements for disposable sanitary products", the antibacterial properties against Escherichia coli and Staphylococcus aureus were investigated using the shaking flask method.
[0096] The test results are shown in Table 1.
[0097] Table 1. Test Results
[0098] As shown in Table 1, the protein wool for spinning obtained in Examples 1-3 has excellent mechanical and antibacterial properties.
[0099] Comparative Example 1, which omitted hydroxylated porous graphene, and Comparative Example 2, which omitted modification treatment, showed a significant deterioration in the mechanical and antibacterial properties of the resulting spinning protein fluff. This indicates that the synergistic effect of hydroxylated porous graphene and chitosan modification jointly improves the mechanical and antibacterial properties.
[0100] While the specific embodiments of the present invention have been described above, they are not intended to limit the scope of protection of the present invention. Based on the technical solutions of the present invention, various modifications or variations that can be made by those skilled in the art without creative effort are still within the scope of protection of the present invention.
Claims
1. A process for processing soy protein isolate into protein velvet for spinning, characterized by, The specific steps are as follows: (1) First, hydroxylated porous graphene is prepared using graphite as raw material; (2) Then the soy protein isolate is enzymatically hydrolyzed to obtain enzymatically hydrolyzed protein, and then the enzymatically hydrolyzed protein is modified by transglutaminase and chitosan to obtain modified protein. (3) Then, the hydroxylated porous graphene and modified protein are ultrasonically dispersed in water, and sodium tripolyphosphate is added and mixed evenly to obtain a spinning solution. The solution is pre-crosslinked and wet-spun to obtain the final product.
2. The process according to claim 1, characterized in that, In step (1), the preparation method of hydroxylated porous graphene is as follows: first, graphite is ultrasonically dispersed in an ethanol aqueous solution, transferred to a reaction vessel, and subjected to a solvothermal reaction to obtain porous graphene; then, the porous graphene is added to a mixed acid solution under stirring conditions, potassium permanganate is added slowly, and the reaction is heated to obtain a suspension; finally, the suspension is poured into cold water, hydrogen peroxide solution is added, and after the reaction stops, it is washed and dried to obtain the hydroxylated porous graphene.
3. The process of claim 2, wherein, The mass ratio of graphite, aqueous ethanol solution, mixed acid solution, and potassium permanganate is 1:12-15:7-9:0.0003-0.0005. The volume concentration of the aqueous ethanol solution is 50-60%. The mixed acid solution is obtained by mixing 98% concentrated sulfuric acid and 85% concentrated phosphoric acid in a volume ratio of 9:
1. The solvothermal reaction conditions are: 140–160℃ for 15–17 hours; the heating reaction conditions are: 45–50℃ for 12–15 hours. The volume ratio of the suspension, cold water, and hydrogen peroxide solution is 1:1:0.3, the temperature of the cold water is 4℃, and the mass concentration of the hydrogen peroxide solution is 30%. The washing process includes sequentially washing with distilled water, 30% hydrochloric acid solution, and anhydrous ethanol; the drying conditions are: drying at 80℃ for 12 hours.
4. The process of claim 2, wherein, In step (2), the enzymatic hydrolysis method is as follows: the soy protein isolate is ultrasonically dispersed in water, the pH is adjusted to 8 using 0.1 mol / L sodium hydroxide solution, alkaline protease is added, and the enzyme is hydrolyzed at 50-60℃ for 3-4 hours. The enzyme is then inactivated, filtered, concentrated, and dried to obtain the hydrolyzed protein.
5. The process of claim 2, wherein, In step (2), the modification treatment method is as follows: the enzymatically hydrolyzed protein is stirred and dispersed in water, transglutaminase and chitosan are added, the reaction is carried out at 40-45℃ for 1-2 hours, the enzyme is inactivated, and then the modified protein is obtained.
6. The process of claim 2, wherein, In step (3), the mass ratio of hydroxylated porous graphene, modified protein, water and sodium tripolyphosphate is 0.03-0.05:1:15-20:0.02-0.
03.
7. The process of claim 2, wherein, In step (3), the pre-crosslinking process conditions are as follows: first, adjust the pH to 6.5 using 0.1 mol / L acetic acid solution, stir at room temperature for 25 to 35 minutes, and then adjust the pH to 9 using 0.1 mol sodium hydroxide solution.
8. The process of claim 2, wherein, In step (3), the wet spinning conditions are as follows: the spinning plate has 6 holes with a hole diameter of 150 μm, the spinning speed is 20 m / min, and the spinning temperature is 80℃; the coagulation bath temperature is 45℃, and the coagulation bath is a mixed aqueous solution including: 300 g / L sodium sulfate, 70 g / L sulfuric acid, and 15 g / L zinc sulfate.
9. The process of claim 2, wherein, In step (3), after wet spinning, the yarn is washed with water until neutral and then subjected to secondary hot stretching. The specific conditions are: 150℃, stretching ratio 1.5 times; 200℃, stretching ratio 3 times.
10. A protein pile for spinning processed from soybean protein isolate, characterized by, It is obtained by the process described in any one of claims 1 to 9.
Citation Information
Patent Citations
Production method of antibacterial soybean protein fiber and product of antibacterial soybean protein fiber
CN103388195B