A three-dimensional crimped bicomponent polyester staple fiber and its preparation method
By employing a core-sheath composite structure and core-shell aerogel microparticles in polyester staple fibers, a continuous three-dimensional crimped and honeycomb porous structure is formed, solving the problems of insufficient crimp stability, fluffy resilience, and thermal insulation performance of polyester staple fibers, and achieving high strength and low thermal conductivity.
Patent Information
- Application Number
- CN202611210712.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-11
- Publication Date
- 2026-11-17
AI Technical Summary
Existing polyester staple fibers have shortcomings in terms of crimp stability, fluffy resilience, and heat insulation properties, making it difficult to simultaneously achieve both high tensile strength and low thermal conductivity.
A core-sheath composite structure is formed using the first and second polyester components. The difference in thermal shrinkage behavior drives continuous three-dimensional crimping. Core-shell aerogel microparticles are introduced into the sheath layer, and a honeycomb porous structure is formed through post-treatment. The hydrophobicity and alkali solubility of the core-shell aerogel microparticles are combined to optimize the internal stress distribution and pore structure of the fiber.
It improves the fiber's fluffiness, resilience, and heat insulation properties while maintaining its tensile strength, reduces the thermal conductivity, and achieves three-dimensional crimping and lightweighting of the fiber.
Smart Images

Figure CN123108772A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of chemical fiber manufacturing technology, specifically to a three-dimensional crimped bicomponent polyester staple fiber and its preparation method. This staple fiber can be used as a functional staple fiber for thermal insulation filling materials, nonwoven materials, textile materials, and discontinuous fiber reinforced composite materials. Background Technology
[0002] Polyester staple fiber is widely used in clothing, home textiles, filling materials, nonwoven materials, and wool-like fabrics due to its advantages such as wide availability of raw materials, moderate cost, stable processing, washability, durability, and good mechanical properties. Ordinary polyester staple fiber is typically a single-component structure with a relatively dense surface and internal structure, high fiber rigidity, and its crimp is mostly formed by mechanical crimping or subsequent processing. This type of crimp is usually biased towards two-dimensional planar crimping, with limited spatial support capacity. After compression, washing, or long-term use, it is prone to problems such as decreased bulk, insufficient resilience, and a stiff feel. In discontinuous fiber reinforced composites, thermal insulation filling materials, and nonwoven materials, the crimp stability, bulk support capacity, interfacial structure, and thermal insulation performance of staple fibers directly affect the material's lightweight, resilience, and thermal insulation performance.
[0003] To improve the bulkiness and resilience of polyester staple fibers, bicomponent polyester composite fibers have been proposed in existing technologies. These fibers typically utilize differences in intrinsic viscosity, crystallization rate, thermal shrinkage, elastic modulus, or heat distortion behavior between the two polyester components to generate internal stress differences during spinning, drawing, heat setting, or post-treatment, causing the fibers to crimp. Compared to ordinary mechanical crimping, the crimp stability of bicomponent polyester composite fibers is improved. However, if crimping relies solely on the shrinkage difference between the two components, the fiber's thermal insulation performance still primarily depends on the air layer between the fiber aggregates, and the fiber itself has limited ability to block heat conduction.
[0004] To improve the thermal insulation performance of polyester fibers, existing technologies include adding low thermal conductivity fillers, inorganic microparticles, or porous particles. Aerogel microparticles, with their low density, porosity, and low thermal conductivity, can reduce the thermal conductivity of the fiber itself to some extent when introduced into polyester fibers. However, if aerogel microparticles are simply dispersed uniformly in the polyester component as ordinary fillers, there is a lack of effective coupling between them and the fiber's crimped structure, resulting in limited improvement on the fiber's bulky resilience. Furthermore, excessive filler may affect spinning stability and fiber strength and elongation properties.
[0005] Existing technologies utilize methods such as alkali reduction, dissolution, extraction, or removable phase removal to create porous structures on or within polyester fibers, thereby reducing fiber density and improving static air retention. However, conventional porous polyester fibers typically suffer from problems such as relatively uniform pore distribution, insufficient structural support, and excessive pore development leading to decreased mechanical properties. If the pore structure cannot synergize with the asymmetric fiber cross-section and the bicomponent internal stress crimping structure, it is difficult to simultaneously achieve low thermal conductivity, fluffy resilience, and high tensile stability.
[0006] Therefore, how to simultaneously construct a three-dimensional crimped structure driven by the difference in thermal shrinkage behavior of the components, a honeycomb porous structure induced by core-shell aerogel microparticles, and a spatial partitioning structure that can retain low thermal conductivity particles in bicomponent polyester staple fibers, thereby improving the fluffy resilience and thermal insulation performance while maintaining usable tensile strength, is a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0007] The purpose of this invention is to provide a three-dimensional crimped bicomponent polyester staple fiber and its preparation method, so as to solve the problems of insufficient crimping stability, limited fluffiness and resilience, and unsatisfactory thermal insulation performance of ordinary polyester staple fibers, as well as the difficulty of existing filler-containing or porous polyester fibers in simultaneously achieving crimping, elongation and thermal insulation performance.
[0008] To achieve the above objectives, the present invention provides a three-dimensional crimped bicomponent polyester staple fiber, comprising a first polyester component and a second polyester component, wherein the first polyester component and the second polyester component are continuously compounded along the fiber length direction to form a bicomponent polyester fiber structure; both the first polyester component and the second polyester component are fiber-forming polyesters, and they have different heat shrinkage behaviors that enable the fiber to form a continuous three-dimensional crimped shape; the second polyester component contains core-shell aerogel microparticles; the three-dimensional crimped bicomponent polyester staple fiber, after being stretched and heat-set, exhibits a continuous three-dimensional crimped shape along the axial direction; after post-treatment, a honeycomb porous structure is formed in the polyester component containing the core-shell aerogel microparticles.
[0009] Preferably, the difference in heat shrinkage behavior can be caused by at least one of the following: intrinsic viscosity, crystallization rate, heat shrinkage rate, elastic modulus, glass transition temperature, or heat distortion behavior. The difference in heat shrinkage behavior is defined as the two polyester components exhibiting different orientation crystallization, heat shrinkage, or heat distortion behaviors after being treated under the same stretching and heat setting conditions, with the degree of difference limited to the extent that the resulting composite fiber can form a continuous three-dimensional crimped shape.
[0010] Preferably, the difference in heat shrinkage behavior can be characterized by the difference in free heat shrinkage rate after dry heat treatment at 180°C for 10 minutes, and the difference in free heat shrinkage rate between the first polyester component and the second polyester component is 5% to 35%, preferably 8% to 25%.
[0011] Preferably, the bicomponent polyester fiber structure is a core-sheath composite structure, which includes a core layer and a sheath layer covering the outer periphery of the core layer. The core layer is composed of a first polyester component, and the sheath layer is composed of a second polyester component. The sheath layer continuously covers the core layer, and the core layer is not exposed.
[0012] Preferably, in the cross-section of the three-dimensional crimped bicomponent polyester staple fiber, the core layer is offset to one side relative to the center of the fiber cross-section, so that the sheath layer forms a thick-walled side and a thin-walled side in the circumferential direction of the fiber.
[0013] Through the above technical solutions, the non-concentric structure can enhance the circumferential asymmetry of the fiber cross section and increase the bending moment of the fiber during the heat setting process, thereby facilitating the formation of three-dimensional crimps in the fiber.
[0014] Preferably, the core-shell aerogel microparticles are dispersed in the sheath layer. After post-processing, a honeycomb-shaped interconnected pore area is formed from the outer surface of the sheath layer to a region of 10% to 60% of the sheath layer thickness, and at least one of the core-shell aerogel microparticles and hydrophobic aerogel core is retained on the inner side of the honeycomb-shaped interconnected pore area.
[0015] Preferably, the equivalent pore size of the pores in the honeycomb interconnected pore area is 0.2 to 5.0 μm.
[0016] Preferably, the average particle size of the core-shell aerogel microparticles is 0.1–5.0 μm, more preferably 0.5–5.0 μm, and even more preferably 0.5–3.0 μm; the content of the core-shell aerogel microparticles is 0.1%–5.0% based on the total fiber mass.
[0017] Preferably, the core-shell aerogel microparticles are core-hydrophobic, shell-alkali-soluble, controllable core-shell aerogel microparticles. The core-shell aerogel microparticles comprise a hydrophobically modified silica-based aerogel core and an alkali-soluble organic shell layer coating the outer surface of the silica-based aerogel core.
[0018] Through the above technical solutions, the aerogel core is used to maintain low thermal conductivity, porosity and lightweight properties in polyester fibers; the alkaline-soluble organic shell layer is used to improve the dispersion compatibility of core-shell aerogel particles in polyester melt, and preferentially hydrolyzes or loosens them during post-processing, so that the core-shell aerogel particles located on or near the surface of the fiber are controllably removed, thereby forming a honeycomb porous structure.
[0019] Preferably, the method for preparing the core-shell aerogel microparticles includes the following steps: P1: Silica aerogel particles are dispersed in an ethanol-water mixture, methyltrimethoxysilane and phenyltrimethoxysilane are added, the pH of the system is adjusted to 4-5 with an acid regulator, and the reaction is carried out at 40-70℃ for 2-6 hours. After hydrolysis, methyltrimethoxysilane and phenyltrimethoxysilane condense with the silanol groups on the surface of silica aerogel particles to obtain a hydrophobic core. In the above process, the silanol groups formed after the hydrolysis of methyltrimethoxysilane can condense with the silanol groups on the surface of silica aerogel particles and introduce methyl hydrophobic groups on the aerogel surface; after the hydrolysis of phenyltrimethoxysilane, phenyl structures can be further introduced, which improves the organic affinity and thermal stability of the aerogel surface.
[0020] P2: The hydrophobic core is dispersed in an ethanol-water mixture, 3-aminopropyltriethoxysilane is added, and the mixture is reacted at 50-75°C for 2-5 hours. After the 3-aminopropyltriethoxysilane is hydrolyzed, it condenses with the remaining silanol groups or siloxane network on the surface of the hydrophobic core to obtain the amino core. In the above process, the triethoxysilane group at one end of 3-aminopropyltriethoxysilane can undergo siloxane condensation with the hydrophobic core surface, while the amino group at the other end remains on the outer surface of the particle. This amino group can improve the interfacial interaction between aerogel particles and polyester, low-polyester, or ring-opening monomers. On the other hand, it can serve as a reaction site for the subsequent introduction of hydroxyl groups and alkaline-soluble polyester shells, transforming aerogel particles from simple inorganic fillers into reactive particles that can be further grafted with organic shells.
[0021] P3: Add glycidol to the dispersion system containing the amino core, and react at 40-70°C for 2-6 hours to allow the epoxy groups in the glycidol to undergo a ring-opening addition reaction with the amino groups on the surface of the amino core to obtain the hydroxyl core; In the above process, glycidol contains both epoxy and hydroxyl groups. Its epoxy groups can undergo a ring-opening reaction with the amino groups on the surface of the amino core, thereby introducing secondary amine linkages and hydroxyl groups onto the surface of the aerogel particles. The hydroxyl groups serve as initiation sites for subsequent ring-opening polymerization of 6-caprolactone or L-lactide, enabling the in-situ growth of alkaline-soluble polyester segments from the surface of the aerogel particles.
[0022] P4: The hydroxyl core is dispersed in an organic solvent, an aliphatic cyclic ester monomer is added, and then stannous octoate is added as a catalyst. The reaction is carried out at 100-150°C for 4-12 hours under nitrogen protection, so that the aliphatic cyclic ester monomer undergoes ring-opening polymerization with the hydroxyl groups on the surface of the hydroxyl core as the initiation site, to obtain core-shell aerogel microparticles coated with at least one of polycaprolactone segments and polylactic acid segments; wherein the aliphatic cyclic ester monomer is selected from at least one of 6-caprolactone and L-lactide.
[0023] In the above process, 6-caprolactone undergoes ring-opening polymerization to form polycaprolactone segments, and L-lactide undergoes ring-opening polymerization to form polylactic acid segments. Both polycaprolactone and polylactic acid segments contain aliphatic ester bonds, and their alkali hydrolysis sensitivity is higher than that of aromatic polyester matrices such as polyethylene terephthalate and polybutylene terephthalate. Under subsequent alkaline post-treatment conditions, the alkali-soluble organic shell of the core-shell aerogel particles located on or near the fiber surface can preferentially undergo hydrolysis, chain breakage, or loosening, causing the corresponding aerogel particles to partially detach from the polyester matrix and form pores on or near the fiber surface; while the core-shell aerogel particles or hydrophobic aerogel core located in the inner region can be at least partially retained due to the restricted diffusion of alkali solution, thus forming an asymmetric structure in which porous regions and particulate residue regions coexist.
[0024] Preferably, in P1, the average particle size of the silica aerogel particles is 0.5–3.0 μm; based on 100 parts by mass of silica aerogel particles, the amount of ethanol is 300–800 parts by mass, the amount of deionized water is 5–50 parts by mass, the amount of methyltrimethoxysilane is 3–12 parts by mass, and the amount of phenyltrimethoxysilane is 1–8 parts by mass; the acidity regulator is selected from at least one of acetic acid, hydrochloric acid, and oxalic acid.
[0025] Preferably, in P2, based on 100 parts by mass of hydrophobic core, the amount of ethanol is 300-800 parts by mass, the amount of deionized water is 5-30 parts by mass, and the amount of 3-aminopropyltriethoxysilane is 2-10 parts by mass.
[0026] Preferably, in P3, the amount of glycidol is 1 to 6 parts by mass, based on 100 parts by mass of amino core.
[0027] Preferably, in P4, based on 100 parts by mass of hydroxyl group, the amount of organic solvent is 100-300 parts by mass, the total amount of aliphatic cyclic ester monomer is 10-120 parts by mass, and the amount of stannous octoate is 0.05-0.5 parts by mass; the aliphatic cyclic ester monomer is selected from at least one of 6-caprolactone and L-lactide; when 6-caprolactone is used, its amount is 10-60 parts by mass; when L-lactide is used, its amount is 10-60 parts by mass; the organic solvent is selected from one of xylene and N,N-dimethylformamide.
[0028] Preferably, the first polyester component is polybutylene terephthalate, and the second polyester component is polyethylene terephthalate.
[0029] This invention also provides a method for preparing three-dimensional crimped bicomponent polyester staple fibers, comprising the following steps: Step (1) The first polyester chips are dried and then melted to obtain the first polyester melt; Step (2) premix the core-shell aerogel microparticles with a portion of the second polyester chips, and then melt-blend, extrude, cool and pelletize them through a twin-screw extruder to obtain a second polyester masterbatch containing core-shell aerogel microparticles; then mix the second polyester masterbatch with the remaining second polyester chips, dry and melt them to obtain a second polyester melt containing core-shell aerogel microparticles. Step (3) The first polyester melt and the second polyester melt are composite spun through a bicomponent composite spinning assembly to obtain bicomponent polyester nascent fibers containing core-shell aerogel microparticles. Step (4) stretches and heat-sets the bicomponent polyester nascent fibers to generate an internal stress difference between the two polyester components, thereby forming a three-dimensional crimped structure that is continuously distributed along the fiber axis. Step (5) Post-processing is performed on the heat-set fibers to cause at least one of the following changes in the core-shell aerogel particles: removal, loosening, and dissolution, and to form a honeycomb porous structure in the second polyester component; Step (6) involves washing, drying and cutting the post-treated fibers to obtain three-dimensional crimped bicomponent polyester staple fibers.
[0030] Preferably, in step (2), the second polyester melt serves as the sheath polyester melt, and the core-shell aerogel particles are introduced into the sheath polyester melt through the second polyester masterbatch.
[0031] Preferably, in step (2), the mass content of core-shell aerogel microparticles in the second polyester masterbatch is 5wt% to 20wt%; the extrusion temperature of the twin-screw melt blend is 270 to 290°C, the screw speed is 100 to 250 r / min, and vacuum exhaust is used.
[0032] Through the above technical solutions, the core-shell aerogel microparticles are first pre-dispersed in the form of a second polyester masterbatch, and then mixed and melted with the remaining second polyester chips. This helps to improve the dispersion uniformity of the core-shell aerogel microparticles in the second polyester component, reduce the risk of powder agglomeration and melt spinning breakage, thereby improving the stability of composite spinning and the uniformity of fiber structure.
[0033] Preferably, in step (3), the bicomponent composite spinning assembly is a core-sheath composite spinning assembly, and the core layer is controlled to be offset relative to the center of the fiber cross-section, so that the fiber forms a non-concentric core-sheath composite structure. During the composite spinning process, the temperature of the first polyester melt is 245-265℃, the temperature of the second polyester melt is 280-295℃, the temperature of the spinning box is 275-290℃, the winding speed is 800-1200m / min, the ring blower temperature is 18-28℃, and the ring blower speed is 0.3-0.8m / s.
[0034] Preferably, in step (4), the draw ratio is 3.0 to 4.0 and the heat setting temperature is 140 to 190°C.
[0035] Preferably, in step (5), the post-treatment is an alkaline post-treatment, the pH of the post-treatment solution is 8.5 to 10.5, the treatment temperature is 65 to 90°C, and the treatment time is 20 to 35 min; the post-treatment solution is a weakly alkaline aqueous solution with pH adjusted by sodium hydroxide.
[0036] Preferably, in step (6), the cutting length is 32-64 mm.
[0037] Preferably, the present invention also provides the application of the above-mentioned three-dimensional crimped bicomponent polyester staple fiber in thermal insulation filling materials, nonwoven materials, textile materials or discontinuous fiber reinforced composite materials.
[0038] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are: 1. This invention utilizes the difference in thermal shrinkage behavior between the first and second polyester components to create an internal stress difference during stretching and heat setting, causing the fibers to form a continuous three-dimensional crimp along the axial direction. Compared to ordinary mechanical crimping, this crimp is driven by the internal stress of the bicomponent structure, which is beneficial for improving the spatial support capacity and compression resilience of the fiber assembly.
[0039] 2. This invention introduces core-shell aerogel microparticles into the second polyester component, namely the sheath polyester component in the core-sheath composite structure, and forms a honeycomb porous structure in the sheath through post-treatment. The honeycomb porous structure can reduce the local density of the fiber and increase the space for stagnant air retention on the fiber surface, near the surface, and in the fiber assembly; at the same time, the incompletely removed core-shell aerogel microparticles or their hydrophobic aerogel cores can still exist as low thermal conductivity particles inside the sheath, so that the pore insulation and low thermal conductivity particle insulation work together to help reduce the thermal conductivity of the fiber assembly.
[0040] 3. The core-shell aerogel microparticles of the present invention adopt a structural design of hydrophobic core and alkaline-soluble shell. The hydrophobic aerogel core is used to maintain a low thermal conductivity porous structure, while the alkaline-soluble organic shell layer is used to improve the melt dispersibility of the second polyester component and serves as a sacrificial layer in the post-processing process. This structure makes the core-shell aerogel microparticles no longer ordinary inert fillers, but simultaneously undertake multiple functions such as melt compatibility, post-processing induced pore formation, and residual thermal insulation.
[0041] 4. This invention distributes core-shell aerogel particles in the sheath layer, rather than primarily in the core layer. Because the sheath layer is close to the outer surface of the fiber, the alkaline post-treatment solution can more easily diffuse into the area containing the core-shell aerogel particles, thereby improving pore-forming efficiency and pore-forming controllability; at the same time, the core layer remains relatively continuous and dense, which is beneficial for maintaining fiber strength, stretching stability, and the internal stress curling effect of the two components.
[0042] 5. In the non-concentric core-sheath composite structure of this invention, the core layer is biased towards one side of the fiber cross-section, while the sheath layer forms thick-walled and thin-walled sides. This structure creates an uneven distribution of stiffness, density, and shrinkage stress in the circumferential direction of the fiber cross-section, further promoting the formation of stable three-dimensional crimp in the fiber. After post-treatment, a honeycomb-like porous structure is formed on the surface or near the surface of the sheath layer. This porous structure works synergistically with the two-component internal stress crimp structure, enabling the fiber to simultaneously possess good three-dimensional crimp, fluffy resilience, and lightweight thermal insulation properties. Attached Figure Description
[0043] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0044] Figure 1 This is a SEM image of the surface of ordinary polyester staple fiber.
[0045] Figure 2 This is a SEM image of the fiber surface of Example 1 of the three-dimensional crimped bicomponent polyester staple fiber of the present invention.
[0046] Figure 3 This is a cross-sectional structural diagram of the core-sheath structure of the three-dimensional crimped bicomponent polyester staple fiber of the present invention.
[0047] Figure 4 This is a schematic diagram of fiber curling morphology, used to illustrate the differences between straight and flat morphology, planar curling morphology, and three-dimensional curling morphology.
[0048] Figure 5 This is a graph showing the bulkiness test results of Example 1 of the three-dimensional crimped bicomponent polyester staple fiber of the present invention. It shows the original height value and the average value under three conditions: light load, heavy load, and after compression and rebound.
[0049] Figure 6 This is a graph showing the test results of the tensile strength of Example 1 of the three-dimensional crimped bicomponent polyester staple fiber of the present invention.
[0050] Figure 7 This is a diagram showing the crimping test results of Example 1 of the three-dimensional crimped bicomponent polyester staple fiber of the present invention.
[0051] Figure 8 This is a graph showing the relationship between breaking strength and breaking elongation of the three-dimensional crimped bicomponent polyester staple fiber in Example 1 of the present invention.
[0052] Figure 9This is a comparison diagram of the light load length L0 and the heavy load length L1 in the three-dimensional crimping test of bicomponent polyester staple fiber in Example 1 of the present invention. Detailed Implementation
[0053] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Example 1
[0054] This embodiment provides a method for preparing three-dimensional crimped bicomponent polyester staple fibers, including the preparation of core-shell aerogel microparticles and the preparation of bicomponent polyester staple fibers.
[0055] The method for preparing the core-shell aerogel microparticles includes the following steps: P1: 100 parts by mass of silica aerogel microparticles with an average particle size of 1.0 μm were added to an ethanol-water mixture consisting of 500 parts by mass of ethanol and 20 parts by mass of deionized water, and ultrasonically dispersed for 30 min to obtain an aerogel solution. 8 parts by mass of methyltrimethoxysilane and 4 parts by mass of phenyltrimethoxysilane were added to the aerogel solution, and the pH of the system was adjusted to 4.5 using acetic acid. The reaction was carried out at 60 °C for 4 h, allowing the methyltrimethoxysilane and phenyltrimethoxysilane to hydrolyze and condense with the silanol groups on the surface of the silica aerogel microparticles. After the reaction was completed, the microparticles were centrifuged, washed sequentially with ethanol and deionized water, and then vacuum dried at 80 °C for 12 h to obtain a hydrophobic core.
[0056] P2: 100 parts by mass of the hydrophobic core were redispersed in an ethanol-water mixture consisting of 500 parts by mass of ethanol and 15 parts by mass of deionized water. 6 parts by mass of 3-aminopropyltriethoxysilane were added, and the mixture was reacted at 65°C for 3 hours. This allowed the 3-aminopropyltriethoxysilane to hydrolyze and condense with the remaining silanol groups or silicon-oxygen network on the surface of the hydrophobic core. After the reaction was complete, the mixture was centrifuged, washed sequentially with ethanol and deionized water, and then vacuum-dried at 80°C for 12 hours to obtain the amino core.
[0057] P3: 100 parts by mass of the amino core were dispersed in 500 parts by mass of ethanol, and 3 parts by mass of glycidol were added. The mixture was reacted at 60°C for 4 hours to allow the epoxy groups in the glycidol to undergo a ring-opening addition reaction with the amino groups on the surface of the amino core. After the reaction was completed, the mixture was centrifuged, washed with ethanol to remove unreacted glycidol, and then vacuum dried at 70°C for 12 hours to obtain the hydroxyl core.
[0058] P4: Take 100 parts by mass of the hydroxyl core and add it to 200 parts by mass of N,N-dimethylformamide. After ultrasonic dispersion for 20 min, add 30 parts by mass of 6-caprolactone and 20 parts by mass of L-lactide, and then add 0.2 parts by mass of stannous octoate as a catalyst. React at 130℃ for 8 h under nitrogen protection, so that 6-caprolactone and L-lactide undergo ring-opening polymerization with the hydroxyl groups on the surface of the hydroxyl core as initiation sites. After the reaction is completed, cool the reaction solution to room temperature, add excess ethanol-water mixture for precipitation and washing, and after centrifugation, wash successively with N,N-dimethylformamide and ethanol to remove free polymer, unreacted monomers and catalyst residues. Then, vacuum dry at 70℃ for 12 h to obtain silicon-based core-shell aerogel microparticles coated with polycaprolactone segments and polylactic acid segments. The silicon-based core-shell aerogel microparticles are core-hydrophobic, shell-base-dissociable controllable core-shell aerogel microparticles with an average particle size of 1.2 μm.
[0059] The core-shell aerogel microparticles are first melt-blended with a portion of the second polyester chips using a twin-screw extruder to prepare a second polyester masterbatch containing core-shell aerogel microparticles. Specifically, the core-shell aerogel microparticles and polyethylene terephthalate chips are vacuum-dried separately, then pre-mixed at a core-shell aerogel microparticle content of 10 wt%, and then melt-blended, extruded, cooled, and pelletized using a twin-screw extruder to obtain the second polyester masterbatch. The twin-screw extrusion temperature is 280℃, the screw speed is 200 r / min, and vacuum degassing is used. Pre-preparing the second polyester masterbatch helps to improve the dispersion uniformity of the core-shell aerogel microparticles in the second polyester component and reduces the risk of agglomeration and breakage during melt spinning.
[0060] The method for preparing the bicomponent polyester staple fiber includes the following steps: Step (1) Based on 100 parts by mass of the total fiber raw materials, 40 parts by mass of polybutylene terephthalate chips are dried and melted to obtain the first polyester melt, which serves as the core layer melt.
[0061] Step (2) involves mixing 45 parts by mass of polyethylene terephthalate chips with 15 parts by mass of the second polyester masterbatch, followed by drying and melting to obtain a second polyester melt, which serves as the sheath melt. The core-shell aerogel microparticles in the second polyester masterbatch contain 10 wt%, therefore, the amount of core-shell aerogel microparticles added to the second polyester melt is 1.5 parts by mass, accounting for 1.5% of the total fiber mass.
[0062] Step (3) Use a core-sheath composite spinning assembly to composite spin the first polyester melt and the second polyester melt, control the cross-sectional area ratio of the core layer to the sheath layer to be 40:60, and make the core layer offset to one side relative to the center of the fiber cross-section, while ensuring that the sheath layer continuously covers the core layer and the core layer is not exposed, to obtain a bicomponent polyester nascent fiber containing core-shell aerogel particles.
[0063] During the composite spinning process, the temperature of the first polyester melt is 250℃, the temperature of the second polyester melt is 285℃, the temperature of the spinning box is 280℃, the winding speed is 1000m / min, the ring blower temperature is 24℃, and the ring blower speed is 0.5m / s.
[0064] Step (4) The bicomponent polyester nascent fibers are cooled, bundled and then stretched with a stretching ratio of 3.4 times; then heat-set at 165°C to generate an internal stress difference between the two polyester components and to form a three-dimensional crimped structure that is continuously distributed along the fiber axis.
[0065] Step (5) The heat-set fiber is treated in a sodium hydroxide aqueous solution at pH 9.5 and temperature 80℃ for 25 minutes to remove, loosen or dissolve some of the core-shell aerogel particles in the sheath, and to form a honeycomb porous structure on the fiber surface and near the surface.
[0066] Step (6) The post-treated fibers are washed, dried and cut to obtain the three-dimensional crimped bicomponent polyester staple fiber of Example 1; the cut length of the obtained staple fiber is 50 mm.
[0067] Depend on Figure 1 and Figure 2 As can be seen from the comparison, the surface of ordinary polyester fiber is relatively smooth and dense, while the surface of the fiber in Example 1 has obvious pore morphology. Figure 3 As can be seen, the fiber in Example 1 has a core-sheath composite cross-sectional structure. Combined with... Figure 4 As can be seen from the indicated criteria for judging the curling morphology, the curling morphology of the fiber in Example 1 is a three-dimensional curling driven by the internal stress of the two components, rather than a normal mechanical curling. Example 2
[0068] This embodiment is basically the same as Example 1, except that: the average particle size of the core-shell aerogel microparticles is 0.8 μm, and the addition amount is 0.5% of the total fiber mass; the cross-sectional area ratio of the core layer to the sheath layer is 30:70; the draw ratio is 3.0 times; the heat setting temperature is 150℃; and the alkaline post-treatment conditions are pH 8.5, 65℃, and 20 min. Example 3
[0069] This embodiment is basically the same as Example 1, except that: the average particle size of the core-shell aerogel microparticles is 2.5 μm, and the addition amount is 3.0% of the total fiber mass; the cross-sectional area ratio of the core layer to the sheath layer is 50:50; the draw ratio is 3.6 times; the heat setting temperature is 175℃; and the alkaline post-treatment conditions are pH 10.0, 85℃, and 30 min. Example 4
[0070] This embodiment is basically the same as Example 1, except that: the average particle size of the core-shell aerogel microparticles is 5.0 μm, and the addition amount is 4.5% of the total fiber mass; the cross-sectional area ratio of the core layer to the sheath layer is 60:40; the draw ratio is 3.9 times; the heat setting temperature is 185℃; and the alkaline post-treatment conditions are pH 10.5, 90℃, and 35 min.
[0071] In this embodiment, the mass content of core-shell aerogel microparticles in the second polyester masterbatch is adjusted to 20 wt%, and the content of core-shell aerogel microparticles in the resulting fiber is 4.5% of the total fiber mass by adjusting the ratio of the second polyester masterbatch to the remaining second polyester chips.
[0072] Comparative Example 1 This comparative example is basically the same as Example 1, except that a concentric core-sheath composite structure is adopted, so that the core layer is located at the center of the fiber cross-section and the thickness of the sheath layer is basically the same in the circumferential direction of the fiber.
[0073] Comparative Example 2 This comparative example is basically the same as Example 1, except that the alkaline post-treatment step is omitted.
[0074] Comparative Example 3 This comparative example is basically the same as Example 1, except that the alkaline post-treatment conditions are strengthened to pH 11, 95°C, and 60 min.
[0075] Comparative Example 4 This comparative example is basically the same as Example 1, except that the core-shell aerogel microparticles are replaced with solid silica microparticles of similar size and added amount.
[0076] Performance testing: The sample area A is 10×10cm, which is 100cm². 2 The sample weight G is 5g.
[0077] Under light load, the heights of the four sides are 2.4cm, 2.3cm, 1.9cm, and 2.0cm respectively, with an average height h1 of 2.15cm. The loft under light load is: V1 = A × h1 / G = 100 × 2.15 / 5 = 43.0 cm 3 / g.
[0078] Under heavy load, the heights of the four sides are 1.0cm, 1.0cm, 0.8cm, and 0.7cm respectively, with an average height h2 of 0.875cm. The loft under heavy load is: V2=A×h2 / G=100×0.875 / 5=17.5cm 3 / g.
[0079] After compression and rebound, the heights of the four sides are 2.0cm, 1.7cm, 1.8cm, and 2.0cm, respectively, with an average height h3 of 1.875cm. The loft after rebound is: V3=A×h3 / G=100×1.875 / 5=37.5cm 3 / g.
[0080] The compression rebound rate R is: R = (h3 - h2) / (h1 - h2) × 100% That is: R = (1.875 - 0.875) / (2.15 - 0.875) × 100% = 78.4%.
[0081] Thermal conductivity was tested using a flat-plate heat flow meter. During the thermal conductivity test, the short fibers obtained in each embodiment and comparative example were opened and prepared into fiber assemblies with the same areal density and thickness. The samples were conditioned for 24 hours at 20±2℃ and 65±5% relative humidity before testing. The test area, thickness, and compression state of each sample were kept consistent. Each group of samples was tested at least three times, and the average value was taken as the thermal conductivity.
[0082] The location and thickness of the honeycomb-like interconnected pore region were determined using scanning electron microscopy (SEM) images of the fiber cross-section. Specifically, the fiber was subjected to liquid nitrogen brittle fracture or embedded sectioning followed by gold sputtering. The fiber cross-section was observed using an SEM, and the distance from the outer surface of the fiber to the outer boundary of the core layer was taken as the sheath thickness. The depth of the continuously distributed pore area was measured along the radial direction of the fiber. The thickness of the honeycomb-like interconnected pore region accounted for 10% to 60% of the sheath thickness. The equivalent pore diameter was calculated by statistically analyzing the equivalent circular diameters of at least 50 pores using image analysis software and then taking the average value.
[0083] The tensile strength and elongation properties were tested according to the test method for the tensile properties of short chemical fibers. Before the test, the samples were conditioned for 24 hours in a standard environment with a temperature of 20±2℃ and a relative humidity of 65±5%. No less than 50 short fibers were randomly selected for single fiber tensile testing. The breaking strength, breaking elongation, breaking strength, breaking elongation, breaking time, initial modulus, elastic modulus, and strength at a given elongation were recorded, and the maximum, minimum, average, and coefficient of variation (CV) were calculated.
[0084] The crimping performance was tested according to GB / T 14338—2022 "Test Method for Crimping Performance of Short Chemical Fibers". Jn represents the number of crimps in a single fiber, in units of crimps / 25mm; JA represents the total number of crimp peaks and crimp valleys in L0 for a single fiber; L0 represents the fiber length under light load, in mm; L1 represents the fiber length under heavy load, in mm. The number of crimps Jn is calculated using the formula Jn=JA / (L0×2)×25; the crimp rate J is calculated using the formula J=(L1-L0) / L1×100%. Wherein, Jn corresponds to Jni in the standard, JA corresponds to JAi in the standard, L0 corresponds to L0i in the standard, and L1 corresponds to L1i in the standard; the subscript i is only used to indicate the i-th single fiber and is omitted in this specification and figures for simplification.
[0085] The three-dimensional curl morphology was confirmed through microscopic observation. Short fibers were laid naturally and loosely on the sample stage, and the fiber curling path was observed from both top and side views. When the fiber was continuously curved along the axial direction, and the curling path was not limited to a single plane, with undulating curves observable in both observation directions, it was determined to be a continuous three-dimensional curl morphology. Two-dimensional planar wavy curls formed by ordinary mechanical indentation do not belong to the continuous three-dimensional curl morphology described in this invention.
[0086] Examples 2-4 and Comparative Examples 1-4 were tested using the same method as Example 1. The results of their bulkiness, resilience, and thermal conductivity are shown in Table 1, and the results of their tensile strength, elongation, and curling properties are shown in Table 2. The original statistical data on tensile strength, elongation, curling, and bulkiness of Example 1 are shown in Tables 3-5, respectively. The comparison results of bulkiness, tensile strength, curling properties, the relationship between breaking strength and elongation at break, and the curling parameters L0 and L1 of Example 1 are shown in Tables 3-5, respectively. Figures 5-9 .
[0087] Table 1. Fluffiness, resilience, and thermal conductivity of Examples 1-4 and Comparative Examples 1-4
[0088] Table 2. Tensile and curl properties of Examples 1-4 and Comparative Examples 1-4
[0089] Table 3. Statistical data of tensile strength test in Example 1
[0090] Table 4. Statistical data of curling test in Example 1
[0091] Table 5 Original test data of fluffiness in Example 1
[0092] As can be seen from Tables 1 and 2, Examples 1 to 4 all employ a combination of non-concentric fully encapsulated core-shell structure, core-shell aerogel microparticles, alkaline post-treatment pore formation, and three-dimensional coiled structure. Therefore, they all exhibit high light-load bulkiness, good compression resilience, and lower thermal conductivity than their counterparts. Among them, Examples 3 and 4 have relatively higher aerogel content and post-treatment strength, resulting in more pronounced pore structures and relatively lower thermal conductivity; however, Example 4, due to its higher filler content and stronger treatment, shows a slight decrease in breaking strength and elongation at break compared to Example 1.
[0093] Compared to Comparative Example 1, Example 1 uses a concentric core-shell structure, lacking the stable bending moment provided by the eccentric cross-section. Therefore, its Jn, J, light-load bulkiness, and compression resilience are all lower than those of Example 1. This demonstrates that a non-concentric fully enclosed core-shell structure is an important structural basis for forming stable three-dimensional curl and improving bulky resilience.
[0094] Compared to Comparative Example 2, Example 2 omitted the alkaline post-treatment step and did not form a distinct surface honeycomb-like interconnected pore region. Therefore, its thermal conductivity was higher than that of Example 1, resulting in weaker weight reduction and insulation effects. This indicates that the surface honeycomb-like interconnected pore region plays an important role in reducing thermal conductivity and improving still air retention capacity.
[0095] Compared to Comparative Example 3, Example 1 employed an excessively alkaline post-treatment, resulting in over-expansion of the sheath pores and weakening of the particle residue area. Although Comparative Example 3 still retained the eccentric core-shell structure, its sheath structure support decreased, and its curl retention ability, tensile strength, elongation at break, and compression resilience were all lower than those of Example 1. This indicates that the present invention does not aim for complete removal of core-shell aerogel particles, but rather emphasizes the formation of a spatially partitioned structure under controllable alkaline post-treatment conditions, characterized by "partial removal of the surface layer to create pores, and retention of particles on the inner side."
[0096] Compared to Comparative Example 4, Example 4 replaced the core-shell aerogel microparticles with ordinary solid silica microparticles. Even with the same eccentric structure and post-processing conditions, its thermal conductivity was still significantly higher than that of Example 1. This indicates that the low thermal conductivity and porous nature of the core-shell aerogel microparticles contribute significantly to the thermal insulation effect of this invention.
[0097] In summary, the technical effect of this invention does not come from a single eccentric core-sheath structure, a single aerogel filler, or a single post-processing pore formation, but from the structural coupling of the three in the same fiber: the eccentric fully covered core-sheath structure provides the crimping driving force, the surface honeycomb interconnected pore area reduces density and increases the ability to retain still air, and the inner particle residue area retains low thermal conductivity particles and maintains cross-sectional asymmetry, ultimately enabling the fiber to have three-dimensional crimp, fluffy resilience, lightweight insulation and usable tensile strength.
[0098] The above description is merely a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. All equivalent substitutions, modifications, or improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A three-dimensional crimped bicomponent polyester staple fiber, characterized in that, The fiber comprises a first polyester component and a second polyester component, which are continuously compounded along the fiber length direction to form a bicomponent polyester fiber structure. Both the first polyester component and the second polyester component are fiber-forming polyesters, and they have different heat shrinkage behaviors that enable the fibers to form a continuous three-dimensional crimped shape. The second polyester component contains core-shell aerogel microparticles. The three-dimensional crimped bicomponent polyester short fibers are in a continuous three-dimensional crimped shape along the axial direction, and the second polyester component has a honeycomb porous structure.
2. The three-dimensional crimped bicomponent polyester staple fiber according to claim 1, characterized in that, The bicomponent polyester fiber structure is a core-sheath composite structure, which includes a core layer and a sheath layer covering the outer periphery of the core layer. The core layer is composed of a first polyester component, and the sheath layer is composed of a second polyester component. The sheath layer continuously covers the core layer, and the core layer is not exposed.
3. The three-dimensional crimped bicomponent polyester staple fiber according to claim 2, characterized in that, On the cross-section of the three-dimensional crimped bicomponent polyester staple fiber, the core layer is offset to one side relative to the center of the fiber cross-section, so that the sheath layer forms a thick-walled side and a thin-walled side in the circumferential direction of the fiber.
4. The three-dimensional crimped bicomponent polyester staple fiber according to claim 3, characterized in that, The core-shell aerogel microparticles are dispersed in the sheath; a honeycomb-shaped interconnected pore area is formed from the outer surface of the sheath to a region of 10% to 60% of the sheath thickness, and at least one of the core-shell aerogel microparticles and the aerogel core of the core-shell aerogel microparticles is retained on the inner side of the honeycomb-shaped interconnected pore area.
5. The three-dimensional crimped bicomponent polyester staple fiber according to claim 4, characterized in that, The equivalent pore size of the pores in the honeycomb interconnected pore region is 0.2–5.0 μm; the average particle size of the core-shell aerogel microparticles is 0.1–5.0 μm; and the content of the core-shell aerogel microparticles is 0.1%–5.0% based on the total fiber mass.
6. The stereocritical crimped bicomponent polyester staple fiber according to any one of claims 1-5, characterized in that, The core-shell aerogel microparticles are core-hydrophobic, shell-alkali-soluble controllable core-shell aerogel microparticles. The core-shell aerogel microparticles include a hydrophobically modified silicon-based aerogel core and an alkali-soluble organic shell layer covering the outer surface of the silicon-based aerogel core. The alkali-soluble organic shell layer includes at least one of polycaprolactone segments and polylactic acid segments.
7. The three-dimensional crimped bicomponent polyester staple fiber according to claim 6, characterized in that, The core-shell aerogel particles were prepared by the following method: P1: Disperse silica aerogel particles in an ethanol-water mixture, add methyltrimethoxysilane and phenyltrimethoxysilane, adjust the pH of the system to 4-5 with an acid regulator, and react at 40-70℃ for 2-6 hours to obtain a hydrophobic core; P2: The hydrophobic core is dispersed in an ethanol-water mixture, 3-aminopropyltriethoxysilane is added, and the mixture is reacted at 50-75°C for 2-5 hours to obtain an amino core; P3: Add glycidol to the dispersion system containing the amino core, and react at 40-70°C for 2-6 hours to obtain the hydroxyl core; P4: The hydroxyl core is dispersed in an organic solvent, an aliphatic cyclic ester monomer is added, and then stannous octoate is added. The mixture is reacted at 100-150°C for 4-12 hours under nitrogen protection to obtain core-shell aerogel microparticles. The aliphatic cyclic ester monomer is selected from at least one of 6-caprolactone and L-lactide; the organic solvent is selected from one of xylene and N,N-dimethylformamide.
8. The stereocripple bicomponent polyester staple fiber according to any one of claims 2-7, characterized in that, The first polyester component is polybutylene terephthalate, and the second polyester component is polyethylene terephthalate.
9. A method for preparing three-dimensional crimped bicomponent polyester staple fiber, characterized in that, Includes the following steps: Step (1) The first polyester chips are dried and then melted to obtain the first polyester melt; Step (2) premix the core-shell aerogel microparticles with a portion of the second polyester chips, and then melt-blend, extrude, cool and pelletize them through a twin-screw extruder to obtain a second polyester masterbatch containing core-shell aerogel microparticles; then mix the second polyester masterbatch with the remaining second polyester chips, dry and melt them to obtain a second polyester melt containing core-shell aerogel microparticles. Step (3) The first polyester melt and the second polyester melt are composite spun through a bicomponent composite spinning assembly to obtain bicomponent polyester nascent fibers containing core-shell aerogel microparticles. Step (4) stretches and heat-sets the bicomponent polyester nascent fibers to generate an internal stress difference between the two polyester components, thereby forming a three-dimensional crimped structure that is continuously distributed along the fiber axis. Step (5) Post-processing is performed on the heat-set fibers to cause at least one of the following changes in the core-shell aerogel particles: removal, loosening, and dissolution, and to form a honeycomb porous structure in the second polyester component; Step (6) involves washing, drying and cutting the post-treated fibers to obtain three-dimensional crimped bicomponent polyester staple fibers.
10. The method for preparing stereo-crimped bicomponent polyester staple fiber according to claim 9, characterized in that, In step (2), the mass content of core-shell aerogel microparticles in the second polyester masterbatch is 5wt% to 20wt%; the extrusion temperature of the twin-screw melt blending is 270 to 290°C, the screw speed is 100 to 250 r / min, and vacuum exhaust is used; the second polyester component is a sheath polyester component, and the core-shell aerogel microparticles are added to the sheath polyester component through the second polyester masterbatch; in step (3), the bicomponent composite spinning assembly is a core-sheath composite spinning assembly, and the core layer is controlled to be offset relative to the center of the fiber cross-section, so that the fiber forms a non-concentric core-sheath composite structure; during the composite spinning process, the first polyester melt The temperature is 245-265℃, the second polyester melt temperature is 280-295℃, the spinning box temperature is 275-290℃, the winding speed is 800-1200m / min, the ring blowing temperature is 18-28℃, and the ring blowing speed is 0.3-0.8m / s; in step (4), the draw ratio is 3.0-4.0, and the heat setting temperature is 140-190℃; in step (5), the post-treatment is alkaline post-treatment, the pH of the post-treatment solution is 8.5-10.5, the treatment temperature is 65-90℃, and the treatment time is 20-35min; in step (6), the cutting length is 32-64mm.