A high UV absorption polyester fiber and its preparation method
By combining a silicon-aluminum inorganic isolation layer co-deposited on the surface of nano zinc oxide and a surface tannic acid/Fe3+ gradient coordination layer in polyester fibers, the problem of unstable absorption performance of polyester fibers under long-term ultraviolet irradiation is solved, achieving both efficient and stable ultraviolet absorption and spinning performance.
Patent Information
- Application Number
- CN202611333727.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-17
AI Technical Summary
Under long-term ultraviolet irradiation, the photo-oxidation loss of the outer organic coordination layer by zinc oxide surface active species in existing polyester fibers leads to unstable ultraviolet absorption performance. Furthermore, when inorganic materials are uniformly distributed inside the fiber, it increases melt filtration pressure and affects fiber strength.
A silicon-aluminum inorganic isolation layer is co-deposited on the surface of nano-zinc oxide to form a core-sheath type polyester fiber, and a tannic acid/Fe3+ gradient coordination layer is constructed on the surface. Through the combination of localized zinc oxide in the skin and the gradient distribution on the surface, a stable ultraviolet absorption layer is formed by low-temperature aqueous phase treatment.
It improves the UV absorption performance and stability of polyester fibers, balances spinning stability and fiber strength, avoids the oxidative loss of the organic layer by zinc oxide active species, and maintains a long-term synergistic effect.
Smart Images

Figure CN123108774A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polyester fiber technology, belonging to patent classification number D01F6 / 92, specifically to a high ultraviolet absorption polyester fiber and its preparation method. Background Technology
[0002] Polyester fiber is widely used in clothing, outdoor sunshade materials, and protective fabrics due to its high strength, good abrasion resistance, dimensional stability, and low production cost. However, ordinary polyester fiber has limited absorption capacity for long-wave ultraviolet (UV) radiation, which can penetrate the pores between fibers and the fiber itself. Long-term exposure can also cause polyester molecular chains to break, leading to decreased strength, embrittlement, and color changes. Therefore, improving the absorption capacity of polyester fiber for UVA and UVB, and ensuring that this property remains stable after long-term use and washing, has practical application value.
[0003] Adding inorganic UV-absorbing materials such as zinc oxide to the interior of polyester fibers can reduce UV transmittance by utilizing the absorption and scattering effects of these materials. Inorganic materials have good heat resistance, capable of withstanding the melt spinning temperature of polyester, and their placement within the fiber can also reduce wash losses. However, if the inorganic material is uniformly added throughout the entire fiber cross-section, a large amount is often required to achieve high UV absorption capacity, which can easily increase melt filtration pressure and potentially affect the fiber's drawability and strength. Concentrating the inorganic material in the fiber sheath can improve its utilization efficiency, but zinc oxide near the fiber surface may still form surface-active species under UV irradiation.
[0004] Constructing an organic ultraviolet absorption layer on the surface of polyester fibers after fiber formation allows the absorption structure to be positioned where light first reaches, and compensates for the insufficient absorption of inorganic materials in certain ultraviolet bands. Tannic acid contains multiple aromatic structures and phenolic hydroxyl groups, which react with Fe... 3+ After forming a coordination structure, it can generate a wide ultraviolet absorption range, making it suitable for deposition on the surface of polyester fibers at lower temperatures, thus avoiding the high temperatures experienced by organic materials during melt spinning. However, when tannic acid / Fe 3+ When the coordination layer is directly combined with the zinc oxide-containing fiber skin, the surface-active species generated by the zinc oxide after being excited by ultraviolet light may gradually oxidize and consume the outer organic coordination layer. Although the fiber has a high initial ultraviolet absorption capacity, after continuous ultraviolet irradiation, the effect of the surface absorption layer gradually weakens, and it is difficult for the internal absorption and surface absorption to maintain a stable synergy for a long time.
[0005] Therefore, the technical problem to be solved by this invention is the application of a zinc oxide absorption structure in the fiber cortex and the tannic acid / Fe on the fiber surface. 3+While the coordination absorption structures jointly improve the ultraviolet absorption performance of polyester fibers, how can we suppress the photo-oxidation loss of the outer organic coordination layer caused by the surface active species formed after zinc oxide is excited by ultraviolet light, so that the two absorption structures can still maintain a stable synergistic effect after long-term ultraviolet irradiation, and at the same time make the materials and processes used adaptable to the conditions of polyester polymerization, melt spinning and subsequent surface treatment? Summary of the Invention
[0006] The purpose of this invention is to provide a high ultraviolet absorption polyester fiber and its preparation method to solve the technical problems mentioned in the background art.
[0007] To achieve the above objectives, the present invention provides the following technical solution: A method for preparing high UV absorption polyester fiber includes the following steps: Nano zinc oxide is dispersed in water, and water glass and aluminum sulfate are used as film-forming materials to co-deposit a silicon-aluminum inorganic isolation layer on the surface of the nano zinc oxide to obtain coated nano zinc oxide. The coated nano zinc oxide is dispersed in polyethylene terephthalate to obtain modified polyethylene terephthalate. The modified polyethylene terephthalate is used to form a skin layer, and polyethylene terephthalate without the coated nano zinc oxide is used to form a core layer. The skin-core type polyester fiber is obtained by composite melt spinning. The core-sheath type polyester fiber was sequentially reacted with an aqueous solution of tannic acid and a Fe-containing solution. 3+ The aqueous solution is contacted at least once to form tannic acid / Fe on the surface of the core-sheath type polyester fiber. 3+ The coordination layer is used to obtain the high UV absorption polyester fiber.
[0008] Preferably, based on 100 parts by mass of the nano-zinc oxide, the amount of water is 800-1000 parts by mass, the amount of water glass is 25-35 parts by mass, and the amount of aluminum sulfate is 12-16 parts by mass; the SiO2 / Na2O molar modulus of the water glass is 2.1-2.3, and the SiO2 mass fraction is 26%-28%; the aluminum sulfate is Al2(SO4)3·18H2O.
[0009] Preferably, the method for forming the silicon-aluminum inorganic isolation layer includes: The nano-zinc oxide aqueous dispersion was heated to 82-88°C. First, a portion of water glass was added to adjust the pH to 8.3-8.8. Then, the remaining water glass and aluminum sulfate aqueous solution were added over 60-90 minutes, maintaining the pH at 8.3-8.8 by adjusting the addition rate of the water glass and aluminum sulfate aqueous solution. After the addition was complete, the mixture was kept at this temperature and stirred for 40-60 minutes. Following filtration, washing, drying, and pre-dehydration, the coated nano-zinc oxide was obtained. The water washing endpoint is when the pH of the filtrate is 6.8–7.5 and the conductivity is not greater than 100 μS / cm, the pre-dehydration temperature is 250–260℃, and the D90 of the resulting coated nano zinc oxide is not greater than 300 nm.
[0010] Preferably, the modified polyethylene terephthalate is prepared by in-situ polymerization, specifically including: Terephthalic acid and the first part of ethylene glycol are esterified at 245–255°C and 0.20–0.35 MPa; the coated nano zinc oxide is dispersed in the second part of ethylene glycol to form an inorganic powder dispersion with a solid content of 15%–22%; after the water generated by esterification reaches more than 95% of the theoretical amount, the inorganic powder dispersion and polycondensation catalyst are added, and then polycondensation is carried out at 270–278°C and a final absolute pressure not exceeding 100 Pa. The total amount of ethylene glycol in the first part and the total amount of ethylene glycol in the second part, in molar ratio with terephthalic acid, is 1.20 to 1.32:1.
[0011] Preferably, the polycondensation catalyst is antimony glycolate, and the amount of antimony glycolate added is based on 180-250 ppm of Sb element as a percentage of the theoretical mass of polyethylene terephthalate; the coated nano zinc oxide accounts for 1.10%-1.50% of the mass of the modified polyethylene terephthalate, and the intrinsic viscosity of the obtained modified polyethylene terephthalate is 0.64-0.68 dL / g.
[0012] Preferably, the intrinsic viscosity difference between the polyethylene terephthalate forming the core layer and the modified polyethylene terephthalate forming the sheath layer is no greater than 0.03 dL / g, and the moisture content before melt spinning is no higher than 30 ppm; the mass ratio of the core layer to the sheath layer is 60-70:40-30; the core-sheath type polyester fiber has a trilobal cross-section; the melt spinning temperature is 280-286℃; the high-temperature residence time of the melt does not exceed 5 min; the draw ratio is 3.2-3.6 times; and the heat setting temperature is 125-135℃.
[0013] Preferably, the tannic acid / Fe 3+ The coordination layer process includes 2 to 4 two-bath deposition cycles; each two-bath deposition cycle includes first treating the core-sheath polyester fiber with an aqueous tannic acid solution, followed by treatment with an Fe-containing solution. 3+ The core-sheath type polyester fibers were treated with an aqueous solution, and in a subsequent two-bath deposition cycle, an aqueous solution of tannic acid and Fe was used. 3+ The concentrations of the aqueous solutions were lower than those of the corresponding solutions in the previous two-bath deposition cycle.
[0014] Preferably, the two-bath deposition cycle consists of three cycles: The first two-bath deposition cycle was treated with a 4.0 g / L tannic acid aqueous solution for 5 min, followed by a 1.0 g / L FeCl3·6H2O aqueous solution for 5 min. The second two-bath deposition cycle was treated with a 2.0 g / L tannic acid aqueous solution for 3 min, followed by a 0.50 g / L FeCl3·6H2O aqueous solution for 3 min. The third two-bath deposition cycle was treated with a 1.0 g / L tannic acid aqueous solution for 2 min, followed by a 0.25 g / L FeCl3·6H2O aqueous solution for 2 min.
[0015] Preferably, before performing the two-bath deposition cycle, the core-sheath type polyester fiber is pre-impregnated with an ethanol aqueous solution of concentration of 20-30 wt% for 1-3 min; a water wash is performed between each tannic acid aqueous solution treatment and FeCl3·6H2O aqueous solution treatment; after each two-bath deposition cycle, the fiber is dried at 65-75°C for 2-4 min; after all two-bath deposition cycles, the fiber is dried at 75-85°C for 8-12 min; and then heat-treated at 115-125°C for 2-4 min.
[0016] A high UV absorption polyester fiber is prepared by the method described above.
[0017] Compared with the prior art, the beneficial effects of the present invention are: 1. The localized inorganic absorption structure in the cortex concentrates nano-zinc oxide in the region near the outer surface of the fiber, allowing ultraviolet light to preferentially contact the zinc oxide after entering the fiber. Zinc oxide absorbs both UVA and UVB rays and scatters ultraviolet light using the difference in refractive index between itself and PET, thus extending the propagation path of ultraviolet light in the fiber cortex and increasing the chance of absorption. Compared to uniformly dispersing zinc oxide throughout the entire fiber cross-section, the localized cortex structure achieves higher inorganic material utilization with a lower overall fiber addition amount. The trilobal cross-section also increases the effective surface area of the fiber and the number of light reflections, while the PET core layer without zinc oxide bears the main tensile load, thus balancing ultraviolet absorption performance, spinning stability, and fiber strength.
[0018] 2. Tannins / Fe on the outer surface of the fiber 3+The gradient coordination layer is located where ultraviolet light first reaches. The multiple aromatic structures contained in tannic acid can absorb short-wave ultraviolet light; after forming a coordination structure, its absorption range is expanded, compensating for the insufficient absorption of zinc oxide in certain wavelength bands. The surface layer is constructed with a gradually decreasing concentration from the inside out. The inner layer, closer to the fiber, has a higher coverage, providing a continuous absorption base; the outer layer uses a lower concentration deposition, which helps fill local gaps and reduce the accumulation of large coordination particles on the surface, avoiding an excessively thick, rough, or brittle surface layer. This coordination layer is formed through low-temperature aqueous phase treatment after spinning and drawing. Tannic acid does not need to undergo the PET melt spinning temperature, thus avoiding thermal decomposition of the organic absorption structure during processing. The surface network formed by multi-point adsorption and coordination also reduces the rapid loss of tannic acid during neutral washing, resulting in better retention of the surface ultraviolet absorption effect.
[0019] 3. A key issue to be addressed when combining the two absorption structures described above is that zinc oxide in the cortex may form surface-active species under continuous ultraviolet irradiation. These active species, in the presence of oxygen and a small amount of moisture, will gradually act on the outer tannic acid / Fe... 3+ The phenolic absorption structure in the coordination layer is oxidized, leading to a decrease in the absorption capacity and structural loosening of the coordination layer, ultimately resulting in a reduced absorption retention rate of the fiber after UV aging. To address this issue, water glass and aluminum sulfate are simultaneously introduced onto the zinc oxide surface to form a silicon-aluminum inorganic isolation layer. The silicon component provided by water glass primarily forms a continuous, transparent, and heat-resistant barrier framework, separating the active surface of zinc oxide from the external organic coordination layer. However, when using the silicon component alone, the isolation layer may develop micropores, pinholes, or insufficient coverage during drying and pre-dehydration, allowing small amounts of oxygen, water, and surface-active species to migrate through these defects. The aluminum component provided by aluminum sulfate can penetrate discontinuous regions of the silicon framework, filling micropores and gaps, and improving the integrity and density of the isolation layer on the zinc oxide surface. However, using the aluminum component alone makes it difficult to form a uniform and continuous thin layer. When both are used together, water glass establishes a continuous barrier framework, while aluminum sulfate seals framework defects and improves density, thus forming an isolation structure that combines continuous barrier and defect sealing. This structure can reduce the chance of oxygen and water approaching the active surface of zinc oxide, limiting the surface-active species generated by zinc oxide to tannic acid / Fe 3+ The coordination layer migrates, thereby mitigating the photo-oxidative loss of the outer organic absorption structure. At the same time, the silicon-aluminum isolation layer is relatively thin and has high UV transmittance, so it does not completely block the zinc oxide absorption core. Therefore, zinc oxide can still perform internal UV absorption and scattering, while the outer coordination layer can continue to perform broadband absorption, allowing the two structures to maintain a relatively stable synergistic effect after long-term UV irradiation. Attached Figure Description
[0020] Figure 1 This is a low-magnification SEM image of the high UV absorption polyester fiber prepared in Example 1 of the present invention.
[0021] Figure 2 This is a high-magnification SEM image of the high UV absorption polyester fiber prepared in Example 1 of the present invention. Detailed Implementation
[0022] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Example 1
[0023] A method for preparing high UV absorption polyester fiber includes the following steps: 1. Preparation of coated nano zinc oxide 30.0g of nano zinc oxide and 130.35g of deionized water were mixed and wet-milled until the laser particle size distribution D90 was no greater than 200nm, thus obtaining an aqueous dispersion of zinc oxide.
[0024] 7.50g of water glass was mixed with 41.25g of deionized water to obtain 48.75g of water glass solution; the water glass had a SiO2 / Na2O molar modulus of 2.1 and a SiO2 mass fraction of 26%, and the SiO2 mass fraction in the diluted solution was 4%.
[0025] 3.60 g of 98% pure Al2(SO4)3·18H2O was dissolved in 68.40 g of deionized water to obtain 72.00 g of 5% aluminum sulfate solution. The total amount of deionized water used in the above steps was 240.00 g, which is equivalent to using 800 parts by mass of deionized water for every 100 parts by mass of nano zinc oxide.
[0026] The zinc oxide aqueous dispersion was heated to 82℃. A portion of the water glass solution was added dropwise to bring the slurry pH to 8.3. Then, the remaining water glass solution and all the aluminum sulfate solution were added through both inlets over 60 minutes. The pH was maintained at 8.3 ± 0.05 by adjusting the feed rates of both inlets. After the addition was complete, the mixture was stirred at 82℃ for 40 minutes and then filtered. The filter cake was redispersed with 150g of deionized water each time and filtered again until the filtrate pH was not lower than 6.8 and the conductivity was not greater than 100 μS / cm.
[0027] The resulting filter cake was dried at 105℃ for 4 hours, then vacuum dried at 145℃ for 4 hours, followed by pre-dehydration at 250℃ for 40 minutes. After cooling, it was air-jet pulverized to a D90 of no more than 300 nm and stored in a sealed container.
[0028] 2. Preparation of core-sheath type polyester fibers The feed was prepared according to the composition for 400.00g of modified PET for the leather layer. 341.99g of terephthalic acid and 130.37g of the first-part ethylene glycol were added to a 1L polyester reactor, and esterification was carried out under nitrogen protection, at 245℃ and 0.20MPa gauge pressure. The stoichiometric theoretical water production corresponding to this feed was 74.17g. The esterification stage ended when the corrected water output reached 70.46g.
[0029] 4.40g of the above-mentioned coated nano zinc oxide and 22.96g of the second part of ethylene glycol were bead-milled in a closed system for 30 minutes to prepare an inorganic powder dispersion with a solid content of 16.1%. The total amount of the first part of ethylene glycol and the second part of ethylene glycol was 153.33g, and the molar ratio of ethylene glycol to terephthalic acid was 1.20:1.
[0030] The reactor temperature was adjusted to 240℃, and inorganic powder dispersion and 0.124g of antimony glycolate were added; the antimony glycolate contained 57.5% Sb by mass, equivalent to 180ppm of Sb element in the theoretical PET mass. Subsequently, the pressure was gradually reduced, and polycondensation was carried out at 270℃ and a final absolute pressure of 100Pa. After sampling and measuring the intrinsic viscosity to reach 0.64dL / g, the vacuum was released, and the material was pressed with nitrogen, cooled, and pelletized.
[0031] The modified PET chips were crystallized at 120℃ for 1 hour, and then vacuum dried at 160℃ for 6 hours. 300g of modified PET chips and 450g of ordinary fiber-grade PET chips with an intrinsic viscosity of 0.65dL / g were weighed separately, and the ordinary PET chips were dried to a moisture content of no more than 30ppm.
[0032] A three-lobed core-sheath composite spinneret was used, with 450g of ordinary PET forming the core layer and 300g of modified PET forming the sheath layer. The core layer to sheath layer was fed at a mass ratio of 60:40, and melt spinning was carried out at 280℃, with the melt residence time controlled to not exceed 5 minutes. The nascent fibers were cooled by side blowing at 20℃ and oiled before being wound, then stretched 3.2 times at 80℃, and heat-set at 125℃.
[0033] 3. Tannic acid / Fe 3+ Surface treatment Weigh 500g of core-sheath polyester fiber from the fiber obtained by stable spinning. Mix 0.500kg of anhydrous ethanol and 2.000kg of deionized water to prepare 2.500kg of ethanol aqueous solution with a mass fraction of 20%. Pre-soak the fiber at 25℃ for 1min and squeeze out the excess liquid.
[0034] Two two-bath deposition cycles were performed, with each treatment bath having a volume of 5.0 L. The first cycle involved treatment with 5.0 L of an aqueous solution containing 20.0 g of tannic acid for 5 min, followed by washing with 5.0 L of deionized water for 1 min; then treatment with 5.0 L of an aqueous solution containing 5.0 g of FeCl3·6H2O for 5 min, followed by washing with 5.0 L of deionized water for 1 min, and drying at 65 °C for 2 min.
[0035] The second cycle involves treating with 5.0 L of an aqueous solution containing 5.0 g of tannic acid for 2 min, followed by washing with 5.0 L of deionized water for 1 min; then treating with 5.0 L of an aqueous solution containing 1.25 g of FeCl3·6H2O for 2 min, followed by washing with 5.0 L of deionized water for 1 min, and drying at 65 °C for 2 min.
[0036] After all processing is completed, the fiber is dried at 75℃ for 8 minutes and then heat-treated at 115℃ for 2 minutes to obtain polyester fiber. Example 2
[0037] A method for preparing high UV absorption polyester fiber includes the following steps: 1. Preparation of coated nano zinc oxide Mix 30.0 g of nano zinc oxide and 175.128 g of deionized water, and wet bead mill until D90 is no greater than 200 nm.
[0038] 8.88g of water glass was mixed with 39.072g of deionized water to obtain 47.952g of water glass solution; the water glass had a SiO2 / Na2O molar modulus of 2.2 and a SiO2 mass fraction of 27%, and the SiO2 mass fraction in the diluted solution was 5%.
[0039] 4.20 g of 98% pure Al2(SO4)3·18H2O was dissolved in 55.80 g of deionized water to obtain 60.00 g of 7% aluminum sulfate solution. The total amount of deionized water used in the above steps was 270.00 g, which is equivalent to using 900 parts by mass of deionized water for every 100 parts by mass of nano zinc oxide.
[0040] The zinc oxide aqueous dispersion was heated to 85°C. A portion of water glass solution was added dropwise to bring the pH to 8.5. The remaining water glass solution and aluminum sulfate solution were then added separately over 75 minutes, maintaining the pH at 8.5 ± 0.05 by adjusting the feed rates of both streams. After the addition was complete, the mixture was stirred at 85°C for 50 minutes and then filtered. The filter cake was redispersed with 150g of deionized water each time and filtered again until the filtrate had a pH of 6.8–7.5 and a conductivity not exceeding 100 μS / cm.
[0041] The filter cake was dried at 110℃ for 4 hours, vacuum dried at 150℃ for 5 hours, pre-dehydrated at 255℃ for 50 minutes, cooled, and then pulverized to a D90 of no more than 300 nm.
[0042] 2. Preparation of core-sheath type polyester fibers The feed was prepared according to the composition for 700.00g of modified PET for the leather layer. 597.16g of terephthalic acid and 240.40g of ethylene glycol (part 1) were added to a 2L polyester reactor, and esterification was carried out under nitrogen protection, 250℃, and 0.28MPa gauge pressure. The stoichiometric theoretical water production corresponding to this feed was 129.51g. The esterification stage ended when the corrected water output reached 123.04g.
[0043] 9.24g of coated nano-zinc oxide and 40.71g of the second part of ethylene glycol were bead-milled in a closed system for 30 minutes to prepare an inorganic powder dispersion with a solid content of 18.5%. The total amount of the first and second parts of ethylene glycol was 281.11g, and the molar ratio of ethylene glycol to terephthalic acid was 1.26:1.
[0044] The esterification temperature was adjusted to 240℃, and an inorganic powder dispersion and 0.264g of antimony glycolate were added. The antimony glycolate contained 57.5% Sb by mass, equivalent to 220ppm of Sb element in the theoretical PET mass. Subsequently, the pressure was gradually reduced, and polycondensation was carried out at 275℃ and a final absolute pressure of 80Pa. After sampling and measuring the intrinsic viscosity to reach 0.66dL / g, the material was discharged, cooled, and pelletized.
[0045] The modified PET chips were crystallized at 120℃ for 1 hour, and then vacuum dried at 160℃ for 6 hours. 525g of modified PET chips and 975g of ordinary fiber-grade PET chips with an intrinsic viscosity of 0.66dL / g were weighed out, and the moisture content of both types of chips was controlled to be below 30ppm.
[0046] A trilobal core-sheath composite spinneret was used, with 975g of ordinary PET forming the core layer and 525g of modified PET forming the sheath layer. The core layer to sheath layer was fed at a mass ratio of 65:35, and melt spinning was performed at 283℃, with the melt residence time controlled to not exceed 5 minutes. The nascent fibers were cooled by side blowing at 20℃, oiled, and wound, then stretched 3.4 times at 85℃ and heat-set at 130℃.
[0047] 3. Tannic acid / Fe 3+ Surface treatment Weigh 1.000 kg of core-sheath type polyester fiber from the fiber obtained by stable spinning. Mix 1.250 kg of anhydrous ethanol and 3.750 kg of deionized water to prepare 5.000 kg of ethanol aqueous solution with a mass fraction of 25%. Pre-soak the fiber at 25°C for 2 min and squeeze out the excess liquid.
[0048] Three two-bath deposition cycles were performed, with each treatment bath having a volume of 10.0 L. The first cycle involved treatment with 10.0 L of an aqueous solution containing 40.0 g of tannic acid for 5 min, followed by washing with 10.0 L of deionized water for 1 min; then treatment with 10.0 L of an aqueous solution containing 10.0 g of FeCl3·6H2O for 5 min, followed by washing with 10.0 L of deionized water for 1 min, and drying at 70 °C for 3 min.
[0049] The second cycle involves treating the sample with a 10.0 L aqueous solution containing 20.0 g tannic acid for 3 min, followed by washing with 10.0 L deionized water for 1 min; then treating it with a 10.0 L aqueous solution containing 5.0 g FeCl3·6H2O for 3 min, followed by washing with 10.0 L deionized water for 1 min, and drying it at 70 °C for 3 min.
[0050] The third cycle involves treatment with 10.0 L of aqueous solution containing 10.0 g tannic acid for 2 min, followed by washing with 10.0 L of deionized water for 1 min; then treatment with 10.0 L of aqueous solution containing 2.50 g FeCl3·6H2O for 2 min, followed by washing with 10.0 L of deionized water for 1 min, and drying at 70 °C for 3 min.
[0051] After all processing is completed, the fibers are dried at 80℃ for 10 minutes and then heat-treated at 120℃ for 3 minutes to obtain polyester fibers. Example 3
[0052] A method for preparing high UV absorption polyester fiber includes the following steps: 1. Preparation of coated nano zinc oxide Mix 30.0g of nano zinc oxide and 206.30g of deionized water, and wet-mill until D90 is no greater than 200nm.
[0053] 10.50g of water glass was mixed with 38.50g of deionized water to obtain 49.00g of water glass solution; the water glass had a SiO2 / Na2O molar modulus of 2.3 and a SiO2 mass fraction of 28%, and the SiO2 mass fraction in the diluted solution was 6%.
[0054] 4.80 g of 98% pure Al2(SO4)3·18H2O was dissolved in 55.20 g of deionized water to obtain 60.00 g of 8% aluminum sulfate solution. The total amount of deionized water used in the above steps was 300.00 g, which is equivalent to using 1000 parts by mass of deionized water for every 100 parts by mass of nano zinc oxide.
[0055] The zinc oxide aqueous dispersion was heated to 88°C. A portion of water glass solution was added dropwise to bring the pH to 8.8. The remaining water glass solution and aluminum sulfate solution were then added separately over 90 minutes, maintaining the pH at 8.8 ± 0.05 by adjusting the feed rates of both streams. After the addition was complete, the mixture was stirred at 88°C for 60 minutes and then filtered. The filter cake was redispersed with 150g of deionized water each time and filtered again until the filtrate pH did not exceed 7.5 and the conductivity did not exceed 100 μS / cm.
[0056] The filter cake was dried at 115℃ for 4 hours, vacuum dried at 155℃ for 6 hours, pre-dehydrated at 260℃ for 60 minutes, cooled, and then pulverized to a D90 of no more than 300 nm.
[0057] 2. Preparation of core-sheath type polyester fibers The feed was prepared according to the composition for 450.00g of modified PET for the leather layer. 383.19g of terephthalic acid and 165.05g of ethylene glycol (part 1) were added to a 1L polyester reactor, and esterification was carried out under nitrogen protection, at 255℃ and 0.35MPa gauge pressure. The stoichiometric theoretical water production corresponding to this feed was 83.11g. The esterification stage ended when the corrected water output reached 78.95g.
[0058] 6.75g of coated nano-zinc oxide and 23.93g of the second part of ethylene glycol were bead-milled in a closed system for 30 minutes to prepare an inorganic powder dispersion with a solid content of 22.0%. The total amount of the first part of ethylene glycol and the second part of ethylene glycol was 188.98g, and the molar ratio of ethylene glycol to terephthalic acid was 1.32:1.
[0059] The temperature of the esterified compound was adjusted to 245℃, and an inorganic powder dispersion and 0.193g of antimony glycolate were added. The antimony glycolate contained 57.5% Sb by mass, which is equivalent to 250ppm of Sb element in the theoretical PET mass. Subsequently, the pressure was gradually reduced, and polycondensation was carried out at 278℃ and a final absolute pressure of 60Pa. After sampling and measuring the intrinsic viscosity, the material was discharged, cooled, and pelletized.
[0060] The modified PET chips were crystallized at 120℃ for 1 hour, and then vacuum dried at 160℃ for 6 hours. 360g of modified PET chips and 840g of ordinary fiber-grade PET chips with an intrinsic viscosity of 0.67dL / g were weighed out, and the moisture content of both types of chips was controlled to be below 30ppm.
[0061] A trilobal core-sheath composite spinneret was used, with 840g of ordinary PET forming the core layer and 360g of modified PET forming the sheath layer. The core layer to sheath layer was fed at a mass ratio of 70:30, and melt spinning was performed at 286℃, controlling the melt residence time at high temperature to not exceed 5 minutes. The nascent fibers were cooled by side blowing at 20℃, oiled, and wound, then stretched 3.6 times at 90℃ and heat-set at 135℃.
[0062] 3. Tannic acid / Fe 3+ Surface treatment 750g of core-sheath polyester fiber was weighed from the fiber obtained by stable spinning. 1.125kg of anhydrous ethanol and 2.625kg of deionized water were mixed to prepare 3.750kg of ethanol aqueous solution with a mass fraction of 30%. The fiber was pre-soaked at 25℃ for 3min and the excess liquid was squeezed off.
[0063] Four two-bath deposition cycles were performed, with each treatment bath having a volume of 7.5 L. The first cycle involved treatment with 7.5 L of aqueous solution containing 30.0 g tannic acid for 5 min, followed by treatment with 7.5 L of aqueous solution containing 7.50 g FeCl3·6H2O for 5 min.
[0064] The second cycle involved treatment with 7.5 L of aqueous solution containing 22.5 g tannic acid for 4 min, followed by treatment with 7.5 L of aqueous solution containing 5.625 g FeCl3·6H2O for 4 min.
[0065] The third cycle involved treatment with 7.5 L of aqueous solution containing 15.0 g tannic acid for 3 min, followed by treatment with 7.5 L of aqueous solution containing 3.750 g FeCl3·6H2O for 3 min.
[0066] The fourth cycle involves treatment with 7.5L of aqueous solution containing 7.50g of tannic acid for 2 minutes, followed by treatment with 7.5L of aqueous solution containing 1.875g of FeCl3·6H2O for 2 minutes.
[0067] Between each treatment with tannic acid aqueous solution and FeCl3·6H2O aqueous solution, the fibers were washed with 7.5 L of deionized water for 1 min. After each two-bath deposition cycle, the fibers were dried at 75 °C for 4 min. After all treatments were completed, the fibers were dried at 85 °C for 12 min and then heat-treated at 125 °C for 4 min to obtain polyester fibers.
[0068] Comparative Example 1: Except for replacing the coated nano zinc oxide in Example 1 with uncoated nano zinc oxide calculated based on the same zinc oxide core mass, the other raw materials, dosages, and process conditions were the same as in Example 1.
[0069] Comparative Example 2: Except for omitting 3.60g of Al2(SO4)3·18H2O during the zinc oxide coating process and using dilute sulfuric acid to maintain the pH of the slurry at 8.3 so that only a siliceous layer is formed on the surface of the zinc oxide, all other conditions were the same as in Example 1.
[0070] Comparative Example 3: Except for omitting 7.50g of water glass during the zinc oxide coating process and using a dilute sodium hydroxide solution to maintain the pH of the slurry at 8.3 so that only an aluminum layer is formed on the surface of the zinc oxide, all other conditions were the same as in Example 1.
[0071] Comparative Example 4: Except for not adding coated nano-zinc oxide to the PET skin layer and using ordinary fiber-grade PET to simultaneously form the core and skin layers, the remaining spinning and tannin / Fe 3+ The surface treatment conditions were the same as in Example 1.
[0072] Comparative Example 5: Except for omitting tannic acid / Fe from Example 1 3+ Except for the two-bath deposition treatment, in which the core-sheath type polyester fibers that have completed stretching and heat setting are directly used as the finished product, all other conditions are the same as in Example 1.
[0073] Comparative Example 6: Except that the coated nano zinc oxide content was uniformly dispersed in all PET fibers in the same way as in Example 1 and single-component melt spinning was used instead of core-sheath composite spinning, the other drawing, heat setting and surface treatment conditions were the same as in Example 1.
[0074] Comparative Example 7: Except for the fact that both two two-bath deposition cycles used 4.0 g / L tannic acid aqueous solution and 1.0 g / L FeCl3·6H2O aqueous solution, and the surface layer was not constructed by a concentration decrease method, all other conditions were the same as in Example 1.
[0075] Performance testing: Sample preparation and conditioning: Polyester filaments with the same nominal linear density obtained in Examples 1-3 and Comparative Examples 1-7 were knitted into plain knit fabrics on the same laboratory single-cylinder circular knitting machine (machine size E24), with a loop length of 2.80 mm and a finished surface density controlled at 120 g / m². 2 No dyeing or resin finishing is performed after weaving; the corresponding roll is taken directly for the filament tensile test. Unless otherwise specified, the fabric is sampled at least 50 mm from the selvage. Before the test, the samples are conditioned for 24 hours without tension in a standard atmosphere with a temperature of (20±2)℃ and a relative humidity of (65±4)% according to GB / T 6529-2008.
[0076] Ultraviolet (UV) protection performance: determined according to GB / T 18830-2009. Five 100mm × 100mm samples were randomly cut from each group, with the outward-facing side of the fabric facing the UV light source. The spectral transmittance was measured using a UV transmittance analyzer equipped with an integrating sphere in the range of 290-400nm, with recording intervals of 5nm and a spectral bandwidth not exceeding 5nm. The UPF of each sample was calculated based on the solar irradiance and erythema spectrum given in the standard. The T(UVA)AV in the 315-400nm range and the T(UVB)AV in the 290-315nm range were also calculated. The table lists the arithmetic mean of the UPF of the five samples, as well as T(UVA)AV and T(UVB)AV, with transmittance rounded to two decimal places.
[0077] Washability: Washing was performed according to GB / T 8629-2017 using the 4N program of a Type A standard washing machine. The washing temperature was (40±3)℃, and the normal agitation washing time was 15min. Each time, (20±1)g of standard detergent 3 without enzymes and fluorescent whitening agents was added, and Type III polyester wash liners were used to make up to a total washing load of (2.0±0.1)kg. The hardness of the test water was less than 0.7mmol / L. One complete wash and hanging drying under Program A was counted as one cycle, and a total of 20 cycles were performed. After the last drying, the product was conditioned in standard atmosphere for 24h, and the average UPF was determined according to GB / T 18830-2009.
[0078] UV aging performance: Accelerated aging was conducted according to test condition 1 of GB / T 31899-2015. A 100mm × 150mm fabric sample was flattened and fixed on the sample holder, with the illuminated side facing the UVA-340 fluorescent ultraviolet lamp; the irradiance at 340nm was 0.89W / (m²). 2 The fabric was irradiated for 8 hours at a blackboard temperature of (60±3)℃ (nm), followed by condensation for 4 hours at a blackboard temperature of (50±3)℃. Each cycle lasted 12 hours, for a total aging period of 120 hours. The filaments used for strength retention testing were uniformly and non-overlappingly wound onto a 150mm long sample frame, and subjected to the same cycle as the fabric. After aging, the fabric was conditioned for 24 hours. The average UPF of the fabric was determined according to GB / T 18830-2009, and the breaking strength of the filaments was determined using the tensile method described below.
[0079] Tensile properties and strength retention of filaments: determined according to GB / T 14344-2022. Five filament packages were randomly selected from each group, and the surface 100m of each package was removed. Four valid samples were obtained from each package, and a total of 20 tests were conducted. A constant-speed elongation tensile tester was used, with a unit linear density pretension of (0.050±0.005) cN / dtex, a clamping distance of (500±1) mm, and a moving clamp speed of 500 mm / min. The breaking strength and elongation at break were recorded. The breaking strength was obtained by dividing the breaking strength by the measured linear density. Results of jaw breakage or significant slippage were disregarded and retested. The arithmetic mean of the 20 valid results was taken for both breaking strength and elongation at break. The strength retention rate after UV aging was calculated as "average breaking strength after aging / average breaking strength before aging × 100%".
[0080] Surface lightness: determined according to GB / T 8424.1-2001. The same tissue was folded into four layers in the same direction and tested using a spectrophotometer under D65 standard illuminant, 10° standard colorimetric observer, d / 8 illumination conditions, and a specular reflection mode. The measuring aperture was 25.4 mm. CIE L*a*b* colorimetric parameters were measured at five non-overlapping locations for each group, and the arithmetic mean of the five L* values was taken. A smaller L* value indicates a darker sample surface color.
[0081] Table 1: sample Initial average UPF T(UVA)AV / % T(UVB)AV / % Average UPF after 20 washes Average UPF after 120h aging Fracture strength / (cN / dtex) Elongation at break / % Strength retention rate after aging / % L* Example 1 62.8 3.12 1.46 55.4 59.0 4.24 23.7 94.1 53.8 Example 2 75.2 2.48 1.18 66.8 70.9 4.38 22.9 94.5 45.2 Example 3 83.7 2.03 1.09 72.0 77.2 4.51 21.8 93.7 37.4 Comparative Example 1 64.5 2.97 1.39 56.2 43.7 4.12 23.4 78.2 53.5 Comparative Example 2 63.7 3.02 1.42 55.8 52.4 4.18 23.6 88.5 53.7 Comparative Example 3 61.5 3.21 1.48 53.9 49.1 4.16 23.5 85.9 53.9 Comparative Example 4 44.8 4.61 2.05 38.6 40.9 4.46 24.5 92.5 53.6 Comparative Example 5 38.6 7.34 2.43 37.9 36.5 4.30 24.0 93.0 88.7 Comparative Example 6 58.3 3.42 1.59 50.5 52.7 3.98 21.6 90.0 53.1 Comparative Example 7 68.9 2.76 1.30 54.3 62.1 4.19 22.8 92.2 46.0 In Table 1, the initial average UPF of Examples 1, 2, and 3 were 62.8, 75.2, and 83.7, respectively; the T(UVA)AV were 3.12%, 2.48%, and 2.03%, respectively; and the T(UVB)AV were 1.46%, 1.18%, and 1.09%, respectively. This indicates that within this set of process parameters, the incremental configuration of the cortex inorganic absorber phase and the surface metal-polyphenol network can continuously reduce UV transmittance. The UPF retention rates after 20 washes were 88.2%, 88.8%, and 86.0%, respectively, and the UPF retention rates after UV aging were 93.9%, 94.3%, and 92.2%, respectively. Example 2 showed better overall stability at a higher initial protection level, while Example 3 had the highest initial protection, but the thicker surface deposition slightly reduced its wash retention rate. The fracture strengths of the three groups of samples were 4.24 cN / dtex, 4.38 cN / dtex, and 4.51 cN / dtex, respectively. The strength retention rate after aging was higher than 93%, indicating that the surface functionalization used did not destroy the main load-bearing function of the pure PET core layer.
[0082] The differences between Example 1 and Comparative Examples 1-3 reflect the role of water glass and aluminum sulfate in constructing the coating layer. Comparative Example 1, without ZnO coating, had an initial average UPF of 64.5 due to complete exposure of the active surface, slightly higher than Example 1's 62.8. However, after aging, the average UPF dropped to 43.7, with a strength retention rate of only 78.2%. Comparative Example 2, which formed only a silica layer, and Comparative Example 3, which formed only an aluminum-containing layer, had average UPFs of 52.4 and 49.1 after aging, respectively, with strength retention rates of 88.5% and 85.9%, both lower than Example 1's 59.0 and 94.1%. Water glass, through hydrolysis and condensation, forms a continuous silicon-oxygen framework, which can expand the coverage of the ZnO surface. The aluminum-containing oxides or hydrated oxides formed by the hydrolysis of aluminum sulfate can fill the micropores and interface defects of the silica layer and improve the density of the deposited layer. The combination of the two reduces the channels through which ultraviolet light and moisture directly contact ZnO via defects, and inhibits the reactive oxygen species reaction induced by photogenerated charge carriers on the ZnO surface. This simultaneously slows down the photo-oxidative damage to the PET molecular chains and the outer tannic acid / Fe³⁺ network. This is a stabilization effect that cannot be achieved when a single silicon layer is prone to leaving microcracks and a single aluminum-containing layer is difficult to form a continuous coverage.
[0083] Comparative Example 4 retained only the surface metal-polyphenol network, with an initial average UPF of 44.8; Comparative Example 5 retained only the skin-coated ZnO, with an initial average UPF of 38.6; Example 1, by employing both types of absorption structures simultaneously, increased the initial average UPF to 62.8, indicating that the absorption and scattering of near-ultraviolet light by ZnO is related to the tannic acid / Fe... 3+ The broadband absorption of the complex network exhibits spatial and spectral complementarity. Comparative Example 6, with the same total amount of ZnO uniformly dispersed in a single-component PET, had an initial average UPF and tensile strength of 58.3 and 3.98 cN / dtex, respectively, both lower than the 62.8 and 4.24 cN / dtex of Example 1. This indicates that concentrating ZnO in the skin layer can improve the light shielding efficiency per unit amount and reduce the disturbance of inorganic particles to the continuity of the carrier phase. Comparative Example 7 underwent two equal-concentration surface treatments, with an initial average UPF of 68.9, but it decreased to 54.3 after 20 washes, with a retention rate of 78.8%. Although Example 1 had an initial average UPF of 62.8, it remained at 55.4 after washing, achieving a retention rate of 88.2%. These results demonstrate that repeated deposition at equal concentrations easily leads to localized accumulation and weak adhesion areas, while decreasing concentration deposition can first establish a continuous underlayer and then fill the gaps with lower concentrations, thus achieving a more stable balance between UV protection, washability, and mechanical retention. L* decreased from 53.8 in Example 1 to 37.4 in Example 3, consistent with the pattern that the color deepens with the increase of surface coordination deposition times.
[0084] Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the essence and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing high ultraviolet absorption polyester fiber, characterized in that, Includes the following steps: Nano zinc oxide is dispersed in water, and water glass and aluminum sulfate are used as film-forming materials to co-deposit a silicon-aluminum inorganic isolation layer on the surface of the nano zinc oxide to obtain coated nano zinc oxide. The coated nano zinc oxide is dispersed in polyethylene terephthalate to obtain modified polyethylene terephthalate. The modified polyethylene terephthalate is used to form a skin layer, and polyethylene terephthalate without the coated nano zinc oxide is used to form a core layer. The skin-core type polyester fiber is obtained by composite melt spinning. The core-sheath type polyester fiber was sequentially reacted with an aqueous solution of tannic acid and a Fe-containing solution. 3+ The aqueous solution is contacted at least once to form tannic acid / Fe on the surface of the core-sheath type polyester fiber. 3+ The coordination layer is used to obtain the high UV absorption polyester fiber.
2. The method for preparing high ultraviolet absorption polyester fiber according to claim 1, characterized in that, Based on 100 parts by mass of the nano zinc oxide, the amount of water used is 800-1000 parts by mass, the amount of water glass used is 25-35 parts by mass, and the amount of aluminum sulfate used is 12-16 parts by mass; the SiO2 / Na2O molar modulus of the water glass is 2.1-2.3, and the SiO2 mass fraction is 26%-28%; the aluminum sulfate is Al2(SO4)3·18H2O.
3. The method for preparing high ultraviolet absorption polyester fiber according to claim 2, characterized in that, The method for forming the silicon-aluminum inorganic isolation layer includes: The nano-zinc oxide aqueous dispersion was heated to 82-88°C. First, a portion of water glass was added to adjust the pH to 8.3-8.
8. Then, the remaining water glass and aluminum sulfate aqueous solution were added over 60-90 minutes, maintaining the pH at 8.3-8.8 by adjusting the addition rate of the water glass and aluminum sulfate aqueous solution. After the addition was complete, the mixture was kept at this temperature and stirred for 40-60 minutes. Following filtration, washing, drying, and pre-dehydration, the coated nano-zinc oxide was obtained. The water washing endpoint is when the pH of the filtrate is 6.8–7.5 and the conductivity is not greater than 100 μS / cm, the pre-dehydration temperature is 250–260℃, and the D90 of the resulting coated nano zinc oxide is not greater than 300 nm.
4. The method for preparing high ultraviolet absorption polyester fiber according to claim 1, characterized in that, The modified polyethylene terephthalate is prepared by in-situ polymerization, specifically including: Terephthalic acid and the first part of ethylene glycol are esterified at 245–255°C and 0.20–0.35 MPa; the coated nano zinc oxide is dispersed in the second part of ethylene glycol to form an inorganic powder dispersion with a solid content of 15%–22%; after the water generated by esterification reaches more than 95% of the theoretical amount, the inorganic powder dispersion and polycondensation catalyst are added, and then polycondensation is carried out at 270–278°C and a final absolute pressure not exceeding 100 Pa. The total amount of ethylene glycol in the first part and the total amount of ethylene glycol in the second part, in molar ratio with terephthalic acid, is 1.20 to 1.32:
1.
5. The method for preparing high ultraviolet absorption polyester fiber according to claim 4, characterized in that, The polycondensation catalyst is antimony glycolate, and the amount of antimony glycolate added is based on 180-250 ppm of Sb element as a percentage of the theoretical mass of polyethylene terephthalate; the coated nano zinc oxide accounts for 1.10%-1.50% of the mass of the modified polyethylene terephthalate, and the intrinsic viscosity of the obtained modified polyethylene terephthalate is 0.64-0.68 dL / g.
6. The method for preparing high ultraviolet absorption polyester fiber according to claim 5, characterized in that, The intrinsic viscosity difference between the polyethylene terephthalate forming the core layer and the modified polyethylene terephthalate forming the sheath layer is no greater than 0.03 dL / g, and the moisture content before melt spinning is no higher than 30 ppm; the mass ratio of the core layer to the sheath layer is 60-70:40-30; the core-sheath type polyester fiber has a trilobal cross-section; the melt spinning temperature is 280-286℃; the high-temperature residence time of the melt does not exceed 5 min; the draw ratio is 3.2-3.6 times; and the heat setting temperature is 125-135℃.
7. The method for preparing high ultraviolet absorption polyester fiber according to claim 1, characterized in that, Formation of the tannic acid / Fe 3+ The coordination layer process includes 2 to 4 two-bath deposition cycles; each two-bath deposition cycle includes first treating the core-sheath polyester fiber with an aqueous tannic acid solution, followed by treatment with an Fe-containing solution. 3+ The core-sheath type polyester fibers were treated with an aqueous solution, and in a subsequent two-bath deposition cycle, an aqueous solution of tannic acid and Fe was used. 3+ The concentrations of the aqueous solutions were lower than those of the corresponding solutions in the previous two-bath deposition cycle.
8. The method for preparing high ultraviolet absorption polyester fiber according to claim 7, characterized in that, The two-bath deposition cycle consists of three parts: The first two-bath deposition cycle was treated with a 4.0 g / L tannic acid aqueous solution for 5 min, followed by a 1.0 g / L FeCl3·6H2O aqueous solution for 5 min. The second two-bath deposition cycle was treated with a 2.0 g / L tannic acid aqueous solution for 3 min, followed by a 0.50 g / L FeCl3·6H2O aqueous solution for 3 min. The third two-bath deposition cycle was treated with a 1.0 g / L tannic acid aqueous solution for 2 min, followed by a 0.25 g / L FeCl3·6H2O aqueous solution for 2 min.
9. The method for preparing high ultraviolet absorption polyester fiber according to claim 8, characterized in that, Before the two-bath deposition cycle, the core-sheath type polyester fiber is pre-impregnated with an ethanol aqueous solution of 20-30 wt% for 1-3 min; water washing is performed between each tannic acid aqueous solution treatment and FeCl3·6H2O aqueous solution treatment; after each two-bath deposition cycle, the fiber is dried at 65-75℃ for 2-4 min; after all two-bath deposition cycles, the fiber is dried at 75-85℃ for 8-12 min and then heat-treated at 115-125℃ for 2-4 min.
10. A high ultraviolet absorption polyester fiber, characterized in that, It is prepared by the method described in any one of claims 1 to 9 above.