A needle-woven composite fabric based on Bletilla striata hydrogel fiber and its preparation method
By preparing a needle-woven composite fabric of Bletilla striata polysaccharide chitosan hydrogel fiber, the problems of poor adhesion and single function of traditional dressings have been solved, realizing intelligent response and multifunctionality of wound exudate, and improving the mechanical properties and skin-friendliness of the dressing.
Patent Information
- Application Number
- CN202611186868.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-06
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional wound dressings suffer from poor bonding between the textile base and hydrogel, easy peeling and shedding between layers, limited functionality, insufficient mechanical strength, inability to balance support and skin-friendliness, inability to respond to the water collapse function of wound exudate, and difficulty in achieving stable loading and controllable release of active ingredients.
A water-collapse functional liquid was prepared using Bletilla striata polysaccharide, chitosan, and nano-reinforcing materials. Composite fibers were obtained through blending treatment, and Bletilla striata polysaccharide-chitosan hydrogel fibers were obtained through wet spinning. The fibers were then woven into a needle-and-machine composite fabric based on Bletilla striata hydrogel fibers.
It improves the interlayer bonding strength and stability of the dressing, enables intelligent response to wound exudate, and has synergistic effects of hemostasis, antibacterial and repair promotion. It also improves the mechanical properties and skin-friendliness of the dressing and extends its service life.
Abstract
Description
Technical Field
[0001] This invention relates to the field of functional textile materials technology, specifically to a knitted composite fabric based on Bletilla striata hydrogel fiber and its preparation method. Background Technology
[0002] Medical wound dressings are key medical materials for wound repair and care. Hydrogel dressings, due to their excellent moisturizing properties, biocompatibility, and healing-promoting abilities, have been widely used in the treatment of acute and chronic wounds. Bletilla striata polysaccharide, as a natural active ingredient, has advantages such as hemostasis, anti-inflammation, and promoting tissue repair. It is often combined with chitosan and nano-reinforcing materials to prepare hydrogels, which can further enhance the biological function and mechanical stability of the dressing.
[0003] Currently, traditional wound dressings generally suffer from structural and functional defects: ordinary textile bases have poor adhesion to hydrogels, and the layers are prone to peeling and falling off; the fibers have not undergone grafting modification and surface treatment, so they cannot provide a stable anchoring interface for the hydrogel; the dressings only have a single moisturizing or protective function, lacking a water-collapse functional layer that can respond to wound exudate, making it difficult to achieve a stable loading of active ingredients; at the same time, knitted and woven structures mostly adopt secondary composite molding, resulting in insufficient overall mechanical strength and poor fit, failing to balance support and skin-friendliness. Summary of the Invention
[0004] In view of the technical problems existing in the background art, this application provides a needle-woven composite fabric based on Bletilla striata hydrogel fiber and its preparation method. The needle-woven composite fabric based on Bletilla striata hydrogel fiber prepared by this method can improve the mechanical properties, interlayer bonding strength and use stability of dressings, realize intelligent response to wound exudate, and simultaneously exert synergistic effects of hemostasis, antibacterial and repair promotion.
[0005] To achieve the above objectives, in a first aspect, the present invention proposes a method for preparing a knitted composite fabric based on Bletilla striata hydrogel fibers, comprising:
[0006] A water-collapse functional fluid is provided, wherein the water-collapse functional fluid comprises Bletilla striata polysaccharide, chitosan, cross-linking agent and organic carboxylic acid;
[0007] At least one of spandex and acrylic fiber is blended with polyester fiber to obtain composite fiber;
[0008] A hydrogel spinning solution of Bletilla striata polysaccharide and chitosan is provided, wherein the hydrogel spinning solution comprises Bletilla striata polysaccharide, chitosan, a dispersion of nano-reinforcing materials, a crosslinking agent, an organic carboxylic acid and water;
[0009] The Bletilla striata polysaccharide-chitosan hydrogel spinning solution was wet-spun and then washed with water to obtain Bletilla striata polysaccharide-chitosan hydrogel fiber.
[0010] The composite fiber is impregnated with the water-collapse functional liquid and then hot-air treated to obtain the first yarn.
[0011] The Bletilla striata polysaccharide chitosan hydrogel fiber was impregnated with the water-slump functional liquid and then hot-air treated to obtain a second yarn;
[0012] The first yarn is woven to obtain a woven layer, and the second yarn is knitted to obtain a knitted layer. The woven layer and the knitted layer are woven together to form a knitted composite fabric based on Bletilla striata hydrogel fiber.
[0013] Furthermore, the degree of deacetylation of the chitosan is at least 85%;
[0014] And / or, the organic carboxylic acid includes at least one of acetic acid, lactic acid, and citric acid;
[0015] And / or, the crosslinking agent includes at least one of sodium tripolyphosphate, genipin, and epichlorohydrin.
[0016] Furthermore, the water-collapse functional fluid is prepared through the following steps:
[0017] Slowly add chitosan to the organic carboxylic acid solution and stir until completely dissolved;
[0018] Add Bletilla striata polysaccharide and continue stirring until the Bletilla striata polysaccharide is evenly distributed in the solution;
[0019] The crosslinking agent is slowly added to the mixture, and then stirred for a period of time to obtain the water-collapse functional liquid.
[0020] Furthermore, in the water-collapse functional liquid, the mass concentration of chitosan is 6 g / L-10 g / L;
[0021] And / or, in the water-collapse functional liquid, the mass concentration of Bletilla striata polysaccharide is 10 g / L-14 g / L;
[0022] And / or, in the water-collapse functional liquid, the mass concentration of the crosslinking agent is 2 g / L-4 g / L;
[0023] And / or, the pH of the water-collapse functional liquid is 4.5-5.0.
[0024] Further, the Bletilla striata polysaccharide-chitosan hydrogel spinning solution is prepared by the following steps:
[0025] The Bletilla striata polysaccharide was mixed with water to obtain a first mixture;
[0026] The chitosan and the organic carboxylic acid are mixed to obtain a second mixture;
[0027] The first mixture and the second mixture are mixed to obtain a polysaccharide mixture;
[0028] The dispersion of nano-reinforced materials was mixed with the polysaccharide mixture, and then a crosslinking agent was added to obtain the Bletilla striata polysaccharide chitosan hydrogel spinning solution.
[0029] Furthermore, the mass ratio of the first mixture to the second mixture is 1:(0.2-0.5);
[0030] And / or, in the first mixture, the mass concentration of the Bletilla striata polysaccharide is 38 g / L-42 g / L;
[0031] And / or, in the second mixture, the mass concentration of chitosan is 8 g / L-12 g / L;
[0032] And / or, the mass concentration of the nano-reinforced material dispersion is 8 g / L-12 g / L;
[0033] And / or, the mass ratio of the nano-reinforced material dispersion to the polysaccharide mixture is 1:(1-3);
[0034] And / or, in the Bletilla striata polysaccharide-chitosan hydrogel spinning solution, the mass concentration of the crosslinking agent is 4 g / L-6 g / L.
[0035] Furthermore, the nano-reinforced material dispersion includes at least one of montmorillonite nanosheet dispersion and nanocellulose dispersion, and the dispersion solvent of the dispersion is water.
[0036] Further, the process of blending at least one of spandex and acrylic fiber with polyester fiber to obtain composite fiber includes:
[0037] Spandex is immersed in a first modification solution to obtain modified spandex, wherein the first modification solution comprises hydroxyethyl methacrylate and an initiator;
[0038] Acrylic fiber is subjected to alkaline hydrolysis and then immersed in a second modification solution to obtain modified acrylic fiber. The second modification solution includes acrylic acid and an initiator.
[0039] Polyester fibers are subjected to alkali reduction treatment to obtain modified polyester fibers.
[0040] At least one of modified spandex and modified acrylic fiber is blended with modified polyester fiber to obtain composite fiber.
[0041] Furthermore, the initiator includes at least one of ammonium persulfate and potassium persulfate;
[0042] And / or, the alkaline hydrolysis treatment uses at least one reagent selected from sodium hydroxide, potassium hydroxide and sodium carbonate;
[0043] And / or, the alkali reduction treatment uses at least one reagent selected from sodium hydroxide, potassium hydroxide, and sodium carbonate.
[0044] Secondly, this application also provides a knitted composite fabric based on Bletilla striata hydrogel fiber, which is prepared by the above-mentioned method for preparing a knitted composite fabric based on Bletilla striata hydrogel fiber.
[0045] The beneficial effects of this application are as follows: This invention obtains composite fibers by blending polyester fibers modified and treated with alkali reduction, either spandex or acrylic fiber. Bletilla striata polysaccharide-chitosan hydrogel is wet-spun to obtain Bletilla striata polysaccharide-chitosan hydrogel fibers. Both fibers are then impregnated in a water-slumping functional solution and knitted together to obtain a knitted composite fabric based on Bletilla striata hydrogel fibers. This fabric achieves the desired combination of interlayer bonding strength, hemostasis, antibacterial activity, and good skin affinity and mechanical properties, making it suitable for the care and repair of various wounds.
[0046] This invention employs an integrated knitted and woven structure, combining the skin-friendly fit of the knitted layer with the support and shaping of the woven layer, thus improving tensile strength and solving the problem of existing dressings struggling to balance fit and stability. By hydrophilic grafting modification of spandex, alkali hydrolysis modification of acrylic fibers, and alkali reduction treatment of polyester fibers, the bonding force between the hydrogel and the substrate interface is improved, the hydrogel shedding rate is reduced, and the dressing's lifespan is extended. The dressing of this invention has a high saturated water absorption rate, which can quickly absorb wound exudate and maintain a moist healing environment, reducing the frequency of dressing changes. Simultaneously, the Bletilla striata polysaccharide-chitosan system is optimized, significantly improving antibacterial rate and cell proliferation rate while meeting biocompatibility requirements. Through precise design, synergistic optimization of function and performance is achieved. Nano-reinforcing materials are introduced into the Bletilla striata polysaccharide-chitosan hydrogel fibers, improving the tensile strength and elongation at break of the hydrogel fibers, balancing strength and flexibility to adapt to the dynamic stress requirements of complex wounds. Detailed Implementation
[0047] Medical wound dressings are key medical materials for wound repair and care. Hydrogel dressings, due to their excellent moisturizing properties, biocompatibility, and healing-promoting abilities, have been widely used in the treatment of acute and chronic wounds. Bletilla striata polysaccharide, as a natural active ingredient, has advantages such as hemostasis, anti-inflammation, and promoting tissue repair. It is often combined with chitosan and nano-reinforcing materials to prepare hydrogels, which can further enhance the biological function and mechanical stability of the dressing.
[0048] Currently, traditional wound dressings generally suffer from structural and functional defects: ordinary textile bases have poor adhesion to hydrogels, and the layers are prone to peeling and falling off; textile fibers have not undergone grafting modification and surface treatment, so they cannot provide a stable anchoring interface for hydrogels; dressings only have a single moisturizing or protective function, lacking a water-collapse functional layer that can respond to wound exudate, making it difficult to achieve stable loading and controllable release of active ingredients; at the same time, knitted and woven structures mostly adopt secondary composite molding, resulting in insufficient overall mechanical strength and poor fit, failing to balance support and skin-friendliness.
[0049] To address the aforementioned technical problems, this application provides a knitted composite fabric based on Bletilla striata hydrogel fiber and its preparation method, comprising:
[0050] A water-collapse functional fluid is provided, wherein the water-collapse functional fluid comprises Bletilla striata polysaccharide, chitosan, cross-linking agent and organic carboxylic acid;
[0051] At least one of spandex and acrylic fiber is blended with polyester fiber to obtain composite fiber;
[0052] A hydrogel spinning solution of Bletilla striata polysaccharide and chitosan is provided, wherein the hydrogel spinning solution comprises Bletilla striata polysaccharide, chitosan, a dispersion of nano-reinforcing materials, a crosslinking agent, an organic carboxylic acid and water;
[0053] The Bletilla striata polysaccharide-chitosan hydrogel spinning solution was wet-spun and then washed with water to obtain Bletilla striata polysaccharide-chitosan hydrogel fiber.
[0054] The composite fiber is impregnated with the water-collapse functional liquid and then hot-air treated to obtain the first yarn.
[0055] The Bletilla striata polysaccharide chitosan hydrogel fiber was impregnated with the water-slump functional liquid and then hot-air treated to obtain a second yarn;
[0056] The first yarn is woven to obtain a woven layer, and the second yarn is knitted to obtain a knitted layer. The woven layer and the knitted layer are woven together to form a knitted composite fabric based on Bletilla striata hydrogel fiber.
[0057] In the technical solution of this application, a composite fiber is prepared by blending polyester fibers that have been modified and treated with alkali reduction, either spandex or acrylic fiber. Bletilla striata polysaccharide-chitosan hydrogel is then wet-spun to obtain Bletilla striata polysaccharide-chitosan hydrogel fibers. Both fibers are then impregnated in a water-slump functional solution and knitted together on a needle-woven machine to obtain a needle-woven composite fabric based on Bletilla striata hydrogel fibers. This achieves the desired combination of interlayer bonding strength, hemostatic and antibacterial activity, as well as good skin affinity and mechanical properties.
[0058] It can be explained that a water-collapse functional fluid is provided, which includes Bletilla striata polysaccharide, chitosan, a cross-linking agent, and organic carboxylic acids. Bletilla striata polysaccharide, as the main active ingredient in the water-collapse functional fluid, provides hemostatic, anti-inflammatory, and healing-promoting effects; the molecular chain of Bletilla striata polysaccharide is rich in hydroxyl groups, which can participate in cross-linking reactions, and it also has good film-forming and moisturizing properties. Chitosan is a cationic polysaccharide, which, as a skeletal reinforcing material, forms a complex network with Bletilla striata polysaccharide through electrostatic interactions or hydrogen bonds. Chitosan also has antibacterial functions and synergistic effects with the hemostatic and anti-inflammatory properties of Bletilla striata polysaccharide. The cross-linking agent forms covalent bonds between the molecular chains of Bletilla striata polysaccharide and chitosan, cross-linking the linear molecular chains into a three-dimensional hydrogel structure, improving the shape stability of the fibers in water or physiological environments. Chitosan needs to dissolve in an acidic environment; organic carboxylic acids are milder than inorganic acids, have less destructive effect on polysaccharide activity, and have a certain antibacterial auxiliary effect.
[0059] It can be explained that a composite fiber is obtained by blending at least one of spandex and acrylic fibers with polyester fibers. Spandex provides high elasticity and resilience, acrylic fibers impart a fluffy and soft feel, and polyester fibers provide high strength, heat resistance, and dimensional stability. Through blending, a composite fiber with multiple properties such as elasticity, softness, strength, and dimensional stability can be obtained.
[0060] It can be explained that a Bletilla striata polysaccharide-chitosan hydrogel spinning solution is provided. This solution comprises Bletilla striata polysaccharide, chitosan, a nano-reinforcing material dispersion, a crosslinking agent, an organic carboxylic acid, and water. The organic carboxylic acid provides an acidic environment, causing the chitosan to protonate and dissolve. Both the amino groups of chitosan and the hydroxyl groups of Bletilla striata polysaccharide can react with the crosslinking agent to form a crosslinked network. After crosslinking, the hydrogel stably swells and forms a hydrogel. Furthermore, the pore structure is uniform and controllable, facilitating subsequent anchoring of functional molecules. The spinning solution prepared using this formulation is environmentally friendly, with mild processing conditions, and retains the bioactivity of both Bletilla striata polysaccharide and chitosan. The mechanical strength, swelling degree, and degradation rate of the fiber can be adjusted by changing the type and amount of the crosslinking agent to meet different application requirements. The resulting fiber combines the healing and hemostatic effects of Bletilla striata polysaccharide with the antibacterial and wet adhesion capabilities of chitosan, making it suitable for the biomedical field.
[0061] It can be explained that the Bletilla striata polysaccharide-chitosan hydrogel spinning solution is wet-spun and then washed with water to obtain Bletilla striata polysaccharide-chitosan hydrogel fibers. Wet spinning is used, with the air pressure at the spinneret controlled at 0.3MPa-0.5MPa and the spinneret orifice diameter at 0.15mm-0.2mm. The air pressure of 0.3MPa-0.5MPa is within a moderate pressurization range, which can overcome spinneret resistance and facilitate the continuous outflow of the spinning solution, thereby obtaining nascent fine streams with uniform diameter and smooth surface. The small orifice diameter of the 0.15mm-0.2mm spinneret limits the initial diameter range of the fibers, and the final Bletilla striata polysaccharide hydrogel fibers generally have a diameter of 100µm-200µm, suitable for subsequent weaving. Small-diameter fibers have a large specific surface area, which can improve the absorption rate and loading capacity of the water-slump functional liquid. The spinning solution is fed into a coagulation bath to solidify and form the fiber. The coagulation bath consists of deionized water and 5% ethanol (by volume). The temperature of the coagulation bath is 25±2℃, and the coagulation time is 30-40 seconds. A pure water coagulation bath would cause the fiber surface to solidify instantly, preventing the internal solvent from diffusing and resulting in large pores or even cracks. Adding a trace amount of ethanol results in a moderate coagulation rate and intact fiber cross-section. The coagulation bath temperature of 25±2℃ is a mild room temperature condition, which allows for appropriate control of the coagulation rate and protects the fiber structure, ensuring its stability and integrity. The 30-40 second coagulation time allows the spinning solution to fully diffuse into the coagulation bath, and the fiber core can also be completely solidified. The solidified nascent fiber is then drawn out by a traction roller with a linear speed of 1.0-1.2 m / min. A traction speed of 1.0 m / min-1.2 m / min applies slight stretching to the fibers, aligning the Bletilla striata polysaccharide macromolecular chains along the fiber axis, improving breaking strength and initial modulus, and facilitating subsequent washing, drying, and weaving processes. A constant traction speed combined with stable extrusion helps maintain a uniform fiber structure. The drawn fibers are then washed with pure water twice, each wash lasting 15-20 seconds. These two short washes remove ethanol from the coagulation bath and residual solvents from the spinning solution, improving fiber purity and reducing chemical residues. The fibers are then dried at an air velocity of 0.6 m / s for 15 minutes, followed by low-ratio stretching and setting at 3%-5%. Hot air drying preserves the internal micropores of the fibers, while stretching and setting eliminates internal stress. This yields Bletilla striata polysaccharide hydrogel fibers.
[0062] It can be explained that the composite fiber is impregnated with the water-slump functional liquid and then hot-air treated to obtain the first yarn. The composite fiber is passed through the functional liquid impregnation tank at a speed of 0.5 m / min, and the impregnation time is controlled at 30-60 s to ensure that the functional liquid fully penetrates into the fiber pores, resulting in a more uniform functional liquid load and a more stable water-slump response. The impregnated fiber is placed in a hot air treatment chamber and subjected to hot air cross-linking and curing at 80℃ and a wind speed of 0.6-0.8 m / s, so that the Bletilla striata polysaccharide-chitosan forms hydrogen bonds and ionic bonds with the hydroxyl / amino groups on the fiber surface, anchoring the functional components. The hot-air treated fiber is naturally cooled for 10 minutes in an environment with room temperature and 40%-50% humidity to stabilize the cross-linked structure and prevent the functional liquid from falling off. Then, a slight stretching of 5% is performed to maintain the fiber shape, finally obtaining the first yarn loaded with functional liquid.
[0063] It can be explained that the second yarn is obtained by impregnating the Bletilla striata polysaccharide-chitosan hydrogel fiber with the water-slump functional liquid followed by hot air treatment. Impregnating the Bletilla striata polysaccharide-chitosan hydrogel fiber in the water-slump functional liquid for 30-60 seconds, followed by hot air treatment at 80°C for 20 minutes, allows the functional liquid to anchor in the fiber pores, improving the structural strength and water resistance of the cross-linked network. The porous structure can regulate the release rate of the functional liquid, thereby improving healing efficiency.
[0064] It can be explained that the first yarn is woven to obtain a woven layer, and the second yarn is knitted to obtain a knitted layer. The woven layer and the knitted layer are integrally woven to form a knitted-knitted composite fabric based on Bletilla striata hydrogel fibers. The woven surface is fed with the first yarn via 2-3 yarn feeders, using a plain weave; the knitted surface is fed with the second yarn via 3 yarn feeders, using a tight weave. The weaving and knitting speeds are controlled at 0.8-1.0 m / min, with knitting at 16-20 stitches / inch and weaving at 10-14 stitches / inch, and the yarn tension at 5-8 cN (knitting) and 12-15 cN (weaving). The woven surface forms the fabric skeleton, providing strength and stability. Due to the presence of spandex, acrylic, and polyester elastic yarns, a speed of 0.8-1.0 m / min allows for more uniform interweaving between yarns, reducing uneven or fluctuating yarn tension and mitigating pilling or breakage caused by friction between the yarn and high-speed moving parts. Controlling the weaving density to 10-14 stitches / inch creates space between yarns, facilitating the formation of a stable interlacing structure. Maintaining the feed tension at 12-15 cN provides tension to straighten the yarns, ensuring clear and stable openings during weaving and creating favorable conditions for weft insertion. The knitted surface offers comfortable, soft, and skin-friendly properties. Adopting a weaving speed consistent with the woven surface (0.8-1.0 m / min) reduces the high temperatures and friction generated by high-speed yarn movement, minimizing damage to the hydrogel network structure. A knitting density of 18 stitches / inch allows for the formation of small, dense loops, resulting in a soft and delicate feel. Controlling the knitting feed tension at 5-8 cN protects the fiber structure during loop formation, reducing breakage caused by excessive stretching and promoting the formation of a soft loop structure.
[0065] After the greige fabric is woven, it undergoes hot air setting at a temperature of 75-80℃ and an air velocity of 0.6-0.8 m / s for 20-30 minutes. This hot air setting of the blended yarns on the woven surface locks in the support layer structure, preventing later shrinkage. Controlling the hot air setting temperature to 75-80℃, lower than the traditional heat setting temperatures for spandex, acrylic, and polyester fiber fabrics, protects the physical and chemical stability of the Bletilla striata polysaccharide hydrogel fibers. Setting at an air velocity of 0.6-0.8 m / s for 20-30 minutes provides a long-term, gentle treatment that reduces internal stress generated during weaving in both the woven and knitted surfaces, while also slowly and evenly drying moisture in the hydrogel areas. The result is a dimensionally stable composite fabric with intact hydrogel functionality.
[0066] In some embodiments, the degree of deacetylation of chitosan is at least 85%.
[0067] In this embodiment, the deacetylated chitosan is introduced with an amino group (-NH2), which is then converted into a protonated amino group (-NH3) in acid. +This process imparts a positive charge to chitosan, making it soluble in acidic aqueous solutions. The positively charged chitosan, after dissolution, can adsorb negatively charged substances, such as bacterial cell walls, lipids, and heavy metal anions, through electrostatic interactions. This is the core source of its antibacterial function. A degree of deacetylation of 85% or higher facilitates the dissolution of chitosan in acidic aqueous solutions, reducing insoluble residues.
[0068] In some embodiments, organic carboxylic acids include at least one of acetic acid, lactic acid, and citric acid.
[0069] In this embodiment, the organic carboxylic acid includes at least one of acetic acid, lactic acid, and citric acid. Organic carboxylic acids provide hydrogen ions, protonating and dissolving chitosan, and are non-toxic, making them suitable for biomedical applications. Acetic acid effectively acidifies solutions; acetate ions maintain chitosan activity and are volatile, facilitating subsequent neutralization and regeneration of chitosan, making them a commonly used chitosan solvent. Lactic acid is stronger than acetic acid, is a natural metabolite in the human body, and has good biocompatibility. Lactate ions can form hydrogen bonds, helping to stabilize chitosan solutions, and are often used in biomedical materials. Citric acid is a tribasic acid that provides multiple hydrogen ions, has strong dissolving power, and possesses antioxidant and chelating properties, making it suitable as a food or pharmaceutical carrier.
[0070] In some embodiments, the crosslinking agent includes at least one of sodium tripolyphosphate, genipin, and epichlorohydrin.
[0071] In this embodiment, the crosslinking agent can transform a flowing polymer solution into a viscoelastic solid gel. The crosslinking density affects the gel's hardness, toughness, and elasticity. The covalent or ionic bonds formed by the crosslinking agent firmly lock the chains together, helping to maintain the complete three-dimensional network structure of the polysaccharide molecules, improving mechanical properties, and enabling it to stably cover wounds and absorb exudate as a dressing. After the crosslinking agent connects the polysaccharide molecular chains, it increases their resistance to enzymatic degradation. The crosslinked network can bind a large amount of water, thereby providing a continuous moist environment and functional support for tissue repair. Sodium tripolyphosphate mainly binds to chitosan molecular chains through electrostatic interactions, with mild action conditions, protecting the activity of functional components. Multiple active sites of genipin covalently bond with the amino groups on chitosan. Genipin is naturally extracted, has good biocompatibility, low cytotoxicity, and is suitable for the field of biomedical dressings. The epoxy groups in epichlorohydrin undergo etherification with the hydroxyl groups of the polysaccharide under alkaline conditions, forming stable covalent bonds that are not easily hydrolyzed, resulting in strong gel strength and resistance to degradation.
[0072] In some embodiments, the water-collapse functional fluid is prepared by the following steps:
[0073] Slowly add chitosan to the organic carboxylic acid solution and stir until completely dissolved;
[0074] Add Bletilla striata polysaccharide and continue stirring until the Bletilla striata polysaccharide is evenly distributed in the solution;
[0075] The crosslinking agent is slowly added to the mixture, and then stirred for a period of time to obtain the water-collapse functional liquid.
[0076] In this embodiment, after deacetylation treatment, chitosan acquires amino groups and forms protonated amino groups in an acidic solution, thereby dissolving and exerting its antibacterial properties. After dispersion, Bletilla striata polysaccharide forms a composite network with chitosan and provides hemostatic and anti-inflammatory effects. The crosslinking agent enables covalent bonds to be formed between the Bletilla striata polysaccharide and chitosan molecular chains, crosslinking the linear molecular chains into a three-dimensional hydrogel structure.
[0077] In some embodiments, the mass concentration of chitosan in the water-collapse functional fluid is 6 g / L-10 g / L.
[0078] In this embodiment, by controlling the chitosan concentration in the water-collapse functional liquid to be 6 g / L-10 g / L, a dense gel network can be formed, maintaining structural integrity while absorbing liquid. Chitosan at this concentration exhibits ideal antibacterial function. The chitosan solution at this concentration has a reasonable viscosity, complementing the concentration of Bletilla striata polysaccharide. Bletilla striata polysaccharide provides the basis for bioactivity, while chitosan at this concentration provides skeletal support and antibacterial function; the two work synergistically.
[0079] In some embodiments, the mass concentration of Bletilla striata polysaccharide in the water-collapse functional liquid is 10 g / L-14 g / L.
[0080] In this embodiment, by controlling the mass concentration of Bletilla striata polysaccharide in the water-collapse functional fluid to 10 g / L-14 g / L, the hemostatic and antibacterial activities of Bletilla striata polysaccharide can be exerted. Increased concentration leads to more entanglement and cross-linking points between Bletilla striata polysaccharide molecular chains, resulting in a more stable network structure. Improved gel strength and adhesion provide a foundation for the subsequent construction of the water-collapse system of the functional fluid.
[0081] In some embodiments, the mass concentration of the crosslinking agent in the water-collapse functional liquid is 2 g / L-4 g / L.
[0082] In this embodiment, by controlling the mass concentration of the cross-linking agent in the water-collapse functional fluid to 2 g / L-4 g / L, a network structure with low cross-linking degree and sparse cross-linking points can be formed. The limited number of cross-linking agent molecular linkages results in a loose network structure, and the resulting pores are conducive to cell growth and proliferation. High swelling degree enhances the water-collapse system's ability to absorb liquid. Soft, high-moisture dressings provide an ideal moist healing environment.
[0083] In some embodiments, the pH of the water-collapse functional fluid is 4.5-5.0.
[0084] In this embodiment, the pH of the water-collapse functional solution is controlled at 4.5-5.0. Chitosan needs to be dissolved in an acidic environment with a pH value below 6.5. A slightly acidic environment with a pH of 4.5-5.0 effectively converts the amino groups in the deacetylated chitosan molecules into positively charged protonated amino groups, thus dissolving them in the acidic aqueous solution. The dissolved chitosan continues to undergo electrostatic cross-linking reactions, exerting its antibacterial effect. The viscosity of Bletilla striata polysaccharide decreases in an alkaline environment, while a slightly acidic environment with a pH of 4.5-5.0 protects the activity of Bletilla striata polysaccharide.
[0085] In some embodiments, the Bletilla striata polysaccharide-chitosan hydrogel spinning solution is prepared by the following steps:
[0086] The Bletilla striata polysaccharide was mixed with water to obtain a first mixture;
[0087] The chitosan and the organic carboxylic acid are mixed to obtain a second mixture;
[0088] The first mixture and the second mixture are mixed to obtain a polysaccharide mixture;
[0089] The dispersion of nano-reinforced materials was mixed with the polysaccharide mixture, and then a crosslinking agent was added to obtain the Bletilla striata polysaccharide chitosan hydrogel spinning solution.
[0090] In this embodiment, Bletilla striata polysaccharide is a neutral polysaccharide, readily soluble in water, and has high viscosity. Pre-dispersion in deionized water improves the uniformity of the Bletilla striata polysaccharide solution and enhances the efficiency of the spinning solution preparation process. Chitosan is insoluble in water; after deacetylation, it acquires amino groups that form protonated amino groups in acidic solutions, thereby dissolving and exerting its antibacterial properties. Thoroughly dissolving and mixing Bletilla striata polysaccharide and chitosan separately yields a macroscopically homogeneous viscous solution, facilitating adjustment of the final total concentration and meeting the uniformity requirements of subsequent spinning. While Bletilla striata polysaccharide and chitosan provide hemostatic and antibacterial activity, their mechanical properties are insufficient; they swell significantly after water absorption, making it difficult to maintain structural strength, and the spinnability of the solution needs improvement. Nanomaterials can compensate for the lack of mechanical strength in the polysaccharide mixture, improving the mechanical strength and swelling stability of the hydrogel. Adding a crosslinking agent can form a stable dynamic crosslinking network while ensuring the spinnability of the spinning solution.
[0091] In some embodiments, the mass ratio of the first mixture and the second mixture is 1:(0.2-0.5).
[0092] In this embodiment, the first mixture is an aqueous solution of Bletilla striata polysaccharide, and the second mixture is a chitosan acid solution. By controlling the mass ratio of the Bletilla striata polysaccharide aqueous solution to the chitosan acid solution to 1:(0.2-0.5), a uniform and dense structure can be formed, and the mechanical properties and stability of the material can be synergistically regulated by the molecules. Moreover, at this ratio, the synergistic efficiency of hemostatic and antibacterial activities is high, which is conducive to giving full play to the respective advantages of Bletilla striata polysaccharide and chitosan.
[0093] In some embodiments, the mass concentration of Bletilla striata polysaccharide in the first mixture is 38 g / L-42 g / L.
[0094] In this embodiment, by controlling the mass concentration of Bletilla striata polysaccharide in the first mixture to be 38 g / L-42 g / L, the viscosity is moderate, which can cause the molecular chains of Bletilla striata polysaccharide to physically entangle, achieve a certain mechanical strength, and at the same time maintain rheological properties, which is beneficial to the continuity and stability of the spinning process.
[0095] In some embodiments, the mass concentration of chitosan in the second mixture is 8 g / L-12 g / L.
[0096] In this embodiment, controlling the chitosan concentration in the second mixture to be 8 g / L-12 g / L ensures the solution has suitable viscosity and good flowability, which is crucial for stable spinning. Since a certain concentration of Bletilla striata polysaccharide already exists in the spinning solution, controlling the overall concentration of the spinning solution by adjusting the chitosan concentration is key to achieving synergistic effects between chitosan and Bletilla striata polysaccharide.
[0097] In some embodiments, the mass concentration of the nano-reinforced material dispersion is 8 g / L-12 g / L.
[0098] In this embodiment, by controlling the mass concentration of the nano-reinforcing material dispersion to be 8 g / L-12 g / L, the nano-reinforcing material can form a stable dispersion existing in the form of individual nanoparticles or small aggregates. A good dispersion state facilitates subsequent uniform mixing with the polysaccharide, and a suitable concentration allows for the introduction of sufficient nano-reinforcing material while limiting the dilution effect on the original polysaccharide system, thus helping to maintain the concentrations of Bletilla striata polysaccharide and chitosan in the spinning solution.
[0099] In some embodiments, the mass ratio of the nano-reinforced material dispersion to the polysaccharide mixture is 1:(1-3).
[0100] In this embodiment, by controlling the mass ratio of the nano-reinforcing material dispersion to the polysaccharide mixture to 1:(1-3), the rigid framework provided by the nano-reinforcing material can withstand and transmit stress, thereby improving strength. The polysaccharide fills the voids and transmits stress. The synergistic effect enables the tensile strength and toughness of the material to be improved simultaneously. At this ratio, a balance can be achieved between the mechanical reinforcement effect, spinnability, and bioactivity of the spinning solution.
[0101] In some embodiments, the mass concentration of the crosslinking agent in the Bletilla striata polysaccharide-chitosan hydrogel spinning solution is 4 g / L-6 g / L.
[0102] In this embodiment, by controlling the mass concentration of the crosslinking agent in the Bletilla striata polysaccharide-chitosan hydrogel spinning solution to 4 g / L-6 g / L, a network with a high degree of crosslinking and dense crosslinking points can be formed, thereby improving mechanical strength. The crosslinking agent molecules form a tight chemical bond network, restricting molecular chain movement and enhancing structural rigidity. Low swelling degree helps maintain the stable structure of the fiber and enhances its resistance to deformation.
[0103] In some embodiments, the nano-reinforced material dispersion includes at least one of montmorillonite nanosheet dispersion and nanocellulose dispersion, and the dispersion solvent is water.
[0104] In this embodiment, the nano-reinforcing material dispersion includes at least one of montmorillonite nanosheet dispersion and nanocellulose dispersion. Montmorillonite nanosheets are natural rigid layered silicates, and nanocellulose is a natural polymer fiber with high aspect ratio and high specific surface area. Both materials exhibit good biocompatibility.
[0105] In some embodiments, at least one of spandex and acrylic fiber is blended with polyester fiber to obtain composite fiber, including:
[0106] Spandex is immersed in a first modification solution to obtain modified spandex. The first modification solution includes hydroxyethyl methacrylate and an initiator.
[0107] After treating the acrylic fiber with an alkaline hydrolysis reagent, it is immersed in a second modification solution to obtain modified acrylic fiber. The first modification solution includes acrylic acid and an initiator.
[0108] Polyester fibers are treated with an alkaline hydrolysis reagent to obtain modified polyester fibers;
[0109] At least one of modified spandex and modified acrylic fiber is blended with modified polyester fiber to obtain composite fiber.
[0110] In this embodiment, at least one of spandex and acrylic fiber is used as the base fiber, and polyester fiber is used as the reinforcing fiber. Spandex has high elasticity and is soft and smooth, but it is difficult to weave alone. Acrylic fiber is fluffy, soft, and skin-friendly, but its moisture absorption is generally poor. Polyester fiber is high-strength, wrinkle-resistant, and crisp, but its moisture absorption is generally poor. Combining at least one of spandex and acrylic fiber with polyester fiber can combine their excellent properties and give full play to the advantages of each fiber.
[0111] In this embodiment, the spandex is modified by introducing hydrophilic side chains with active hydroxyl groups, which improves the hydrophilicity of the spandex surface and enhances the interfacial bonding force with the hydrogel, thus facilitating the stable bonding with the water-collapse functional fluid in the subsequent process.
[0112] In this embodiment, the acrylonitrile fiber undergoes alkaline hydrolysis modification. The hydrophobic cyano groups of the acrylonitrile fiber are first hydrolyzed into amide groups, and then further converted into strongly hydrophilic carboxyl groups, increasing the surface free energy of the acrylonitrile fiber. The alkaline-hydrolyzed acrylonitrile fiber is then grafted, with acrylic monomers linked to the active sites of the acrylonitrile fiber under the action of an initiator, forming polyacrylic acid side chains, further enhancing hydrophilicity. The modified acrylonitrile fiber achieves hydrogen / ionic bonding with the hydrogel through hydrophilic modification, enhancing interlayer adhesion and simultaneously possessing drug-carrying and antibacterial functions.
[0113] In this embodiment, the polyester fibers undergo alkali reduction treatment, forming a micro-nano rough structure on the fiber surface, which enhances their anchoring ability with the water-collapse system. The polyester fibers are treated with a 30 g / L NaOH solution at 95°C for 40 minutes, achieving a weight reduction rate of 8% ± 0.5%. This process creates a micro-nano rough structure on the fiber surface, further improving their anchoring ability with the water-collapse system. The polyester fibers enhance structural stability and mechanical properties.
[0114] In this embodiment, the spandex yarn twist is adjusted to 80-90 twists / 10cm, achieving a breaking strength retention rate of over 92%. The acrylic yarn twist is adjusted to 80-90 twists / 10cm to ensure smooth yarn feeding. The polyester fiber yarn twist is adjusted to 110-130 twists / 10cm, enhancing the structural stability and mechanical properties of the polyester fiber.
[0115] In some embodiments, the initiator includes at least one of ammonium persulfate and potassium persulfate.
[0116] In this embodiment, the initiator includes at least one of ammonium persulfate and potassium persulfate. Ammonium persulfate and potassium persulfate are inorganic peroxide initiators, soluble in water, and generate sulfate free radicals that can be used in aqueous systems.
[0117] In some embodiments, the alkaline hydrolysis reagent includes at least one of sodium hydroxide, potassium hydroxide, and sodium carbonate.
[0118] In this embodiment, the alkaline hydrolysis reagent includes at least one of sodium hydroxide, potassium hydroxide, and sodium carbonate.
[0119] Sodium hydroxide, potassium hydroxide, and sodium carbonate all provide hydroxide ions in water. These hydroxide ions are crucial for attacking the cyano groups in acrylic fibers and the ester bonds in polyester fibers. Sodium hydroxide and potassium hydroxide are strong bases and are highly efficient alkaline hydrolysis reagents. Sodium carbonate has a milder effect, causing less damage to fibers, and can be used for gentle modification.
[0120] Secondly, embodiments of this application also provide a knitted composite fabric based on Bletilla striata hydrogel fiber, which is prepared by the above-described method for preparing a knitted composite fabric based on Bletilla striata hydrogel fiber.
[0121] It is understood that the knitted composite fabric based on Bletilla striata hydrogel fiber has all the beneficial effects of all the above-mentioned embodiments of the preparation method of knitted composite fabric based on Bletilla striata hydrogel fiber, and will not be repeated here.
[0122] The following are some specific embodiments. It should be noted that the embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially.
[0123] I. Preparation Method
[0124] Example 1
[0125] (1) Preparation of water collapse functional liquid: Weigh 0.8g of chitosan and add it to 100mL of acetic acid solution with a volume fraction of 1%. Stir until completely dissolved, add 1.2g of Bletilla striata polysaccharide, and continue stirring until the Bletilla striata polysaccharide is evenly dispersed in the solution. Slowly add 0.3g of sodium tripolyphosphate as a crosslinking agent and stir evenly to obtain a water collapse functional liquid with a pH of 4.5.
[0126] (2) Preparation of composite fiber: Take 10g of spandex fiber with a fineness of 20D, add 100mL of deionized water, and then add 1g of hydroxyethyl methacrylate (HEMA) monomer. Stir and purge with nitrogen for 30min to remove oxygen, and then add 0.02g of ammonium persulfate (APS). Heat the reaction system to 60℃ and stir at a constant temperature for 2h. After the reaction is completed, take out the fiber, wash it three times with deionized water and three times with anhydrous ethanol, and dry it in a vacuum drying oven at 60℃ until constant weight to obtain modified spandex.
[0127] Take 10g of 30D acrylic fiber and add 100mL of 5% sodium hydroxide solution. Place the beaker in a constant temperature water bath, heat to 70℃, maintain the temperature for 30min and stir. After the reaction, remove the acrylic fiber and wash it three times each with deionized water, 0.5% acetic acid solution, and deionized water until the washing solution is neutral. Place the washed acrylic fiber in a vacuum drying oven at 60℃ and dry to constant weight to obtain alkali-hydrophilicated acrylic fiber. Take the above alkali-pretreated acrylic fiber and add 100mL of deionized water, then add 5g of acrylic acid (AA) monomer, stir and purge with nitrogen to remove oxygen for 30min, then add 0.02g of ammonium persulfate (APS). Heat the reaction system to 70℃ and stir for 2h. After the reaction, remove the fiber and wash it three times each with deionized water and anhydrous ethanol, then dry it in a vacuum drying oven at 60℃ to constant weight to obtain acrylic acid grafted modified acrylic fiber.
[0128] Take 10g of 50D polyester fiber and add it to 100mL of 3% sodium hydroxide solution. Place the beaker in a constant temperature water bath, heat to 95℃, and maintain the temperature for 40min while stirring. After treatment, remove the fiber and wash it three times each with deionized water, 0.5% acetic acid solution, and deionized water until the washing solution is neutral. Place the fiber in an 80℃ vacuum drying oven and dry to constant weight to obtain alkali-reduced modified polyester fiber.
[0129] The three modified fibers were blended in a ratio of 4:3:3 to obtain composite fibers.
[0130] (3) Preparation of Bletilla striata polysaccharide-chitosan hydrogel fibers:
[0131] Add ≥92% purity Bletilla striata polysaccharide to deionized water to prepare a 40 g / L Bletilla striata polysaccharide solution, and stir at 300 rpm for 1.5 h at 45℃ until completely dissolved.
[0132] Take chitosan with a degree of deacetylation ≥ 85% and add it to a 1% acetic acid solution to prepare a 10 g / L chitosan solution. Stir at 200 rpm for 1 hour at 37°C until completely dissolved.
[0133] The chitosan solution was slowly added to the Bletilla striata polysaccharide solution at a mass ratio of 1:5, and stirred at 250 rpm for 30 min at 45°C.
[0134] Montmorillonite nanosheets with a diameter of 100-200 nm were dispersed in deionized water to prepare a 10 g / L montmorillonite nanosheet dispersion. The dispersion was stirred at 600 rpm for 30 min and then sonicated at 300 W for 20 min.
[0135] The montmorillonite dispersion was slowly added dropwise to the polysaccharide mixture at a mass ratio of 1:3. The mixture was stirred at 200 rpm for 1 hour at 45°C and then sonicated for 15 minutes.
[0136] Sodium tripolyphosphate was added to the mixture after ultrasonic treatment to achieve a concentration of 4 g / L. The mixture was stirred at 150 rpm for 20 min at 30°C.
[0137] Wet spinning was employed, with the air pressure at the spinneret set at 0.3 MPa and the spinneret diameter at 0.15 mm. The coagulation bath consisted of deionized water and 5% ethanol (by volume), and coagulation was carried out at 25°C for 30 seconds. The traction roller speed was 1.0 m / min, and the fibers were washed twice with water for 15 seconds each time. The fibers were then dried at 60°C with an air velocity of 0.6 m / s for 15 minutes, followed by 3% low-ratio stretching and setting to obtain Bletilla striata polysaccharide-chitosan hydrogel fibers.
[0138] (4) Preparation of the first and second yarns: The composite fiber is passed through the functional liquid impregnation tank at a speed of 0.5 m / min, and the impregnation time is controlled at 30 s; the impregnated composite fiber is placed in a hot air treatment box and cross-linked and cured by hot air at 80℃ and wind speed of 0.6 m / s; then it is cooled for 10 min in an environment with room temperature and 40% humidity. Then it is slightly stretched by 5% stretch rate to maintain the fiber shape, and finally the first yarn loaded with functional liquid is obtained.
[0139] The Bletilla striata polysaccharide chitosan fiber was immersed in a water-slump functional liquid for 30-60 seconds, and then treated with hot air at 80℃ for 20 minutes to obtain a second yarn loaded with functional liquid.
[0140] (5) Preparation of composite fabric with water collapse function: The second yarn is connected to the needle bed (knitted surface) of the knitting machine and fed evenly using a 3-way yarn feeder. The knitting density is controlled at 18 needles / inch, the yarn tension is 5cN, and the knitting speed is 0.8m / min. A single-layer knitted skin-friendly base is formed, ensuring that there are no gaps in the fiber distribution.
[0141] The first yarn is fed into the lower needle bed (woven surface) of the knitting machine using a three-way yarn feeder, controlling the weaving density at 12 stitches / inch, the yarn tension at 12 cN, and the weaving speed at 0.8 m / min. The fabric is then formed in one pass through a double-sided jacquard weave to obtain a knitting-woven composite fabric. After weaving, the fabric is hot-air set for 20 minutes at 75℃ and an air velocity of 0.6 m / s to lock the support layer structure, resulting in a composite fabric with water-slump functionality.
[0142] Example 2
[0143] Unlike Example 1, when preparing the water-collapse functional liquid, 1g of Bletilla striata polysaccharide and 1g of chitosan were weighed out. The remaining steps are roughly the same and will not be repeated here.
[0144] Example 3
[0145] Unlike Example 1, the pH of the water collapse functional liquid is 5.0. The remaining steps are roughly the same and will not be described again here.
[0146] Example 4
[0147] Unlike Example 1, lactic acid was used instead of acetic acid in the organic carboxylic acid. The remaining steps are roughly the same and will not be repeated here.
[0148] Example 5
[0149] Unlike Example 1, genipin was used instead of sodium tripolyphosphate as the crosslinking agent. The remaining steps are roughly the same and will not be described in detail here.
[0150] Example 6
[0151] Unlike Example 1, when preparing the Bletilla striata polysaccharide-chitosan spinning solution, the concentration of the Bletilla striata polysaccharide solution was 42 g / L, the concentration of the chitosan solution was 12 g / L, and the mass ratio of the Bletilla striata polysaccharide solution to the chitosan solution was 2:1. The remaining steps were roughly the same and will not be described in detail here.
[0152] Example 7
[0153] Unlike Example 1, when preparing the Bletilla striata polysaccharide-chitosan spinning solution, the mass ratio of the polysaccharide solution to the montmorillonite nano-dispersion was controlled at 1:1. The remaining steps were roughly the same and will not be described in detail here.
[0154] Example 8
[0155] Unlike Example 1, the modification time for spandex was 2.2 h and the modification temperature was 65 °C; the alkali hydrolysis time for acrylic fiber was 35 min and the modification temperature was 95 °C; the alkali reduction treatment temperature for polyester fiber was 100 °C and the alkali reduction treatment time was 45 min. The remaining steps were roughly the same and will not be described in detail here.
[0156] Example 9
[0157] Unlike Example 1, only a composite fiber made of spandex and polyester fiber is used, and the mass ratio of spandex to polyester fiber is 7:3. The remaining steps are roughly the same and will not be described in detail here.
[0158] Example 10
[0159] Unlike Example 1, the first and second yarns were immersed in the functional liquid for 5 minutes, the hot air treatment time was 30 minutes, and the hot air treatment temperature was 90°C. The remaining steps were roughly the same and will not be described in detail here.
[0160] Comparative Example 1
[0161] Unlike Example 1, neither the composite fiber nor the Bletilla striata polysaccharide chitosan hydrogel fiber is impregnated in the functional liquid. The remaining steps are roughly the same and will not be described again here.
[0162] Comparative Example 2
[0163] Unlike Example 1, the composite fibers are not impregnated in the functional liquid. The remaining steps are largely the same and will not be described in detail here.
[0164] Comparative Example 3
[0165] Unlike Example 1, the Bletilla striata polysaccharide chitosan hydrogel fibers are not impregnated in the functional liquid. The remaining steps are largely the same and will not be described in detail here.
[0166] II. Testing Methods
[0167] Testing of elongation at break and tensile strength: According to GB / T 3923.1-2013, the electronic fabric tensile testing machine (model: YG26H) was used. Test conditions: temperature 23±2℃, relative humidity 50±5%, samples cut into 200mm×50mm strips, clamping distance 100mm, tensile speed 100mm / min, pre-tension 2cN. After equilibration under standard conditions for 24 hours, the samples were tested. The instrument automatically recorded the tensile strength (unit: cN / tax) and the rate of fracture initiation (unit: %). Five tests were performed for each group, and the average value was taken.
[0168] Water absorption rate: Tested according to YY / T 0471.1-2004 using an electronic analytical balance (model: FA2004, accuracy 0.1mg) and a constant temperature water bath (model: HH-S). Test conditions: The test liquid was 0.9% sodium chloride injection solution, temperature 37±1℃, and the sample was equilibrated for 24 hours at a temperature of 23±2℃ and a relative humidity of 50±5%. The initial mass of the dried sample was weighed. Immerse the sample completely in 37℃ physiological saline for 30 minutes, remove it and let it drain naturally for 30 seconds before weighing the wet mass. According to the formula: Water absorption rate (%) = ( - ) / Calculate using ×100%, and take the average value of 3 tests for each group.
[0169] Shedding rate: Referencing YY / T 1294.2-2015, the test was conducted using a constant temperature water bath shaker (model: THZ-82A), an electronic analytical balance (model: FA2004), and an electric heating drying oven (model: DHG-9070A). Test conditions: The test medium was 0.9% sodium chloride injection solution, temperature 37±1℃, and shaker speed 100 rpm. The initial mass of the sample from the water-loaded collapse system was weighed. The sample was placed in an Erlenmeyer flask containing 200 mL of physiological saline, and shaken at 37 °C and 100 rpm for 24 h. The sample was then removed and dried in a 60 °C oven to constant weight, and the mass was measured. According to the formula: shedding rate (%) = ( - / ) / Calculate using ×100%, and take the average value of 3 tests for each group.
[0170] Inhibition rate: According to GB / T 20944.3-2008, the test was conducted using a constant temperature shaking incubator (model: THZ-300), a clean bench (model: SW-CJ-1F), and a high-pressure steam sterilizer (model: LDZX-50KBS). Test conditions: The test strains were Staphylococcus aureus (ATCC 6538) and Escherichia coli (ATCC 25922). The temperature was 37±1℃, the shaking speed was 150 rpm, and the shaking time was 18-24 h. The samples and blank control samples were cut into 0.75g±0.01g fragments and sterilized. PBS buffer and bacterial suspension were added to the conical flasks, and after shaking and incubation, plate counting was performed. The inhibition rate (%) was calculated according to the formula: Inhibition rate (%) = (Number of viable bacteria in blank control - Number of viable bacteria in test sample) / Number of viable bacteria in blank control × 100%.
[0171] Cell proliferation rate: Based on GB / T 16886.5-2017, using... The tests were conducted using an incubator (Thermo 3111), a microplate reader (Multiskan FC), and a clean bench (SW-CJ-1F). Test conditions: The cells were mouse fibroblast L929 cells, and the culture environment was 37℃. The cell proliferation rate was determined by the following methods: saturated humidity; extraction medium: serum-containing DMEM medium; extraction ratio: 0.2 g / mL; extraction temperature: 37℃; extraction time: 24 h. The extract was then added to 96-well plates inoculated with L929 cells and cultured for 24 h. CCK-8 reagent was added and incubated for 2 h. The absorbance at 450 nm was measured using a microplate reader. The cell proliferation rate (%) was calculated using the formula: Cell proliferation rate (%) = (OD value of sample group - OD value of blank well) / (OD value of control group - OD value of blank well) × 100%.
[0172] III. Analysis of Test Results for Each Embodiment and Comparative Example
[0173] Table 1 shows the test results of the woven and knitted composite fabrics based on Bletilla striata hydrogel fibers in Examples 1-10 and Comparative Examples 1-3, including tensile strength, elongation at break, water absorption, shedding rate, antibacterial rate, and cell proliferation rate.
[0174] Fracture strength (cN / tax) Elongation at break (%) Water absorption rate (%) Shedding rate (%) Antibacterial rate (%) Cell proliferation rate (%) Example 1 3.8 480 230 4.1 92.5 118.5 Example 2 3.7 475 218 4.5 89.6 115.3 Example 3 3.6 470 225 4.3 90.2 116.7 Example 4 3.5 465 215 4.7 88.7 114.2 Example 5 3.6 472 222 4.4 91.1 117.0 Example 6 3.7 468 220 4.6 90.0 115.8 Example 7 3.5 455 210 4.9 87.3 113.5 Example 8 3.4 450 205 5.1 86.5 112.8 Example 9 3.2 430 190 6.8 82.0 108.0 Example 10 3.3 440 195 6.2 83.5 110.0 Comparative Example 1 2.2 320 125 28.5 68.0 92.5 Comparative Example 2 2.5 350 135 22.0 72.0 95.0 Comparative Example 3 2.7 370 145 18.0 75.0 98.0
[0175] Conclusion:
[0176] Tensile strength reflects the ability of knitted and woven composite fabrics based on Bletilla striata hydrogel fibers to resist tensile forces, and affects the mechanical integrity of these fabrics in moving parts. Insufficient strength leads to breakage, while excessive strength may damage newly formed granulation tissue.
[0177] Elongation at break characterizes the elasticity or extensibility of knitted or woven composite fabrics based on Bletilla striata hydrogel fibers, reflecting their ability to deform synchronously with the skin.
[0178] Water absorption rate measures the ability of knitted composite fabrics based on Bletilla striata hydrogel fibers to absorb wound exudate.
[0179] Shedding rate measures the structural integrity of knitted composite fabrics based on Bletilla striata hydrogel fibers after liquid absorption.
[0180] The antibacterial rate reflects the ability of knitted and woven composite fabrics based on Bletilla striata hydrogel fibers to kill or inhibit bacteria and prevent wound infection.
[0181] Cell proliferation rate reflects the biocompatibility of knitted and woven composite fabrics based on Bletilla striata hydrogel fibers. A proliferation rate greater than 100% indicates promotion of cell growth, while a proliferation rate less than 100% indicates inhibition of toxicity.
[0182] Table 1 shows that the fracture strength, elongation at break, water absorption rate, detachment rate, antibacterial rate, and cell proliferation rate of all embodiments are superior to those of the comparative example. The fracture strength of all embodiments is between 3.2 cN / tax and 3.8 cN / tax, achieving a balance between flexibility and strength, maintaining structural integrity while protecting the growth of new tissue; the elongation at break is between 430% and 480%, indicating high elasticity, meeting the needs of highly mobile areas; the water absorption rate is between 190% and 230%, with an absorption capacity of 1.9 to 2.3 times its own weight, indicating good water absorption; the detachment rate is between 4.1% and 6.8%, indicating good structural integrity after water absorption and resistance to detachment; the antibacterial rate is between 82% and 92.5%, meeting clinical needs; and the cell proliferation rate is between 108% and 118.5%, showing no cytotoxicity, promoting cell proliferation, and facilitating wound healing. Regarding the shedding rate, Comparative Example 1 did not load the water collapse system, while Comparative Examples 2 and 3 only partially loaded the water collapse system. In the comparative examples, the composite fabrics were soaked and the weaving sizing dissolved, the fabric delaminated and shed fibers, resulting in a large amount of shedding and a high value. In contrast, in the examples, the water collapse system filled the gaps between the fibers, bonded the double-layer base, locked the fibers and prevented shedding, and only a small amount of surface gel shed, so the shedding rate was lower. Therefore, the shedding rates of the comparative examples were all higher than those of the examples.
[0183] In Example 2, the concentrations of Bletilla striata polysaccharide and chitosan in the water-collapse functional liquid were adjusted compared to Example 1. The concentration of Bletilla striata polysaccharide was reduced and the concentration of chitosan was increased. As a result, the breaking strength and breaking elongation of the knitted composite fabric based on Bletilla striata hydrogel fiber were slightly reduced, the water absorption rate was reduced, the shedding rate was increased, and the antibacterial rate and cell proliferation rate were reduced.
[0184] In Example 3, the pH value of the water-collapse functional liquid was adjusted compared to Example 1, and the pH value was increased from 4.5 to 5. The breaking strength and breaking elongation of the knitted composite fabric based on Bletilla striata hydrogel fiber decreased slightly, the water absorption rate decreased, the shedding rate increased, and the antibacterial rate and cell proliferation rate decreased, but the overall level remained quite high.
[0185] Compared with Example 1, Example 4 changed the choice of organic carboxylic acid, replacing acetic acid with lactic acid. The breaking strength and breaking elongation of the knitted composite fabric based on Bletilla striata hydrogel fiber were slightly reduced, the water absorption rate was reduced, the shedding rate was increased, and the antibacterial rate and cell proliferation rate were reduced, but the overall level was still maintained at a considerable level.
[0186] Compared with Example 1, Example 5 changed the crosslinking agent, replacing sodium tripolyphosphate with genipin. The breaking strength and breaking elongation of the knitted composite fabric based on Bletilla striata hydrogel fiber decreased slightly, the water absorption decreased, the shedding rate increased, and the antibacterial rate and cell proliferation rate decreased, but the overall level remained quite high.
[0187] Compared with Example 1, Example 6 increased the concentration of Bletilla striata polysaccharide solution and chitosan solution in the Bletilla striata polysaccharide-chitosan spinning solution, and increased the proportion of Bletilla striata polysaccharide solution. The breaking strength and breaking elongation of the knitted composite fabric based on Bletilla striata hydrogel fiber decreased slightly, the water absorption rate decreased, the shedding rate increased, and the antibacterial rate and cell proliferation rate decreased.
[0188] Compared with Example 1, Example 7 increased the proportion of montmorillonite nano-dispersion in the Bletilla striata polysaccharide chitosan spinning solution. The breaking strength and breaking elongation of the knitted composite fabric based on Bletilla striata hydrogel fiber were slightly reduced, the water absorption rate was reduced, the shedding rate was increased, and the antibacterial rate and cell proliferation rate were reduced.
[0189] Compared with Example 1, Example 8 improved the modification degree of spandex, acrylic and polyester fibers. The breaking strength and breaking elongation of the knitted composite fabric based on Bletilla striata hydrogel fiber were slightly reduced, the water absorption rate was reduced, the shedding rate was increased, and the antibacterial rate and cell proliferation rate were reduced.
[0190] Compared to Example 1, Example 9 only uses a composite fiber made of spandex and polyester fibers, and the mass ratio of spandex to polyester fibers is 7:3. The breaking strength and breaking elongation of the knitted composite fabric based on Bletilla striata hydrogel fiber are slightly reduced, the water absorption rate is reduced, the shedding rate is increased, and the antibacterial rate and cell proliferation rate are reduced.
[0191] Compared to Example 1, Example 10 increased the immersion time of the composite fiber and Bletilla striata polysaccharide chitosan hydrogel fiber in the functional liquid, as well as the time and temperature of hot air treatment. The breaking strength and breaking elongation of the knitted composite fabric based on Bletilla striata hydrogel fiber were slightly reduced, the water absorption rate was reduced, the shedding rate was increased, and the antibacterial rate and cell proliferation rate were reduced.
[0192] Therefore, the preparation method of the knitted composite fabric based on Bletilla striata hydrogel fiber of the present invention can control the breaking strength, breaking elongation, water absorption rate and shedding rate by adjusting the concentration of Bletilla striata polysaccharide and chitosan in the water-collapse functional solution, the concentration of Bletilla striata polysaccharide solution and chitosan solution in the Bletilla striata polysaccharide-chitosan spinning solution, the composition of the composite fiber, the degree of modification of spandex, acrylic fiber and polyester fiber, the immersion time of composite fiber and Bletilla striata polysaccharide-chitosan hydrogel in the functional solution and the temperature and time of hot air treatment, thereby affecting the antibacterial rate and cell proliferation rate, and achieving a balance between interlayer bonding force, hemostasis, antibacterial activity and mechanical properties of the knitted composite fabric based on Bletilla striata hydrogel fiber.
[0193] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.
Claims
1. A method for preparing a knitted composite fabric based on Bletilla striata hydrogel fibers, characterized in that, include: A water-collapse functional fluid is provided, wherein the water-collapse functional fluid comprises Bletilla striata polysaccharide, chitosan, cross-linking agent and organic carboxylic acid; At least one of spandex and acrylic fiber is blended with polyester fiber to obtain composite fiber; A hydrogel spinning solution of Bletilla striata polysaccharide and chitosan is provided, wherein the hydrogel spinning solution comprises Bletilla striata polysaccharide, chitosan, a dispersion of nano-reinforcing materials, a crosslinking agent, an organic carboxylic acid and water; The Bletilla striata polysaccharide-chitosan hydrogel spinning solution was wet-spun and then washed with water to obtain Bletilla striata polysaccharide-chitosan hydrogel fiber. The composite fiber is impregnated with the water-collapse functional liquid and then hot-air treated to obtain the first yarn. The Bletilla striata polysaccharide chitosan hydrogel fiber was impregnated with the water-slump functional liquid and then hot-air treated to obtain a second yarn; The first yarn is woven to obtain a woven layer, and the second yarn is knitted to obtain a knitted layer. The woven layer and the knitted layer are woven together to form a knitted composite fabric based on Bletilla striata hydrogel fiber.
2. The method for preparing the knitted composite fabric based on Bletilla striata hydrogel fiber according to claim 1, characterized in that: The degree of deacetylation of the chitosan is at least 85%; And / or, the organic carboxylic acid includes at least one of acetic acid, lactic acid, and citric acid; And / or, the crosslinking agent includes at least one of sodium tripolyphosphate, genipin, and epichlorohydrin.
3. The method for preparing the knitted composite fabric based on Bletilla striata hydrogel fiber according to claim 1, characterized in that: The water-collapse functional fluid is prepared through the following steps: Slowly add chitosan to the organic carboxylic acid solution and stir until completely dissolved; Add Bletilla striata polysaccharide and continue stirring until the Bletilla striata polysaccharide is evenly distributed in the solution; The crosslinking agent is slowly added to the mixture, and then stirred for a period of time to obtain the water-collapse functional liquid.
4. The method for preparing the knitted composite fabric based on Bletilla striata hydrogel fiber according to claim 3, characterized in that: In the water-collapse functional fluid, the mass concentration of chitosan is 6 g / L-10 g / L; And / or, in the water-collapse functional liquid, the mass concentration of Bletilla striata polysaccharide is 10 g / L-14 g / L; And / or, in the water-collapse functional liquid, the mass concentration of the crosslinking agent is 2 g / L-4 g / L; And / or, the pH of the water-collapse functional liquid is 4.5-5.
0.
5. The method for preparing the knitted composite fabric based on Bletilla striata hydrogel fiber according to claim 1, characterized in that: The Bletilla striata polysaccharide-chitosan hydrogel spinning solution is prepared by the following steps: The Bletilla striata polysaccharide was mixed with water to obtain a first mixture; The chitosan and the organic carboxylic acid are mixed to obtain a second mixture; The first mixture and the second mixture are mixed to obtain a polysaccharide mixture; The dispersion of nano-reinforced materials was mixed with the polysaccharide mixture, and then a crosslinking agent was added to obtain the Bletilla striata polysaccharide chitosan hydrogel spinning solution.
6. The method for preparing the knitted composite fabric based on Bletilla striata hydrogel fiber according to claim 5, characterized in that: The mass ratio of the first mixture to the second mixture is 1:(0.2-0.5); And / or, in the first mixture, the mass concentration of the Bletilla striata polysaccharide is 38 g / L-42 g / L; And / or, in the second mixture, the mass concentration of chitosan is 8 g / L-12 g / L; And / or, the mass concentration of the nano-reinforced material dispersion is 8 g / L-12 g / L; And / or, the mass ratio of the nano-reinforced material dispersion to the polysaccharide mixture is 1:(1-3); And / or, in the Bletilla striata polysaccharide-chitosan hydrogel spinning solution, the mass concentration of the crosslinking agent is 4 g / L-6 g / L.
7. The method for preparing the knitted composite fabric based on Bletilla striata hydrogel fiber according to claim 5, characterized in that: The nano-reinforced material dispersion includes at least one of montmorillonite nanosheet dispersion and nanocellulose dispersion, and the dispersion solvent is water.
8. The method for preparing the knitted composite fabric based on Bletilla striata hydrogel fiber according to claim 1, characterized in that: The method of blending at least one of spandex and acrylic fiber with polyester fiber to obtain composite fiber includes: Spandex is immersed in a first modification solution to obtain modified spandex, wherein the first modification solution comprises hydroxyethyl methacrylate and an initiator; Acrylic fiber is subjected to alkaline hydrolysis and then immersed in a second modification solution to obtain modified acrylic fiber. The second modification solution includes acrylic acid and an initiator. Polyester fibers are subjected to alkali reduction treatment to obtain modified polyester fibers. At least one of modified spandex and modified acrylic fiber is blended with modified polyester fiber to obtain composite fiber.
9. The method for preparing the knitted composite fabric based on Bletilla striata hydrogel fiber according to claim 8, characterized in that: The initiator includes at least one of ammonium persulfate and potassium persulfate; And / or, the alkaline hydrolysis treatment uses at least one reagent selected from sodium hydroxide, potassium hydroxide and sodium carbonate; And / or, the alkali reduction treatment uses at least one reagent selected from sodium hydroxide, potassium hydroxide, and sodium carbonate.