A method for preparing perovskite-type piezoelectric particle-doped PVDF-based piezoelectric nanofiber thin films and their applications

By synthesizing BCZT-Tb piezoelectric particles with CTAB modification via solid-state method and combining them with PVDF, the problems of low β-phase content and easy filler detachment in PVDF-based piezoelectric materials were solved. This enabled the preparation of nanofiber films with high β-phase content and good cycle stability, thereby improving the mechanical stability and signal output of the sensor.

CN123108835APending Publication Date: 2026-11-17CHANGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611268230.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing PVDF-based piezoelectric materials are prone to generating non-polar α phases without piezoelectric activity during the preparation process. Furthermore, inorganic fillers tend to agglomerate in the polymer matrix and have poor interfacial compatibility, which leads to filler detachment and output signal attenuation in sensor devices under long-term cyclic stress.

Method used

BCZT-Tb piezoelectric particles were synthesized by solid-state method and modified with CTAB surface. The modified piezoelectric particles were then combined with PVDF by electrospinning process to prepare nanofiber films with high β phase content and good cycle stability.

Benefits of technology

The β phase content was increased to 85%, which enhanced the interfacial bonding strength and ensured that the output voltage of the sensor remained stable after 5,000 cycles of loading. The piezoelectric particles on the fiber surface did not fall off, demonstrating excellent cycle stability and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108835A_ABST
    Figure CN123108835A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing PVDF-based piezoelectric nanofiber films doped with perovskite-type piezoelectric particles and their applications, belonging to the field of flexible piezoelectric materials. The preparation method includes the following steps: BCZT piezoelectric particles are prepared using a solid-state method; BCZT is doped with mixed-valence Tb elements to enhance the performance of the piezoelectric particles; subsequently, the particles are surface-modified using CTAB, purifying the surface while simultaneously forming a coating structure through electrostatic self-assembly; finally, the modified particles are uniformly dispersed in a PVDF precursor solution, and the nucleation and growth of the polar β phase of PVDF are induced in situ based on the high-voltage electric field and jet stretching of electrospinning technology. The synergistic modification of Tb doping and CTAB in this invention improves the dispersion of the particles and the β phase content. The prepared flexible sensor exhibits excellent piezoelectric output and stability, showing broad application prospects in wearable devices, pulse monitoring, and human-computer interaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer piezoelectric materials and discloses a method for preparing a perovskite-type piezoelectric particle-doped PVDF-based homopolymer piezoelectric film. Background Technology

[0002] With the rapid development of the Internet of Things and human-computer interaction technologies, the demand for applications involving complex curved surfaces and dynamic deformation is increasing. Traditional rigid piezoelectric ceramics, limited by their physical form and mechanical properties, are difficult to adapt to the requirements of technological development. In contrast, flexible sensors based on polymers possess unique flexibility compared to piezoelectric ceramics, and their mechanical tensile strength is also superior.

[0003] In recent years, flexible electronics technology has been widely used in wearable devices, human-computer interaction, and health monitoring. Flexible sensors need to possess certain mechanical compliance and wear resistance to achieve stable monitoring of physical signals under complex deformation conditions.

[0004] Among numerous energy conversion mechanisms, piezoelectric materials can convert mechanical energy caused by environmental vibrations into electrical energy. Among various piezoelectric material systems, polyvinylidene fluoride (PVDF) stands out as a flexible and highly effective piezoelectric polymer medium, possessing characteristics such as smooth surface, lightweight, and fatigue resistance. Its polarized films can achieve piezoelectric constants as high as 6–7 pC·N. -1 Its piezoelectricity is approximately ten times that of other common polymers, exhibiting superior combined piezoelectric, pyroelectric, ferroelectric, and dielectric properties, making it particularly suitable for various portable electronic devices. Furthermore, introducing an inorganic filler phase during the PVDF crystallization process can effectively promote the preferred formation of the polar piezoelectric phase. However, pure PVDF readily generates a non-polar α-phase without piezoelectric activity during conventional preparation. To improve its piezoelectric properties, it is usually necessary to introduce inorganic piezoelectric particles as fillers during the crystallization process to promote the formation of the polar β-phase.

[0005] Currently, lead zirconate titanate (PZT)-based ceramics are widely used in piezoelectric applications. However, due to the toxicity and high-temperature volatility of lead oxide, they face severe environmental and health challenges, making the development of high-performance lead-free piezoelectric materials an urgent issue in the field of functional materials. Among many candidate systems, barium calcium zirconate titanate (Ba... 0.85 Ca 0.15 (Zr) 0.1 Ti 0.9 O3 (BCZT) has attracted much attention because it also has the characteristics of rhombohedral-tetragonal phase coexistence and MPB behavior similar to PZT. As an environmentally friendly lead-free piezoelectric material, its excellent piezoelectric and ferroelectric properties have been proven, and it is regarded as one of the most promising lead-free systems.

[0006] Introducing highly electroactive inorganic piezoelectric particles into a PVDF matrix can optimize the electromechanical conversion efficiency and mechanoelectric response behavior of the composite material from multiple dimensions. Besides adding fillers to PVDF, the preparation process is also a key factor affecting the piezoelectric properties of PVDF. In most cases, a stable nonpolar α phase is formed inside the prepared PVDF film, lacking piezoelectric properties. To ensure that the dipole moments of disordered molecules in PVDF can be oriented along a specific direction, thereby forming an excellent piezoelectric β phase, the content of the polar phase in PVDF can be increased through methods such as stretching, applying a strong electric field for polarization, and thermal annealing, thus inducing dipole orientation. Common preparation methods include spin coating, electrospinning, and hot pressing.

[0007] Despite the progress made in the research and development of various PVDF functional devices, the field still faces several challenges: inorganic fillers tend to agglomerate in polymer matrices, exhibiting poor interfacial compatibility; and filler detachment and output signal attenuation occur under long-term cyclic stress. Therefore, improving the dispersibility of inorganic particles, increasing the β-phase content of composite films, and ensuring the long-term mechanical stability of sensor devices through material modification and structural design are key technical issues that need to be addressed. Summary of the Invention

[0008] The purpose of this invention is to provide a method for preparing BCZT-Tb piezoelectric particle-doped PVDF nanofiber thin films. This method first synthesizes BCZT-Tb piezoelectric particles with excellent ferroelectric properties using a solid-state method, and then modifies their surface using CTAB. Finally, using an electrospinning process, the modified piezoelectric particles are combined with PVDF to prepare nanofiber thin films with high β-phase content and good cycling stability, which can be used for flexible piezoelectric sensors.

[0009] This invention is achieved through the following technical solution:

[0010] A method for preparing perovskite-type piezoelectric particle-doped PVDF-based piezoelectric nanofiber thin films includes the following steps:

[0011] (1) Weigh the raw materials required for preparing BCZT-Tb piezoelectric particles according to the stoichiometric ratio, including BaCO3, CaCO3, TiO2, ZrO2 and Tb4O7. The chemical formula of the piezoelectric particles prepared by solid-state reaction is (Ba 0.85 Ca 0.15 ) 1-x Tb x (Zr) 0.1 Ti 0.9 O3; 0.001≤x≤0.007.

[0012] The above raw materials were dispersed in ethanol, thoroughly ground, and the solvent was allowed to evaporate naturally. The grinding process was repeated five times until the powder was uniformly mixed. The powder was then sieved through a 200-mesh sieve to obtain a uniform and fine powder. The powder was then placed in a calcination furnace and treated at a high temperature of 1100~1300°C to finally obtain BCZT-Tb piezoelectric particles.

[0013] BCZT belongs to the ABO3 type perovskite structure, where the B site is composed of Ti. 4+ With Zr 4+ Ions occupy the site and form an oxygen octahedral coordination environment; the A site is occupied by Ba. 2+ or Ca 2+ Ions occupy the octahedron, forming a network structure with shared vertices with oxygen octahedrons. As a rare earth element, terbium (Tb) exhibits mixed valence states, primarily existing in +3 and +4 oxidation states. Under the solid-state reaction conditions described in this invention, Tb primarily exists in the +3 oxidation state, and its ionic radius (0.92 Å) is similar to that of Ca. 2+ (1.00 Å) similar, tending to enter the A-site of the perovskite structure, partially replacing Ba. 2+ or Ca 2+ Small amount of Tb 4+ It may enter the B site, but the dominant role comes from the lattice distortion and oxygen vacancy generation caused by the substitution of the A site, thereby optimizing the ferroelectric and piezoelectric properties of the material.

[0014] (2) Surface modification of the piezoelectric particles obtained in step (1). The surface of the particles is modified by using the cationic surfactant CTAB, which adsorbs onto the negatively charged sites on the surface of the BCZT-Tb particles through electrostatic interaction, and then self-assembles to form an ordered coating structure.

[0015] The specific steps are as follows: Prepare a cationic surfactant solution of hexadecyltrimethylammonium bromide (CTAB) with a concentration of 2-6 mg / mL in a mixed solvent of ethanol and water (volume ratio 1:1). After dissolution, add the above-mentioned BCZT-Tb piezoelectric particles at a ratio of 80-150 mL: 1 g, disperse ultrasonically, and heat and stir at 50-60 °C. After the reaction is complete, centrifuge and wash to remove unbound free CTAB from the surface, and dry to obtain surface-modified BCZT-Tb@CTAB particles. The mass ratio of CTAB to BCZT-Tb is 0.2:1 to 0.9:1.

[0016] This invention further reveals that surface modification of BCZT-Tb particles using CTAB not only achieves uniform dispersion of the particles in the PVDF matrix, but more importantly, this modification process effectively removes the inherent carbonate and amorphous contamination layer on the surface of the BCZT-Tb particles, exposing clean and ordered crystal faces. Raman spectroscopy characterization confirms that the intensity of the characteristic Raman peaks of the modified BCZT-Tb particles is increased, indicating a reduction in surface defects and improved crystallinity. This surface purification effect significantly enhances the activity of BCZT-Tb particles as heterogeneous nucleation sites in PVDF. Simultaneously, Tb... 3+ / Tb 4+ Mixed valence states introduce local defect dipoles in the BCZT lattice. These defect dipoles can be oriented under the action of a high voltage electric field (preferably 19 kV) during electrospinning, forming a dual polarization synergy with the electric field orientation of the PVDF molecular chain.

[0017] (3) The surface-modified BCZT-Tb piezoelectric particles obtained in step (2) are dispersed in a PVDF solution of a specific concentration to prepare a uniform and stable spinning precursor solution. The spinning solution is then processed into a nanofiber film using electrospinning technology.

[0018] Specifically, a PVDF solution with a mass fraction of 14 wt% to 18 wt% was prepared, using N,N-dimethylformamide (DMF) and acetone in a volume ratio of 7:3 to 8:2. The aforementioned BCZT-Tb@CTAB particles were added to the PVDF solution, with a particle doping amount of 3 wt% to 18 wt% (preferably 13 wt%) of the PVDF mass. After stirring to form a homogeneous precursor solution, electrospinning was performed to obtain a nanofiber film. Following annealing, a perovskite-type piezoelectric particle-doped PVDF-based homopolymer piezoelectric film was obtained.

[0019] Furthermore, the annealing temperature is 50-70 ℃, and the annealing time is 1-3 h.

[0020] Furthermore, the purity of the raw materials required for the preparation of BCZT-Tb in step (1) is ≥99%.

[0021] Furthermore, the weighing accuracy of all raw materials in step (1) is 0.001g.

[0022] Furthermore, in step (1), the doping amount of Tb element is 0.1 mol%-0.7 mol%.

[0023] Furthermore, in step (3), in order to eliminate the electrostatic interference caused by friction on the sample surface, the sample is placed in a 60°C oven and left to stand for 2 hours.

[0024] Furthermore, the applied positive polarization high voltage is 15-25 kV, the distance from the syringe needle to the receiving roller is 10-20 cm, the solution propulsion rate is 1.0-2.0 mL / h, the receiving roller rotation speed is 300-500 rpm, the spinning environment temperature is controlled at 20-30 ℃, and the relative humidity is controlled at 15%-30%.

[0025] The present invention also provides a flexible piezoelectric sensor device, which uses the above-mentioned preparation method to obtain a perovskite-type piezoelectric particle-doped PVDF-based piezoelectric nanofiber film as a dielectric layer, attaches conductive electrodes to the upper and lower surfaces of the dielectric layer, and encapsulates it with a flexible polymer layer to form a sandwich structure.

[0026] The flexible piezoelectric sensor is used to collect environmental mechanical energy or is attached to the surface of the human body for real-time monitoring of motion and pulse physiological signals.

[0027] This invention uniformly incorporates BCZT-Tb piezoelectric particles into a PVDF matrix. The electrostatic interaction between the polar functional groups on the surface of the CTAB-modified piezoelectric particles and the polymer molecular chains effectively improves the dispersion of the inorganic phase in the polymer medium, suppresses the aggregation tendency of the piezoelectric particles, and results in a highly uniform distribution of the filler within the matrix. During the subsequent crystallization process, the surface of the uniformly dispersed BCZT-Tb particles serves as heterogeneous nucleation sites, inducing the preferred formation of the polar β-phase crystal form by lowering the activation energy barrier for conformational adjustment of the PVDF molecular chains. Simultaneously, the localized electric field concentration effect caused by dielectric mismatch at the interface between the high-dielectric-constant ceramic phase and the PVDF matrix further promotes the directional alignment of dipoles along the electric field direction, thereby constructing enhanced local piezoelectric response microregions within the composite system. Building upon this foundation, an electrospinning process was employed to perform in-situ stretching and electric field polarization treatment on the composite precursor solution. Utilizing the mechanical stretching and high-voltage electric field induction during high-speed jet stretching, direct polarization was achieved, forcing the PVDF molecular chains to highly oriented and solidify into a β-phase-rich nanofiber configuration. This successfully prepared a flexible nanofiber film with high specific surface area and excellent piezoelectric activity. Subsequent encapsulation and integration resulted in functional devices that not only fully retained the material's intrinsic flexibility but also reduced manufacturing costs and environmental impact. BCZT-Tb, as a lead-free and environmentally friendly ferroelectric material, effectively avoids the ecological pollution risks caused by lead in discarded traditional lead-containing capacitors, aligning with the strategic direction of sustainable development in green electronic devices.

[0028] Compared with the prior art, the present invention has the following technical effects:

[0029] (1) High voltage response under low filler content: The doping amount of CTAB modified BCZT-Tb particles can be optimized to increase the β phase content to up to 85%. This indicates that Tb doping and CTAB modification produce a synergistic enhancement of heterogeneous nucleation effect.

[0030] (2) Raman spectroscopy showed that the Raman characteristic peak intensity of BCZT-Tb particles was increased after CTAB modification, proving that CTAB not only acts as a dispersant but also plays a role in surface purification by removing the surface contaminant layer and reducing lattice defects. Furthermore, during 5000 cyclic loading tests (constant pressure 15 N), the output voltage of the composite film remained stable (approximately 1.6 V), and no piezoelectric particles on the fiber surface detached. These results indicate that CTAB continues to play a persistent interfacial coupling role in the final composite film, enhancing the interfacial bonding strength between BCZT-Tb particles and the PVDF matrix.

[0031] (3) Excellent cyclic stability and durability: After 5000 consecutive cycles of loading (15 N, 5 Hz), the output voltage decay rate of the flexible piezoelectric sensor manufactured in this invention is less than 5%, and there is no obvious shedding or leakage of piezoelectric particles on the fiber surface and inside. In contrast, the conventional BCZT / PVDF system is prone to filler-matrix interface debonding, particle shedding, and output signal attenuation under long-term cyclic stress. The excellent durability of this invention is attributed to: Tb doping causes moderate shrinkage of the BCZT lattice and introduces oxygen vacancies, changing the chemical state of the particle surface and enhancing the electrostatic adsorption with the CTAB head group; at the same time, the long alkyl chain of CTAB forms a strong hydrophobic / van der Waals interaction with the PVDF molecular chain, forming a strong interface anchoring structure. Attached Figure Description

[0032] Figure 1 XPS image of BCZT piezoelectric particles prepared by solid-state method (Example 1).

[0033] Figure 2 SEM images and particle size distributions of piezoelectric particles with different Tb doping concentrations are shown in Figures (a)-(e). The Tb concentrations are 0% for Comparative Example 3, 0.1% for Example 2, 0.3% for Example 3, 0.5% for Example 1, and 0.7% for Example 4.

[0034] Figure 3 Hysteresis loop diagrams of the prepared piezoelectric ceramic samples (Examples 1-4).

[0035] Figure 4 Raman diagram of the modified BCZT-Tb@CTAB piezoelectric particles (piezoelectric particles prepared in step (2) of Example 1).

[0036] Figure 5XRD pattern of the modified BCZT-Tb@CTAB piezoelectric particles (piezoelectric particles prepared in step (2) of Example 1).

[0037] Figure 6 FTIR images of nanofiber films with different doping concentrations (corresponding to Examples 1, 5, 6, and 7).

[0038] Figure 7 The response voltage test diagrams of flexible sensors prepared for pure PVDF films and fiber films with different doping concentrations (Comparative Example 1 and Examples 1, 5, 6, 7) under different forces are shown.

[0039] Figure 8 This is a SEM image of the fiber film with a doping concentration of 13 wt%.

[0040] Figure 9 The output voltage of the sensor at different frequencies under a fixed pressure (Example 1).

[0041] Figure 10 To prepare tactile sensing signals of a simple flexible sensor in different scenarios (Example 1).

[0042] Figure 11 To prepare a stability map of a simple flexible sensor in 5000 cycles of testing (Example 1). Detailed Implementation

[0043] This invention is not limited to the specific embodiments listed below. Those skilled in the art can implement this invention using various other specific embodiments based on the content disclosed herein. Any modifications or alterations made to the design structure and concept of this invention fall within the protection scope of this invention. It should be noted that, unless otherwise specified, the embodiments and features described in this invention can be combined with each other.

[0044] The present invention will be further described in detail below with reference to the embodiments:

[0045] I. All reagents used in this invention are commercially available, and the testing instruments include:

[0046] X-ray photoelectron spectroscopy (XPS): The elemental composition of the piezoelectric particles was confirmed using an X-ray photoelectron spectrometer (XPS, Thermo Scientific K-Alpha type, USA).

[0047] X-ray diffractometer (XRD): Used to analyze the crystal structure and phase composition of test samples.

[0048] SEM testing: The surface morphology of inorganic particles was observed using a scanning electron microscope (FEG250, Quanta, USA). The voltage was set to 15kV, and the samples were sputter-coated with gold. The surface morphology was then observed at 5000x magnification.

[0049] Ferroelectric performance testing: The piezoelectric ceramic samples coated with electrodes were tested using the Radiant Precision Premier LC ferroelectric testing system. The electrodes used were low-temperature silver paste, and the samples were fired at 650°C for 30 minutes.

[0050] Raman spectroscopy test: The instrument used was a Thermo Fischer DXR.

[0051] Infrared spectroscopy (FTIR): The prepared samples were analyzed using a Fourier transform infrared spectrometer (model Avatar 370) (Thermoelectric Nigel Instruments, USA).

[0052] Dielectric property testing: The fiber film sample was simply compacted, and electrodes were added to both sides. The test was performed using a Partulab HDMS-1000 measurement system.

[0053] Sensor signal testing: A linear motor was used to realize the contact separation movement under different conditions, and an oscilloscope (KEYSIGHT DSO-X 3024T) was used for testing. The piezoelectric signal measurement experimental platform was built in the laboratory.

[0054] II. Specific steps in the preparation of PVDF piezoelectric fiber films:

[0055] Example 1

[0056] A method for preparing PVDF piezoelectric fiber films, comprising the following steps:

[0057] Step 1: According to chemistry (Ba 0.85 Ca 0.15 ) 0.995 Tb 0.005 (Zr) 0.1 Ti 0.9 To determine the stoichiometric ratio of O3, 4.53 g BaCO3, 0.404 g CaCO3, 1.95 g TiO2, 0.33 g ZrO2, and 0.02 g Tb4O7 were ground in an agate mortar with anhydrous ethanol until the ethanol was completely evaporated. This process was repeated five times to ensure uniform mixing. The mixture was then dried and sieved. The sample was dried at 60°C for 4 hours, followed by sieving through a 200-mesh sieve. Finally, the powder was placed in a crucible, heated to 1200°C at a rate of 2°C / min, and held at that temperature for 4 hours. The mixture was then cooled to room temperature in the furnace to obtain the perovskite phase.

[0058] Step 2: First, in a mixed solvent of ethanol and water (v 乙醇 / v 水 A CTAB solution with a concentration of 3 mg / mL was prepared in a 1:1 ratio and stirred at 60°C for 1.5 h to ensure complete dissolution. 1 g of BCZT-Tb powder obtained in step 1 was added to 100 mL of the above CTAB solution, and the mixture was first sonicated for 30 min to ensure uniform dispersion, then stirred at 50°C for 4 h. After the reaction was complete, the product was centrifuged, washed, and dried at 60°C for 24 h to obtain the CTAB-modified BCZT-Tb powder.

[0059] Step 3: First, 3.2 g of PVDF was dissolved in a mixed solvent of 16.8 g DMF and acetone (volume ratio 7:3), and ultrasonically treated for 30 min to ensure complete dissolution, preparing a PVDF precursor solution with a mass concentration of 16 wt%. The solution was then magnetically stirred at 60°C for 3 h. Next, 0.4 g of the modified BCZT-Tb@CTAB powder from Step 2, representing 13 wt% of the PVDF mass, was uniformly dispersed in the precursor solution, and stirring was continued for 1 h to obtain the composite spinning solution. Then, in a spinning environment at 25°C and 20% relative humidity, a 0.5 mm inner diameter metal needle was used, with the needle 15 cm from the receiving roller, the roller speed 350 rpm, the solution feed rate 1.5 mL / h, and a positive polarization high voltage of 19 kV was applied. Silicone-coated release paper was used as the receiving substrate, and the solution was received for 4 h. Finally, the obtained fiber membrane was annealed at 60°C for 2 h to eliminate internal stress, and the final PVDF composite piezoelectric fiber membrane (PVDF / BCZT-Tb@CTAB) sample was obtained.

[0060] Step 4: The core structure of a flexible piezoelectric sensor typically includes a piezoelectric functional layer and an electrode layer. In this invention, the flexible piezoelectric sensor has a sandwich structure and is encapsulated with a flexible encapsulation layer. The PVDF composite piezoelectric fiber film (PVDF / BCZT-Tb@CTAB) prepared in Step 3 serves as the dielectric layer, with an area of ​​1 × 1 cm. 2 The upper and lower copper foil layers are responsible for generating electrical signals. The copper foil on both sides serves as electrodes to receive the signals generated by the dielectric layer and leads them out to an external oscilloscope via wires. The flexible PI layer is the encapsulation layer, which mainly provides protection for the device, resulting in the final flexible piezoelectric sensor.

[0061] Example 2

[0062] The only difference from Example 1 is that the amount of Tb4O7 in step (1) is adjusted so that the Tb doping amount is 0.1 mol%. All other operations and parameters are exactly the same as in Example 1.

[0063] Example 3

[0064] The only difference from Example 1 is that the amount of Tb4O7 in step (1) is adjusted so that the Tb doping amount is 0.3 mol%. All other operations and parameters are exactly the same as in Example 1.

[0065] Example 4

[0066] The only difference from Example 1 is that the amount of Tb4O7 in step (1) is adjusted so that the Tb doping amount is 0.7 mol%. All other operations and parameters are exactly the same as in Example 1.

[0067] Example 5

[0068] The only difference from Example 1 is that the mass of BCZT-Tb@CTAB powder weighed in step (3) is 0.096 g (3 wt% of the mass of PVDF), and the rest of the operation and parameters are exactly the same as in Example 1.

[0069] Example 6

[0070] The only difference from Example 1 is that in step (3), the mass of BCZT-Tb@CTAB powder weighed is 0.256 g (8 wt% of the mass of PVDF), and the rest of the operation and parameters are exactly the same as in Example 1.

[0071] Example 7

[0072] The only difference from Example 1 is that the mass of BCZT-Tb@CTAB powder weighed in step (3) is 0.576 g (relative to 18 wt% of the mass of PVDF), and the rest of the operation and parameters are exactly the same as in Example 1.

[0073] Comparative Example 1 (Pure PVDF)

[0074] The only difference from Example 1 is that no piezoelectric particles are added, and the 16 wt% PVDF solution is directly electrospun. All other operations and parameters are exactly the same as in Example 1.

[0075] Comparative Example 2 (CTAB modification omitted)

[0076] After preparing 0.5 mol% Tb-doped BCZT-Tb powder according to step (1) of Example 1, the CTAB surface modification treatment in step (2) was omitted, and the unmodified powder was directly added to the PVDF spinning solution at a ratio of 13 wt%. The remaining steps, electrospinning and encapsulation were exactly the same as in Example 1.

[0077] Comparative Example 3 (Tb doping omitted)

[0078] The only difference from Example 1 is that Tb4O7 is not added in step (1), according to chemical (Ba 0.85 Ca 0.15 (Zr) 0.1 Ti 0.9 The raw materials were weighed according to the stoichiometric ratio of O3 to prepare pure BCZT inorganic particles (i.e., Tb doping amount is 0). The remaining operations (2)-(4) and parameters are exactly the same as in Example 1.

[0079] Comparative Example 4 (CTAB replaced with SDBS)

[0080] The only difference from Example 1 is that in step (2), the CTAB surfactant is replaced with sodium dodecylbenzenesulfonate (SDBS) at an equimolar concentration. All other operations and parameters are exactly the same as in Example 1.

[0081] Comparative Example 5 (Scraping + Corona Polarization as an Alternative to Electrospinning)

[0082] The spinning precursor solution used was exactly the same as that used in steps (1) to (3) of Example 1, but instead of electrospinning, the spinning solution was coated into a film and dried. After drying, it was subjected to conventional corona polarization treatment (polarization field 25 kV, temperature 80°C, time 30 min). The remaining encapsulation steps were the same as those in Example 1.

[0083] Table 1. Performance test results of the composite films in the examples and comparative examples:

[0084]

[0085] Characterization and performance testing:

[0086] Ferroelectric property testing of inorganic fillers: Preparation of BCZT-Tb piezoelectric ceramic samples: First, the pre-synthesized powder was ball-milled twice with the same parameters. After drying and sieving, BCZT-Tb nanoparticles were obtained. The powder was then ground uniformly with 0.8% PVA binder in a mortar, dried at 80°C, and sieved through a 200-mesh sieve to obtain granulated powder with uniform particle size. Subsequently, the powder was pressed into cylindrical green bodies using a mold at 4 MPa. The green bodies were held at 550°C for 2 h to completely remove PVA, and then sintered at 1450°C for 3 h to finally obtain BCZT-Tb piezoelectric ceramic samples for subsequent ferroelectric testing.

[0087] Figure 1The XPS spectra of the prepared BCZT piezoelectric particles are shown. The XPS results not only confirmed the successful synthesis of BCZT but also revealed the chemical states of each element. The full XPS spectrum of the BCZT powder clearly shows the characteristic peaks of Ba 3d, Ca 2p, Zr 3d, Ti 2p, and O 1s, as well as a residual carbon peak at C 1s at 284.08 eV. No other contaminants were detected. The Ba 3d spectrum can be decomposed into two peaks: Ba 3d5 / 2 (777.78 eV) and Ba 3d3 / 2 (793.12 eV), with a binding energy difference of approximately 15.3 eV, which are attributed to Ba. 2+ The Ca 2p spectrum shows a double peak with a binding energy difference of 3.6 eV, indicating that Ca... 2+ Yes, it exists. The Zr 3d5 / 2 peak in the Zr 3d spectrum is located at 180.48 eV, corresponding to Zr 4+ The spin orbital splits into 2.2 eV. The peaks at 457.28 eV and 463.08 eV in the Ti 2p spectrum are attributed to Ti 2p3 / 2 and Ti 2p1 / 2, respectively. After peak fitting, sub-peaks appear at 456.08 eV and 461.98 eV, indicating the presence of Ti in the sample. 3+ This can be attributed to the electronic compensation mechanism that accompanies the formation of oxygen vacancies.

[0088] Figure 2 Images (a)-(e) show SEM images of Tb doping concentrations of 0%, 0.1%, 0.3%, 0.5%, and 0.7%, respectively. It can be seen that the particles at different Tb doping concentrations all exhibit good spherical crystal morphology with clear boundaries and particle sizes ranging from 0.4 to 1.2 μm, indicating that all samples have good phase structure consistency. Statistical analysis shows that Tb doping further promotes grain growth and increases the average particle size, which is attributed to the increased Tb doping concentration. 3+ Ti is produced by partial substitution in ABO3 perovskite. 4+ and Ba 2+ Vacancies, such defects, can enhance mass transport, thereby accelerating grain growth. When the Tb doping concentration is 0.1% and 0.3%, the average grain size is concentrated at 0.7 μm and 0.75 μm, respectively, with little change; when the concentration is increased to 0.5%, the average grain size increases to 0.9 μm, and the grain growth is most complete; however, when the doping concentration is further increased to 0.7%, excessive substitution will inhibit grain growth.

[0089] Figure 3 The hysteresis loops of the piezoelectric ceramic samples pressed using the aforementioned particles are shown. All samples exhibit a typical ferroelectric butterfly-shaped hysteresis loop, indicating spontaneous polarization reversal under an alternating electric field, demonstrating a perovskite ferroelectric structure. Under a 25 kV polarization field, the residual polarization intensity (Pr) of the Tb-doped samples is higher than that of the undoped samples. This is because Tb...3+ By entering the A and B sites of the perovskite lattice, the lattice parameters are altered, causing the structure to approach the quasi-isomorphic phase boundary (MPB). The MPB region contains multiple ferroelectric phases with similar energies and a low energy barrier, promoting domain wall movement and thus increasing ferroelectric ore (Pr). With increasing Tb doping concentration, Pr first increases and then decreases: at 0.1%, Pr is 9.56 μC / cm², a 19% increase compared to undoped; at 0.3%, it increases to 11.14 μC / cm²; at 0.5%, it reaches a maximum of 11.91 μC / cm², at which concentration the oxygen vacancy concentration is optimal, resulting in the best ferroelectric performance. Further increasing the concentration leads to a decrease in Pr due to excessive oxygen vacancies pinning the domain walls. Therefore, 0.5% is the optimal doping concentration.

[0090] Figure 4 The images show the Raman spectra before and after modification. The samples all have Raman spectra at approximately 181, 290, 303, 505, and 719 cm⁻¹. -1 A characteristic peak appeared at the position, consistent with the reported BCZT-Tb Raman peak. The Raman peak intensity of the modified sample was significantly improved, indicating improved crystallinity. This demonstrates that CTAB modification helps reduce surface defects, suppress amorphous formation, and enhance the structural stability of the material.

[0091] Figure 5 The XRD patterns before and after modification are shown. The modified ceramic filler exhibits sharp diffraction peaks at 22.3° (100), 31.6° (110), 38.9° (111), 45.4° (200), 56.3° (211), and 66.0° (220) without any impurity phases, indicating that it retains its perovskite structure. Magnified patterns in the 44°–46° range show reflection splitting between the (002) and (200) crystal planes, confirming the coexistence of rhombohedral and tetragonal phases in BCZT-Tb. The results indicate that surface modification did not alter the crystal structure of the inorganic particles.

[0092] Figure 6 The image shows the infrared spectrum of the PVDF fiber film. Films prepared by electrospinning all exhibit high piezoelectric phase content. FTIR analysis shows that at 763 cm⁻¹... -1 872 cm -1 and 1405 cm -1 The absorption peaks at 840 cm⁻¹ belong to the α phase of PVDF, corresponding to the bending vibrations of CH₂ and CF₂, the asymmetric stretching vibrations of C–C–C, and the stretching vibrations of CH₂; while the absorption peaks at 840 cm⁻¹ belong to the α phase of PVDF, corresponding to the bending vibrations of CH₂ and CF₂, the asymmetric stretching vibrations of C–C– -1 and 1175 cm -1The absorption peaks at these locations belong to the β phase, corresponding to the stretching vibrations of CH2 and CF2, and the stretching vibration of CH2, respectively. With increasing doping concentration, the piezoelectric β phase fraction gradually increases. This is due to the local electric field generated during spinning, which exerts strong Coulomb forces on the polymer chains, promoting their arrangement and formation of the β phase. The introduction of piezoelectric particles amplifies this effect.

[0093] When the doping concentration was 13 wt%, the piezoelectric phase content of the sample reached a maximum of 85%. Subsequently, with further doping to 18 wt%, the β phase fraction decreased to 81%. This is because, under appropriate doping concentrations, the CTAB-modified piezoelectric particles promote the transformation of the α phase to the β phase; while excessive doping leads to shorter distances between piezoelectric particles, making them prone to agglomeration or merging. Agglomeration can damage the morphology of the fiber film and the distribution of piezoelectric particles, and affect β phase nucleation.

[0094] The β phase content F(β) in PVDF can be calculated using Beer-Lambert's law, with the following formula:

[0095]

[0096] In the formula, X α X β This represents the content of α and β phases in PVDF. K α It is 6.1 × 10⁴ cm 2 ·mol -1 K β It is 7.7 × 10⁴ cm 2 ·mol -1 , for PVDF in FTIR spectrum at 763 cm⁻¹ -1 and 840cm -1 The absorption coefficient at point A, while A α and A β The PVDF in the FTIR spectrum at 763 cm⁻¹ is respectively -1 and 840 cm -1 Absorption band at that location.

[0097] Figure 7This paper presents the voltage response of a laboratory-made sensor under applied force. As the applied external pressure increases, the sensor's output voltage also increases. This is because the internal structure of the piezoelectric film changes during the stress process. With increasing external pressure, the degree of deformation within the material increases accordingly, leading to an increase in the generation of polarization charges in the piezoelectric composite film. This, in turn, increases the charge density accumulated on the electrode surface, ultimately manifesting as an increase in output voltage on a macroscopic scale. When the pressure increases to 15 N, the film sample doped with 13 wt% piezoelectric particles exhibits a maximum output voltage of 1.85 V, which is twice that of the pure PVDF film. This experimental result demonstrates that the introduction of an appropriate amount of piezoelectric particles can induce the formation of a piezoelectric β phase. Furthermore, the piezoelectric particles themselves, after being polarized by an electric field, also possess piezoelectricity, strengthening the polarization effect at the interface with the PVDF matrix. This synergistically enhances the mechanical-electric coupling efficiency of the material, thereby improving the piezoelectric output performance. When the doping amount is too high (18 wt%), the piezoelectric particles are too numerous and difficult to disperse in the spinning solution. Particle agglomeration can easily lead to instability in the spinning process, destroying the effective separation and transport path of charge, and ultimately resulting in a decrease in piezoelectric output performance.

[0098] Figure 8 The image shows a SEM image of the fiber film with a 13 wt% doping concentration. The fiber distribution uniformity is lower than that of pure PVDF. This is mainly because the introduction of piezoelectric particles disrupts the viscoelastic balance of the polymer spinning solution. The presence of rigid piezoelectric particles restricts the migration ability of polymer chains, promoting local aggregation, which in turn leads to instability in the electrospinning jet and the formation of entangled structures. This microscopic roughness and entangled structure formed by the introduction of fillers not only effectively serve as concentration points for external mechanical stress but also promote the improvement of macroscopic piezoelectric output performance.

[0099] Figure 9 The output voltage of the sensor is shown at different frequencies under a fixed pressure. When the fixed pressure is 15N, the output voltage of the piezoelectric sensor shows a significant upward trend as the frequency increases from 1Hz to 5Hz. This trend is highly consistent with the dynamic response characteristics of piezoelectric materials: when the external excitation frequency increases, the number of stress cycles experienced by the piezoelectric composite material per unit time increases accordingly, and the polarization and depolarization processes within the material accelerate. This acceleration effect comprehensively improves the efficiency of charge generation, separation, and collection, thus macroscopically manifesting as a continuous increase in output voltage. At a frequency of 1Hz, the sensor output voltage reaches approximately 1.2V; when the frequency increases to 3Hz, the output voltage further increases to approximately 2.7V; and at a frequency of 5Hz, the output voltage reaches approximately 5.6V. This experimental data shows that the sensor has a stronger power output capability as the frequency increases.

[0100] Figure 10The voltage response of the self-made sensor prepared in the laboratory using the optimal formulation of Example 1 (13 wt% doping, 0.5 mol% Tb) under different application scenarios is shown in Figure (a). During walking, the sensor output remains stable at approximately 1.05 V, indicating that the flexible device has good responsiveness and reliability in motion sensing, making it suitable for real-time monitoring of human movement. Figure (b) shows that when the sensor is attached to the wrist pulse point, a stable voltage output of approximately 9 mV can still be measured in the resting state, clearly reflecting the pulsating characteristics of the human pulse. This result confirms that the developed composite piezoelectric nanogenerator can effectively detect weak physiological signals under wearable conditions, possessing potential for application in wearable medical diagnostic devices and high-sensitivity biosensing.

[0101] Figure 11 The sensor prepared in Example 1 underwent 5000 fatigue cycle tests at a constant pressure of 15 N. During the cycles, the output voltage remained stable around 1.6 V, demonstrating its good output stability. Furthermore, after 5000 stress cycles, there was no significant shedding or leakage of piezoelectric particles on the fiber, verifying the excellent stability of BCZT-Tb@CTAB on nanofibers.

[0102] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a perovskite-type piezoelectric particle-doped PVDF-based piezoelectric nanofiber thin film, characterized in that, Includes the following steps: (1) Weigh the raw materials according to the stoichiometric ratio, and prepare the chemical formula (Ba) through solid-phase reaction. 0.85 Ca 0.15 ) 1-x Tb x (Zr) 0.1 T i0.9 Lead-free perovskite piezoelectric particles of O3, denoted as BCZT-Tb, where 0.001≤x≤0.007; (2) The BCZT-Tb piezoelectric particles obtained in step (1) were surface modified with hexadecyltrimethylammonium bromide. After washing and drying, the surface-modified piezoelectric particles were obtained and denoted as BCZT-Tb@CTAB. (3) The BCZT-Tb@CTAB piezoelectric particles obtained in step (2) are uniformly dispersed in a polyvinylidene fluoride solution to form a uniform spinning precursor solution. Then, the precursor solution is processed into a nanofiber film by electrospinning. After annealing, a perovskite-type piezoelectric particle-doped PVDF-based piezoelectric nanofiber film is obtained.

2. The method for preparing perovskite-type piezoelectric particle-doped PVDF-based piezoelectric nanofiber thin films according to claim 1, characterized in that: The raw materials for step (1) include BaCO3, CaCO3, TiO2, ZrO2 and Tb4O7 with a purity of ≥99%; the above raw materials are dispersed in anhydrous ethanol, ground evenly, dried and sieved, and then calcined at a high temperature of 1100~1300 ℃ to obtain the BCZT-Tb piezoelectric particles; the doping amount of Tb element x is 0.

005.

3. The method for preparing perovskite-type piezoelectric particle-doped PVDF-based piezoelectric nanofiber thin films according to claim 1, characterized in that: Step (2) specifically includes: preparing a CTAB solution with a mass concentration of 2~6 mg / mL in a mixed solvent of ethanol and water; adding BCZT-Tb piezoelectric particles into the solution and dispersing them ultrasonically, followed by stirring and reacting at 50~60 ℃; after the reaction is completed, centrifuging and washing, and finally drying to obtain BCZT-Tb@CTAB particles; wherein, the ratio of the mixed solvent to the piezoelectric particles is 80~150 mL:1 g; the mass ratio of CTAB to BCZT-Tb is 0.2 : 1~ 0.9 :

1.

4. The method for preparing perovskite-type piezoelectric particle-doped PVDF-based piezoelectric nanofiber thin films according to claim 1, characterized in that: The PVDF solution in step (3) is prepared by PVDF powder and mixed solvent, with the mass fraction of PVDF being 14 wt% to 18 wt%; the mixed solvent is a mixture of N,N-dimethylformamide (DMF) and acetone, with a volume ratio of 7:3 to 8:

2.

5. The method for preparing perovskite-type piezoelectric particle-doped PVDF-based piezoelectric nanofiber thin films according to claim 1, characterized in that: In step (3), the doping amount of the BCZT-Tb@CTAB piezoelectric particles is 3 wt% to 18 wt% of the PVDF mass.

6. The method for preparing perovskite-type piezoelectric particle-doped PVDF-based piezoelectric nanofiber thin films according to claim 5, characterized in that: The doping amount of the BCZT-Tb@CTAB piezoelectric particles is 13 wt% of the PVDF mass.

7. The method for preparing perovskite-type piezoelectric particle-doped PVDF-based piezoelectric nanofiber thin films according to claim 1, characterized in that: The parameters of the electrospinning process in step (3) include: the working environment temperature is 20-30℃, the applied positive polarization voltage is 15-25 kV, the distance between the spinning needle and the receiving roller is 10-20 cm, the solution propulsion rate is 1.0-2.0 mL / h; the annealing temperature is 50-70℃, and the annealing time is 1-3 h.

8. A flexible piezoelectric sensor, characterized in that: Using the preparation method described in any one of claims 1-7, a perovskite-type piezoelectric particle-doped PVDF-based piezoelectric nanofiber film is obtained as a dielectric layer. Conductive electrodes are attached to the upper and lower surfaces of the dielectric layer, and a flexible polymer layer is used for external encapsulation to form a sandwich structure.

9. The application of the flexible piezoelectric sensor according to claim 8 in the field of flexible wearable devices, characterized in that: The flexible piezoelectric sensor is used to collect environmental mechanical energy or is attached to the surface of the human body for real-time monitoring of motion and pulse physiological signals.