A flame-retardant and smoke-suppressing polyester fabric and its preparation method

By constructing a reactive phosphorus and nitrogen smoke-catching layer on the surface of PET fabric and introducing Zn2+ and Al3+ to form a gradient confined flame-retardant and smoke-suppressing layer, the problem of synergistic improvement of flame retardancy, smoke suppression, drip suppression and washability of PET fabric in flame-retardant finishing was solved, and comprehensive performance improvement under low weight gain conditions was achieved.

CN123108931APending Publication Date: 2026-11-17DONGHUA UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611630774.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

There are difficulties in the synergistic improvement of flame retardancy, smoke suppression, drip suppression and washability in the flame retardant finishing of existing PET fabrics, and there are also difficulties in the dispersion and fixation of metal or inorganic nano flame retardant and smoke suppressant components in the fabric finishing process.

Method used

A reactive phosphorus and nitrogen smoke-catching layer is constructed on the surface of PET fabric. Phosphorus compounds, amino polymers and modified attapulgite are fixed by ionic crosslinking and coordination crosslinking. Then, Zn2+ is introduced under weakly acidic conditions to form inner catalytic sites, and Al3+ is introduced under slow-release alkaline conditions to form outer Al-OP skeleton, thus constructing a gradient confined flame-retardant and smoke-suppressing layer. Finally, wet heat treatment or baking treatment is performed.

Benefits of technology

Under conditions of low finishing weight gain, it achieves a synergistic improvement in flame retardancy, smoke suppression, drip suppression and washability, reduces peak heat release rate, smoke generation rate and total smoke release, and maintains the softness and breathability of the fabric.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108931A_ABST
    Figure CN123108931A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of PET flame retardant and smoke-suppressing finishing technology, and relates to a flame retardant and smoke-suppressing polyester fabric and its preparation method. The preparation process involves first constructing a reactive phosphorus-nitrogen smoke-catching layer on the surface of a PET fabric that has undergone shallow activation treatment. Then, the PET fabric with the reactive phosphorus-nitrogen smoke-catching layer is sequentially immersed in a first finishing solution and a second finishing solution to form a gradient-confined flame retardant and smoke-suppressing layer with enriched Zn catalytic sites on the inner side and Al-O-P skeleton sites on the outer side. Finally, the immersed PET fabric undergoes post-treatment to obtain the fabric. The fabric includes a PET base fabric, a reactive phosphorus-nitrogen smoke-catching layer fixed to the surface of the PET base fabric, and a gradient-confined flame retardant and smoke-suppressing layer located on the surface of the reactive phosphorus-nitrogen smoke-catching layer. This invention improves the utilization rate of metal active sites and the stability of the char layer; the fabric achieves a synergistic improvement in flame retardancy, smoke suppression, drip suppression, and washability with low weight gain.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of PET flame retardant and smoke suppressant finishing technology, and relates to a flame retardant and smoke suppressant polyester fabric and its preparation method. Background Technology

[0002] PET fabrics inherently have a low limiting oxygen index (LOI). Reference 1 (Durable flame retardant and anti-dripping of PET fabric using bio-based covalent crosslinking intumescent system of chitosan and phytic acid. Progress in Organic Coatings, 2023, 183:107785.) reports that its LOI is typically only 20%–22%. During combustion, it is prone to melting and dripping, which can ignite underlying combustibles. Therefore, flame-retardant finishing of PET requires addressing both flame retardancy and drip suppression simultaneously. Furthermore, polyester fibers themselves have weak char-forming ability, making it difficult to form a stable protective char layer during combustion. Thus, there is a challenge in achieving synergistic improvement in flame retardancy, char formation, smoke suppression, and drip suppression.

[0003] Existing PET finishing systems mostly rely on electrostatic adsorption, hydrogen bonding, physical coating, or weak coordination to fix flame-retardant components. Reference 1 points out that layer-by-layer flame-retardant finished fabrics suffer from poor wash durability due to the lack of covalent bonds between the flame retardant and the fabric, and the water solubility of some bio-based flame-retardant components. Therefore, the weak bonding of flame-retardant and smoke-suppressing components to the PET fiber surface, as well as their migration or loss during washing, are objectively existing problems.

[0004] While metallic or inorganic nano-flame retardant and smoke-suppressing components can promote catalytic char formation and smoke suppression, they face difficulties in dispersion and fixation during fabric finishing. Reference 2 (Construction of durable flame retardant, anti-dripping, and smoke-suppressing recycled polyester fabric. PolymerDegradation and Stability, 2024, 226: 110827.) points out that inorganic nano-flame retardant components suffer from problems such as high addition amounts, poor dispersibility, impact on mechanical properties, and difficulty in adsorption and fixation on textiles. Reference 3 (ZnOnanostructured materials and their potential applications. NanoscaleAdvances, 2022, 4: 1868-1925.) indicates that ZnO and other metal oxide nanoparticles are also prone to aggregation due to their high surface energy. Therefore, metallic flame retardant and smoke-suppressing components are prone to aggregation, migration, and low utilization of active sites in conventional co-bath finishing or direct application systems.

[0005] Therefore, it is of great significance to study a flame-retardant and smoke-suppressing polyester fabric and its preparation method, so as to achieve a synergistic improvement in flame retardancy, smoke suppression, drip suppression and washability under low weight gain conditions. Summary of the Invention

[0006] The purpose of this invention is to solve the problems existing in the prior art and to provide a flame-retardant and smoke-suppressing polyester fabric and its preparation method.

[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0008] A method for preparing flame-retardant and smoke-suppressing polyester fabric involves first constructing a reactive phosphorus and nitrogen smoke-catching layer on the surface of a PET fabric that has undergone shallow activation treatment, then immersing the PET fabric with the reactive phosphorus and nitrogen smoke-catching layer in a first finishing solution and a second finishing solution in sequence to form a gradient confined flame-retardant and smoke-suppressing layer with enriched Zn catalytic sites on the inner side and enriched Al-OP skeleton sites on the outer side, and finally performing post-treatment on the PET fabric after immersion treatment to obtain the flame-retardant and smoke-suppressing polyester fabric.

[0009] The reactive phosphorus-nitrogen smoke trapping layer contains phosphorus compounds, amino-containing polymers, and modified attapulgite, and is fixed to the surface of PET fibers through at least one of ionic crosslinking and coordination crosslinking. The phosphorus compound is phytic acid or phytate, and the amino-containing polymer is chitosan or polyethyleneimine. The modified attapulgite is attapulgite surface-modified with phosphate, phytic acid, or silane coupling agents. Ionic crosslinking is formed by the electrostatic interaction between the phosphate groups in phytic acid or phytate and the protonated amino groups in chitosan or polyethyleneimine. Zn is subsequently introduced... 2+ And Al 3+ It can coordinate with multiple sites such as phosphate groups, hydroxyl groups and amino groups in the phosphorus and nitrogen smoke trapping layer, and can coordinate or exchange with hydroxyl groups or exchangeable ion sites on the surface of modified attapulgite, thereby improving the fixation stability of the phosphorus and nitrogen smoke trapping layer. Compared with unmodified ordinary attapulgite, modified attapulgite can improve its interfacial bonding with the phosphorus and nitrogen smoke trapping network and improve the effective utilization at low addition levels.

[0010] The first finishing solution contains Zn. 2+ A weak complexing agent, which is one or more of citric acid, lactic acid, and gluconic acid, is used. The pH of the first finishing solution is 4.2~5.5. Under weakly acidic conditions, the pH of the first finishing solution can make Zn... 2+ It forms a complex with weak complexing agents, possessing a certain migration capability, thus reducing Zn. 2+ The possibility of premature hydrolysis or surface deposition allows it to diffuse into regions closer to the PET matrix and coordinate or be fixed by ion exchange at sites such as phosphate groups, amino groups, and hydroxyl groups.

[0011] The second finishing solution contains Al 3+ The solution contains a slow-release alkali component, which is one or more of urea and hexamethylenetetramine. The pH of the second finishing solution is 4.5–5.2. The impregnation treatment in the second finishing solution is divided into two stages: the first stage treatment temperature is 25–45 °C, and the second stage treatment temperature is 50–70 °C. After the second stage treatment, the pH of the second finishing solution gradually increases to 6.5–7.8. The first stage uses a lower temperature impregnation treatment, the main purpose of which is to allow the Al to... 3+ The phosphorus and nitrogen smoke traps fully penetrate and diffuse into the reactive phosphorus and nitrogen smoke trapping layer, preventing premature hydrolysis or rapid deposition on the fabric surface. The second stage employs a higher temperature treatment to promote the slow-release alkaline components' effectiveness, gradually increasing the system pH and promoting Al2O3 production. 3+ Hydrolysis, hydroxyl bridging, and coordination fixation with phosphate groups make it easier for confined cross-linking and deposition to occur in the region of the reactive phosphorus and nitrogen smoke trapping layer near the air side, thereby forming a more stable Al-OP framework structure on the outer side.

[0012] Post-treatment is either wet heat treatment or baking treatment;

[0013] The weight gain rate of flame-retardant and smoke-suppressing polyester fabrics is 1.5-5.0%.

[0014] The weight gain rate, calculated only for the mass increase resulting from subsequent phosphorus and nitrogen smoke trapping layers, Zn / Al finishing, and post-treatment, is determined using the following formula:

[0015] Weight gain rate = (m1 - m0) / m0 × 100%;

[0016] Wherein, m0 is the mass of the PET fabric after drying to constant weight after shallow activation treatment and before constructing the reactive phosphorus and nitrogen smoke-catching layer, and m1 is the mass of the PET flame-retardant and smoke-suppressing fabric after drying to constant weight after completing all finishing and post-treatment.

[0017] Under low finishing weight gain conditions, this invention constructs a Zn / Al flame-retardant and smoke-suppressing layer with functional partitions in the thickness direction through stepwise diffusion of Zn followed by Al, pH control, and gradient confinement in-situ transformation, thereby achieving simultaneous improvement in flame retardancy, smoke suppression, drip suppression, and washability.

[0018] Specifically, this invention differs from conventional metal salt co-bath finishing, direct external addition of metal oxides, or ordinary phosphorus-nitrogen coatings. In conventional systems, metal components such as Zn and Al are usually randomly deposited or uniformly distributed, easily leading to low utilization of metal active sites, local agglomeration, and washing loss. In contrast, this invention employs a Zn-first, then Al treatment sequence. Under weakly acidic conditions, Zn is first diffused and fixed towards the region near the PET matrix, forming inner Zn-P / N / O catalytic sites. Then, under slow-release alkaline conditions, Al is introduced, causing it to primarily form Al-OP framework sites near the air side. This results in a gradient confinement structure of "inner Zn catalytic secondary carbonization and outer Al-OP stable shielding for carbonization."

[0019] As a preferred technical solution:

[0020] The preparation method of flame-retardant and smoke-suppressing polyester fabric as described above, the shallow activation treatment refers to at least one of alkali reduction micro-etching, low-temperature plasma treatment and ultraviolet-ozone synergistic treatment. The ultraviolet-ozone synergistic treatment is to generate ozone and active oxygen species by ultraviolet light irradiation in an oxygen-containing atmosphere, and to oxidize and activate the surface of PET fibers, thereby introducing oxygen-containing active groups such as hydroxyl and carboxyl groups. The depth of the shallow activation treatment is 10~300nm.

[0021] In the method for preparing a flame-retardant and smoke-suppressing polyester fabric as described above, the mass ratio of phosphorus compound, amino-containing polymer and modified attapulgite is 1~5:1~5:0.2~3.

[0022] As described above, in the preparation method of a flame-retardant and smoke-suppressing polyester fabric, Zn in the first finishing solution 2+The source is one or more of zinc acetate, zinc nitrate, and zinc gluconate, Zn 2+ The concentration is 0.03~0.18 mol / L, and the weak complexing agent is combined with Zn. 2+ The molar ratio is 0.3~1.5:1;

[0023] The first finishing solution is applied at a temperature of 25~70℃ for 10~45 minutes.

[0024] As described above, in the preparation method of a flame-retardant and smoke-suppressing polyester fabric, Al in the second finishing solution 3+ The source is one or more of aluminum nitrate, aluminum acetate, and aluminum lactate, Al 3+ The concentration is 0.03~0.18 mol / L, and the slow-release alkali component is related to Al. 3+ The molar ratio is 0.5~3.0:1;

[0025] The sample is immersed in the second finishing solution for 5-20 minutes in the first stage and 10-30 minutes in the second stage.

[0026] As described above, in the preparation method of a flame-retardant and smoke-suppressing polyester fabric, Zn in the first finishing solution 2+ With Al in the second finishing solution 3+ The molar ratio is 0.5~3:1.

[0027] The method for preparing a flame-retardant and smoke-suppressing polyester fabric as described above involves a wet heat treatment at a temperature of 80-120°C for 20-90 minutes.

[0028] The baking temperature is 120~170℃ and the time is 2~15min.

[0029] The present invention also provides a flame-retardant and smoke-suppressing polyester fabric prepared by the method described above, comprising a PET base fabric, a reactive phosphorus and nitrogen smoke-catching layer fixed on the surface of the PET base fabric, and a gradient confinement flame-retardant and smoke-suppressing layer located on the surface of the reactive phosphorus and nitrogen smoke-catching layer.

[0030] The reactive phosphorus and nitrogen smoke trapping layer includes a phosphorus and nitrogen smoke trapping network and modified attapulgite dispersed and fixed in the phosphorus and nitrogen smoke trapping network. The phosphorus and nitrogen smoke trapping network is composed of phosphorus compounds and amino-containing polymers.

[0031] The inner side of the gradient-confined flame-retardant and smoke-suppressing layer is enriched with Zn catalytic sites, while the outer side is enriched with Al-OP framework sites.

[0032] Based on the inner 30% thickness region and the outer 30% thickness region of the gradient confined flame retardant and smoke suppressant layer, the Zn / Al atomic ratio in the inner region is more than 1.5 times that in the outer region, and the Al / P atomic ratio in the outer region is higher than that in the inner region.

[0033] As a preferred technical solution:

[0034] The flame-retardant and smoke-suppressing polyester fabric described above has a reactive phosphorus and nitrogen smoke-catching layer with a thickness of 80~800nm.

[0035] The thickness of the gradient-confined flame-retardant and smoke-suppressing layer is 120~1200nm;

[0036] The Zn catalytic sites enriched on the inner side of the gradient confined flame-retardant and smoke-suppressing layer contain one or more of the following coordination structures: Zn-OP, Zn-N, and Zn-O.

[0037] The Al-OP framework sites enriched on the outer side of the gradient-confined flame-retardant and smoke-suppressing layer contain one or more of the following bridging structures: Al-OP, Al-O-Al, and Al-OH.

[0038] The flame-retardant and smoke-suppressing polyester fabric described above has a limiting oxygen index of not less than 30.0%, a vertical combustion afterflame time of not more than 2 seconds, a smoldering time of not more than 2 seconds, and the molten droplets generated during vertical combustion do not ignite the degreased cotton. Under the same cone calorimetry test conditions, compared with the untreated PET fabric of the same specification, the peak heat release rate of the flame-retardant and smoke-suppressing polyester fabric is reduced by not less than 50%, the peak smoke generation rate is reduced by not less than 60.0%, and the total smoke release is reduced by not less than 55%. After 10 standard washes, the limiting oxygen index of the flame-retardant and smoke-suppressing polyester fabric is not less than 26.0%, it can still self-extinguish, and the molten droplets generated during vertical combustion do not ignite the degreased cotton.

[0039] Compared with existing technologies, the LOI of chitosan / phytic acid flame-retardant PET fabric reported in Literature 1 can reach 34.0%, but it mainly reflects the flame-retardant and anti-dripping effects of the chitosan / phytic acid covalently cross-linked intumescent flame-retardant system. Although the LOI of this invention does not aim to significantly exceed that of the literature, it achieves good smoke suppression, anti-dripping performance, and post-wash performance retention under relatively low finishing weight gain conditions. In particular, the reduction in peak heat release rate (pkHRR), total smoke release (TSR), and peak smoke generation rate (pSPR) of this invention demonstrates its significant effect in low smoke and heat release suppression. Reference 2 also points out that inorganic nano-flame retardant and smoke suppressant components have problems with dispersion, fixation and durability in the finishing of polyester fabrics; Reference 3 further points out that metal oxide nanomaterials such as ZnO are prone to agglomeration due to their high surface energy; Reference 4 (Flame retardant challenges for textiles and fibres: New chemistry versus innovative solutions. Polymer Degradation and Stability, 2011, 96(3): 377–392.) points out that polyester fibers such as PET have weak char-forming ability, and it is difficult to take into account char-forming, flame retardant and wearability properties in flame retardant modification.

[0040] Therefore, the superiority of this invention should be understood as the comprehensive synergistic advantage of multiple indicators under low finishing weight gain conditions, rather than the absolute highest value of a single LOI indicator. This invention, through a specific gradient-confined Zn / Al structure, achieves a balance between increased LOI, reduced heat release, reduced smoke release, anti-dripping, and post-wash stability at a relatively low weight gain, representing a significant advancement over existing PET flame-retardant finishing technologies.

[0041] Invention principle:

[0042] This invention is based on the characteristic that combustible volatiles and flue gas precursors are mainly released from the fiber surface during the pyrolysis of PET, and utilizes Zn 2+ With Al 3+ Differences in complexation migration, hydrolysis deposition, phosphate coordination and cross-linking fixation capabilities allow for the formation of a gradient flame-retardant and smoke-suppressing layer with functional partitions in the thickness direction on the surface of PET fibers through a continuous control process of "surface activation - phosphorus and nitrogen smoke-capturing layer construction - Zn internal diffusion fixation - Al outer layer confined cross-linking - wet heat / baking in-situ conversion".

[0043] Specifically, the shallow activation treatment generates reactive sites such as carboxyl and hydroxyl groups on the surface of PET fibers, providing an interfacial anchoring basis for the stable binding of subsequent phosphorus and nitrogen components.

[0044] Phytic acid or phytate, chitosan or polyethyleneimine, and modified attapulgite components in reactive phosphorus and nitrogen-containing smoke traps can, on the one hand, provide functional groups such as phosphate groups, amino groups, and hydroxyl groups, as well as inorganic adsorption / skeletal sites, thereby playing the roles of acid source, nitrogen source, carbon layer promotion, and flue gas adsorption; on the other hand, these components can provide Zn 2+ And Al 3+ It provides coordination, ion exchange, or cross-linking fixation sites, so that Zn and Al metal sites are confined and fixed in the phosphorus and nitrogen smoke trapping layer.

[0045] Under weakly acidic conditions, Zn 2+ It forms a complex migration state with a certain diffusion capability with a weak complexing agent, which can penetrate into the phosphorus and nitrogen smoke trap layer towards the side closer to the PET matrix. There, it undergoes decomplexing or ion exchange fixation with phosphorus, nitrogen, and oxygen coordinating groups, forming inner-enriched Zn-P / N / O catalytic sites. During combustion or thermal decomposition, these inner Zn catalytic sites are close to the PET thermal decomposition source region, preferentially acting on flue gas precursors such as benzene series compounds, aromatic esters, and aldehydes, promoting their condensation, aromatization, cross-linking, and deposition carbonization, thereby reducing the release of combustible volatiles and flue gas.

[0046] Al was then introduced under near-neutral or slow-release alkaline conditions. 3+ Using AI 3+ Its strong hydrolysis, hydroxyl bridging, phosphate coordination, and cross-linking fixation capabilities enable it to undergo confined cross-linking, deposition, or gelation transformation primarily in the air-side region of the phosphorus and nitrogen smoke trapping layer, forming an outer Al-OP enriched char layer framework structure. During combustion, this outer Al-OP framework enhances the continuity, density, thermal stability, and oxidation resistance of the char layer, and provides a shielding coating and physical constraint for molten PET, reducing the risk of droplet generation and ignition.

[0047] After wet heat treatment or baking, Zn and Al sites undergo further confined in-situ transformation within the phosphorus and nitrogen smoke-collecting layer, forming dispersed Zn-Al-P / N / O amorphous nanoclusters, low-crystallinity zinc aluminum phosphate structures, or metal-phosphorus / nitrogen / oxygen coordination networks. This constructs a gradient confined flame-retardant and smoke-suppressing structure with "inner layer Zn catalyzing secondary carbonization and outer layer Al stabilizing and shielding carbonization," enabling PET fabrics to achieve synergistic improvements in flame retardancy, low smoke, drip suppression, and washability stability under relatively low finishing weight gain conditions.

[0048] Beneficial effects:

[0049] (1) A method for preparing a flame-retardant and smoke-suppressing polyester fabric according to the present invention involves stepwise diffusion of Zn followed by Al, pH control and confined in-situ conversion, forming a gradient confined structure in the reactive phosphorus and nitrogen smoke-catching layer on the surface of PET fibers, with the inner Zn-P / N / O catalytic sites enriched and the outer Al-OP carbon layer skeleton enriched. This improves the dispersion stability of metal components, the interfacial bonding stability and the protective effect of the carbon layer, so as to achieve a synergistic improvement in flame retardancy, smoke suppression, drip suppression and washability stability under low finishing weight gain conditions, and is conducive to maintaining the softness, breathability and mechanical properties of the fabric.

[0050] (2) The flame-retardant and smoke-suppressing polyester fabric of the present invention, compared with metal salt co-bath finishing, metal oxide addition and ordinary phosphorus and nitrogen coating, can avoid random distribution, agglomeration and detachment of metal components and migration precipitation, and improve the utilization efficiency of metal active sites; wherein the inner Zn sites are close to the PET thermal decomposition source area, which can promote the condensation, aromatization and deposition carbonization of flue gas precursors such as benzene series, aromatic esters and aldehydes, thereby reducing the release of flue gas and combustible volatiles from the source; the outer Al-OP skeleton can enhance the continuity, density, thermal stability of the carbon layer and the encapsulation and constraint effect on molten PET, reducing the risk of dripping and ignition. Attached Figure Description

[0051] Figure 1 The FTIR spectra of PET, PET-PN, PET-PN-Zn, and PET-PN-Zn-Al in Example 1 are shown below.

[0052] Figure 2 XPS full spectra of PET, PET-PN, and PET-PN-Zn in Example 1;

[0053] Figure 3 The O 1s high-resolution spectrum of the PET-PN-Zn sample in Example 1. Detailed Implementation

[0054] The present invention will be further described below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.

[0055] The test methods involved in the performance indicators in the embodiments and comparative examples of this invention are as follows:

[0056] Limiting Oxygen Index (LOI): Tested according to GB / T 5454-1997 "Test for Burning Performance of Textiles - Oxygen Index Method". Specimens measuring 150 mm × 58 mm were cut, and the number of specimens and sampling direction were in accordance with the standard. Before testing, the specimens were conditioned for 24 hours under standard atmospheric conditions of 20±2 ℃ and 65±4% relative humidity. The specimen was vertically clamped in the center of the combustion chamber of the oxygen index tester. The top of the specimen was ignited under conditions where the oxygen-nitrogen mixture stably passed through the combustion chamber from bottom to top. The oxygen concentration was adjusted using a lifting method. The lowest oxygen concentration at which the combustion time or combustion length after the specimen left the ignition source reached the standard-specified criterion was used as the limiting oxygen index. The result was expressed as the volume fraction of oxygen in the oxygen-nitrogen mixture, rounded to 0.1%.

[0057] Vertical burning: The test was conducted according to GB / T 5455-2014 "Determination of Vertical Damage Length, Afterflame and Afterburning Time of Textiles". Five samples of 300 mm × 89 mm were cut along both the warp and weft directions of the fabric, with the sampling position at least 100 mm from the fabric edge. After conditioning the samples for 24 h under standard atmospheric conditions of 20 ± 2 ℃ and 65 ± 4% relative humidity, they were vertically mounted in the sample holder of the burning test apparatus. Using propane as fuel, the flame height was adjusted to 40 ± 2 mm, and the flame was applied to the center of the bottom edge of the sample for 12 s. After removing the igniter, the afterburning time, afterflame time and damage length were recorded. The average value of the test results for each direction was calculated separately.

[0058] Post-wash performance testing: Washing was conducted according to GB / T 8629-2017 "Domestic Washing and Drying Procedures for Testing Textiles". A type A horizontal drum front-door feeding standard washing machine was used, with the 4N washing program selected and the washing temperature set at 40±3℃. Standard detergent 3 as specified in the standard was used, and polyester accompaniment was added to make the total dry weight of the sample and accompaniment 2.0±0.1 kg. After each washing cycle, the sample was hung to dry according to program A. One washing and drying process was recorded as one standard wash, and a total of 10 washes were repeated. After the 10th wash and drying, the sample was conditioned for 24 h under standard atmospheric conditions of 20±2℃ and 65±4% relative humidity. Subsequently, the limiting oxygen index after washing was determined according to GB / T 5454-1997, and the vertical flammability after washing was determined according to GB / T 5455-2014.

[0059] Conical calorimetry test: at 35 kW / m 2 Cone calorimetry was performed according to ISO 5660-1 under thermal radiation flux; the peak heat release rate (pkHRR) of the untreated raw material PET fabric was measured to be 88.14 kW / m². 2The peak time was 28 s; the peak smoke generation rate (pSPR) of untreated PET fabric was 0.0360 m. 2 / s; Total smoke emission (TSR) was 59.1 m³ / s. 2 / m 2 .

[0060] In the embodiments of the present invention, the feeding mass ratio of phosphorus compound, amino-containing polymer and modified attapulgite is calculated based on the oven-dry mass of each component; when polyethyleneimine is used in the form of an aqueous solution, its feeding mass is calculated based on the effective solid content of polyethyleneimine therein.

[0061] The original attapulgite was Acti-Gel® 208 dry powder attapulgite manufactured by Active Minerals International. Before use, it was dried in an 80 °C vacuum drying oven for 12 h, cooled to room temperature, and then sealed for storage. The mass of attapulgite and each modifier was calculated based on dry weight. Four types of modified attapulgite were prepared by the following methods.

[0062] Sodium dihydrogen phosphate modified attapulgite: Weigh 10.0 g of dried Acti-Gel® 208 attapulgite and add it to 200 mL of deionized water. Stir at 500 r / min for 30 min, then ultrasonically disperse at 40 kHz and 300 W for 30 min, controlling the system temperature not to exceed 35 ℃ during ultrasonication, to obtain an attapulgite dispersion. Separately, dissolve 1.0 g of sodium dihydrogen phosphate in 20 mL of deionized water and add it to the attapulgite dispersion under stirring. Heat the mixture to 60 ℃ and stir at 500 r / min for 4 h. After the reaction, cool to room temperature, separate the solid by centrifugation, and wash with deionized water to remove unadsorbed free sodium dihydrogen phosphate. Dry the obtained solid under vacuum at 60 ℃ for 12 h, grind and pass through a 200-mesh sieve to obtain sodium dihydrogen phosphate modified attapulgite.

[0063] Phytic acid-modified attapulgite: Weigh 10.0 g of dried Acti-Gel® 208 attapulgite, add 200 mL of deionized water, stir at 500 r / min for 30 min, and then ultrasonically disperse at 40 kHz and 300 W for 30 min, controlling the system temperature not to exceed 35 ℃. Weigh the commercial phytic acid solution according to the dry basis mass ratio of attapulgite to phytic acid of 8:1 or 6:1, where the phytic acid mass is calculated according to the effective content of the product. Dilute the commercial phytic acid solution with 20 mL of deionized water and add it to the attapulgite dispersion under stirring. Heat the mixture to 60 ℃ and stir at 500 r / min for 4 h. After the reaction is complete, cool to room temperature, separate the solid by centrifugation, and wash three times with deionized water to remove unfixed free phytic acid. The obtained solid is vacuum dried at 60 ℃ for 12 h, ground, and passed through a 200-mesh sieve to obtain phytic acid-modified attapulgite.

[0064] KH560 modified attapulgite: Weigh 1.0 g of KH560 and add it to a mixed solvent consisting of 80 mL of anhydrous ethanol and 20 mL of deionized water. Adjust the pH of the system to 4.5±0.2 using an aqueous acetic acid solution under stirring. Pre-hydrolyze the mixture at 25±2 °C and 500 r / min for 30 min to obtain a KH560 pre-hydrolyzed solution. Separately weigh 10.0 g of dried Acti-Gel®208 attapulgite and add it to the KH560 pre-hydrolyzed solution. Disperse the mixture ultrasonically at 40 kHz and 300 W for 30 min, controlling the system temperature not to exceed 35 °C. Then, heat the system to 70 °C and stir at 500 r / min for 4 h. After the reaction, cool to room temperature and separate the solid by centrifugation. Wash the solid sequentially with ethanol and deionized water to remove unreacted or physically adsorbed KH560. The obtained solid was vacuum dried at 60 °C for 12 h, then cured at 100 °C for 2 h, cooled, ground and passed through a 200-mesh sieve to obtain KH560 modified attapulgite.

[0065] KH570 modified attapulgite: Except for replacing KH560 with an equal mass of KH570, the other raw material dosages, pre-hydrolysis conditions, ultrasonic dispersion conditions, reaction temperature, reaction time, washing, drying and curing conditions are the same as those for KH560 modified attapulgite.

[0066] Example 1

[0067] A method for preparing a flame-retardant and smoke-suppressing polyester fabric, comprising the following specific steps:

[0068] (1) Alkali reduction micro-etching;

[0069] The PET fabric was placed in a 5 g / L sodium hydroxide aqueous solution at a bath ratio of 1:30 and treated at 50 °C for 10 min. After treatment, it was neutralized with a 1 g / L acetic acid aqueous solution for 2 min, then washed with deionized water until neutral, and dried at 60 °C for 2 h to obtain the PET fabric after alkali reduction micro-etching treatment. The depth of the alkali reduction micro-etching treatment was 10 nm.

[0070] (2) Construct a reactive phosphorus and nitrogen smoke trapping layer on the surface of the PET fabric treated in step (1);

[0071] (2.1) Add 2.0 g of chitosan to an appropriate amount of acetic acid aqueous solution with a mass fraction of 1.0%, stir at 500 r / min for 4 h at 25±2 ℃ to fully dissolve the chitosan, and adjust the pH of the system to 3.5±0.2;

[0072] Chitosan is a low molecular weight chitosan, manufactured by Sigma-Aldrich, with product number 448869, a degree of deacetylation of 75%~85%, and a nominal molecular weight of 50,000~190,000.

[0073] (2.2) Add 0.5 g of sodium dihydrogen phosphate modified attapulgite to the chitosan solution obtained in step (2.1), and ultrasonically disperse it for 30 min at a frequency of 40 kHz and a power of 300 W. During the ultrasonic process, control the system temperature to not exceed 35 ℃. Then stir at 500 r / min for 30 min, and then make up the system to 100.0 g with acetic acid aqueous solution with a mass fraction of 1.0% to obtain a finishing solution containing 2.0 wt% chitosan and 0.5 wt% sodium dihydrogen phosphate modified attapulgite, i.e. chitosan / sodium dihydrogen phosphate modified attapulgite finishing solution;

[0074] In sodium dihydrogen phosphate modified attapulgite, the mass ratio of attapulgite to sodium dihydrogen phosphate is 10:1.

[0075] (2.3) The PET fabric treated in step (1) was immersed in chitosan / sodium dihydrogen phosphate modified attapulgite finishing solution at a ratio of 1:30 according to the ratio of fabric mass to finishing solution mass. The solution was shaken and immersed at 100 r / min for 30 min at 40 ℃. After the fabric was removed, it was rolled in a one-dip-one-rolling manner. The roller pressure was 0.20 MPa and the roller linear speed was 1.0 m / min. The roll residue was controlled to be 80±5%.

[0076] (2.4) According to the ratio of fabric mass to finishing solution mass of 1:30, the fabric after padding is immersed in phytic acid aqueous solution with a mass fraction of 2.0% and a pH of 2.5±0.2, and shaken at 100 r / min for 20 min at 30 ℃, so that the phosphate groups in phytic acid and the protonated amino groups in chitosan undergo ionic cross-linking to form a phosphorus nitrogen smoke catching network, and the modified attapulgite is embedded and fixed in the formed phosphorus nitrogen smoke catching network.

[0077] (2.5) After the treatment in step (2.4) is completed, the fabric is rinsed in deionized water at 25±2℃ for 30 s according to the ratio of fabric mass to deionized water volume of 1 g: 50 mL, then lightly rolled once under 0.10 MPa pressure, and finally dried under vacuum at 60℃ for 2 h to obtain a PET fabric with a reactive phosphorus and nitrogen smoke trapping layer on the surface, denoted as PET-PN;

[0078] (3) The PET fabric with the reactive phosphorus and nitrogen smoke trapping layer constructed in step (2) was placed in the first finishing solution with pH 4.2 and immersed at 25 °C for 45 min. The resulting product was denoted as PET-PN-Zn.

[0079] The first finishing solution is a mixed solution of zinc acetate and citric acid, Zn 2+ The concentration is 0.03 mol / L, citric acid and Zn 2+ The molar ratio is 0.3:1;

[0080] (4) The PET fabric treated in step (3) is immersed in the second finishing solution to form a gradient confined flame retardant and smoke suppressing layer with enriched Zn catalytic sites on the inner side and enriched Al-OP skeleton sites on the outer side.

[0081] The immersion treatment in the second finishing solution was divided into two stages. The first stage was treated at a temperature of 25 ℃ for 20 min, and the second stage was treated at a temperature of 50 ℃ for 30 min. After the second stage treatment, the pH of the second finishing solution was gradually increased to 6.5.

[0082] The second finishing solution is a mixed solution of aluminum nitrate and urea, with a pH of 4.5; the second finishing solution contains Al 3+ At a concentration of 0.03 mol / L, urea and Al 3+ The molar ratio of Zn in the first finishing solution is 0.5:1. 2+ With Al in the second finishing solution 3+ The molar ratio is 1.0:1;

[0083] (5) The PET fabric after impregnation in step (4) is subjected to wet heat treatment for 90 min under normal pressure, 80 ℃ and relative humidity of 90±5% to obtain flame-retardant and smoke-suppressing polyester fabric, denoted as PET-PN-Zn-Al.

[0084] The resulting flame-retardant and smoke-suppressing polyester fabric comprises a PET base fabric, a reactive phosphorus-nitrogen smoke-catching layer fixed to the surface of the PET base fabric, and a gradient-confined flame-retardant and smoke-suppressing layer located on the surface of the reactive phosphorus-nitrogen smoke-catching layer. The reactive phosphorus-nitrogen smoke-catching layer consists of a phosphorus-nitrogen smoke-catching network and attapulgite dispersed and fixed within the phosphorus-nitrogen smoke-catching network. The inner side of the gradient-confined flame-retardant and smoke-suppressing layer is enriched with Zn catalytic sites, while the outer side is enriched with Al-OP framework sites. Based on a 30% thickness region on both the inner and outer sides of the gradient-confined flame-retardant and smoke-suppressing layer, the Zn / Al atomic ratio in the inner region is 1.6 times that in the outer region, and the Al / P atomic ratio in the outer region is 1.2 times that in the inner region. The thickness of the reactive phosphorus-nitrogen smoke-catching layer is 80 nm, and the thickness of the gradient-confined flame-retardant and smoke-suppressing layer is 120 nm. nm; The Zn catalytic sites enriched on the inner side of the gradient-confined flame-retardant and smoke-suppressing layer contain Zn-OP and Zn-O coordination structures; The Al-OP skeleton sites enriched on the outer side of the gradient-confined flame-retardant and smoke-suppressing layer contain Al-OP and Al-OH bridging structures; The finishing weight gain of the flame-retardant and smoke-suppressing polyester fabric is 1.5%, the limiting oxygen index is 30%, the vertical combustion afterflame time is 2 s, the smoldering time is 2 s, and the molten droplets generated during vertical combustion do not ignite the degreased cotton; Under the same cone calorimetry test conditions, compared with the unfinished PET fabric of the same specification, the peak heat release rate of the flame-retardant and smoke-suppressing polyester fabric is reduced by 58.5%, the peak smoke generation rate (pSPR) is reduced by 60%, and the total smoke release is reduced by 65%; After 10 standard washes, the limiting oxygen index of the flame-retardant and smoke-suppressing polyester fabric is 26%, it can still self-extinguish, and the molten droplets generated during vertical combustion do not ignite the degreased cotton.

[0085] Zn using FTIR and XPS 2+ The interaction between the P / N / O functional groups in the reactive phosphorus-nitrogen smoke trap was analyzed. Figure 1 In comparison with PET-PN, the peak positions, shapes, and relative intensities of the P=O / PO, POC, -NH / -OH, and NH related absorption bands in the PET-PN-Zn sample changed to some extent. Furthermore, absorption signals attributable to Zn-O related vibrations appeared in the low wavenumber region, indicating that Zn... 2+ Coordination, ion exchange, or cross-linking fixation occurred between the P / N / O functional groups such as phosphate, amino, and hydroxyl groups.

[0086] Figure 2XPS full spectrum showed that the PET-PN-Zn sample exhibited a distinct Zn 2p characteristic peak; its O 1s high-resolution spectrum ( Figure 3 The oxygen-containing components belonging to POC and Zn-O / PO-Zn can be identified. These results collectively demonstrate that Zn species have been introduced into the phosphorus-nitrogen smoke trap and support their interaction with oxygen-containing sites such as phosphate groups and hydroxyl groups, providing characterization evidence for the formation of Zn-containing catalytic sites.

[0087] Further introduction of AI 3+ After being subjected to damp heat treatment, the absorption bands of P=O / PO, POC, and -NH / -OH in the PET-PN-Zn-Al sample changed relative to PET-PN, and the Al-OP / PO-Al related absorption signal appeared, indicating that the Al species coordinated, bridged or cross-linked with phosphate groups and other oxygen-containing groups, supporting the formation of Al-OP related framework structures.

[0088] Based on the preparation sequence and FTIR and XPS results, it can be concluded that Zn and Al species are immobilized in the reactive phosphorus-nitrogen smoke trap layer, forming dispersed Zn / Al composite coordination sites. This structure is beneficial for improving the dispersion and immobilization stability of the metal components; among them, the Zn-related sites may promote the catalytic carbonization and secondary condensation of PET pyrolysis products, while the Al-OP-related structure may improve the continuity, density, and thermal stability of the carbon layer, thereby contributing to improved flame retardant, smoke suppression, and drip suppression performance.

[0089] Comparative Example 1

[0090] A method for preparing a PET flame-retardant and smoke-suppressing fabric is basically the same as in Example 1, except that step (3) of the first finishing liquid impregnation treatment is omitted, i.e., a Zn-containing solution is not used. 2+ The PET-PN fabric obtained in step (2) is treated with a first finishing solution containing a weak complexing agent; the PET-PN fabric obtained in step (2) is then directly processed according to step (4) using Al 3+ After sorting, and performing wet heat post-treatment according to step (5), a PET flame-retardant and smoke-suppressing fabric containing only the outer Al-based fixed structure and without Zn catalytic sites is finally obtained, denoted as PET-PN-Al.

[0091] The final PET-PN-Al fabric had a finishing weight gain of 1.2%, a limiting oxygen index of 28.6%, a vertical burning afterflame time of 3.5 s, and a smoldering time of 2.8 s. Under the same cone calorimetry test conditions, compared with the unfinished PET fabric of the same specification, the peak heat release rate was reduced by 43%, the peak smoke generation rate was reduced by 33.3%, and the total smoke release was reduced by 40%. After 10 standard washes, the limiting oxygen index of the fabric was 24.5%.

[0092] Comparing Comparative Example 1 and Example 1, it can be seen that Zn is omitted. 2+ After finishing, the limiting oxygen index of the obtained PET flame-retardant and smoke-suppressing fabric decreased from 30% to 28.6%, the peak heat release rate decreased from 58.5% to 43%, the peak smoke generation rate decreased from 60% to 33.3%, the total smoke release decreased from 65% to 40.0%, and the limiting oxygen index after 10 standard washes decreased from 26% to 24.5%. The results indicate that while retaining the phosphorus-nitrogen smoke-catching layer and Al-based framework alone can still produce certain flame-retardant, char-forming, and shielding effects, its suppression effect on heat release and smoke generation is weaker than in Example 1. This is because omitting the first finishing liquid treatment prevents the formation of Zn-OP, Zn-O, and other Zn-based catalytic sites near the PET matrix in the reactive phosphorus-nitrogen smoke-catching layer. Consequently, oxygen-containing low-molecular-weight compounds, aromatic pyrolysis products, and other combustible volatiles generated by the thermal decomposition of PET cannot undergo timely secondary condensation and deposition carbonization, leading to an increase in combustible components and smoke precursors entering the gas phase. Therefore, the peak heat release rate, peak smoke generation rate, and total smoke release of Comparative Example 1 are all higher than those of Example 1. Meanwhile, the absence of Zn... 2+ The coordination and immobilization between phosphoric acid groups, hydroxyl groups, and other sites also reduces the degree of cross-linking and washing stability of the phosphorus and nitrogen smoke trapping layer, resulting in a decrease in the limiting oxygen index after washing.

[0093] Comparative Example 2

[0094] A method for preparing a PET flame-retardant and smoke-suppressing fabric is basically the same as in Example 1, except that step (4) of the second finishing liquid impregnation treatment is omitted, i.e., Al-containing liquid is not used. 3+ The second finishing solution containing the slow-release alkali component is used for treatment; the PET-PN-Zn fabric obtained in step (3) is directly subjected to wet heat treatment at 80 °C for 90 min according to the conditions in step (5). Finally, a PET flame-retardant and smoke-suppressing fabric containing Zn catalytic sites but not Al-OP skeleton sites is obtained, denoted as PET-PN-Zn-HT, where "HT" indicates wet heat treatment.

[0095] The final PET-PN-Zn-HT fabric had a finishing weight gain of 1.1%, a limiting oxygen index of 28.2%, a vertical burning afterflame time of 4 s, and a smoldering time of 3.2 s. During the combustion process, some of the molten droplets produced by the sample could ignite the degreased cotton below. Under the same cone calorimetry test conditions, compared with the unfinished PET fabric of the same specification, the peak heat release rate was reduced by 47%, the peak smoke generation rate was reduced by 52%, and the total smoke release was reduced by 50%. After 10 standard washes, the limiting oxygen index of the fabric was 24.2%.

[0096] Comparing Comparative Example 2 and Example 1, it can be seen that Al is omitted. 3+After finishing, the limiting oxygen index of the resulting fabric decreased from 30% to 28.2%, the vertical burning afterflame time increased from 2 s to 4 s, and the smoldering time increased from 2 s to 3.2 s. Furthermore, the molten droplets changed from not igniting the absorbent cotton to some samples being able to ignite it. The peak heat release rate decreased from 58.5% to 47%, the peak smoke generation rate decreased from 60% to 52%, and the total smoke release decreased from 65% to 50%. The limiting oxygen index after 10 standard washes decreased from 26% to 24.2%. This is because the Zn catalytic sites in the fabric of Comparative Example 2 can still promote the secondary condensation and deposition carbonization of some pyrolysis products, thus maintaining a certain smoke suppression and heat release inhibition effect. However, due to the lack of Al treatment... 3+ In practice, the outer side of the phosphorus and nitrogen smoke-catching layer cannot form a continuous and stable Al-OP, Al-OH, or Al-O-Al framework structure, resulting in reduced continuity, density, and thermal stability of the obtained char layer, and weakened barrier effect against heat, oxygen, and combustible volatiles. Simultaneously, the lack of Al-based framework for coating and physically constraining molten PET increases the risk of molten dripping and its ignition. Furthermore, the lack of Al... 3+ The multi-site coordination and bridging fixation between the finishing layer and sites such as phosphate groups and hydroxyl groups reduce the crosslinking stability and wash resistance of the finishing layer.

[0097] Comparative Example 3

[0098] A method for preparing Zn / Al catalytic carbonization PET flame-retardant and smoke-suppressing fabric is basically the same as in Example 1, except that the first stage of treatment is omitted in step (4) when the fabric is immersed in the second finishing solution. Specifically, the PET-PN-Zn fabric obtained in step (3) is directly immersed in the second finishing solution with an initial pH of 4.5, the temperature of the second finishing solution is directly raised to 50°C, and the fabric is treated at 50°C for 30 min. At the end of the treatment, the pH of the second finishing solution is 6.5. Then, according to the conditions of step (5) in Example 1, the fabric is subjected to wet heat treatment at 80°C for 90 min to obtain the fabric with Al omitted. 3+ The Zn / Al catalytic carbonization of PET flame-retardant and smoke-suppressing fabric during the low-temperature diffusion stage is denoted as PET-PN-Zn-Al-D.

[0099] The final PET-PN-Zn-Al-D fabric had a finishing weight gain of 1.3%, a limiting oxygen index of 29.1%, a vertical burning afterflame time of 2.8 s, and a smoldering time of 2.5 s. The molten droplets generated during combustion did not ignite the degreased cotton. Under the same cone calorimetry test conditions, compared with the unfinished PET fabric of the same specification, the PET-PN-Zn-Al-D fabric had a 52% lower peak heat release rate, a 54% lower peak smoke generation rate, and a 53% lower total smoke release. After 10 standard washes, the limiting oxygen index of the fabric was 24.8%.

[0100] Comparing Comparative Example 3 and Example 1, it can be seen that after omitting the second finishing liquid in the first-stage low-temperature impregnation treatment, the limiting oxygen index of the resulting fabric decreased from 30.0% to 29.1%, the vertical burning afterflame time increased from 2 s to 2.8 s, and the smoldering time increased from 2 s to 2.5 s; the peak heat release rate decreased from 58.5% to 52.0%, the peak smoke generation rate decreased from 60% to 54.0%, the total smoke release rate decreased from 65% to 53%, and the limiting oxygen index after 10 standard washes decreased from 26% to 24.8%. This is because the first-stage low-temperature impregnation treatment was able to achieve the desired effect before the slow-release alkali significantly promoted Al2O3 production. 3+ Under hydrolysis conditions, Al 3+ First, it enters the reactive phosphorus and nitrogen smoke-collecting layer and fully contacts the coordination sites such as phosphate groups and hydroxyl groups; when the low-temperature impregnation treatment stage is omitted and the treatment is carried out directly at 50 °C, the slow-release alkali effect and Al 3+ The hydrolysis process occurs relatively early, and some Al components readily form hydroxyl-bridged structures or aluminum phosphate deposits on the outer surface of the phosphorus-nitrogen smoke eliminator, reducing the diffusion depth of Al components into the interior of the smoke eliminator and potentially leading to localized surface deposits. Therefore, although Comparative Example 3 still contains Zn and Al components and can form a certain degree of catalytic char formation and outer layer shielding, the uniformity of Zn / Al site distribution in the thickness direction, the degree of interfacial bonding between Al components and the phosphorus-nitrogen smoke eliminator, and the washing stability of the finishing layer are all weaker than in Example 1, ultimately resulting in a decline in its flame retardant, smoke suppression, and post-washing performance.

[0101] Comparative Example 4

[0102] A method for preparing Zn / Al catalytic carbonization PET flame-retardant and smoke-suppressing fabric is basically the same as in Example 1, except that: in step (4), the second stage of treatment is omitted when immersing the fabric in the second finishing solution. Specifically, the PET-PN-Zn fabric obtained in step (3) is immersed in the second finishing solution with an initial pH of 4.5, and the first stage of immersion treatment is carried out at 25 °C for 20 min. After the first stage, the second finishing solution is not heated to 50 °C for 30 min. At this time, the pH of the second finishing solution is still 4.5±0.2. After the first stage of immersion treatment, the fabric is immediately taken out and rinsed in deionized water at 25±2 °C for 30 s according to the fabric mass to deionized water volume ratio of 1 g: 50 mL to remove unfixed Al salt and slow-release alkali components. Then, according to the conditions of step (5) in Example 1, the fabric is wet-heat treated at 80 °C for 90 min. min, the Zn / Al catalytic carbonization PET flame retardant and smoke-suppressing fabric with the second stage of heating and fixing treatment omitted was obtained, denoted as PET-PN-Zn-Al-L.

[0103] The final PET-PN-Zn-Al-L fabric had a finishing weight gain of 1.2%, a limiting oxygen index of 28.7%, a vertical burning afterflame time of 3.4 s, and a smoldering time of 2.8 s. During the combustion process, some of the molten droplets produced by the sample could ignite the degreased cotton below. Under the same cone calorimetry test conditions, compared with the unfinished PET fabric of the same specification, the peak heat release rate of the PET-PN-Zn-Al-L fabric was reduced by 50%, the peak smoke generation rate was reduced by 53%, and the total smoke release was reduced by 51%. After 10 standard washes, the limiting oxygen index of the fabric was 24.3%.

[0104] Comparing Comparative Example 4 and Example 1, it can be seen that omitting the second-stage heating treatment resulted in a decrease in the weight gain of the finished fabric from 1.5% to 1.2%, a decrease in the limiting oxygen index from 30% to 28.7%, an increase in the vertical burning afterflame time from 2 s to 3.4 s, an increase in the smoldering time from 2 s to 2.8 s, and the phenomenon of some molten droplets igniting the degreased cotton; the reduction rate of peak heat release rate decreased from 58.5% to 50%, the reduction rate of peak smoke generation rate decreased from 60% to 53%, the reduction rate of total smoke release decreased from 65% to 51%, and the limiting oxygen index after 10 standard washes decreased from 26% to 24.3%. This is because the first-stage low-temperature impregnation treatment mainly caused Al 3+ It enters and diffuses into the reactive phosphorus and nitrogen smoke trapping layer, but under conditions of 25 ℃ and pH 4.5±0.2, the slow-release alkali has not yet fully exerted its effect. 3+ The degree of hydrolysis, hydroxyl bridging, and coordination fixation with phosphate groups is relatively low. Without omitting the second-stage heating treatment, the pH of the second finishing solution cannot be gradually increased from 4.5 to 6.5, allowing some Al to enter the phosphorus and nitrogen smoke trapping layer. 3+ The Al-OP, Al-OH, and Al-O-Al frameworks formed in Comparative Example 4 are reduced in number, resulting in decreased cross-linking of the finishing layer, continuity of the char layer, and ability to confine the molten PET. Although the Zn catalytic sites retained in the fabric can still play a certain role in catalytic char formation and smoke suppression, their flame retardancy, drip suppression, and washing stability are all weaker than those of fabrics that have completed two stages of Al formation. 3+ Example 1 of the processing.

[0105] Comparative Example 5

[0106] A method for preparing Zn / Al catalytic carbonization PET flame-retardant and smoke-suppressing fabric is basically the same as in Example 1, except that: in step (4), the treatment temperature of the second stage in the second finishing solution is 75°C and the treatment time of the second stage is still 30 min; after the second stage treatment, the pH of the second finishing solution is 8.2; then, according to the conditions of step (5) in Example 1, a wet heat treatment is performed at 80°C for 90 min to obtain Zn / Al catalytic carbonization PET flame-retardant and smoke-suppressing fabric with a second stage treatment temperature of 75°C, denoted as PET-PN-Zn-Al-75.

[0107] The final PET-PN-Zn-Al-75 fabric had a finishing weight gain of 1.7%, a limiting oxygen index of 29.4%, a vertical burning afterflame time of 2.6 s, and a smoldering time of 2.3 s. The molten droplets generated during combustion did not ignite the degreased cotton. Under the same cone calorimetry test conditions, compared with the unfinished PET fabric of the same specification, the PET-PN-Zn-Al-75 fabric had a 54% lower peak heat release rate, a 56% lower peak smoke generation rate, and a 55% lower total smoke release. After 10 standard washes, the limiting oxygen index of the fabric was 24.9%.

[0108] Comparing Comparative Example 5 and Example 1, it can be seen that increasing the second-stage treatment temperature from 50°C to 75°C increases the weight gain of the finished fabric from 1.5% to 1.7%, but decreases the limiting oxygen index from 30.0% to 29.4%, extends the vertical burning afterflame time from 2 s to 2.6 s, and extends the smoldering time from 2 s to 2.3 s; the peak heat release rate reduction rate decreases from 58.5% to 54%, the peak smoke generation rate reduction rate decreases from 60% to 56%, the total smoke release reduction rate decreases from 65% to 55%, and the limiting oxygen index after 10 standard washes decreases from 26% to 24.9%. This is because when the second-stage temperature is increased to 75°C, the slow-release alkali component takes effect more quickly, causing the pH of the second finishing solution to rise to 8.2 in a shorter time, promoting Al 3+ Rapid hydrolysis. Partial Al 3+ Before fully diffusing and coordinating with the phosphate and hydroxyl groups in the phosphorus and nitrogen smoke trapping layer, Al-OH, Al-O-Al, or aluminophosphate aggregates form in the finishing solution or on the outer surface of the fabric. This rapidly forming surface deposit may also hinder subsequent Al... 3+ The phosphorus and nitrogen smoke-catching layer diffuses into the interior, causing the Al component to concentrate mainly on the outermost surface of the fabric.

[0109] Therefore, although Comparative Example 5 exhibits a higher finishing weight gain due to increased surface inorganic deposition, the dispersion and effective utilization of Al active sites decrease, making it difficult to form a uniform, continuous Al-OP framework that is stably integrated with the phosphorus and nitrogen smoke-collecting layer. Some surface deposits are easily detached during rinsing and washing, resulting in lower flame-retardant and smoke-suppressing efficiency and washing stability of the fabric compared to Example 1.

[0110] Comparative Example 6

[0111] A method for preparing Zn / Al catalytic carbonization PET flame-retardant and smoke-suppressing fabric is basically the same as in Example 1, except that: in step (4), the treatment temperature of the second stage in the second finishing solution is 45°C and the treatment time of the second stage is still 30 min; after the second stage treatment, the pH of the second finishing solution is 5.8; after the second stage treatment, the fabric is taken out and rinsed in deionized water at 25±2°C for 30 s according to the ratio of fabric mass to deionized water volume of 1 g: 50 mL to remove unfixed Al salt and slow-release alkali components; then, according to the conditions of step (5) in Example 1, it is subjected to wet heat treatment at 80°C for 90 min to obtain Zn / Al catalytic carbonization PET flame-retardant and smoke-suppressing fabric with a second stage treatment temperature of 45°C, which is denoted as PET-PN-Zn-Al-45.

[0112] The final PET-PN-Zn-Al-45 fabric had a finishing weight gain of 1.3%, a limiting oxygen index of 29.5%, a vertical burning afterflame time of 2.5 s, and a smoldering time of 2.2 s. The molten droplets generated during combustion did not ignite the degreased cotton. Under the same cone calorimetry test conditions, compared with the unfinished PET fabric of the same specification, the peak heat release rate decreased by 55.5%, the peak smoke generation rate decreased by 57%, and the total smoke release decreased by 56%. After 10 standard washes, the limiting oxygen index of the fabric was 25.1%.

[0113] Comparing Comparative Example 6 and Example 1, it can be seen that after reducing the second-stage treatment temperature from 50 °C to 45 °C, the final pH of the second finishing solution decreased from 6.5 to 5.8, the weight gain of the resulting fabric decreased from 1.5% to 1.3%, the limiting oxygen index decreased from 30% to 29.5%, the afterflame time increased from 2 s to 2.5 s, and the smoldering time increased from 2 s to 2.2 s; the peak heat release rate decreased from 58.5% to 55.5%, the peak smoke generation rate decreased from 60% to 57%, the total smoke release rate decreased from 65% to 56%, and the limiting oxygen index after 10 standard washes decreased from 26% to 25.1%. This is because after the second-stage treatment temperature was reduced to 45 °C, the rate at which the slow-release alkali component took effect decreased, and the pH of the second finishing solution only increased to 5.8, failing to reach 6.5 as in Example 1. Under relatively low pH conditions, Al3+ The Al components mainly exist in hydrated ionic or weakly coordinated forms, and their hydrolysis, hydroxyl bridging, and coordination fixation with phosphate groups are reduced. Some of the Al components entering the reactive phosphorus-nitrogen smoke trapping layer are lost during subsequent rinsing. Therefore, the number of Al-OP, Al-OH, and Al-O-Al framework structures formed in Comparative Example 6 is reduced, and the continuity, density, and thermal stability of the outer carbon layer framework are weaker than in Example 1. Although the Zn catalytic sites retained in the fabric can still promote the secondary condensation and deposition carbonization of PET pyrolysis products, maintaining certain flame retardant and smoke-suppressing properties, the insufficient construction of the Al-based framework results in a decrease in heat release inhibition, smoke release inhibition, and washing stability of the resulting fabric.

[0114] Example 2

[0115] A method for preparing a flame-retardant and smoke-suppressing polyester fabric, comprising the following specific steps:

[0116] (1) Alkali reduction micro-etching;

[0117] The PET fabric was placed in a 20 g / L sodium hydroxide aqueous solution at a bath ratio of 1:30 and treated at 70 °C for 30 min. After treatment, it was neutralized with a 1 g / L acetic acid aqueous solution for 2 min, then washed with deionized water until neutral, and dried at 60 °C for 2 h to obtain the PET fabric after alkali reduction micro-etching treatment. The depth of the alkali reduction micro-etching treatment was 300 nm.

[0118] (2) Construct a reactive phosphorus and nitrogen smoke trapping layer on the surface of the PET fabric treated in step (1);

[0119] (2.1) Add 3.0 g of polyethyleneimine to an appropriate amount of acetic acid aqueous solution with a mass fraction of 1.0%, stir at 500 r / min for 4 h at 25±2 ℃ to fully dissolve the polyethyleneimine, and adjust the pH of the system to 3.5±0.2;

[0120] Polyethyleneimine: Manufacturer: Sigma-Aldrich, Product No. 408727, Weight Average Molecular Weight 25000;

[0121] (2.2) Add 0.2 g of phytic acid modified attapulgite to the polyethyleneimine solution obtained in step (2.1), and ultrasonically disperse it for 30 min at a frequency of 40 kHz and a power of 300 W. During the ultrasonic process, control the system temperature to not exceed 35 ℃. Then stir at 500 r / min for 30 min, and then make up the system to 100.0 g with 1.0% acetic acid aqueous solution to obtain a finishing solution containing 3.0 wt% polyethyleneimine and 0.2 wt% phytic acid modified attapulgite, namely polyethyleneimine / phytic acid modified attapulgite finishing solution;

[0122] In phytic acid-modified attapulgite, the mass ratio of attapulgite to phytic acid is 8:1.

[0123] (2.3) The PET fabric treated in step (1) was immersed in polyethyleneimine / phytic acid modified attapulgite finishing solution at a ratio of 1:30 according to the ratio of fabric mass to finishing solution mass. The immersion was carried out at 40 °C with 100 r / min for 30 min. After the fabric was removed, it was rolled in a one-dip-one-rolling method with a roller pressure of 0.20 MPa and a roller linear speed of 1.0 m / min. The roll residue was controlled to be 80±5%.

[0124] (2.4) According to the mass ratio of fabric to sodium phytate aqueous solution of 1:30, the fabric after padding is immersed in sodium phytate aqueous solution with a mass fraction of 1.0% and a pH of 2.5±0.2, and shaken at 100 r / min for 20 min at 30 ℃, so that the phosphate groups in sodium phytate and the protonated amino groups in polyethyleneimine undergo ionic cross-linking to form a phosphorus nitrogen smoke catching network, and the modified attapulgite soil is embedded and fixed in the formed phosphorus nitrogen smoke catching network.

[0125] (2.5) After the treatment in step (2.4) is completed, the fabric is rinsed in deionized water at 25±2℃ for 30 s according to the ratio of fabric mass to deionized water volume of 1 g: 50 mL, then lightly rolled once under 0.10 MPa pressure, and finally dried under vacuum at 60℃ for 2 h to obtain a PET fabric with a reactive phosphorus and nitrogen smoke trapping layer on the surface, denoted as PET-PN;

[0126] (3) Place the PET fabric with the reactive phosphorus and nitrogen smoke trapping layer constructed in step (2) in the first finishing solution with pH 4.5 and immerse it at 35 °C for 30 min;

[0127] The first finishing solution is a mixed solution of zinc nitrate and lactic acid, Zn 2+ The concentration is 0.18 mol / L, lactic acid and Zn 2 + The molar ratio is 0.6:1;

[0128] (4) The PET fabric treated in step (3) is immersed in the second finishing solution to form a gradient confined flame retardant and smoke suppressing layer with enriched Zn catalytic sites on the inner side and enriched Al-OP skeleton sites on the outer side.

[0129] The immersion treatment in the second finishing solution was divided into two stages. The first stage was treated at a temperature of 30 ℃ for 18 min, and the second stage was treated at a temperature of 55 ℃ for 25 min. After the second stage treatment, the pH of the second finishing solution gradually increased to 6.8.

[0130] The second finishing solution is a mixed solution of aluminum acetate and hexamethylenetetramine, with a pH of 4.7; the second finishing solution contains Al 3+ At a concentration of 0.06 mol / L, hexamethylenetetramine and Al 3+ The molar ratio of Zn in the first finishing solution is 1.0:1. 2+ With Al in the second finishing solution 3+ The molar ratio is 3.0:1;

[0131] (5) The PET fabric after impregnation in step (4) is subjected to wet heat treatment at 100 °C saturated steam and 100% RH for 50 min to obtain flame-retardant and smoke-suppressing polyester fabric.

[0132] The resulting flame-retardant and smoke-suppressing polyester fabric comprises a PET base fabric, a reactive phosphorus-nitrogen smoke-catching layer fixed to the surface of the PET base fabric, and a gradient-confined flame-retardant and smoke-suppressing layer located on the surface of the reactive phosphorus-nitrogen smoke-catching layer. The reactive phosphorus-nitrogen smoke-catching layer consists of a phosphorus-nitrogen smoke-catching network and attapulgite dispersed and fixed within the phosphorus-nitrogen smoke-catching network. The inner side of the gradient-confined flame-retardant and smoke-suppressing layer is enriched with Zn catalytic sites, while the outer side is enriched with Al-OP framework sites. Based on a 30% thickness region on both the inner and outer sides of the gradient-confined flame-retardant and smoke-suppressing layer, the Zn / Al atomic ratio in the inner region is 1.9 times that in the outer region, and the Al / P atomic ratio in the outer region is 1.3 times that in the inner region. The thickness of the reactive phosphorus-nitrogen smoke-catching layer is 220 nm, and the thickness of the gradient-confined flame-retardant and smoke-suppressing layer is 350 nm. nm; The Zn catalytic sites enriched on the inner side of the gradient-confined flame-retardant and smoke-suppressing layer contain Zn-N and Zn-O coordination structures; the Al-OP skeleton sites enriched on the outer side of the gradient-confined flame-retardant and smoke-suppressing layer contain Al-OP and Al-O-Al bridging structures; the finishing weight gain of the flame-retardant and smoke-suppressing polyester fabric is 2.3%, the limiting oxygen index is 31.2%, the vertical combustion afterflame time is 1.5 s, the smoldering time is 1.3 s, and the molten droplets generated during vertical combustion do not ignite the degreased cotton; under the same cone calorimetry test conditions, compared with the unfinished PET fabric of the same specification, the peak heat release rate of the flame-retardant and smoke-suppressing polyester fabric is reduced by 54%, the peak smoke generation rate (pSPR) is reduced by 60.5%, and the total smoke release is reduced by 65.5%; after 10 standard washes, the limiting oxygen index of the flame-retardant and smoke-suppressing polyester fabric is 26.8%, it can still self-extinguish, and the molten droplets generated during vertical combustion do not ignite the degreased cotton.

[0133] Example 3

[0134] A method for preparing a flame-retardant and smoke-suppressing polyester fabric, comprising the following specific steps:

[0135] (1) Low-temperature plasma treatment;

[0136] Oxygen plasma was used at a temperature of 25±2 ℃, a working pressure of 30 Pa, an oxygen flow rate of 50 mL / min, and a discharge power of 100 W. Both sides of the PET fabric were treated for 5 min each, and the depth of the low-temperature plasma treatment was 100 nm.

[0137] (2) Construct a reactive phosphorus and nitrogen smoke trapping layer on the surface of the PET fabric treated in step (1);

[0138] (2.1) Add 2.0 g of chitosan to an appropriate amount of acetic acid aqueous solution with a mass fraction of 1.0%, stir at 500 r / min for 4 h at 25±2 ℃ to fully dissolve the chitosan, and adjust the pH of the system to 3.5±0.2;

[0139] Chitosan is a low molecular weight chitosan, manufactured by Sigma-Aldrich, with product number 448869, a degree of deacetylation of 75%~85%, and a nominal molecular weight of 50,000~190,000.

[0140] (2.2) Add 1.0 g of KH560 modified attapulgite to the chitosan solution obtained in step (2.1), and ultrasonically disperse it for 30 min at a frequency of 40 kHz and a power of 300 W. During the ultrasonic process, control the system temperature to be no higher than 35 ℃. Then stir at 500 r / min for 30 min, and then make up the system to 100.0 g with 1.0% acetic acid aqueous solution to obtain a finishing solution containing 2.0 wt% chitosan and 1.0 wt% KH560 modified attapulgite, i.e. chitosan / KH560 modified attapulgite finishing solution;

[0141] In KH560 modified attapulgite, the mass ratio of attapulgite to KH560 is 10:1.

[0142] (2.3) The PET fabric treated in step (1) was immersed in chitosan / KH560 modified attapulgite finishing solution at a ratio of 1:30 between the fabric mass and the finishing solution mass. The solution was shaken and immersed at 100 r / min for 30 min at 40 ℃. After the fabric was removed, it was rolled in a one-dip-one-rolling manner. The roller pressure was 0.20 MPa and the roller linear speed was 1.0 m / min. The roll residue was controlled to be 80±5%.

[0143] (2.4) The fabric after padding was immersed in a phytic acid aqueous solution with a mass fraction of 3.0% and a pH of 2.5±0.2 at 30 °C and shaken at 100 r / min for 20 min to allow the phosphate groups in the phytic acid to undergo ionic cross-linking with the protonated amino groups in the chitosan to form a phosphorus nitrogen smoke-catching network, and the modified attapulgite soil was embedded and fixed in the formed phosphorus nitrogen smoke-catching network.

[0144] (2.5) After the treatment in step (2.4) is completed, the fabric is rinsed in deionized water at 25±2℃ for 30 s according to the ratio of fabric mass to deionized water volume of 1 g: 50 mL, then lightly rolled once under 0.10 MPa pressure, and finally dried under vacuum at 60℃ for 2 h to obtain a PET fabric with a reactive phosphorus and nitrogen smoke trapping layer on the surface, denoted as PET-PN;

[0145] (3) Place the PET fabric with the reactive phosphorus and nitrogen smoke trapping layer constructed in step (2) into the first finishing solution with pH 4.8 and immerse it at 50 °C for 20 min;

[0146] The first finishing solution is a mixed solution of zinc gluconate and gluconic acid, Zn 2+ The concentration is 0.16 mol / L, gluconic acid and Zn 2+ The molar ratio is 0.9:1;

[0147] (4) The PET fabric treated in step (3) is immersed in the second finishing solution to form a gradient confined flame retardant and smoke suppressing layer with enriched Zn catalytic sites on the inner side and enriched Al-OP skeleton sites on the outer side.

[0148] The immersion treatment in the second finishing solution was divided into two stages. The first stage was treated at a temperature of 35 ℃ for 15 min, and the second stage was treated at a temperature of 60 ℃ for 20 min. After the second stage was completed, the pH of the second finishing solution was gradually increased to 7.

[0149] The second finishing solution contains a mixed solution of aluminum lactate and hexamethylenetetramine, and its pH is 4.9; the second finishing solution contains Al 3+ At a concentration of 0.1 mol / L, hexamethylenetetramine and Al 3+ The molar ratio of Zn in the first finishing solution is 1.5:1. 2+ With Al in the second finishing solution 3+ The molar ratio is 1.6:1;

[0150] (5) The PET fabric after impregnation in step (4) is subjected to wet heat treatment for 20 min under saturated steam at 120 ℃ and pressure of 0.199 MPa to obtain flame-retardant and smoke-suppressing polyester fabric.

[0151] The resulting flame-retardant and smoke-suppressing polyester fabric comprises a PET base fabric, a reactive phosphorus-nitrogen smoke-catching layer fixed to the surface of the PET base fabric, and a gradient-confined flame-retardant and smoke-suppressing layer located on the surface of the reactive phosphorus-nitrogen smoke-catching layer. The reactive phosphorus-nitrogen smoke-catching layer consists of a phosphorus-nitrogen smoke-catching network and attapulgite dispersed and fixed within the phosphorus-nitrogen smoke-catching network. The inner side of the gradient-confined flame-retardant and smoke-suppressing layer is enriched with Zn catalytic sites, while the outer side is enriched with Al-OP framework sites. Based on a 30% thickness region on both the inner and outer sides of the gradient-confined flame-retardant and smoke-suppressing layer, the Zn / Al atomic ratio in the inner region is 2.3 times that in the outer region, and the Al / P atomic ratio in the outer region is 1.5 times that in the inner region. The thickness of the reactive phosphorus-nitrogen smoke-catching layer is 380 nm, and the thickness of the gradient-confined flame-retardant and smoke-suppressing layer is 620 nm. nm; The Zn catalytic sites enriched on the inner side of the gradient-confined flame-retardant and smoke-suppressing layer contain Zn-OP, Zn-N, and Zn-O coordination structures; The Al-OP skeleton sites enriched on the outer side of the gradient-confined flame-retardant and smoke-suppressing layer contain Al-OP, Al-O-Al, and Al-OH bridging structures; The finishing weight gain of the flame-retardant and smoke-suppressing polyester fabric is 3.2%, the limiting oxygen index is 32.5%, the vertical combustion afterflame time is 0.8 s, the smoldering time is 0.6 s, and the molten droplets generated during vertical combustion do not ignite the degreased cotton; Under the same cone calorimetry test conditions, compared with the unfinished PET fabric of the same specification, the peak heat release rate of the flame-retardant and smoke-suppressing polyester fabric is reduced by 62%, the peak smoke generation rate (pSPR) is reduced by 62%, and the total smoke release is reduced by 64%; After 10 standard washes, the limiting oxygen index of the flame-retardant and smoke-suppressing polyester fabric is 27.9%, it can still self-extinguish, and the molten droplets generated during vertical combustion do not ignite the degreased cotton.

[0152] Example 4

[0153] A method for preparing a flame-retardant and smoke-suppressing polyester fabric, comprising the following specific steps:

[0154] (1) Ultraviolet-ozone synergistic treatment;

[0155] A dual-wavelength ozone-type ultraviolet lamp with 185 nm and 254 nm wavelengths was used, with an irradiance of 15 mW / cm² at 254 nm. 2 The irradiation intensity at 185 nm is 2 mW / cm². 2 With a lamp distance of 20 mm, in an atmospheric pressure air atmosphere, 185 nm ultraviolet light is used to generate ozone in situ from oxygen in the air, and under the action of 254 nm ultraviolet light, active oxygen species that participate in surface oxidation are formed. The PET fabric is irradiated on both sides for 20 min, and the depth of action of ultraviolet-ozone synergistic treatment is 20 nm.

[0156] (2) Construct a reactive phosphorus and nitrogen smoke trapping layer on the surface of the PET fabric treated in step (1);

[0157] (2.1) Add 4 g of polyethyleneimine to an appropriate amount of acetic acid aqueous solution with a mass fraction of 1.0%, stir at 500 r / min for 4 h at 25±2 ℃, and adjust the pH of the system to 3.5±0.2;

[0158] Polyethyleneimine: Manufacturer: Sigma-Aldrich, Product No. 408727, Weight Average Molecular Weight 25000;

[0159] (2.2) Add 2 g of phytic acid modified attapulgite to the polyethyleneimine solution obtained in step (2.1), and ultrasonically disperse it for 30 min at a frequency of 40 kHz and a power of 300 W. During the ultrasonic process, control the system temperature to not exceed 35 ℃. Then stir at 500 r / min for 30 min, and then make up the system to 100.0 g with 1.0% acetic acid aqueous solution to obtain a finishing solution containing 4.0 wt% polyethyleneimine and 2.0 wt% phytic acid modified attapulgite, namely polyethyleneimine / phytic acid modified attapulgite finishing solution;

[0160] In phytic acid-modified attapulgite, the mass ratio of attapulgite to phytic acid is 6:1.

[0161] (2.3) The PET fabric treated in step (1) was immersed in polyethyleneimine / phytic acid modified attapulgite finishing solution at a ratio of 1:30 according to the ratio of fabric mass to finishing solution mass. The immersion was carried out at 40 °C with 100 r / min for 30 min. After the fabric was removed, it was rolled in a one-dip-one-rolling method with a roller pressure of 0.20 MPa and a roller linear speed of 1.0 m / min. The roll residue was controlled to be 80±5%.

[0162] (2.4) The fabric after padding was immersed in a phytic acid aqueous solution with a mass fraction of 2.0% and a pH of 2.5±0.2 at 30 °C and shaken at 100 r / min for 20 min to allow the phosphate groups in the phytic acid to undergo ionic cross-linking with the protonated amino groups in the polyethyleneimine to form a phosphorus nitrogen smoke-catching network, and the modified attapulgite soil was embedded and fixed in the formed phosphorus nitrogen smoke-catching network.

[0163] (2.5) After the treatment in step (2.4) is completed, the fabric is rinsed in deionized water at 25±2℃ for 30 s according to the ratio of fabric mass to deionized water volume of 1 g: 50 mL, then lightly rolled once under 0.10 MPa pressure, and finally dried under vacuum at 60℃ for 2 h to obtain a PET fabric with a reactive phosphorus and nitrogen smoke trapping layer on the surface, denoted as PET-PN;

[0164] (3) Place the PET fabric with the reactive phosphorus and nitrogen smoke trapping layer constructed in step (2) in the first finishing solution with pH 5 and immerse it at 60 °C for 15 min.

[0165] The first finishing solution is a mixed solution of zinc gluconate and citric acid, Zn 2+ The concentration is 0.15 mol / L, citric acid and Zn 2+ The molar ratio is 1.2:1;

[0166] (4) The PET fabric treated in step (3) is immersed in the second finishing solution to form a gradient confined flame retardant and smoke suppressing layer with enriched Zn catalytic sites on the inner side and enriched Al-OP skeleton sites on the outer side.

[0167] The immersion treatment in the second finishing solution was divided into two stages. The first stage was treated at a temperature of 40 ℃ for 10 min, and the second stage was treated at a temperature of 65 ℃ for 15 min. After the second stage treatment, the pH of the second finishing solution gradually increased to 7.5.

[0168] The second finishing solution contains aluminum nitrate (purchased from Sigma-Aldrich, grade 237973) and a slow-release alkali component. The slow-release alkali component is a mixture of urea and hexamethylenetetramine in a 1:1 mass ratio. The pH of the second finishing solution is 5. The second finishing solution contains Al... 3+ The concentration is 0.15 mol / L, and the slow-release alkali component reacts with Al. 3+ The molar ratio of Zn in the first finishing solution is 2.0:1. 2+ With Al in the second finishing solution 3+ The molar ratio is 1.0:1;

[0169] (5) The PET fabric after impregnation in step (4) is baked at normal pressure and 120 °C for 15 min to obtain flame-retardant and smoke-suppressing polyester fabric.

[0170] The resulting flame-retardant and smoke-suppressing polyester fabric comprises a PET base fabric, a reactive phosphorus-nitrogen smoke-catching layer fixed to the surface of the PET base fabric, and a gradient-confined flame-retardant and smoke-suppressing layer located on the surface of the reactive phosphorus-nitrogen smoke-catching layer. The reactive phosphorus-nitrogen smoke-catching layer consists of a phosphorus-nitrogen smoke-catching network and attapulgite dispersed and fixed within the phosphorus-nitrogen smoke-catching network. The inner side of the gradient-confined flame-retardant and smoke-suppressing layer is enriched with Zn catalytic sites, while the outer side is enriched with Al-OP framework sites. Based on a 30% thickness region on both the inner and outer sides of the gradient-confined flame-retardant and smoke-suppressing layer, the Zn / Al atomic ratio in the inner region is 2.6 times that in the outer region, and the Al / P atomic ratio in the outer region is 1.6 times that in the inner region. The thickness of the reactive phosphorus-nitrogen smoke-catching layer is 600 nm, and the thickness of the gradient-confined flame-retardant and smoke-suppressing layer is 900 nm. nm; The Zn catalytic sites enriched on the inner side of the gradient-confined flame-retardant and smoke-suppressing layer contain Zn-OP and Zn-O coordination structures; the Al-OP skeleton sites enriched on the outer side of the gradient-confined flame-retardant and smoke-suppressing layer contain Al-OP and Al-O-Al bridging structures; the finishing weight gain of the flame-retardant and smoke-suppressing polyester fabric is 4.1%, the limiting oxygen index is 33.1%, the vertical combustion afterflame time is 0.5 s, the smoldering time is 0.3 s, and the molten droplets generated during vertical combustion do not ignite the degreased cotton; under the same cone calorimetry test conditions, compared with the unfinished PET fabric of the same specification, the peak heat release rate of the flame-retardant and smoke-suppressing polyester fabric is reduced by 57.6%, the peak smoke generation rate (pSPR) is reduced by 61.5%, and the total smoke release is reduced by 64.5%; after 10 standard washes, the limiting oxygen index of the flame-retardant and smoke-suppressing polyester fabric is 28.3%, it can still self-extinguish, and the molten droplets generated during vertical combustion do not ignite the degreased cotton.

[0171] Example 5

[0172] A method for preparing a flame-retardant and smoke-suppressing polyester fabric, comprising the following specific steps:

[0173] (1) Ultraviolet-ozone synergistic treatment;

[0174] A dual-wavelength ozone-type ultraviolet lamp with 185 nm and 254 nm wavelengths was used, with an irradiance of 20 mW / cm² at 254 nm. 2 The irradiance at 185 nm is 2.5 mW / cm². 2 With a lamp distance of 15 mm, in an atmospheric pressure air atmosphere, 185 nm ultraviolet light is used to generate ozone in situ from oxygen in the air, and under the action of 254 nm ultraviolet light, active oxygen species that participate in surface oxidation are formed. The PET fabric is irradiated on both sides for 30 min, and the depth of action of ultraviolet-ozone synergistic treatment is 30 nm.

[0175] (2) Construct a reactive phosphorus and nitrogen smoke trapping layer on the surface of the PET fabric treated in step (1);

[0176] (2.1) Add 5.0 g of chitosan to an appropriate amount of acetic acid aqueous solution with a mass fraction of 1.0%, stir at 500 r / min for 4 h at 25±2 ℃ to fully dissolve the chitosan, and adjust the pH of the system to 3.5±0.2;

[0177] Chitosan is a low molecular weight chitosan, manufactured by Sigma-Aldrich, with product number 448869, a degree of deacetylation of 75%~85%, and a nominal molecular weight of 50,000~190,000.

[0178] (2.2) Add 3 g of KH570 modified attapulgite to the obtained chitosan solution, and ultrasonically disperse it for 30 min at a frequency of 40 kHz and a power of 300 W. During the ultrasonic process, control the system temperature to not exceed 35 ℃. Then stir at 500 r / min for 30 min, and then make up the system to 100.0 g with 1.0% acetic acid aqueous solution to obtain a finishing solution containing 5.0 wt% chitosan and 3.0 wt% KH570 modified attapulgite, i.e. chitosan / KH570 modified attapulgite finishing solution;

[0179] In KH570 modified attapulgite, the mass ratio of attapulgite to KH570 is 10:1.

[0180] (2.3) The PET fabric treated in step (1) was immersed in chitosan / KH570 modified attapulgite finishing solution at a ratio of 1:30 between the fabric mass and the finishing solution mass. The solution was shaken and immersed at 100 r / min for 30 min at 40 ℃. After the fabric was removed, it was rolled in a one-dip-one-rolling manner. The roller pressure was 0.20 MPa and the roller linear speed was 1.0 m / min. The roll residue was controlled to be 80±5%.

[0181] (2.4) According to the mass ratio of fabric to sodium phytate aqueous solution of 1:30, the fabric after padding is immersed in sodium phytate aqueous solution with a mass fraction of 5.0% and a pH of 2.5±0.2, and shaken at 100 r / min at 30 ℃ for 20 min, so that the phosphate groups in sodium phytate and the protonated amino groups in chitosan undergo ionic cross-linking to form a phosphorus nitrogen smoke catching network, and the modified attapulgite soil is embedded and fixed in the formed phosphorus nitrogen smoke catching network.

[0182] (2.5) After the treatment in step (2.4) is completed, the fabric is rinsed in deionized water at 25±2℃ for 30 s according to the ratio of fabric mass to deionized water volume of 1 g: 50 mL, then lightly rolled once under 0.10 MPa pressure, and finally dried under vacuum at 60℃ for 2 h to obtain a PET fabric with a reactive phosphorus and nitrogen smoke trapping layer on the surface, denoted as PET-PN;

[0183] (3) Place the PET fabric with the reactive phosphorus and nitrogen smoke trapping layer constructed in step (2) in the first finishing solution with pH 5.5 and immerse it at 70 °C for 10 min.

[0184] The first finishing solution contains Zn 2+ And weak complexing agents, Zn 2+ The source is a mixture of zinc acetate and zinc nitrate in a mass ratio of 1:1, Zn 2+ The concentration is 0.09 mol / L, and the weak complexing agent is a mixture of lactic acid and gluconic acid in a 1:1 mass ratio. The weak complexing agent reacts with Zn. 2+ The molar ratio is 1.5:1;

[0185] (4) The PET fabric treated in step (3) is immersed in the second finishing solution to form a gradient confined flame retardant and smoke suppressing layer with enriched Zn catalytic sites on the inner side and enriched Al-OP skeleton sites on the outer side.

[0186] The immersion treatment in the second finishing solution was divided into two stages. The first stage was treated at a temperature of 45 ℃ for 5 min, and the second stage was treated at a temperature of 70 ℃ for 10 min. After the second stage treatment, the pH of the second finishing solution gradually increased to 7.8.

[0187] The second finishing liquid contains Al 3+ With hexamethylenetetramine, the pH of the second finishing solution is 5.2; Al in the second finishing solution 3+ The source is a mixture of aluminum nitrate and aluminum acetate in a mass ratio of 1:1, Al 3+ At a concentration of 0.18 mol / L, hexamethylenetetramine and Al 3+ The molar ratio of Zn in the first finishing solution is 3.0:1. 2+ With Al in the second finishing solution 3+ The molar ratio is 0.5:1;

[0188] (5) The PET fabric after impregnation in step (4) is baked at normal pressure and 170 °C for 2 min to obtain flame-retardant and smoke-suppressing polyester fabric.

[0189] The resulting flame-retardant and smoke-suppressing polyester fabric comprises a PET base fabric, a reactive phosphorus-nitrogen smoke-catching layer fixed to the surface of the PET base fabric, and a gradient-confined flame-retardant and smoke-suppressing layer located on the surface of the reactive phosphorus-nitrogen smoke-catching layer. The reactive phosphorus-nitrogen smoke-catching layer consists of a phosphorus-nitrogen smoke-catching network and attapulgite dispersed and fixed within the phosphorus-nitrogen smoke-catching network. The inner side of the gradient-confined flame-retardant and smoke-suppressing layer is enriched with Zn catalytic sites, while the outer side is enriched with Al-OP framework sites. Based on a 30% thickness region on both the inner and outer sides of the gradient-confined flame-retardant and smoke-suppressing layer, the Zn / Al atomic ratio in the inner region is three times that in the outer region, and the Al / P atomic ratio in the outer region is 1.8 times that in the inner region. The thickness of the reactive phosphorus-nitrogen smoke-catching layer is 800 nm, and the thickness of the gradient-confined flame-retardant and smoke-suppressing layer is 1200 nm. nm; The Zn catalytic sites enriched on the inner side of the gradient-confined flame-retardant and smoke-suppressing layer contain Zn-OP, Zn-N, and Zn-O coordination structures; The Al-OP skeleton sites enriched on the outer side of the gradient-confined flame-retardant and smoke-suppressing layer contain Al-OP, Al-O-Al, and Al-OH bridging structures; The finishing weight gain of the flame-retardant and smoke-suppressing polyester fabric is 5%, the limiting oxygen index is 32.8%, the vertical combustion afterflame time is 0.7 s, the smoldering time is 0.5 s, and the molten droplets generated during vertical combustion do not ignite the degreased cotton; Under the same cone calorimetry test conditions, compared with the unfinished PET fabric of the same specification, the peak heat release rate of the flame-retardant and smoke-suppressing polyester fabric is reduced by 63.8%, the peak smoke generation rate (pSPR) is reduced by 61%, and the total smoke release is reduced by 64%; After 10 standard washes, the limiting oxygen index of the flame-retardant and smoke-suppressing polyester fabric is 28%, it can still self-extinguish, and the molten droplets generated during vertical combustion do not ignite the degreased cotton.

Claims

1. A method for preparing a flame-retardant and smoke-suppressing polyester fabric, characterized in that: First, a reactive phosphorus and nitrogen smoke-catching layer is constructed on the surface of a PET fabric that has undergone shallow activation treatment. Then, the PET fabric with the reactive phosphorus and nitrogen smoke-catching layer is immersed in the first finishing solution and the second finishing solution in sequence to form a gradient confined flame-retardant and smoke-suppressing layer with enriched Zn catalytic sites on the inner side and enriched Al-OP skeleton sites on the outer side. Finally, the PET fabric after immersion treatment is post-treated to obtain a flame-retardant and smoke-suppressing polyester fabric. The reactive phosphorus and nitrogen smoke trapping layer contains phosphorus compounds, amino-containing polymers, and modified attapulgite, and is fixed to the surface of PET fibers through at least one of ionic crosslinking and coordination crosslinking; the phosphorus compound is phytic acid or phytate, the amino-containing polymer is chitosan or polyethyleneimine; the modified attapulgite is attapulgite that has been surface modified with phosphate, phytic acid, or silane coupling agent. The first finishing liquid contains Zn 2+ and a weak complexing agent, the weak complexing agent being one or more of citric acid, lactic acid, and gluconic acid, the pH of the first finishing liquid being 4.2 to 5.5; The second finishing liquid contains Al 3+ and a slow-release alkali component, the slow-release alkali component being one or more of urea and hexamethylenetetramine, the pH of the second finishing liquid being 4.5-5.2; the dipping treatment in the second finishing liquid is divided into two stages, the treatment temperature of the first stage being 25-45 ℃, the treatment temperature of the second stage being 50-70 ℃, and after the end of the second stage treatment, the pH of the second finishing liquid gradually increases to 6.5-7.8; Post-treatment is either wet heat treatment or baking treatment; The weight gain rate of flame-retardant and smoke-suppressing polyester fabrics is 1.5-5.0%.

2. The method for preparing a flame-retardant and smoke-suppressing polyester fabric according to claim 1, characterized in that, Shallow activation treatment refers to at least one of alkali reduction micro-etching, low-temperature plasma treatment and ultraviolet-ozone synergistic treatment, with an activation depth of 10~300nm.

3. The method for preparing a flame-retardant and smoke-suppressing polyester fabric according to claim 1, characterized in that, The mass ratio of phosphorus compounds, amino-containing polymers, and modified attapulgite is 1~5:1~5:0.2~3.

4. The method for preparing a flame-retardant and smoke-suppressing polyester fabric according to claim 1, characterized in that, Zn in the first finishing liquid 2+ Zn is derived from one or more of zinc acetate, zinc nitrate and zinc gluconate 2+ The concentration of the weak complexing agent is 0.03-0.18 mol / L, and the molar ratio of the weak complexing agent to Zn 2+ is 0.3-1.5:

1. The first finishing solution is applied at a temperature of 25~70℃ for 10~45 minutes.

5. The method for preparing a flame-retardant and smoke-suppressing polyester fabric according to claim 1, characterized in that, Al in the second finishing solution 3+ The source is one or more of aluminum nitrate, aluminum acetate, and aluminum lactate, Al 3+ The concentration is 0.03~0.18 mol / L, and the slow-release alkali component is related to Al. 3+ The molar ratio is 0.5~3.0:1; The sample is immersed in the second finishing solution for 5-20 minutes in the first stage and 10-30 minutes in the second stage.

6. The method for preparing a flame-retardant and smoke-suppressing polyester fabric according to claim 1, characterized in that, Zn in the first finishing solution 2+ With Al in the second finishing solution 3+ The molar ratio is 0.5~3:

1.

7. The method for preparing a flame-retardant and smoke-suppressing polyester fabric according to claim 1, characterized in that, The temperature for damp heat treatment is 80~120℃, and the time is 20~90min; The baking temperature is 120~170℃ and the time is 2~15min.

8. A flame-retardant and smoke-suppressing polyester fabric prepared by the method according to any one of claims 1 to 7, characterized in that: It includes a PET base fabric, a reactive phosphorus and nitrogen smoke trapping layer fixed to the surface of the PET base fabric, and a gradient confined flame-retardant and smoke-suppressing layer located on the surface of the reactive phosphorus and nitrogen smoke trapping layer; The reactive phosphorus and nitrogen smoke trapping layer includes a phosphorus and nitrogen smoke trapping network and modified attapulgite dispersed and fixed in the phosphorus and nitrogen smoke trapping network. The phosphorus and nitrogen smoke trapping network is composed of phosphorus compounds and amino-containing polymers. The inner side of the gradient-confined flame-retardant and smoke-suppressing layer is enriched with Zn catalytic sites, while the outer side is enriched with Al-OP framework sites. Based on the inner 30% thickness region and the outer 30% thickness region of the gradient confined flame retardant and smoke suppressant layer, the Zn / Al atomic ratio in the inner region is more than 1.5 times that in the outer region, and the Al / P atomic ratio in the outer region is higher than that in the inner region.

9. The flame-retardant and smoke-suppressing polyester fabric according to claim 8, characterized in that, The thickness of the reactive phosphorus and nitrogen smoke trap is 80~800 nm; The thickness of the gradient-confined flame-retardant and smoke-suppressing layer is 120~1200nm; The Zn catalytic sites enriched on the inner side of the gradient confined flame-retardant and smoke-suppressing layer contain one or more of the following coordination structures: Zn-OP, Zn-N, and Zn-O. The Al-OP framework sites enriched on the outer side of the gradient-confined flame-retardant and smoke-suppressing layer contain one or more of the following bridging structures: Al-OP, Al-O-Al, and Al-OH.

10. A flame-retardant and smoke-suppressing polyester fabric according to claim 9, characterized in that, The limiting oxygen index is not less than 30.0%, the afterflame time during vertical combustion is not more than 2 seconds, the smoldering time is not more than 2 seconds, and the molten droplets generated during vertical combustion do not ignite the degreased cotton; under the same cone calorimetry test conditions, compared with untreated PET fabric of the same specification, the peak heat release rate of the flame-retardant and smoke-suppressing polyester fabric is reduced by not less than 50%, the peak smoke generation rate is reduced by not less than 60.0%, and the total smoke release is reduced by not less than 55%; after 10 standard washes, the limiting oxygen index of the flame-retardant and smoke-suppressing polyester fabric is not less than 26.0%, it can still self-extinguish, and the molten droplets generated during vertical combustion do not ignite the degreased cotton.