A hydrophilic synthetic short-cut fiber and its preparation method
By modifying the oil and chemically etching the surface of the synthetic fiber, a stable hydrophilic film layer is formed, which solves the problems of hydrophilicity and dispersibility of synthetic fibers in aqueous systems, achieves rapid wetting and uniform dispersion, and improves the durability of the fiber.
Patent Information
- Application Number
- CN202611315384.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-27
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to achieve the excellent hydrophilicity and good dispersibility of synthetic fibers in aqueous systems, and the modification process is complex and costly, making it difficult to meet diverse and small-batch customization needs.
The modified oil is composed of isomeric tridecyl alcohol polyoxyethylene ether, APG0810, PEG400 and nano silica. Through impregnation and chemical etching treatment, a stable hydrophilic film layer is formed, which enhances the hydrophilicity and dispersibility of the fiber, and improves the durability through the synergistic effect of KH570 and PEG400DA.
It achieves rapid wetting and uniform dispersion of synthetic fibers in water, with a sinking time as low as ≤4s, reduced agglomeration rate, and significantly improved durability, meeting the needs of high-frequency washing and long-term use scenarios.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_6
Abstract
Description
Technical Field
[0001] This invention belongs to the field of hydrophilic modification technology of chopped fiber surface, specifically relating to a hydrophilic synthetic chopped fiber and its preparation method. Background Technology
[0002] Chopped strand fibers are reinforcing materials made by cutting continuous fibers to a predetermined length. Common types include polyester fibers, polyamide fibers, polylactic acid fibers, and polypropylene fibers. These materials have advantages such as strong adaptability to molding processes and relatively low cost, showing broad application prospects in composite materials, papermaking, textiles, and building reinforcement. However, most synthetic fibers are inherently hydrophobic polymers with low surface energy and a lack of polar groups, making them difficult to effectively wet in aqueous substrates and difficult to achieve uniform dispersion. This inherent defect severely restricts the efficient application of chopped strand fibers in aqueous systems.
[0003] To address the aforementioned issues, the industry has explored various approaches. Patents CN104328531B, CN114214742B, and CN202968795U modify fibers from the source by adjusting raw material formulations, compounding multiple fibers, or performing grooving treatments. While the resulting products possess good hydrophilic properties, downstream users must purchase corresponding types of modified fibers based on different application needs, easily leading to inventory backlogs. Furthermore, source modification involves complex process parameter control, making it difficult to respond promptly to diverse market demands and small-batch customization needs, resulting in insufficient versatility. Patent CN122257256A uses physical blending or surface coating to modify fibers for hydrophilicity, but the resulting fibers show limited improvement in hydrophilicity and are prone to agglomeration during cutting and processing, leading to poor dispersibility and uneven distribution. Patent CN105818398B uses a bio-based surface modifier to improve the hydrophilicity of fibers and their dispersibility in aqueous media. However, it still suffers from problems such as a long treatment cycle, unsatisfactory hydrophilicity modification effect, and high cost.
[0004] In summary, existing modification methods struggle to simultaneously achieve excellent hydrophilicity and good dispersion stability. Therefore, developing a method for preparing hydrophilic synthetic short-cut fibers with good dispersibility through surface treatment of ordinary synthetic fibers remains a pressing technical problem to be solved in this field. Summary of the Invention
[0005] To address the problems existing in the above-mentioned background art, the first aspect of the present invention provides a method for preparing hydrophilic synthetic short-cut fibers: The hydrophilic synthetic short-cut fiber involved in this invention is made from ordinary synthetic fiber by modifying it with a modifying oil agent; The synthetic fibers include one or more of polyester fibers, polyamide fibers, polylactic acid fibers, or polypropylene fibers; The modified oil agent includes surfactant, antistatic agent, double-terminated PEG and nano silica. The total weight of the modified oil agent is 100 parts. Each functional component is added according to the corresponding part number. The distribution ratio of each component is shown in Table 1. The remainder is made up to 100 parts by weight with deionized water. Table 1: Modified Oil Formulation
[0006] Isomeric tridecyl alcohol polyoxyethylene ether has excellent emulsifying properties and can spread rapidly on the fiber surface; APG0810 is highly hydrophilic and can be adsorbed onto the fiber surface through hydrogen bonds. When the two are combined, the oil can be quickly and uniformly adsorbed onto the fiber surface, forming a continuous and stable mixed hydrophilic film layer.
[0007] After PEG400 forms a film, it leaves an extremely thin lubricating film on the fiber surface, which can enhance the moisturizing and film-forming properties of the oil, thereby reducing friction and assisting in antistatic properties. The addition of nano-silica forms a nano-scale rough structure on the fiber surface, which further enhances the hydrophilicity brought by the surfactant and improves the smoothness, reducing the adhesion between fibers.
[0008] The synergistic effect of the components gives the oil excellent hydrophilicity and dispersibility.
[0009] The preparation of the hydrophilic synthetic short-cut fibers of the present invention includes the following steps: S1: The synthetic fiber bundle is introduced into a water washing tank for cleaning to remove the original spinning or processing oil on the fiber surface and obtain deoiled fiber bundles. S2: The deoiled fiber bundles obtained in step S1 are introduced into the drying unit to remove the residual moisture on the fiber surface and obtain dried deoiled fiber bundles. S3: The dried and deoiled fiber bundles obtained in step S2 are introduced into an oil soaking tank, immersed in a modified oiling agent, and then pressed and controlled by extrusion rollers to keep the oiling rate stable at 0.4wt% to 0.7wt% to obtain modified oiled fiber bundles. S4: The modified oiled fiber bundle obtained in step S3 is introduced into a cutting machine and cut into short fibers to obtain hydrophilic synthetic short fibers.
[0010] Preferably, in step S1, the washed fiber filaments or fiber bundles can be dehydrated by means of extrusion rollers, etc. This can save drying costs on the one hand, and further reduce the original oil residue on the fiber surface on the other hand.
[0011] To address the problem of extremely low adhesion strength to surfactants caused by the lack of polar anchor points on the surface of polypropylene fibers, this invention employs a manganese dioxide-sulfuric acid system for chemical etching of polypropylene fibers. The etching principle is as follows: sulfuric acid provides a strongly acidic environment, enhancing the oxidizing power of MnO2, which attacks the CH bonds on the fiber surface, thereby introducing polar groups such as hydroxyl, carbonyl, and carboxyl groups onto the fiber surface through oxidation.
[0012] For polypropylene fibers, three additional steps—chemical etching, reduction decolorization, and fiber cleaning—are added between steps S1 and S2. Specifically: S1a Chemical Etching: Prepare an etching working solution with a MnO2 concentration of 70–85 g / L and a volume ratio of 98% concentrated sulfuric acid to deionized water of 2.8–3.2:1. Completely immerse the deoiled fiber bundles obtained from S1 into the etching working solution, control the temperature at 75–85℃, and etch at a constant temperature for 80–120 min. During the etching process, gently stir the fiber bundles once every 5–15 min to obtain etched fiber bundles. S1b Reduction Decolorization: Prepare a reduction and decolorization solution with an oxalic acid dihydrate concentration of 25-30 g / L and an addition of 98% concentrated sulfuric acid of 95-105 mL / L. Immerse the etched fibers in the reduction and decolorization solution and maintain the temperature at 48-53℃ for 5-15 min. During this time, shake the fiber bundle until the brown color on the fiber surface completely disappears and returns to white, thus obtaining a decolorized fiber bundle. S1c fiber cleaning: The decolorized fibers are first washed with flowing deionized water at 35-45℃ for 3-8 minutes, then rinsed with room temperature deionized water until the pH of the effluent is 6-7 and there are no manganese ions or oxalate residues. After that, they are squeezed and dewatered by pressure rollers to obtain etched and cleaned fiber bundles.
[0013] The preparation of the modified oil agent of the present invention includes the following steps: M1: Take a portion of the deionized water used to make up the balance and heat it to 40-45°C. Slowly add nano-silica under low-speed stirring and disperse it for 20-30 minutes under high-speed shearing or ultrasonic conditions to obtain a silicon pre-dispersion. M2: Add PEG400, isomeric tridecyl alcohol polyoxyethylene ether, and APG0810 sequentially to the silicon predispersant prepared in M1, and stir at 40-45℃ until fully dissolved to obtain a compound intermediate; M3: Under stirring conditions of 40-45℃, AEP-K is slowly added dropwise to the compound intermediate, and the mixture is kept warm and stirred until all components are completely compatible to obtain the compound oil intermediate; M4: Add the remaining deionized water to make the total weight reach 100 parts, keep warm at 40-45℃ for aging, then cool down and let stand to defoam, to obtain the modified oil concentrate stock solution.
[0014] When using, dilute the original solution with deionized water at a weight ratio of 1:5 to form the working solution.
[0015] Preferably, to further address the problem that the modified oil layer easily detaches from the fiber surface under long-term water washing and mechanical friction, leading to a decrease in hydrophilic dispersion performance, this invention also provides a method for preparing highly durable hydrophilic synthetic chopped fibers. This method, based on the aforementioned basic preparation process, introduces a synergistic enhancement mechanism of "fiber surface chemical anchoring" and "oil curing into a film."
[0016] Among them, "fiber surface chemical anchoring" is achieved by introducing γ-methacryloxypropyltrimethoxysilane (KH570), which utilizes its bifunctional characteristics. After hydrolysis, one end forms a covalent bond with the polar groups on the fiber surface, while the other end has a pre-reserved reactive methacryloxy group as an exposed linker. "Oil-cured film formation" is achieved by partially or completely replacing PEG400 in the original formula with PEG400 diacrylate (PEG400DA) and compounding it with 0.1 to 0.3 parts of photoinitiator. The diacrylate functional group of PEG400DA forms a three-dimensional cross-linked network after curing.
[0017] The specific changes to the steps in this preferred embodiment include the following three aspects: adding a fiber coupling pretreatment step, adjusting the modified oil agent, and adding a curing and film-forming step, as detailed below: The fiber surface coupling pretreatment is added between steps S2 and S3, and specifically includes: S2a is used to prepare a coupling pretreatment solution. The pretreatment solution contains 0.5-2.0 wt% KH570, a pH adjuster, and 5-10 vol% ethanol as a co-solvent, and should be prepared and used immediately. The pH adjuster includes one or more of glacial acetic acid, formic acid, oxalic acid, etc., and the pH adjuster should be added dropwise slowly until the pH of the system stabilizes at 3-5.5.
[0018] S2b involves immersing the dried, degreased fiber bundles obtained in S2 completely into the above pretreatment solution for 30–60 seconds. After removal, the liquid is controlled by extrusion rollers, and then pre-cured at 80–90°C for 1–2 minutes to obtain the coupling-treated fiber bundles.
[0019] It should be noted that in the above coupling pretreatment step, the pH adjuster is used to regulate the acidity of the pretreatment solution, so as to promote the hydrolysis of the methoxy group on the KH570 molecule into a highly active silanol group, and inhibit the premature condensation of the hydrolysis product to form a gel. The generated active silanol group can undergo a dehydration condensation reaction with the polar groups on the fiber surface to form a covalent bond, thereby firmly "anchoring" one end of KH570 to the fiber surface. This provides reaction sites for the subsequent chemical bonding between the modified oil layer and the fiber, fundamentally improving the bonding strength and durability of the modified interface.
[0020] The modified oil is adjusted by replacing 50% to 100% of the weight of PEG400 in the original formula with PEG400DA, or by adding 2 to 6 parts by weight of PEG400DA, and adding 0.1 to 0.3 parts by weight of photoinitiator 1173.
[0021] The curing and film-forming step is added between steps S3 and S4. Specifically, the modified oiled fiber bundle obtained in S3 is irradiated under 365nm ultraviolet light at 200-400mJ / cm² for 5-10s to obtain the cured fiber bundle.
[0022] It should be noted that the above-described coupling pretreatment and curing film-forming steps are not essential steps for implementing this invention. In applications where extreme durability is not required, these steps can be omitted, and excellent hydrophilicity and dispersibility can be achieved solely through the adsorption of the modified oil itself. However, when applied to fields requiring repeated hydrophilicity and high durability, the above-described preferred steps are preferably introduced to obtain short-cut fibers with significantly improved wash resistance.
[0023] Compared with the prior art, the present invention has the following beneficial technical effects: (1) Significantly improved hydrophilicity. This invention modifies the surface of synthetic fibers by modifying the oil, transforming the fibers from hydrophobic to hydrophilic. Tests show that the modified synthetic chopped fibers can sink in water in as little as ≤4s, which is far superior to unmodified synthetic fibers, achieving true high hydrophilicity modification.
[0024] (2) Excellent dispersibility in water and significantly reduced agglomeration rate. After impregnation with modified oil, the fiber of this invention exhibits a coefficient of variation of dry weight in aqueous suspension as low as 2%, and the overall variation can be controlled within 2.46%. The synergistic effect of nano-silica, surfactant, and antistatic agent effectively improves the dispersibility of the fiber.
[0025] (3) Significantly improved durability. The present invention introduces KH570 and PEG400DA through an optimal solution. After testing, the fiber prepared by the optimal solution has a sinking time of less than 25 seconds in water after 10 cycles of washing, which is far superior to conventional physically adsorbed modified fiber, and meets the needs of high-frequency washing and long-term use scenarios.
[0026] In summary, this invention modifies synthetic fibers by impregnation with a modified oil agent of a specific composition. The synergistic effect of the components gives the fibers both excellent hydrophilicity and dispersibility, and has good application prospects. Detailed Implementation
[0027] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0028] The raw materials used in the specific embodiments of the present invention are all commercially available conventional industrial raw materials: isomeric tridecyl alcohol polyoxyethylene ether; APG0810; AEP-K; PEG400; nano silica; and unmodified polyamide fibers, polyester fibers, polylactic acid and polypropylene fiber filaments.
[0029] Example 1 This embodiment provides a method for preparing hydrophilic polyamide chopped fibers, comprising two stages: preparation of a modifying oil and fiber modification treatment. The specific steps are as follows: (1) Preparation of modified oil The modified oil formulation in this embodiment, by weight, is as follows: 30 parts of isomeric tridecyl alcohol polyoxyethylene ether, 30 parts of APG0810, 8 parts of AEP-K, 6 parts of PEG400, 3 parts of nano-silica with a native particle size of 15nm, and 23 parts of deionized water, for a total weight of 100 parts.
[0030] Specific steps for preparing the oil: M1: Take 50% of the total amount of deionized water in the formula and heat it to 43°C. Slowly add the amount of nano-silica in the formula while stirring at a low speed of 400 r / min. After the addition is complete, shear and disperse it at a high speed of 10000 r / min for 25 min to obtain a silicon pre-dispersion without visible particle agglomeration. M2: Keep the system temperature at 43℃, and add PEG400, isotridecyl alcohol polyoxyethylene ether and APG0810 to the silicon predispersion in sequence under stirring at 400r / min. After the addition is completed, keep the temperature and stir until all components are completely dissolved to obtain the compound intermediate. M3: Keep the temperature constant at 43℃ and stir. Slowly add 8 parts of AEP-K at a rate of 2mL / min. After the addition is complete, keep the temperature and stir until the system is completely homogeneous and transparent to obtain the composite oil intermediate. M4: Add the remaining amount of deionized water, continue to keep warm and stir for 15 minutes, then let it cool naturally to room temperature, stand for 2 hours to defoam, and obtain the modified oil concentrate stock solution.
[0031] When using, dilute the above-mentioned modified oil concentrate with deionized water at a weight ratio of 1:5, stir evenly to obtain the modified oil working solution, and set aside for later use.
[0032] (2) Fiber modification treatment S1: The polyamide fiber filament bundle is introduced into a 60℃ deionized water washing tank at a speed of 10m / min and immersed and washed 3 times, each time for 10min. After washing, most of the water in the fiber bundle is removed by squeezing with a pair of rubber pressure rollers at a pressure of 0.3MPa to obtain deoiled fiber bundle. S2: Introduce the cleaned fibers into the hot air drying unit, dry at 105℃ for 2 minutes, control the fiber moisture regain to ≤0.5%, and dry the deoiled fiber bundles. S3: The dried fiber is introduced into a room temperature modified oiling agent immersion tank for 10 seconds to ensure that the fiber bundle is completely wetted. After exiting the immersion tank, it is rolled and oiled by a pair of polyurethane rollers with a roller pressure of 0.25 MPa to control the fiber oiling rate of 0.5 wt% and obtain modified oiled fiber bundle. S4: Introduce the oiled fiber into the cutting machine, adjust the cutting blade distance, and cut it into short fibers with a length of 6mm to obtain the hydrophilic polyamide short fibers of this embodiment.
[0033] Example 2 This embodiment provides a method for preparing hydrophilic polyester chopped fibers, which differs from Example 1 only in that: (1) The modified oil formulation was adjusted to: 35 parts of isomeric tridecyl alcohol polyoxyethylene ether, 25 parts of APG0810, 6 parts of AEP-K, 8 parts of PEG400, 2 parts of nano silica with a native particle size of 20nm, and 24 parts of deionized water. (2) The process parameters for oil preparation were adjusted as follows: M1 pre-dispersion temperature 42℃, high-speed shear dispersion time 27min; M2 and M3 step temperatures were both 42℃. (3) The fiber used is polyester fiber filament; (4) The oiling rate in step S3 is controlled to be 0.4 wt%.
[0034] The remaining oil preparation steps and fiber processing parameters are exactly the same as in Example 1, and finally, hydrophilic polyester short-cut fibers with a length of 6 mm are obtained.
[0035] Example 3 This embodiment provides a method for preparing hydrophilic polylactic acid chopped fibers, which differs from Example 1 only in that: (1) The modified oil formulation was adjusted to: 25 parts of isomeric tridecyl alcohol polyoxyethylene ether, 35 parts of APG0810, 10 parts of AEP-K, 6 parts of PEG400, 5 parts of nano silica with a native particle size of 8nm, and 19 parts of deionized water. (2) The process parameters for oil preparation were adjusted as follows: M1 pre-dispersion temperature 45℃, high-speed shear dispersion time 30min; M2 and M3 step temperatures were both 45℃. (3) The fiber used is polylactic acid fiber filament; (4) The oiling rate in step S3 is controlled to be 0.7 wt%.
[0036] The remaining steps for preparing the modified oil and the fiber processing parameters were exactly the same as in Example 1, and finally, hydrophilic polylactic acid short-cut fibers with a length of 6 mm were obtained.
[0037] Example 4 This embodiment provides a method for preparing hydrophilic polypropylene short-cut fibers, which differs from Example 1 only in that three steps—chemical etching, reduction decolorization, and fiber cleaning—are added between steps S1 and S2. S1a: Chemical etching The etching working solution composition ratio is as follows: MnO2 concentration is 80g / L, and the volume ratio of 98% industrial concentrated sulfuric acid to deionized water is 2.8~3.2:1; Preparation steps: Slowly pour 98% industrial concentrated sulfuric acid into deionized water along the container wall, stir and cool. When the temperature drops below 60℃, add MnO2 and continue stirring for 30 minutes until uniform suspension is obtained to obtain the etching working solution.
[0038] Etching: The fiber bundle after extrusion and dehydration in step S1 is completely immersed in the etching solution, the temperature is controlled at 80°C, and the constant temperature immersion etching is carried out for 100 minutes. During the etching process, the fiber bundle is gently stirred once every 10 minutes to obtain the etched fiber bundle.
[0039] S1b: Reduction decolorization Preparation of reduction and decolorization cleaning solution: Add 28g of oxalic acid dihydrate and 100mL of 98% concentrated sulfuric acid to each liter of deionized water, and stir until completely dissolved; Reduction and decolorization: Take out the etched fibers and immerse them in the reduction cleaning solution. Soak them at a constant temperature of 50°C for 10 minutes. During the soaking process, gently shake the fiber bundle continuously until the brown color on the fiber surface is completely removed and the fiber returns to its original white color, thus obtaining a decolorized fiber bundle.
[0040] S1c: Fiber Cleaning Soak the fiber bundle in 40℃ flowing deionized water for 5 minutes to initially remove oxalic acid, manganese salt, and sulfuric acid residue from the fiber surface. Then, continuously rinse the fiber bundle with room temperature deionized water and continuously monitor the effluent until the pH of the effluent stabilizes at 6-7 and there are no manganese ions or oxalate residues. After rinsing, squeeze the fiber bundle with a pair of rubber rollers to remove most of the water, resulting in an etched and cleaned fiber bundle.
[0041] Example 5 This embodiment provides a method for preparing highly durable hydrophilic polyamide chopped fibers, which differs from Example 1 in that: (1) The modified oil formulation was adjusted to: 30 parts of isomeric tridecyl alcohol polyoxyethylene ether, 30 parts of APG0810, 8 parts of AEP-K, 3 parts of PEG400, 3 parts of PEG400DA, 3 parts of nano silica with a native particle size of 15nm, 0.2 parts of photoinitiator 1173, and 22.8 parts of deionized water.
[0042] (2) The preparation steps for the modified oil are adjusted as follows: M2: Keep the system temperature at 43℃, and add PEG400, PEG400DA, isotridecyl alcohol polyoxyethylene ether and APG0810 to the silicon predispersion in sequence under stirring at 400r / min. After the addition is completed, keep the temperature and stir until all components are completely dissolved to obtain the compound intermediate. M4: Add 0.2 parts of photoinitiator 1173 to the compound intermediate, then add the remaining amount of deionized water, continue to keep warm and stir for 15 minutes, then let it cool naturally to room temperature, stand for 2 hours to defoam, and obtain the modified oil concentrate stock solution.
[0043] (3) An additional fiber surface coupling pretreatment step is added between steps S2 and S3, specifically including: S2a Preparation of Coupling Pretreatment Solution: Take a clean and dry reaction vessel, add 92 parts of deionized water, and then slowly add 8 vol% anhydrous ethanol to the deionized water. Stir continuously at 250 r / min for 4 min. While stirring, slowly add glacial acetic acid dropwise until the pH of the system is 4.0, then stop adding glacial acetic acid. After 2 min, add 0.8 wt% KH570 and adjust the stirring speed to 350 r / min. Stir continuously at room temperature for 40 min to hydrolyze, and then let it stand for 12 min to obtain the coupling pretreatment solution.
[0044] S2b involves immersing the dried, degreased fiber bundle obtained in S2 completely into the above pretreatment solution for 50 seconds. After removal, the fiber bundle is squeezed by a pair of rubber rollers to remove most of the moisture. The roller pressure is 0.3 MPa. The fiber bundle is then pre-cured at 85°C for 1.5 minutes to obtain the coupling-treated fiber bundle.
[0045] (4) An additional curing and film-forming process is added between steps S3 and S4, as follows: S3a introduces the modified oiled fiber bundles prepared by S3 into a UV curing chamber, irradiates them with a 365nm ultraviolet lamp, sets the radiation energy to 300mJ / cm², and irradiates for 8s to obtain cured fiber bundles. Comparative Example 1 This comparative example uses unmodified polyamide fibers, which are only subjected to S1 degreasing and cleaning and S2 drying steps in sequence, without oiling or soaking, and are directly cut into 6mm short fibers.
[0046] Comparative Examples 2-6 The preparation steps and fiber treatment processes of the modified oils in Comparative Examples 2-6 are exactly the same as those in Example 1, with the only difference being the adjustment of the modified oil formulation, as follows: Comparative Example 2: Without the addition of isomeric tridecyl alcohol polyoxyethylene ether, the amount of APG0810 was adjusted to 60 parts; Comparative Example 3: Without adding APG0810, the amount of isomeric tridecyl alcohol polyoxyethylene ether was adjusted to 60 parts; Comparative Example 4: No AEP-K was added, and the amount of deionized water was increased accordingly; Comparative Example 5: No PEG400 was added, and the amount of deionized water was increased accordingly; Comparative Example 6: No nano-silica was added, and the amount of deionized water was increased accordingly.
[0047] Comparative Examples 7-11 The preparation steps and fiber treatment processes of the modified oils in Comparative Examples 7-11 were exactly the same as those in Example 1. The only difference was that the weight parts of some components of the modified oils used in each comparative example were adjusted compared to the formulation of Example 1, and the amount of deionized water was adjusted accordingly to keep the total weight parts at 100 parts. The results of the adjustment of the weight parts of each component of the modified oils in Comparative Examples 7-11 are detailed in Table 2.
[0048] Table 2: Formulations of the modified oils used in Comparative Examples 7–11
[0049] Comparative Example 12 This comparative example uses the hydrophilic wear-resistant fiber preparation method described in Example 2 of CN122257256A to treat polyamide fibers: the functional modification layer is composed of 35% polyvinylpyrrolidone, 30% nano alumina, and 35% epoxy resin emulsion. The functional slurry is prepared according to the steps described in the patent, sprayed and cured at high temperature. After curing, the fibers are cut into 6mm short fibers. The washing and drying steps are the same as in Example 1.
[0050] Comparative Example 13 This comparative example uses the short-cut fiber dispersion preparation method described in Example 3 of CN105818398B to modify polyamide fibers: after cutting the polyamide fibers into 6mm pieces, surface modification is performed by ultrasonic reaction with dopamine at pH 8.0 for 10h to obtain hydrophilic modified short-cut fibers.
[0051] Comparative Example 14 This comparative example uses the polyolefin hydrophilic modification method described in Example 4 of CN106397821B to treat polypropylene fibers: instead of etching the polypropylene fibers, corona discharge treatment is performed on the surface of the polypropylene material at 10 kV between S2 and S3 for 30 seconds, and the remaining treatment methods are the same as in Example 4.
[0052] Comparative Examples 15–22 The preparation steps and fiber treatment processes of the modified oils in Comparative Examples 15-22 were the same as those in Example 1, the only difference being the substitution of a single component in the modified oil formulation. Specifically, each comparative example replaced the corresponding component in Example 1 with the following components in the same weight parts as the original components: Comparative Example 15 replaced isomeric tridecyl alcohol polyoxyethylene ether with fatty alcohol polyoxyethylene ether (AEO-8); Comparative Example 16 replaced APG0810 with sodium dodecyl sulfate (SDS); Comparative Example 17 replaced PEG400 with glycerol (glycerol); Comparative Example 18: PEG200 was used instead of PEG400; Comparative Example 19: PEG600 was used instead of PEG400; Comparative Example 20 replaced nano-silica (original particle size 8-20 nm) with ordinary precipitated silica (original particle size 1 μm).
[0053] Comparative Example 21 replaced the original 15nm nano-silica with nano-silica with an original particle size of 7nm.
[0054] Comparative Example 22 replaced the original 15nm nano-silica with nano-silica with an original particle size of 21nm.
[0055] Comparative Examples 23 and 24 Comparative Examples 23 and 24 are basically the same as Example 5, except that: Comparative Example 23 omitted the fiber surface coupling pretreatment step; Comparative Example 24 omitted the curing and film-forming process.
[0056] Performance testing methods (1) Hydrophilicity test: In accordance with FZ / T 50040-2018, the sedimentation method was adopted, and the sinking time of the fiber in water was used as the hydrophilicity evaluation index.
[0057] (2) Dispersion test: Refer to CN116151147B, and measure the dispersion by the coefficient of variation of dry weight of fiber in water suspension.
[0058] The monitoring steps for dispersibility testing mainly refer to the wet water suspension testing approach disclosed in CN101876139B. The fiber dispersion and sampling are completed in an aquatic environment throughout the process. The coefficient of variation of fiber dry weight in the water suspension is calculated by the fiber dry weight fluctuation of multiple sets of samples to quantify the fiber dispersion uniformity and accurately characterize the water dispersibility performance of short-cut fibers.
[0059] The specific operation and calculation steps are as follows: ① Pre-dispersion preparation of suspension: Accurately weigh 1.0g of the short-cut fiber to be tested and put it into the dispersion cylinder, add 4L of deionized water, and stir at a high speed of 1500r / min for 2min to initially disperse and break up the fiber; ② Dilution and mixing: Add deionized water to the cylinder to a total volume of 8L, reduce the stirring speed to 200r / min, and stir at low speed for 2min to eliminate local concentration differences and form a uniform fiber suspension; ③ Multi-point equal volume sampling: Let stand for 30 seconds to eliminate fluid turbulence, open the liquid discharge valve at the bottom of the dispersion cylinder to let the suspension flow out naturally, and use a graduated cylinder to randomly select 5 200mL suspension samples each. ④ Drying and weighing: Vacuum filter each of the 5 suspensions to collect all fibers; dry them in a 105℃ oven until constant weight, cool to room temperature, and weigh each fiber portion. Record the dry weight as follows: , unit g.
[0060] ⑤ Data Calculation: The first step is to calculate the average dry weight of the fibers in the five samples: The second step is to calculate the standard deviation of fiber dry weight for the five samples. :
[0061] The third step is to calculate the coefficient of variation of the dry weight of the fiber in the aqueous suspension (a dispersion evaluation index): In the formula: —Coefficient of variation of dry weight of fiber in aqueous suspension, % —Standard deviation of fiber dry weight for 5 samples, g; —Average dry weight of fibers from 5 samples, g; ——No. The dry weight of the fiber in the sampled specimen ( ), g.
[0062] (3) Durability test: The sinking time of the fiber in water was measured before and after washing, and the rate of change of the sinking time of the fiber in water was calculated. At the same time, the CV of the fiber before and after washing was measured and calculated, and its rate of change was further calculated to evaluate the durability of the hydrophilic modification of the fiber. The fiber washing was carried out in accordance with GB / T 8629-2017 standard, and a total of ten washing cycles were performed.
[0063] The formula for calculating the rate of change is: The rate of change of fiber sinking time in water (%) = (sinking time of fiber in water after 10 washes - sinking time of fiber in water before washing) / sinking time of fiber in water before washing × 100%.
[0064] Formula for calculating the rate of change of coefficient of variation: CV change rate (%) = (CV of fiber after 10 washes - CV of fiber before washing) / CV of fiber before washing × 100%.
[0065] Performance test results The performance test results of each embodiment and comparative example are detailed in Tables 3 to 7.
[0066] Table 3: Performance test results of Examples 1-5
[0067] Table 4: Performance test results of comparative examples 1-6
[0068] Table 5: Performance test results of comparative examples 7-11
[0069] Table 6: Performance test results of comparative examples 12-14
[0070] Table 7: Performance test results of comparative examples 15-22
[0071] Table 8: Results of Hydrophilic Modification Durability Test of Fibers
[0072] Table 9: Durability Test Results of Fiber Dispersion Modification
[0073] The test results above show that: Comparing Example 1 with Comparative Example 1, the unmodified polyamide fiber had a sinking time >1200s and could not form a uniform suspension, indicating that its strong hydrophobicity severely restricted its application in aqueous systems. However, in Example 1 treated with the modified oil agent of the present invention, the sinking time of the fiber in water dropped sharply to 5s, and the CV value was only 2.00%, proving that the modified oil agent of the present invention can fundamentally change the surface properties of the fiber and endow it with excellent hydrophilicity and dispersion uniformity.
[0074] Examples 2-4 used polyester fiber, polylactic acid fiber, and etched polypropylene fiber as substrates, respectively. The sinking times of the resulting fibers in water were 7s, 7s, and 6s, respectively, and the CV values were 2.31%, 2.46%, and 2.38%, respectively, all close to the level of Example 1. This indicates that the modified oil and preparation process of the present invention have good universality for different types of synthetic fibers. In particular, the chemical etching treatment can effectively solve the problem of non-polar anchor points in polypropylene fibers, making the modification effect equally excellent.
[0075] Comparing Example 1 with Comparative Examples 2-6, Comparative Examples 2-6 each lacked a specific component in the modified oil, and their fiber sinking time and / or dispersibility in water were significantly worse than those of Example 1. Specifically: In Comparative Example 2, the fiber settling time increased to 45 s with a CV value as high as 10.96% after the absence of isotridecyl alcohol polyoxyethylene ether, indicating that the emulsifying and spreading effect of isotridecyl alcohol polyoxyethylene ether is indispensable for the rapid and uniform film formation of the oil. In Comparative Example 3, the settling time was 32 s with a CV value of 8.58% after the absence of APG0810, indicating that APG0810 significantly contributes to improving hydrophilicity due to its strong hydrogen bond adsorption capacity, and only the combination of the two can achieve the shortest settling time and the lowest CV value. In Comparative Example 4, the antistatic agent AEP was missing. After -K, although the settling time was 6s, the CV value increased to 7.19%, indicating that although the antistatic agent is not a hydrophilic core component, it plays an important role in reducing electrostatic aggregation between fibers and improving dispersibility. After PEG400 was missing in Comparative Example 5, the settling time was 22s and the CV value was 5.85%. After nano silica was missing in Comparative Example 6, the settling time was 18s and the CV value was 6.5%. The absence of both resulted in a simultaneous decrease in hydrophilicity and dispersibility, confirming that PEG400 and nano silica are crucial for the synergistic improvement of performance.
[0076] Comparing Example 1 with Comparative Examples 7-11, which adjusted the amount of a certain component in the modified oil to deviate from the preferred range defined by this invention (e.g., less than 25 parts of nonionic surfactant, less than 4 parts of PEG400, and more than 5 parts of nano-silica), the results showed that the fibers produced by all formulations deviating from the preferred range had significantly higher CV values than the 2.00% of Example 1, and the sinking time of fibers in some of the comparative examples also increased to varying degrees. For example, in Comparative Example 7, the amount of isomeric tridecyl alcohol polyoxyethylene ether was reduced to 24 parts, the settling time increased to 35 s, and the CV value was 8.46%; in Comparative Example 8, APG0810 was reduced to 24 parts, the settling time was 25 s, and the CV value was 6.92%; in Comparative Example 9, PEG400 was reduced to 3 parts, the settling time was 16 s, and the CV value was 4.73%; in Comparative Example 10, nano-silica was increased to 6 parts, the settling time was 14 s, and the CV value was 4.46%; and in Comparative Example 11, nano-silica was reduced to 1 part, the settling time was 8 s, and the CV value was 3.92%. This indicates that insufficient addition of nonionic surfactants or PEG400, or deviation of the amount of nano-silica from the range of 2-5 parts, will impair the synergistic effect of fiber hydrophilicity and dispersibility. Optimal performance can only be obtained within the limits defined by this invention.
[0077] Comparing Example 1 with Comparative Examples 12 and 13, Comparative Example 12 modifies polyamide fibers using a functional coating composed of polyvinylpyrrolidone, nano-alumina, and epoxy resin, as described in existing technologies. Its sinking time is 35 seconds, and its CV value is 3.65%, both of which are inferior to those of the present invention in terms of hydrophilicity and dispersibility. Comparative Example 13 uses dopamine surface modification; although its CV value is only 1.85%, its sinking time is as long as 25 seconds, indicating severely insufficient hydrophilicity. This fails to meet the high hydrophilicity application scenarios sought by the present invention, and the modification process is complex and time-consuming. In contrast, Example 1 of the present invention maintains a CV value as low as 2.00%, while the fiber sinking time in water is only 5 seconds, achieving both excellent hydrophilicity and good dispersibility, and the process is simple and efficient.
[0078] Comparing Example 4 with Comparative Example 14, which uses the prior art corona treatment to treat polypropylene fibers, the sinking time of the fibers in water was 16s and the CV value was 3.92%. Although corona treatment improves the hydrophilicity of polypropylene fibers to some extent through surface oxidation, its sinking time is still significantly higher than that of Example 4 (6s) and its CV value is also higher than that of Example 4 (2.38%). This indicates that its hydrophilic modification effect and dispersion uniformity in water are not as good as the chemical etching synergistic oil agent modification scheme of the present invention.
[0079] Compare Example 1 with Comparative Examples 15-22 In Comparative Example 15, after replacing isomeric tridecyl alcohol polyoxyethylene ether with fatty alcohol polyoxyethylene ether, the settling time increased to 42s and the CV value increased to 8.45%, indicating that the emulsifying and spreading ability of fatty alcohol polyoxyethylene ether is far inferior to that of isomeric tridecyl alcohol polyoxyethylene ether, and it cannot form a uniform hydrophilic film layer. In Comparative Example 16, after replacing APG0810 with SDS, the settling time increased to 38s and the CV value increased to 9.46%. It is speculated that the reason is that the non-ionic mild adsorption characteristics of APG0810 and its ability to form hydrogen bonds with the fiber surface are not possessed by SDS. On the contrary, the anionic surfactant may affect the uniform adsorption of the oil agent due to electrostatic repulsion. Comparative Example 17, which replaced PEG400 with glycerol, only increased the settling time to 30s, but the CV value increased to 7.62%, indicating that PEG400 is crucial for dispersibility; Comparative Examples 18 and 19 replaced PEG400 with PEG200 and PEG600 respectively, and the CV values were 5.19% and 5.46% respectively, both higher than Example 1. This indicates that the molecular weight of PEG400 has the best match for the formulation of the present invention. It is speculated that the reason is that if the molecular weight of PEG is too low, it may lead to insufficient film-forming properties, while if it is too high, it may increase the viscosity of the oil and affect uniform coating. Comparative Example 20 replaced nano-silica with ordinary precipitated silica, and the CV value was 6.42%, which was also higher than that of Example 1. This indicates that micron-sized silica cannot provide a nanoscale rough structure, and the synergistic hydrophilic enhancement effect with surfactants is greatly weakened, which is not helpful in improving dispersibility. Comparative Examples 21 and 22, with nano-silica particle sizes adjusted to 7 nm and 21 nm respectively, yielded fibers with sinking times in water of 6 s and 11 s, and CV values of 6.54% and 1.98%, respectively. It is speculated that the 7 nm nano-silica, due to its extremely high surface energy, is prone to agglomeration in oil-based agents, leading to uneven distribution on the fiber surface and localized defects, thus significantly affecting the overall dispersion stability of the fiber. For the 21 nm nano-silica, it is speculated that the increased particle size significantly reduces the specific surface area, weakening its ability to synergistically construct a hydrophilic rough interface with surfactants, resulting in a slight increase in sinking time. This indicates that the nano-silica particle size needs to be within the 8–20 nm range specified in this invention to simultaneously achieve excellent dispersibility and hydrophilicity.
[0080] Example 5 introduced KH570 coupling pretreatment and PEG400DA curing to form a film based on the basic formulation. Its initial settling time was 4 seconds, with a CV value of 2.15%, comparable to Example 1. However, after 10 cycles of washing, the settling time only increased from 4 seconds to 5 seconds, a change rate of only 25%, while in Example 1, under the same washing conditions, the settling time increased from 5 seconds to 25 seconds, a change rate as high as 400%. Meanwhile, as shown in Table 9, the CV change rate of Example 5 was only 12.6%, while that of Example 1 was as high as 504%, indicating that the preferred solution of the present invention also has a significant advantage in maintaining dispersion stability. This shows that the preferred solution of the present invention significantly improves the bonding strength between the modified oil layer and the fiber and its wash resistance durability through the synergistic effect of chemical anchoring and cross-linking networks.
[0081] Comparing Example 5 with Comparative Examples 23 and 24, Comparative Example 23 omitted the fiber surface coupling pretreatment step, and Comparative Example 24 omitted the curing film-forming treatment step. After 10 water washes, the sinking time change rates of the fibers in Comparative Examples 23 and 24 were 160% and 375%, respectively, both significantly higher than the 25% of Example 5, and their CV change rates were 232% and 102%, respectively. The reason for this in Comparative Example 23 is speculated to be the lack of chemical anchoring in the cross-linked film, leading to its overall peeling and loss of nano-silica and antistatic agents, resulting in a severe deterioration in dispersibility. Although Comparative Example 24 had a CV change rate of 102%, the loss of a large number of uncross-linked hydrophilic molecules resulted in a sinking time change rate of 375% for the obtained fibers. The above comparisons demonstrate that both coupling pretreatment and curing film-forming are indispensable; only through their synergy can a balanced and long-lasting balance of hydrophilicity and dispersibility be achieved. However, it should be noted that even without these two preferred steps, the basic schemes of Examples 1-4 still guarantee excellent initial hydrophilicity and dispersibility, meeting the requirements of conventional applications. In summary, this invention modifies synthetic fibers by impregnating them with a modified oil agent of specific composition and ratio. The synergistic effect of the components significantly reduces the fiber's sinking time in water to ≤7s, with an optimal value of 4s, while maintaining a CV value of ≤2.46%. This achieves a balance between hydrophilicity and dispersibility, making it suitable for water-based systems such as wet papermaking and nonwoven materials. Furthermore, the coupling-crosslinking reinforcement scheme imparts excellent washability and durability to the fibers, making them suitable for applications requiring high durability, such as washable filter media and reusable industrial wipes. Compared to existing technologies, this invention offers versatility, high efficiency, and adjustable performance, meeting diverse application needs and demonstrating significant potential for industrial application.
Claims
1. A method for preparing hydrophilic synthetic short-cut fibers, characterized in that, It is prepared by hydrophilic modification of synthetic fibers using a modified oil agent; Based on 100 parts by weight of the modified oil agent, the raw materials of the modified oil agent include: 50-70 parts of nonionic surfactant, 6-10 parts of antistatic agent, 4-14 parts of double-terminated PEG, and 2-5 parts of nano-silica. The nonionic surfactant is one or more of isotridecyl alcohol polyoxyethylene ether and alkyl glycoside; The dual-terminated PEG is one or more of PEG400 and PEG400 diacrylate; The original particle size of the nano-silica is 8–20 nm.
2. The method for preparing hydrophilic synthetic short-cut fibers according to claim 1, characterized in that, The isomeric tridecyl alcohol polyoxyethylene ether has an EO number of 8 and is used in an amount of 25-35 parts, and the alkyl glycoside is APG0810, used in an amount of 25-35 parts.
3. The method for preparing hydrophilic synthetic short-cut fibers according to claim 1, characterized in that, The amount of PEG400 used is 4 to 8 parts, and the amount of PEG400 diacrylate used is 0 to 6 parts.
4. The method for preparing hydrophilic synthetic short-cut fibers according to claim 1, characterized in that, The antistatic agent is potassium C12 fatty alcohol polyoxyethylene ether phosphate, with an EO number of 3.
5. The method for preparing hydrophilic synthetic short-cut fibers according to claim 1, characterized in that, The synthetic fiber is one or more of polyester fiber, polyamide fiber, polylactic acid fiber, or polypropylene fiber.
6. The method for preparing hydrophilic synthetic short-cut fibers according to claim 1, characterized in that, The preparation of the chopped fibers also includes the following steps: S1: The synthetic fiber bundle is introduced into a water washing tank for cleaning to remove the original spinning or processing oil on the fiber surface and obtain deoiled fiber bundles. S2: The deoiled fiber bundles obtained in step S1 are introduced into the drying unit to remove the residual moisture on the fiber surface and obtain dried deoiled fiber bundles. S3: The dried and deoiled fiber bundles obtained in step S2 are introduced into an oil soaking tank, immersed in a modified oiling agent, and then pressed and controlled by extrusion rollers to keep the oiling rate stable at 0.4wt% to 0.7wt% to obtain modified oiled fiber bundles. S4: The modified oiled fiber bundle obtained in step S3 is introduced into a cutting machine and cut into short fibers to obtain hydrophilic synthetic short fibers.
7. The method for preparing hydrophilic synthetic short-cut fibers according to claim 6, characterized in that, When the synthetic fiber is polypropylene fiber, the steps between steps S1 and S2 include chemical etching, reduction decolorization, and fiber cleaning, as follows: S1a Chemical Etching: Prepare an etching working solution with a MnO2 concentration of 70–85 g / L and a volume ratio of 98% concentrated sulfuric acid to deionized water of 2.8–3.2:
1. Completely immerse the deoiled fiber bundles obtained in S1 into the etching working solution, control the temperature at 75–85°C, and etch at a constant temperature for 80–120 min. Stir the fiber bundles intermittently during etching to obtain etched fiber bundles. S1b Reduction Decolorization: Prepare a reduction and decolorization solution with an oxalic acid dihydrate concentration of 25-30 g / L and an addition of 98% concentrated sulfuric acid of 95-105 mL / L. Immerse the etched fibers in the reduction and decolorization solution and maintain the temperature at 48-53℃ for 5-15 min. During this time, shake the fiber bundle until the brown color on the fiber surface completely disappears and returns to white, thus obtaining a decolorized fiber bundle. S1c fiber cleaning: The decolorized fibers are first washed with flowing deionized water at 35-45℃ for 3-8 minutes, then rinsed with room temperature deionized water until the pH of the effluent is 6-7 and there are no manganese ions or oxalate residues. After that, they are squeezed and dewatered by pressure rollers to obtain etched and cleaned fiber bundles.
8. The method for preparing hydrophilic synthetic short-cut fibers according to any one of claims 1 to 6, characterized in that, It also includes the preparation method of modified oils, the specific steps of which are as follows: M1: Take a portion of the deionized water used to make up the balance, heat it to 40-45°C, slowly add nano-silica under low-speed stirring, and disperse it under high-speed shearing or ultrasonic conditions to obtain a silicon pre-dispersion. M2: Add PEG400 diacrylate and / or PEG400, isomeric tridecyl alcohol polyoxyethylene ether, and APG0810 sequentially to the silicon predispersant prepared in M1, and stir at 40-45℃ until fully dissolved to obtain a compound intermediate. M3: Under stirring conditions of 40-45℃, slowly add potassium C12 fatty alcohol polyoxyethylene ether phosphate to the compound intermediate, and keep it warm and stir until all components are completely compatible to obtain the compound oil intermediate; M4: Add the remaining deionized water to make the total weight reach 100 parts, keep warm at 40-45℃ for aging, then cool down and let stand to defoam, to obtain the modified oil concentrate stock solution.
9. The method for preparing hydrophilic synthetic short-cut fibers according to claim 6, characterized in that, It also includes steps to enhance the durability of the modified material: Between step S2 and step S3, a fiber surface coupling pretreatment step is also included: the dried and degreased fiber bundle is introduced into the coupling agent treatment tank, the tank solution containing 0.5-2.0 wt% γ-methacryloyloxypropyltrimethoxysilane, pH adjuster and 5-10 vol% ethanol co-solvent; the fiber bundle is immersed for 30-60 seconds and then the liquid is controlled by rollers, and then pre-cured at 80-90℃ for 1-2 minutes; Between step S3 and step S4, a curing and film-forming step is also included: the modified oiled fiber bundle is irradiated under ultraviolet light at 200-400 mJ / cm² for 5-10 seconds; The modified oil also contains a photoinitiator in its raw materials. The amount of photoinitiator added is 0.1 to 0.3 parts by weight, based on 100 parts by weight of the total weight of the modified oil.
10. A hydrophilic synthetic chopped fiber, characterized in that, It is prepared by the preparation method described in any one of claims 1 to 7 and 9.
Citation Information
Patent Citations
Device and method for detecting dispersing performance of chemical synthesized short fibers
CN101876139B
Manufacturing Method of Hydrophilic Polyester Staple Fibers for Direct Spinning Spunlace Nonwovens
CN104328531B
A kind of chopped fiber dispersion and preparation method thereof
CN105818398B
A method for durable hydrophilic modification of polyolefin material surfaces
CN106397821B
Preparation method of HDPE-PET multiple hydrophilic composite short fiber
CN114214742B