A method for modifying the pore wall interface of an alkali-resistant porous substrate using a eutectic solvent-compatible cosolvent for organic solvent slurry lamination, and a composite membrane.

By forming a non-clogging interface modification layer on the inner wall of the porous substrate pores through a ternary synergistic system of eutectic solvent and compatible cosolvent, the wetting and bonding problems between the porous substrate and the polar organic solvent slurry are solved, thereby improving the performance of the composite membrane.

CN123108935APending Publication Date: 2026-11-17HEFEI MEMBRANE TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610952419.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-29
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The porous substrate of existing composite membranes has difficulty forming stable wetting and interfacial bonding with polar organic solvent slurry on its inner pore wall, which leads to problems such as uneven pore filling, trapped air bubbles in the pores, local unwetting, interfacial voids and debonding of the composite layer. In addition, the eutectic solvent has high viscosity and slow entry into the pores when used alone, which affects the liquid permeation flux and long-term stability.

Method used

A ternary synergistic system of eutectic solvent and compatible cosolvent is adopted. By preparing an interface modification liquid of eutectic solvent and compatible cosolvent, it enters the inner wall of the pores of the porous substrate and is fixed with the surface modification components to form a non-pore-blocking interface modification layer, which improves the pore wall permeability and compatibility with subsequent functional slurries.

Benefits of technology

It improves the wetting, penetration and interfacial bonding of functional slurries, enhances the peel strength, bubble point pressure and operational stability of composite membranes, and avoids pore blockage and decrease in liquid flux.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108935A_ABST
    Figure CN123108935A_ABST
Patent Text Reader

Abstract

This invention discloses a method for modifying the pore wall interface of an alkali-resistant porous substrate using a low-eutectic solvent-compatible co-solvent for composite slurry containing a polar organic solvent in alkaline water electrolysis composite membranes, and the composite membrane itself. The method includes: providing an alkali-resistant inert porous substrate; preparing a ternary interface modification liquid consisting of a low-eutectic solvent component, a first co-solvent, and a surface modification component; wherein the mass ratio of the low-eutectic solvent component to the first co-solvent is 1:2 to 1:6, the mass fraction of the surface modification component is 0.05 wt% to 5 wt%, the system does not undergo macroscopic stratification or gelation after standing at 25 ℃ for 24 h, and the viscosity at the treatment temperature is 5-500 mPa·s; allowing the liquid to enter the interconnecting pores and contact the inner wall of the pores; after liquid control, heating, moist heat treatment, crosslinking, curing, or drying to fix the surface modification component to the pore wall, forming a non-clogging interface modification layer. After treatment, the pore blockage area ratio is not higher than 10%, and the liquid permeation flux retention rate is not less than 70%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical fields of alkaline water electrolysis membrane materials, functional composite membranes, porous substrate interface modification and organic solvent slurry composites. Specifically, it relates to a method for modifying the pore wall interface of an alkali-resistant porous substrate with a low eutectic solvent-compatible cosolvent for composite with a functional slurry containing polar organic solvents, the interface-modified porous substrate obtained by the method, and a composite membrane containing the interface-modified porous substrate. Background Technology

[0002] Alkaline water electrolysis hydrogen production devices typically require the use of diaphragm materials to separate the gases generated on the cathode and anode sides, while allowing ion conduction in the electrolyte. As alkaline electrolyzers develop towards higher current density, lower energy consumption, larger size, and longer lifespan, composite diaphragms need to simultaneously possess low sheet resistivity, high bubble point pressure, good alkali resistance, high mechanical strength, and stable interfacial bonding capabilities.

[0003] Existing composite membranes often use alkali-resistant, inert porous substrates such as polyphenylene sulfide, polyetheretherketone, polytetrafluoroethylene, and polyvinylidene fluoride as the support layer, and coat, impregnate, or laminate functional slurries containing polar organic solvents onto the surface and pores of the porous substrate. These functional slurries typically include inorganic functional particles such as zirconium oxide, titanium oxide, alumina, and barium sulfate, as well as polymer binders or film-forming polymers such as polysulfone, polyethersulfone, and polyvinylidene fluoride, with N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, or γ-butyrolactone as the main dispersion or dissolution medium.

[0004] However, alkali-resistant inert porous substrates typically have low surface energy and few polar interaction sites, making it difficult for the inner walls of the pores to form stable wetting and interfacial bonding with the aforementioned polar organic solvent slurries. Insufficient slurry penetration into the pores can easily lead to problems such as uneven pore filling, trapped air bubbles, localized lack of wetting, interfacial voids, debonding of the composite layer, decreased bubble point pressure, and insufficient long-term stability under alkaline conditions.

[0005] Conventional hydrophilication, plasma treatment, chemical oxidation, coupling agent treatment, or surface primer can improve the wettability of the substrate's outer surface to some extent, but their effect on the deep regions of the pore walls is limited, and the resulting modified layer lacks compatibility and long-term stability with subsequent organic solvent slurries. Eutectic solvents have strong hydrogen bonding, ionic interaction, and solvation capabilities, and can be used for surface treatment of various materials; however, eutectic solvents typically have high viscosity when used alone, resulting in slow penetration into micropores or complex channels, and their compatibility with subsequent NMP, DMAc, DMF, DMSO, or GBL-based functional slurries may not be sufficient.

[0006] Therefore, there is an urgent need for a pore wall interface modification method for the composite process of functional slurries containing polar organic solvents. This method can utilize the hydrogen bonding and solvation capabilities of eutectic solvents, reduce the viscosity of the system and improve the pore wall permeability through a first cosolvent compatible with the subsequent slurry, and stably introduce and fix the surface modification components into and fix them to the inner wall of the porous substrate pores. This improves the wetting, permeation and interfacial bonding stability of the subsequent functional slurry without causing pore blockage. Summary of the Invention

[0007] Furthermore, this invention utilizes a compatible eutectic solvent to regulate the viscosity, single-phase stability, and pore wall retention behavior of the eutectic solvent system, solving the problems of high viscosity and slow entry into the pore channel of a single eutectic solvent, as well as insufficient pore wall retention of ordinary organic solvents, which is different from simple solvent replacement or ordinary formulation optimization.

[0008] The purpose of this invention is to provide a method for modifying the pore wall interface of alkali-resistant porous substrates with low eutectic solvent-compatible cosolvent for composite with functional slurries containing polar organic solvents. This method solves the problems of the inner wall of the pores of alkali-resistant inert porous substrates being difficult to be fully wetted by organic solvent slurries, uneven slurry penetration in the pores, and unstable interface bonding. At the same time, it avoids the pore blockage and reduced liquid permeation caused by ordinary thick coatings or sealing films.

[0009] To achieve the above objectives, the present invention provides a method for modifying the pore wall interface of an alkali-resistant porous substrate using a eutectic solvent-compatible cosolvent, the technical solution of which includes the following steps:

[0010] Step 1: Provide an alkali-resistant inert porous substrate with interconnected channels, wherein the alkali-resistant inert porous substrate is a PPS woven mesh, PPS nonwoven fabric, PTFE porous membrane, PEEK porous membrane, PVDF porous membrane or a composite porous substrate thereof. Step 2: Prepare a eutectic solvent-compatible cosolvent interface modification solution comprising a eutectic solvent component, a first cosolvent, and a surface modification component. The eutectic solvent component is choline chloride-urea, choline chloride-ethylene glycol, or choline chloride-glycerol. The first cosolvent is N-methylpyrrolidone, N,N-dimethylacetamide, or dimethyl sulfoxide. The surface modification component is polyvinylpyrrolidone, polysulfone, polyethersulfone, dopamine, tannic acid, or polyethyleneimine. Step 3: Allow the eutectic solvent-compatible cosolvent interface modification liquid to enter the interconnecting pores and contact the inner wall of the pores, the edge of the pores and / or the fiber crossing area inside the pores; Step 4: Remove excess eutectic solvent-compatible cosolvent interface modification liquid from the outer surface, pore openings and / or the outer side of the pores of the alkali-resistant inert porous substrate, so that no continuous closed liquid film is formed at the pore openings. Step 5: The alkali-resistant inert porous substrate treated with the interface modification liquid is subjected to heating, moist heat, crosslinking, curing, drying and shaping or a combination thereof, so that the surface modification components are at least partially fixed on the inner wall of the pores, the edge of the pores and / or the fiber crossing area inside the pores, forming a non-pore-blocking interface modification layer, and thus obtaining an interface-modified porous substrate.

[0011] In a preferred embodiment, the mass ratio of the eutectic solvent component to the first cosolvent is 1:2 to 1:6, and the mass fraction of the surface modification component is 0.05 wt% to 5 wt%; the molar ratio of choline chloride to urea, ethylene glycol, or glycerol in the eutectic solvent component is 1:1 to 1:3; the eutectic solvent-compatible cosolvent interface modification solution does not undergo macroscopic stratification or gelation after standing at 25 °C for 24 h, and its viscosity at the treatment temperature is 5 mPa·s to 500 mPa·s; the eutectic solvent-compatible cosolvent interface modification solution is a single-phase or macroscopically stratified system at 20 °C to 100 °C.

[0012] In a preferred embodiment, after the interface modification treatment, the mass increase of the interface modification layer relative to the alkali-resistant inert porous substrate is 0.05 wt% to 5 wt%, the pore blockage area ratio is not higher than 10%, and the liquid permeability retention rate is not lower than 70% of that before the treatment; the non-blocking interface modification layer is used to improve the wetting, penetration and interfacial bonding of the subsequent functional slurry containing polar organic solvent with a solid content of 40 wt% to 90 wt% in the pores.

[0013] In a preferred embodiment, the eutectic solvent component is choline chloride-urea, the first cosolvent is N-methylpyrrolidone, and the surface modification component is polyvinylpyrrolidone; or, the eutectic solvent component is choline chloride-glycerol, the first cosolvent is N,N-dimethylacetamide, and the surface modification component is polysulfone or polyethersulfone.

[0014] In a preferred embodiment, step (3) is carried out by dip coating, spray coating, roller coating, scraping coating, vacuum-assisted impregnation, pressure-assisted impregnation, circulating injection or filtration penetration; step (4) is carried out by scraping liquid, roller pressing and squeezing liquid, air knife blowing, centrifugal liquid removal, negative pressure suction, filtration and drainage, quantitative roller control of liquid or a combination thereof.

[0015] In a preferred embodiment, the temperature of the shaping treatment in step (5) is 40 ℃ to 120 ℃, and the treatment time is 10 min to 6 h; preferably, after the interface modification treatment, the mass increase of the interface modification layer relative to the alkali-resistant inert porous substrate is 0.10 wt% to 3 wt%, the pore blockage area ratio is not higher than 5%, and the liquid permeability retention rate is not lower than 80% of that before the treatment.

[0016] The present invention also provides an interface-modified porous substrate prepared by the above method, wherein the interface-modified porous substrate comprises an alkali-resistant inert porous substrate and a non-blocking interface modification layer located on the inner wall of the pores, the edge of the pores and / or the fiber crossing area within the pores.

[0017] The present invention also provides a composite membrane, comprising the interface-modified porous substrate and a functional composite layer composited with the interface-modified porous substrate. The functional composite layer at least partially enters the communicating channels and contacts, entangles, bonds, or interpenetrates with the non-pore-blocking interface modification layer; the functional composite layer is formed from a functional slurry containing a polar organic solvent, the solid content of which is 40 wt% to 90 wt%, and at least partially enters the communicating channels.

[0018] Compared with the prior art, the present invention improves the ability of the interface modification liquid to enter the inner wall of the pores, the compatibility with the subsequent polar organic solvent functional slurry, and the pore wall fixation stability through a ternary synergistic system of eutectic solvent component, first cosolvent and surface modification component. This improves the wetting, penetration and interfacial bonding of the subsequent functional slurry, and improves the peel strength, bubble point pressure and operational stability of the composite membrane while keeping the pore openings unblocked and the liquid permeation flux high. Attached Figure Description

[0019] Figure 1 This is a schematic flowchart of the pore wall interface modification method of the eutectic solvent-compatible cosolvent described in this invention.

[0020] Figure 2 This is a schematic diagram comparing the pore wall state of an untreated porous substrate and an interface-modified porous substrate.

[0021] Figure 3 This is a schematic diagram showing how the eutectic solvent component, the first co-solvent, and the surface modification component synergistically enter the inner wall of the pores to form an interface modification layer.

[0022] Figure 4 This is a schematic diagram comparing the wetting and penetration behavior of untreated porous substrates and interface-modified porous substrates on functional slurries containing polar organic solvents.

[0023] Figure 5 This is a schematic diagram of the cross-sectional structure of a composite membrane prepared using an interface-modified porous substrate.

[0024] Figure 6 This is a scanning electron microscope comparison image of an untreated alkali-resistant porous substrate and an interface-modified porous substrate.

[0025] Figure 7 Comparison of X-ray diffraction patterns of PPS substrate, interface-modified substrate, and composite membrane.

[0026] Figure 8Optical photographs of untreated and interface-modified substrates, and a comparison of their wetting behavior with polar organic solvent slurries.

[0027] Explanation of reference numerals in the attached figures 1. Alkali-resistant inert porous substrate; 11. Connecting pores; 12. Pore inner wall; 13. Pore opening; 14. Fiber cross-section area within the pore; 2. Eutectic solvent-cosolvent interface modification liquid; 21. Eutectic solvent component; 22. First cosolvent; 23. Surface modification component; 24. Excess interface modification liquid; 3. Interface modification layer; 31. Polar organic solvent-affinity polymer layer; 32. Adhesion and fixing layer; 33. Polar group modification layer; 4. Functional slurry containing polar organic solvent; 41. Inorganic functional particles; 42. Polymer binder; 43. Polar organic solvent; 5. Functional composite layer; 6. Composite membrane; 7. Pore defects or interface voids; 8. Continuous pore plugging layer. Detailed Implementation

[0028] The present invention will be further described below with reference to the accompanying drawings and embodiments. It should be understood that the following embodiments are only used to illustrate the technical solutions and effects of the present invention, and are not intended to limit the scope of protection of the present invention. Without departing from the core concept of the present invention, those skilled in the art can adjust, replace, or combine the substrate type, eutectic solvent component, first co-solvent, surface modification component, introduction method, shaping method, and subsequent functional slurry composition.

[0029] like Figure 1 As shown, the method of the present invention includes providing an alkali-resistant inert porous substrate 1, preparing a low eutectic solvent-cosolvent interface modification liquid 2, allowing it to enter the connecting channel 11 and contact the inner wall 12 of the pore, removing excess interface modification liquid 24, forming an interface modification layer 3 after shaping treatment, obtaining an interface-modified porous substrate, and further compounding it with a functional slurry containing a polar organic solvent 4 to prepare a composite membrane 6.

[0030] like Figure 2 As shown, the surface of the pore wall of the untreated alkali-resistant inert porous substrate lacks polar interaction sites, and subsequent functional slurries are prone to local dewetting and defect formation in the pores. After treatment by the present invention, the interface modification layer 3 is at least partially located on the inner wall 12 of the pores, which can provide a wetting, entanglement, bonding or interpenetration interface for subsequent functional slurries containing polar organic solvents.

[0031] like Figure 3 As shown, the eutectic solvent component 21, the first cosolvent 22, and the surface modification component 23 form a synergistic system. The eutectic solvent component 21 provides hydrogen bonding, ionic interaction, and solvation environment; the first cosolvent 22 reduces the viscosity of the system and improves compatibility with subsequent functional slurries; and the surface modification component 23 is fixed to the pore wall after the shaping process to form an interface modification layer 3.

[0032] like Figure 4 As shown, the untreated substrate has poor wetting and pore penetration of functional slurries containing polar organic solvents, which easily leads to defects in the pores or interfacial voids. The porous substrate after interface modification enables the functional slurry to spread faster and enter the interconnected pores, reducing defects in the pores.

[0033] like Figure 5 As shown, the composite membrane 6 includes an interface-modified porous substrate and a functional composite layer 5. The functional composite layer 5 at least partially enters the connecting channel 11 and is in continuous contact, entangled, bonded or interpenetrated with the interface modification layer 3.

[0034] Figure 1 This is a schematic flowchart of the method for modifying the eutectic solvent-co-solvent interface of alkali-resistant porous substrates according to the present invention. Figure 1 As shown, the method includes: (1) providing an alkali-resistant inert porous substrate; (2) cleaning and degreasing; (3) preparing a eutectic solvent-cosolvent interface modification solution; (4) introducing it onto the surface and pore walls of the substrate; (5) heating / humidifying / crosslinking / curing / shaping; (6) washing / drying; (7) obtaining an interface-modified porous substrate.

[0035] Figure 2 This is a schematic diagram comparing the interface state of the pore inner wall of an untreated alkali-resistant inert porous substrate and an interface-modified porous substrate treated by the method of this invention. Figure 2 As shown, the untreated alkali-resistant inert porous substrate exhibits smooth inner pore walls, inertness, and difficulty in interacting with resin solvents. However, the interface-modified porous substrate treated by the method of this invention exhibits easily interacting inner pore wall interfaces with resins / solvents.

[0036] Figure 3 This is a schematic diagram illustrating the mechanism by which the eutectic solvent component, the first co-solvent, and the surface modification component synergistically enter the inner wall of the pores and form an interface modification layer, as described in this invention. Figure 3 As shown, the mechanism includes: 1. preparation of solution components, 2. synergistic penetration into the pores, and 3. formation of an interface modification layer on the pore wall.

[0037] Figure 4 This is a schematic diagram comparing the wetting and penetration behavior of polar organic solvent functional slurries on an untreated alkali-resistant inert porous substrate and an interface-modified porous substrate treated by the method of this invention. Figure 4 As shown, the untreated substrate exhibits a large contact angle and poor wettability; while the interface-modified porous substrate treated by the method of this invention exhibits a small contact angle and good wettability.

[0038] Figure 5 This is a schematic diagram of the structure of an alkaline water electrolysis composite membrane prepared using the interface-modified porous substrate of this invention. Figure 5As shown, an interface modification layer is formed on the inner wall of the pores, and the functional composite layer partially enters the pore channels. For example... Figure 5 As shown, the untreated porous substrate exhibits uneven functional slurry regions formed on the inner walls of the pores; while the interface-modified porous substrate treated by the method of the present invention forms an interface modification layer, and the inner walls of the pores are functionalized and roughened.

[0039] Figure 6 This is a comparison image using scanning electron microscopy (SEM) of untreated alkali-resistant porous substrates and interface-modified porous substrates. Among them, (a) is a surface morphology image of the untreated porous substrate; (b) is a surface morphology image of the interface-modified porous substrate; (c) is a cross-sectional morphology image of the untreated porous substrate; and (d) is a cross-sectional morphology image of the interface-modified porous substrate.

[0040] Figure 7 Comparison of X-ray diffraction (XRD) images of PPS substrate, interface-modified substrate, and composite membrane.

[0041] The figure shows that the main characteristic peaks of the PPS substrate are basically maintained after the interface modification treatment, while the characteristic diffraction peaks of inorganic functional particles further appear in the composite membrane.

[0042] Figure 8 Optical photographs of untreated and interface-modified substrates, and a comparison of their wetting behavior with polar organic solvent slurries.

[0043] Among them, (a) is a dry optical photograph of the untreated substrate; (b) is a dry optical photograph of the interface-modified substrate; (c) is the initial wetting state of the polar organic solvent slurry on the surface of the untreated substrate; and (d) is the initial wetting state of the polar organic solvent slurry on the surface of the interface-modified substrate.

[0044] Depend on Figure 8 As can be seen, the surface of the untreated substrate is uneven, the contact angle is large, and the wettability is poor; while the surface of the interface-modified substrate is uniform, the contact angle is small, and the wettability is good.

[0045] The following embodiments are used to further illustrate the technical solutions of the present invention, but should not be construed as limiting the scope of protection of the present invention. All equivalent substitutions, modifications, or combinations made based on the concept of the present invention without departing from the essential content of the present invention should fall within the scope of protection of the present invention.

[0046] Example 1: Interfacial Modification of Polyphenylene Sulfide Nonwoven Fabric with Choline Chloride-Urea / NMP / PVP Step 1: Provide polyphenylene sulfide nonwoven fabric as an alkali-resistant, inert, porous substrate. Step 2: Mix choline chloride and urea in a molar ratio of 1:2 to form a choline chloride-urea eutectic solvent component; add N-methylpyrrolidone as a first cosolvent, making the mass ratio of the eutectic solvent component to N-methylpyrrolidone 1:2; subsequently, add polyvinylpyrrolidone as a surface modification component, making its mass fraction 2 wt%, to obtain a eutectic solvent-cosolvent interface modification solution.

[0047] Step 3: Immerse the polyphenylene sulfide nonwoven fabric in the above-mentioned interface modification solution, allowing the interface modification solution to penetrate the substrate surface and at least part of the pore inner wall. Step 4: Remove excess interface modification solution from the outer surface and pore openings, followed by heat treatment to allow polyvinylpyrrolidone to adhere to and fix to the inner wall of the polyphenylene sulfide pores; after washing and drying, obtain the interface-modified polyphenylene sulfide porous substrate.

[0048] The results showed that the contact angle of untreated polyphenylene sulfide nonwoven fabric with N-methylpyrrolidone was approximately 68°, which decreased to approximately 22° after treatment in this embodiment. The complete wetting time of the functional slurry containing N-methylpyrrolidone in the untreated substrate was greater than 90 s, while it was shortened to approximately 8 s in the interface-modified substrate. Cross-sectional SEM showed that the functional slurry could penetrate more uniformly into the pores of the interface-modified substrate, and no obvious interfacial voids were observed between the pore walls and the functional composite layer. The peel strength of the functional layer of the composite membrane increased from approximately 0.18 N / cm in the control sample to approximately 0.62 N / cm, the bubble point pressure increased from approximately 0.31 MPa to approximately 0.52 MPa, and the sheet resistivity remained at approximately 0.30 Ω·cm².

[0049] Example 2: Interfacial Modification of Polyphenylene Sulfide Mesh with Choline Chloride-Glycerol / DMAc / Polysulfone Step 1: Provide polyphenylene sulfide mesh as an alkali-resistant, inert porous substrate. Step 2: Mix choline chloride and glycerol in a molar ratio of 1:2 to form a choline chloride-glycerol eutectic solvent component; add N,N-dimethylacetamide as a first cosolvent, making the mass ratio of the eutectic solvent component to N,N-dimethylacetamide 1:3; add polysulfone as a polar organic solvent polymer, making its mass fraction 3 wt%, to obtain a eutectic solvent-cosolvent interface modified solution.

[0050] Step 3: The polyphenylene sulfide (PPS) mesh is placed in the above-mentioned interface modification solution for treatment, allowing polysulfone to enter and adhere to the surface of the PPS mesh and the inner walls of the pores. Step 4: Excess interface modification solution is removed from the pore openings and outer surface. After heat treatment, washing, and drying, the interface-modified PPS mesh is obtained.

[0051] The results showed that after treatment, the contact angle of the polyphenylene sulfide (PPS) mesh with N,N-dimethylacetamide decreased from approximately 64° to approximately 19°. The DMAc-containing ceramic / polymer functional slurry spread more uniformly in the interface-modified PPS mesh, forming a continuous composite interface on the inner walls of the pores. The resulting composite membrane exhibited a peel strength of approximately 0.68 N / cm, significantly higher than the approximately 0.20 N / cm of the sample prepared from the untreated substrate. The bubble point pressure increased from approximately 0.33 MPa to approximately 0.55 MPa, and the sheet resistivity was approximately 0.32 Ω·cm².

[0052] Example 3: Interfacial Modification of Polyphenylene Sulfide Nonwoven Fabric with Choline Chloride-Lactic Acid / DMSO / Polyethylene Imine Step 1: Provide polyphenylene sulfide nonwoven fabric as an alkali-resistant, inert, porous substrate. Step 2: Mix choline chloride and lactic acid in a molar ratio of 1:2 to form a choline chloride-lactic acid eutectic solvent component; add dimethyl sulfoxide as a first cosolvent, making the mass ratio of the eutectic solvent component to dimethyl sulfoxide 1:2; add polyethyleneimine as an adhesion and fixing component, making its mass fraction 1.5 wt%, to obtain a eutectic solvent-cosolvent interface modified solution.

[0053] Step 3: Treat the polyphenylene sulfide nonwoven fabric with the above-mentioned interface modification solution to allow polyethyleneimine to enter the inner wall of the pores. Step 4: Remove excess interface modification solution and fix the polyethyleneimine to the inner wall of the pores through hydrogen bonding, ionic interaction, and entanglement. After washing and drying, the interface-modified polyphenylene sulfide porous substrate is obtained.

[0054] The results showed that after treatment, the contact angle of polyphenylene sulfide nonwoven fabric with dimethyl sulfoxide decreased from approximately 71° to approximately 25°. The wetting time of the functional slurry in the treated substrate was shortened from approximately 110 s in the control sample to approximately 15 s. In the cross-section of the composite diaphragm, the functional composite layer and the substrate were tightly bonded, and no obvious debonding areas were observed. The peel strength increased from approximately 0.16 N / cm to approximately 0.57 N / cm. After immersion in alkaline solution, the composite layer still maintained good integrity, with a peel strength retention rate of approximately 91% and a bubble point retention rate of approximately 93%.

[0055] Example 4: Interfacial Modification of Polyphenylene Sulfide Fiber Porous Membranes with Choline Chloride-Ethylene Glycol / NMP / Dopamine Step 1: Provide a polyphenylene sulfide fiber porous membrane as an alkali-resistant inert porous substrate. Step 2: Mix choline chloride and ethylene glycol in a molar ratio of 1:2 to form a eutectic solvent component; add N-methylpyrrolidone as a first cosolvent, making the mass ratio of the eutectic solvent component to N-methylpyrrolidone 1:4; add dopamine as an adhesion and fixation component to obtain a eutectic solvent-cosolvent interface modified solution.

[0056] Step 3: Place the polyphenylene sulfide fiber porous membrane in the above-mentioned interface modification solution for treatment, so that the interface modification solution contacts the fiber surface and the inner wall of the pores. Step 4: Remove excess interface modification solution, and allow dopamine to be deposited or fixed on the fiber surface and the inner wall of the pores to form an adhesive interface modification layer; after washing and drying, the interface-modified polyphenylene sulfide fiber porous membrane is obtained.

[0057] The results showed that after treatment, a continuous and uniform thin-layer interface modification structure appeared on the surface of the polyphenylene sulfide fiber. The contact angle of the substrate with N-methylpyrrolidone decreased from approximately 69° to approximately 20° after treatment. After functional slurry lamination, cross-sectional SEM showed that the ceramic / polymer composite layer could be tightly bonded to the fiber surface. The composite diaphragm peel strength reached approximately 0.74 N / cm, the bubble point pressure reached approximately 0.56 MPa, and the sheet resistivity was approximately 0.31 Ω·cm².

[0058] Example 5: Interfacial Modification of Polyphenylene Sulfide Nonwoven Fabric with Choline Chloride-Oxalic Acid / DMAc / Tanolic Acid-Polyethyleneimine Step 1: Provide polyphenylene sulfide nonwoven fabric as an alkali-resistant, inert, porous substrate. Step 2: Mix choline chloride and oxalic acid in a molar ratio of 1:1 to form a choline chloride-oxalic acid eutectic solvent component; add N,N-dimethylacetamide as a first cosolvent, making the mass ratio of the eutectic solvent component to N,N-dimethylacetamide 1:3; add tannic acid and polyethyleneimine as adhesion and fixation components to obtain a eutectic solvent-cosolvent interface modification solution.

[0059] Step 3: Treat the polyphenylene sulfide nonwoven fabric with the aforementioned interface modification solution, allowing the solution to enter the pores and contact the inner walls of the pores. Step 4: Remove excess interface modification solution and fix the tannic acid-polyethyleneimine composite modification layer to the inner walls of the polyphenylene sulfide pores; after washing and drying, obtain the interface-modified polyphenylene sulfide porous substrate.

[0060] The results showed that after treatment, the contact angle of the substrate with DMAc decreased from approximately 66° to approximately 24°. The functional slurry formed a continuous filling structure in the pores of the interface-modified substrate, while in the untreated sample, local unfilled or insufficiently filled pores were visible. The bubble point pressure of the resulting composite membrane increased from approximately 0.34 MPa in the control sample to approximately 0.58 MPa, and the peel strength increased from approximately 0.19 N / cm to approximately 0.65 N / cm. The bubble point retention rate after alkali immersion was approximately 94%.

[0061] Example 6: Interfacial Modification of Polytetrafluoroethylene Porous Membranes with Choline Chloride-Urea / DMF / Dopamine-Silane Coupling Agent Step 1: Provide a polytetrafluoroethylene porous membrane as an alkali-resistant inert porous substrate. Step 2: Mix choline chloride and urea in a molar ratio of 1:2 to form a eutectic solvent component; add N,N-dimethylformamide as a first cosolvent, making the mass ratio of the eutectic solvent component to N,N-dimethylformamide 1:4; add dopamine and a silane coupling agent as surface modification components to obtain a eutectic solvent-cosolvent interface modified solution.

[0062] Step 3: Treat the polytetrafluoroethylene porous membrane with the aforementioned interface modification solution, allowing the solution to penetrate the membrane surface and at least part of the pore inner walls. Step 4: Remove excess interface modification solution from the pore openings and outer surface, allowing a dopamine-silane composite interface layer to form on the polytetrafluoroethylene surface and at least part of the pore inner walls; after washing and drying, obtain the interface-modified polytetrafluoroethylene porous substrate.

[0063] The results showed that the contact angle of the untreated PTFE porous membrane with DMF was approximately 92°, which decreased to approximately 37° after treatment in this embodiment. The functional slurry containing DMF showed slow and uneven wetting in the untreated PTFE porous membrane, while significant channel penetration was achieved in the treated substrate. The peel strength of the resulting composite membrane increased from approximately 0.08 N / cm in the control sample to approximately 0.46 N / cm, and the bubble point pressure increased from approximately 0.24 MPa to approximately 0.43 MPa.

[0064] Example 7: Betaine-glycerol / NMP / PAA-PVP interface modification of polyvinylidene fluoride porous membranes Step 1: Provide a polyvinylidene fluoride porous membrane as an alkali-resistant inert porous substrate. Step 2: Mix betaine and glycerol in a molar ratio of 1:2 to form a betaine-glycerol eutectic solvent component; add N-methylpyrrolidone as a first cosolvent, making the mass ratio of the eutectic solvent component to N-methylpyrrolidone 1:3; add polyacrylic acid and polyvinylpyrrolidone as surface modification components to obtain a eutectic solvent-cosolvent interface modification solution.

[0065] Step 3: Treat the polyvinylidene fluoride porous membrane with the above-mentioned interface modification solution, allowing the interface modification solution to penetrate into the inner wall of the pores. Step 4: Remove excess interface modification solution and fix polyacrylic acid and polyvinylpyrrolidone to the inner wall of the polyvinylidene fluoride pores; after washing and drying, obtain the interface-modified polyvinylidene fluoride porous substrate.

[0066] The results showed that, after treatment, the contact angle of the polyvinylidene fluoride porous membrane with N-methylpyrrolidone decreased from approximately 78° to approximately 26°. The NMP-containing functional slurry penetrated more fully into the treated substrate, resulting in a tighter bond between the composite layer and the substrate. The peel strength of the composite membrane increased from approximately 0.14 N / cm to approximately 0.53 N / cm, the bubble point pressure increased from approximately 0.30 MPa to approximately 0.49 MPa, and the sheet resistivity was approximately 0.34 Ω·cm².

[0067] Example 8: Interfacial Modification of Polyetheretherketone Porous Substrates with Choline Chloride-Ethylene Glycol / γ-Butyrolactone / PES-PVP Step 1: Provide a polyetheretherketone (PEEK) porous substrate as an alkali-resistant, inert porous substrate. Step 2: Mix choline chloride and ethylene glycol in a molar ratio of 1:2 to form a eutectic solvent component; add γ-butyrolactone as a first cosolvent, making the mass ratio of the eutectic solvent component to γ-butyrolactone 1:3; add polyethersulfone and polyvinylpyrrolidone as polar-loving organic solvent polymers to obtain a eutectic solvent-cosolvent interface modified solution.

[0068] Step 3: The polyetheretherketone porous substrate is treated with the above-mentioned interface modification solution to allow polyethersulfone and polyvinylpyrrolidone to enter the inner wall of the pores. Step 4: Excess interface modification solution is removed, and polyethersulfone and polyvinylpyrrolidone are fixed to the inner wall of the polyetheretherketone pores; after washing and drying, the interface-modified polyetheretherketone porous substrate is obtained.

[0069] The results showed that after treatment, the contact angle of the polyetheretherketone porous substrate with γ-butyrolactone decreased from approximately 73° to approximately 29°. The degree of continuous filling of the functional slurry in the pores of the treated substrate was significantly higher than that of the untreated substrate. The peel strength of the resulting composite membrane increased from approximately 0.17 N / cm to approximately 0.50 N / cm, and the bubble point pressure increased from approximately 0.35 MPa to approximately 0.51 MPa. After immersion in alkaline solution, no significant interfacial debonding occurred in the composite layer.

[0070] Example 9: Continuous Eutectic Solvent-Cosolvent Interface Modification of Polyphenylene Sulfide Rolls Step 1: Provide wide-width polyphenylene sulfide nonwoven fabric rolls as alkali-resistant, inert, porous substrates. Step 2: Prepare a choline chloride-urea / N-methylpyrrolidone / polyvinylpyrrolidone eutectic solvent-cosolvent interface modification solution, wherein the molar ratio of choline chloride to urea is 1:2, the mass ratio of the eutectic solvent component to N-methylpyrrolidone is 1:2, and the mass fraction of polyvinylpyrrolidone is 2 wt%.

[0071] Step 3: The polyphenylene sulfide nonwoven fabric roll is continuously passed through the interface modification liquid, allowing the liquid to penetrate the substrate surface and at least part of the pore inner walls. Step 4: The liquid is controlled, heated and shaped, washed, dried and wound up sequentially to obtain a continuous interface-modified polyphenylene sulfide porous substrate.

[0072] The results showed that the continuously treated polyphenylene sulfide (PPS) roll material exhibited good uniformity of interfacial modification along both the width and length directions. The contact angles of samples at different locations with N-methylpyrrolidone were concentrated between approximately 21° and 28°. After preparing composite membranes using samples from different locations, the bubble point pressures ranged from approximately 0.48 MPa to 0.54 MPa, and the sheet resistivity ranged from approximately 0.29 Ω·cm² to 0.33 Ω·cm², indicating that the method of this invention is suitable for continuous processing of roll materials.

[0073] Example 10: Preparation of an alkaline water electrolysis composite membrane using an interface-modified polyphenylene sulfide porous substrate. Step 1: Take the interface-modified polyphenylene sulfide porous substrate obtained in Example 1. Step 2: Prepare a functional slurry containing N-methylpyrrolidone, wherein the functional slurry comprises zirconium oxide inorganic functional particles, polysulfone film-forming polymer, binder, and dispersant. Step 3: Apply the functional slurry to the interface-modified polyphenylene sulfide porous substrate, allowing at least a portion of the functional slurry to enter the substrate pores and bond with the interface modification layer located on the inner wall of the pores. Step 4: After drying and setting, an alkaline electrolytic water composite membrane is obtained.

[0074] The results showed that in the composite membrane prepared using interface-modified polyphenylene sulfide porous substrate, the zirconium oxide / polysulfone functional composite layer was uniformly distributed within the substrate pores, and the bond between the pore inner walls and the functional composite layer was tight. Compared with the composite membrane prepared using untreated polyphenylene sulfide substrate, the peel strength of the composite membrane in this embodiment increased from approximately 0.18 N / cm to approximately 0.66 N / cm, the bubble point pressure increased from approximately 0.32 MPa to approximately 0.55 MPa, and the sheet resistivity decreased from approximately 0.34 Ω·cm² to approximately 0.30 Ω·cm². After immersion in alkaline solution, no significant peeling or flaking of the composite layer was observed, with a bubble point retention rate of approximately 93% and a peel strength retention rate of approximately 90%.

[0075] Comparative Example 1: Untreated polyphenylene sulfide porous substrate Step 1: Provide the same polyphenylene sulfide nonwoven fabric as in Example 1. Step 2: Without eutectic solvent-cosolvent interface modification treatment, directly apply to the composite of functional slurry containing N-methylpyrrolidone.

[0076] The results showed that the contact angle of untreated polyphenylene sulfide nonwoven fabric with N-methylpyrrolidone was approximately 68°, and the complete wetting time of the functional slurry was greater than 90 s. Local areas of the composite membrane exhibited insufficient pore filling and interfacial voids. The peel strength of the functional layer was approximately 0.18 N / cm, the bubble point pressure was approximately 0.31 MPa, and the sheet resistivity was approximately 0.34 Ω·cm².

[0077] Comparative Example 2 only used the first co-solvent treatment Step 1: Provide the same polyphenylene sulfide nonwoven fabric as in Example 1. Step 2: Impregnate with only N-methylpyrrolidone, without adding eutectic solvent components or surface modification components. Step 3: After treatment, dry to obtain the control substrate.

[0078] The results showed that treatment with N-methylpyrrolidone alone improved the initial wettability of the substrate to N-methylpyrrolidone, but the wetting effect was significantly weakened after drying. The resulting composite diaphragm had a peel strength of approximately 0.25 N / cm and a bubble point pressure of approximately 0.36 MPa, which were lower than those of the sample obtained in Example 1.

[0079] Comparative Example 3 was treated with only a eutectic solvent. Step 1: Provide the same polyphenylene sulfide nonwoven fabric as in Example 1. Step 2: Treat with only a choline chloride-urea eutectic solvent, without adding a first co-solvent or surface modification components.

[0080] The results showed that when only a eutectic solvent was used for treatment, the system viscosity was high, limiting the ability of the treatment liquid to enter the pores. The resulting composite membrane had a peel strength of approximately 0.29 N / cm and a bubble point pressure of approximately 0.38 MPa, indicating that the distribution of the functional composite layer in the local pores remained uneven.

[0081] Comparative Example 4 uses a eutectic solvent and a first co-solvent, but without adding surface modification components. Step 1: Provide the same polyphenylene sulfide nonwoven fabric as in Example 1. Step 2: Use a treatment solution composed of choline chloride-urea and N-methylpyrrolidone, but without adding polyvinylpyrrolidone or other surface-modifying components.

[0082] The results showed that this treatment method could improve the ability of the treatment liquid to enter the pores, but due to the lack of surface modification components that could be fixed to the inner wall of the pores, the resulting interface modification effect was unstable. The peel strength of the obtained composite membrane was approximately 0.34 N / cm, and the bubble point pressure was approximately 0.41 MPa, both lower than the sample obtained in Example 1.

[0083] Comparative Example 5 was treated with a eutectic solvent and a second cosolvent. Step 1: Provide the same polyphenylene sulfide nonwoven fabric as in Example 1. Step 2: Use choline chloride-urea eutectic solvent and ethanol as the main co-solvents, and add polyvinylpyrrolidone for treatment.

[0084] The results showed that while using ethanol as the main co-solvent could reduce the system viscosity, it resulted in insufficient compatibility with the subsequent N-methylpyrrolidone-based functional slurry. The resulting composite membrane had a peel strength of approximately 0.39 N / cm and a bubble point pressure of approximately 0.44 MPa, which were still lower than those of Example 1 treated with the first co-solvent N-methylpyrrolidone.

[0085] Table 1 Summary of Results of Examples

[0086] As can be seen from the results of the above embodiments and comparative examples, the interface-modified porous substrate provided by the present invention can improve the wettability, pore permeability, and interfacial bonding stability of subsequent polar organic solvent functional slurries. Compared with untreated samples, samples treated only with the first cosolvent, samples treated only with the eutectic solvent, samples treated with the eutectic solvent and the first cosolvent but without surface modification components, and samples treated with an incompatible second cosolvent, the ternary interface modification liquid of the present invention can simultaneously achieve pore wall permeability, slurry compatibility, and interface fixation, and is suitable for the preparation of alkaline water electrolysis composite membranes.

[0087] Other embodiments of this disclosure will readily occur to those skilled in the art upon consideration of the specification and practice of the disclosure herein. This application is intended to cover any variations, uses, or adaptations of this disclosure that follow the general principles of this disclosure and include common knowledge or customary techniques in the art not disclosed herein. The specification and examples are to be considered exemplary only, and the true scope and spirit of this disclosure are indicated by the following claims.

Claims

1. A method for modifying the pore wall interface of an alkali-resistant porous substrate using a low-eutectic solvent-compatible co-solvent for composite slurry containing polar organic solvents in alkaline water electrolysis composite membranes, characterized in that, Includes the following steps: (1) Provide an alkali-resistant inert porous substrate having interconnected channels, wherein the interconnected channels have an inner wall of pores, a channel edge, an opening and an outer surface; (2) Prepare a eutectic solvent-compatible cosolvent interface modification solution, wherein the interface modification solution comprises a eutectic solvent component, a first cosolvent and a surface modification component; (3) The eutectic solvent-compatible cosolvent interface modification liquid is introduced into the communicating channel and contacts the inner wall of the pore, the edge of the pore and / or the fiber crossing area inside the pore; (4) Remove excess eutectic solvent-compatible cosolvent interface modification liquid from the outer surface, orifice and / or outer side of the pores of the alkali-resistant inert porous substrate so that no continuous closed liquid film is formed at the orifice. (5) The alkali-resistant inert porous substrate treated with the interface modification liquid is subjected to heating, moist heat, crosslinking, curing, drying and shaping or a combination thereof, so that the surface modification component is at least partially fixed on the inner wall of the pores, the edge of the pores and / or the fiber cross area inside the pores, forming a non-clogging interface modification layer, and obtaining an interface-modified porous substrate; wherein, after the interface modification treatment, the mass increase of the interface modification layer relative to the alkali-resistant inert porous substrate is 0.05 wt% to 5 wt%, the pore blockage area ratio is not higher than 10%, and the liquid permeation flux retention rate is not lower than 70% before the treatment. The non-clogging interface modification layer is used to improve the wetting, penetration and interface bonding of the subsequent functional slurry containing polar organic solvent with a solid content of 40 wt% to 90 wt% in the pores.

2. The method according to claim 1, characterized in that, The alkali-resistant inert porous substrate is PPS woven mesh, PPS nonwoven fabric, PTFE porous membrane, PEEK porous membrane, PVDF porous membrane or a composite porous substrate thereof.

3. The method according to claim 1, characterized in that, The eutectic solvent component is choline chloride-urea, choline chloride-ethylene glycol, or choline chloride-glycerol; the first cosolvent is N-methylpyrrolidone, N,N-dimethylacetamide, or dimethyl sulfoxide; the surface modification component is polyvinylpyrrolidone, polysulfone, polyethersulfone, dopamine, tannic acid, or polyethyleneimine.

4. The method according to claim 3, characterized in that, The mass ratio of the eutectic solvent component to the first cosolvent is 1:2 to 1:6, and the mass fraction of the surface modification component in the eutectic solvent-compatible cosolvent interface modification solution is 0.05 wt% to 5 wt%; the molar ratio of choline chloride to urea, ethylene glycol or glycerol in the eutectic solvent component is 1:1 to 1:

3.

5. The method according to claim 1, characterized in that, The eutectic solvent-compatible cosolvent interface modification solution does not undergo macroscopic stratification or gelation after standing at 25 °C for 24 h, and its viscosity is 5 mPa·s to 500 mPa·s at the treatment temperature; the eutectic solvent-compatible cosolvent interface modification solution is a single-phase or macroscopically stratified system at 20 °C to 100 °C.

6. The method according to claim 1 or 3, characterized in that, The eutectic solvent component is choline chloride-urea, the first cosolvent is N-methylpyrrolidone, and the surface modification component is polyvinylpyrrolidone; or, the eutectic solvent component is choline chloride-glycerol, the first cosolvent is N,N-dimethylacetamide, and the surface modification component is polysulfone or polyethersulfone.

7. The method according to claim 1, characterized in that, Step (3) is carried out by dip coating, spray coating, roller coating, scraping coating, vacuum-assisted impregnation, pressure-assisted impregnation, circulating injection or filtration penetration; Step (4) is carried out by scraping liquid, roller pressing and squeezing liquid, air knife blowing, centrifugal liquid removal, negative pressure suction, filtration and drainage, quantitative roller control liquid or a combination thereof.

8. The method according to claim 1, characterized in that, In step (5), the temperature for the shaping treatment is 40 ℃ to 120 ℃, and the treatment time is 10 min to 6 h. Preferably, after the interface modification treatment, the mass increase of the interface modification layer relative to the alkali-resistant inert porous substrate is 0.10 wt% to 3 wt%, the pore blockage area ratio is not higher than 5%, and the liquid permeability retention rate is not lower than 80% of that before the treatment.

9. An interface-modified porous substrate, characterized in that, The interface-modified porous substrate is prepared by the method according to any one of claims 1 to 8, and includes an alkali-resistant inert porous substrate and a non-blocking interface modification layer located on the inner wall of the pores, the edge of the pores and / or the fiber crossing area within the pores.

10. A composite diaphragm, characterized in that, It includes the interface-modified porous substrate as described in claim 9 and a functional composite layer compounded with the interface-modified porous substrate, wherein the functional composite layer at least partially enters the communicating channels and contacts, entangles, combines with, or interpenetrates the non-blocking interface modification layer.