A method for modifying the pore wall interface by antisolvent and a composite membrane
By using an antisolvent-induced pore wall interface modification method, the problems of insufficient wetting of composite membranes in the pores and discontinuous slurry penetration were solved, achieving efficient interface bonding and stability, and meeting the requirements of high current density, low energy consumption and long life of alkaline water electrolysis devices.
Patent Information
- Application Number
- CN202610952427.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-29
- Publication Date
- 2026-11-17
Smart Images

Figure CN123108941A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of porous substrate interface modification, functional composite membranes and alkaline water electrolysis membrane materials, specifically relating to an antisolvent-induced pore wall interface modification method and a composite membrane. Background Technology
[0002] Alkaline water electrolysis hydrogen production devices typically require the use of diaphragm materials to separate the gases on the cathode and anode sides while allowing ion conduction in the electrolyte. As alkaline electrolyzers develop towards higher current density, lower energy consumption, larger size, and longer lifespan, composite diaphragms need to simultaneously possess low sheet resistance, high bubble point pressure, good alkali resistance, and stable interfacial bonding capabilities.
[0003] Existing composite membranes typically use alkali-resistant, inert porous substrates such as polyphenylene sulfide, polyetheretherketone, polytetrafluoroethylene, and polyvinylidene fluoride as a support layer, and coat, impregnate, infuse, or composite a functional slurry containing organic solvents onto the surface and / or channels of the porous substrate. The functional slurry typically contains inorganic particles, polymer binders, dispersants, and organic solvents, such as N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, or dimethyl sulfoxide as the dispersion or dissolution medium.
[0004] However, alkali-resistant, inert porous substrates such as polyphenylene sulfide, polytetrafluoroethylene, and polyetheretherketone typically have low surface energy and few polar interaction sites, making it difficult for functional slurries containing organic solvents to quickly and uniformly wet the inner walls of their pores. When the slurry does not penetrate sufficiently into the pores, problems such as uneven pore filling, interfacial voids, localized debonding, discontinuous distribution of inorganic particles, and unstable bonding between the composite layer and the substrate can easily occur, thus affecting the bubble point pressure, gas barrier properties, interfacial durability, and long-term operational stability of the composite membrane.
[0005] In existing technologies, methods such as plasma treatment, oxidation treatment, coupling agent treatment, hydrophilic polymer coating, or simple immersion treatment are commonly used to improve the compatibility between porous substrates and functional slurries. However, these methods primarily affect the outer surface of the porous substrate, limiting the depth, uniformity, and stability of modification on the inner walls of the deep pores. This makes it particularly difficult to meet the requirements for rapid wetting, stable penetration, and interfacial bonding within the pores during the continuous fabrication of large-area roll-to-roll composite membranes.
[0006] In addition, conventional coating-type interface modification methods also have the problem of difficulty in balancing thickness. When the modification layer is thin, the inner wall of the pores is not sufficiently modified, and subsequent slurry still has difficulty entering the pores continuously; when the modification layer is thick, a blocking layer is easily formed at the pore opening or in the pores, which affects the entry of subsequent functional slurry into the pores and reduces the effective open porosity of the porous substrate.
[0007] Therefore, there is a need for an interface modification method that enables interface modification components to enter the pores of a porous substrate and be stably fixed at the inner wall of the pores, while avoiding pore blockage. Summary of the Invention
[0008] Furthermore, the present invention does not form an integral continuous film on the outer surface of the porous substrate by means of the interface modification component, but rather, after liquid control treatment, the interface modification component is confined and fixed to the inner wall of the pores, the edge of the pores and / or the fiber crossing area within the pores by antisolvent induction, thereby distinguishing it from ordinary antisolvent film formation and integral phase inversion treatment.
[0009] The purpose of this invention is to provide an antisolvent-induced pore wall interface modification method to solve the problems of insufficient wetting inside the pores, discontinuous slurry penetration, interface voids, local debonding, and the formation of a continuous filling layer at the pore openings by ordinary antisolvent precipitation or overall phase transformation treatment in porous substrates during subsequent organic solvent slurry composite processes.
[0010] To achieve the above objectives, the present invention provides an antisolvent-induced pore wall interface modification method, comprising the following steps:
[0011] Step 1: Provide a porous substrate with communicating channels, wherein the communicating channels have an opening, an outer surface, and an inner wall of the pores; Step 2: Prepare an organic solvent modification solution, wherein the organic solvent modification solution includes an organic solvent and an interface modification component; Step 3: Introduce the organic solvent modification liquid into the interconnecting channels of the porous substrate, so that the organic solvent modification liquid contacts the inner wall of the pores, the edge of the channels and / or the fiber crossing area inside the pores; Step 4: Perform liquid control treatment on the porous substrate after treatment with the organic solvent modification liquid to remove excess organic solvent modification liquid from the outer surface, pore opening and / or outside of the pore channel of the porous substrate, so that the thickness of the residual organic solvent modification liquid film on the outer surface is not higher than 10 μm, and the area of the continuous organic solvent modification liquid film on the outer surface accounts for less than 10% of the observation area of the outer surface. Step 5: The porous substrate after liquid control treatment is brought into contact with the antisolvent, so that the interface modification component is deposited, precipitated, entangled or fixed in the inner wall of the pores, the edge of the pores and / or the fiber crossing area inside the pores, and forms an interface modification layer on the inner wall of the pores. Step six: The porous substrate with the pore inner wall interface modification layer is washed, solvent replaced, dried and / or heat-treated to obtain an anti-solvent-induced interface-modified porous substrate.
[0012] In a preferred embodiment, the mass increase of the pore inner wall interface modification layer is 0.05 wt% to 5 wt% of the porous substrate mass, the pore blockage area ratio is not higher than 10%, the liquid permeability retention rate is not lower than 70% of that before treatment, and the porosity retention rate is not lower than 80% of that before treatment.
[0013] In a preferred embodiment, the porous substrate is an alkali-resistant inert porous substrate, selected from polyphenylene sulfide woven mesh, polyphenylene sulfide nonwoven fabric, polytetrafluoroethylene porous membrane, polyether ether ketone porous membrane, polyvinylidene fluoride porous membrane or composite porous substrate thereof.
[0014] In a preferred embodiment, the organic solvent is selected from N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, or a mixture thereof; the interface modification component is selected from polyvinylpyrrolidone, polysulfone, polyethersulfone, polyvinylidene fluoride, polyacrylic acid, polyvinyl alcohol, dopamine, polyethyleneimine, or a combination thereof.
[0015] In a preferred embodiment, the mass fraction of the interface modification component in the organic solvent modification liquid is from 0.05 wt% to 5 wt%, and the viscosity of the organic solvent modification liquid at 25 °C is from 1 mPa·s to 1000 mPa·s.
[0016] In a preferred embodiment, the organic solvent modification liquid in step three is introduced into the interconnecting channels of the porous substrate by dip coating, spraying, roller coating, scraping, vacuum-assisted wetting, pressure-assisted wetting, circulating injection, ultrasonic-assisted wetting, or a combination thereof. And / or, the liquid control process described in step four includes methods such as scraping, roller pressing and squeezing, air knife blowing, centrifugal slinging, negative pressure suction, filtration and drainage, quantitative roller control, contact of liquid-absorbing materials, or combinations thereof.
[0017] In a preferred embodiment, after the liquid control treatment in step four, the thickness of the residual organic solvent modification liquid film on the outer surface of the porous substrate is not higher than 5 μm, and / or the area of the continuous organic solvent modification liquid film on the outer surface accounts for less than 5% of the observation area of the outer surface.
[0018] In a preferred embodiment, the antisolvent is selected from water, ethanol, isopropanol, acetone, water / ethanol mixture, water / isopropanol mixture, water / acetone mixture, alkaline aqueous solution, salt aqueous solution, or a combination thereof. The antisolvent contact method is single-sided contact, double-sided contact, immersion contact, spray contact, or gradient displacement. The antisolvent contact time is 5 s to 30 min.
[0019] In a preferred embodiment, the pore inner wall interface modification layer in step five is a thin layer, a semi-continuous layer, an island layer, a dotted layer, a mesh layer, or a discontinuous interface layer, and does not constitute a continuous filling layer that fills the pores; and / or, the thickness of the pore inner wall interface modification layer is 5 nm to 1 μm, and the pore inner wall interface modification layer accounts for 2% to 15% of the pore volume of the porous substrate.
[0020] In a preferred embodiment, the contact angle of the porous substrate with the corresponding organic solvent or the functional slurry containing the organic solvent after treatment is less than 40°; and / or, after the anti-solvent-induced interface-modified porous substrate is combined with the functional slurry containing the organic solvent, the resulting composite membrane has a higher peel strength and a higher bubble point pressure than the composite membrane obtained from the untreated porous substrate.
[0021] The present invention also provides an antisolvent-induced interface-modified porous substrate, comprising a porous substrate and an inner pore wall interface modification layer located on the inner wall of the pores of the porous substrate, wherein the inner pore wall interface modification layer is fixedly formed by the above-mentioned confined antisolvent-induced process; the inner pore wall interface modification layer is a thin layer, a semi-continuous layer, an island layer, a dot layer, a network layer or a discontinuous interface layer, and does not constitute a continuous filling layer that fills the pores.
[0022] The present invention also provides a composite membrane comprising the antisolvent-induced interface-modified porous substrate and a functional composite layer thereof; the functional composite layer is formed of a functional slurry containing organic solvents, the functional slurry containing organic solvents comprising inorganic particles, polymer binders, dispersants and organic solvents, and at least partially entering the pores of the antisolvent-induced interface-modified porous substrate and forming a continuous intrapore bond structure with the interface modification layer of the pore wall.
[0023] Compared with the prior art, the present invention has at least the following beneficial effects: First, by allowing the organic solvent-modified liquid to enter the pores and contact the inner wall of the pores, the interface modification components have a basis for distribution within the pores; Second, by limiting the residual liquid film on the outer surface and at the pore opening through liquid control treatment, the risk of accumulation on the outer surface and blockage at the pore opening during the anti-solvent induction process is reduced; Third, by inducing confined deposition, precipitation, entanglement, or fixation through anti-solvent induction, the interface modification components are preferentially fixed to the inner wall of the pores without filling the pores; Fourth, the resulting anti-solvent-induced interface-modified porous substrate can improve the wetting, penetration, and interfacial bonding stability of subsequent organic solvent-containing functional slurries within the pores. Attached Figure Description
[0024] Figure 1 This is a schematic flowchart of the antisolvent-induced pore inner wall interface modification method of the present invention; Figure 2 This is a schematic diagram of the structure of the pore inner wall interface modification layer formed on the pore inner wall of a porous substrate according to the present invention; Figure 3 This is a comparative schematic diagram of the pore inner wall interface modification layer described in this invention and a conventional surface thick coating; Figure 4 This is a schematic diagram comparing the penetration of subsequent functional slurries and the continuity within the pores of an untreated porous substrate and a porous substrate modified by antisolvent-induced interface modification. Figure 5 This is a schematic diagram of the structure of the composite diaphragm described in this invention.
[0025] Figure reference numerals: 1-Porous substrate; 2-Pore channel; 3-Pore inner wall; 4-Organic solvent modification liquid; 5-Interface modification component; 6-Antisolvent; 7-Pore inner wall interface modification layer (7a-Thin layer, 7b-Semi-continuous layer, 7c-Island layer, 7d-Dot layer, 7e-Network layer); 8-Antisolvent-induced interface modification porous substrate; 9-Slurry containing organic solvent; 10-Inorganic particles; 11-Polymer binder; 12-Functional composite layer; 13-Pore clogging layer; 14-Interface voids; 15-Continuous bonding structure within the pores. Detailed Implementation
[0026] Embodiments of the present invention are described in detail below, examples of which are illustrated in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.
[0027] like Figure 1 As shown, the method of the present invention includes: providing a porous substrate 1; preparing an organic solvent modification liquid 4 containing an interface modification component 5; introducing the organic solvent modification liquid 4 into the pores 2 of the porous substrate 1; subjecting the porous substrate 1 treated with the organic solvent modification liquid 4 to a controlled liquid treatment, such that the thickness of the residual organic solvent modification liquid 4 liquid film on the outer surface is not higher than 10 μm and the area of the continuous liquid film on the outer surface accounts for less than 10% of the observed area of the outer surface; contacting the porous substrate 1 after the controlled liquid treatment with an antisolvent 6, so that the interface modification component 5 is fixed on the inner wall 3 of the pores; and obtaining an antisolvent-induced interface-modified porous substrate 8 after washing, solvent replacement, drying and / or heat treatment.
[0028] like Figure 2 As shown, the pore inner wall interface modification layer 7 is located on the pore inner wall 3 of the porous substrate 1, and can be in the form of a thin layer 7a, a semi-continuous layer 7b, an island layer 7c, a dot layer 7d, or a mesh layer 7e. The pore inner wall interface modification layer 7 does not form a continuous filling layer that blocks the pores 2, thus keeping the pores 2 of the porous substrate 1 open.
[0029] like Figure 3As shown, the pore inner wall interface modification layer 7 of the present invention differs from ordinary surface thick coatings. Ordinary surface thick coatings tend to accumulate on the outer surface or at the pore openings of the porous substrate 1, producing a pore opening blockage layer 13 (as shown on the left side of the figure), causing pore opening blockage or reducing the ability of subsequent slurry to enter the pore channel 2; while the present invention (as shown on the right side of the figure) uses an organic solvent modification liquid 4 to enter the pore channel 2, liquid control treatment, and anti-solvent 6 to induce fixation, so that the interface modification component 5 mainly forms a pore inner wall interface modification layer 7 on the pore inner wall 3, which can be a thin layer 7a, a semi-continuous layer 7b, an island layer 7c, a dot layer 7d, or a network layer 7e, thereby taking into account both the pore interface modification and the pore channel connectivity (see the rightmost figure on the right).
[0030] like Figure 4 As shown, in the subsequent composite process of the untreated porous substrate 1 containing organic solvent functional slurry 9, interfacial voids 14 are easily formed on the outer surface or at the pore interface of the porous substrate 1, leading to insufficient slurry penetration (as shown in local areas A and B on the left), uneven filling of the pores (as shown in area C on the left), and interfacial bonding defects such as discontinuous particle distribution. However, in the porous substrate treated with anti-solvent-induced interface modification of the present invention (as shown in local areas A and B on the left), the interfacial voids 14 are easily formed on the outer surface or at the pore interface, leading to insufficient slurry penetration (as shown in local areas A and B on the left), uneven filling of the pores (as shown in area C on the left), and discontinuous particle distribution. Figure 4 As shown on the right, the organic solvent-containing slurry 9 can more fully wet and penetrate downwards along the interface modification layers 7 formed on the inner walls of the pores, such as the thin layer 7a, semi-continuous layer 7b, island layer 7c, dot layer 7d, or network layer 7e, thereby forming an excellent continuous bonding structure 15 within the pores 2 (as shown in region E on the right and the enlarged attached figure on the right). This structure significantly improves the continuity of the functional slurry within the pores and the interfacial bonding stability of the interconnected channels.
[0031] like Figure 5 As shown, the composite membrane of the present invention comprises an antisolvent-induced interface-modified porous substrate 8 and a functional composite layer 12. The functional composite layer 12 (containing inorganic particles 10 and / or polymer binder 11) at least partially enters the pores 2 of the porous substrate 8, and after passing through the substrate surface, forms a continuous intrapore bonding structure 15 with the pore inner wall interface modification layer 7. During the composite process, the inorganic particles 10 and / or polymer binder 11 in the functional composite layer 12 can achieve more thorough wetting and capillary penetration along the pre-modified pore inner wall interface modification layer 7. This allows the functional components to not only form a film on the surface, but also achieve more stable deposition, bridging, and anchoring along the longitudinal direction of the pores, thereby forming a longitudinally extending continuous intrapore bonding structure 15 inside the pores, significantly improving the interfacial bonding stability and overall structural continuity between the functional composite layer 12 and the antisolvent-induced interface-modified porous substrate 8.
[0032] The technical solution of the present invention will be described in detail below with reference to specific embodiments.
[0033] Example The following embodiments are all described according to steps one to six of claim 1. Unless otherwise specified, the organic solvent-containing functional slurry is a composite slurry containing inorganic particles, polymer binders, dispersants, and organic solvents, and the composite diaphragm is used as an alkaline water electrolysis diaphragm material; the liquid control treatment aims to ensure that the thickness of the residual organic solvent-modified liquid film on the outer surface is not higher than 10 μm and the area of the continuous liquid film on the outer surface accounts for less than 10% of the observed area of the outer surface.
[0034] Example 1: PPS / NMP / PVP-water / ethanol antisolvent system Step 1: Provide a porous substrate. Using polyphenylene sulfide (PPS) nonwoven fabric as the porous substrate, it is washed sequentially with ethanol and deionized water to remove surface impurities and soluble residues, and then dried at 60 °C for 2 h for later use.
[0035] Step 2: Prepare the organic solvent modification solution. Prepare an N-methylpyrrolidone (NMP) modification solution, wherein the organic solvent modification solution comprises N-methylpyrrolidone and polyvinylpyrrolidone (PVP); the polyvinylpyrrolidone is used as an interface modification component, and its mass fraction is 0.1 wt% to 5.0 wt%; the organic solvent modification solution has a viscosity of 120 mPa·s at 25 °C.
[0036] Step 3: Introduce the organic solvent modification solution into the pores of the porous substrate. Immerse the polyphenylene sulfide nonwoven fabric obtained in Step 1 into the NMP / PVP modification solution prepared in Step 2, and perform vacuum-assisted wetting for 10 to 30 minutes to allow the organic solvent modification solution to enter the pores of the polyphenylene sulfide nonwoven fabric and contact the inner wall of the pores.
[0037] Step four involves controlling the liquid flow of the porous substrate treated with the organic solvent modification solution. The polyphenylene sulfide (PPS) nonwoven fabric treated with the organic solvent modification solution is removed and subjected to liquid control treatment via roller pressing and air knife blowing to remove free NMP / PVP modification solution from the outer surface and pores of the PPS nonwoven fabric. This ensures that a continuous film of modification solution does not form on the outer surface and pores of the PPS nonwoven fabric, and that the thickness of the residual organic solvent modification solution film on the outer surface is no more than 10 μm, with the area of the continuous organic solvent modification solution film on the outer surface accounting for less than 10% of the observed area of the outer surface.
[0038] Step 5: Contact the porous substrate after liquid control treatment with the antisolvent to fix the interface modification component onto the inner pore walls of the porous substrate. Transfer the polyphenylene sulfide nonwoven fabric after liquid control treatment to a water / ethanol mixed antisolvent, wherein the volume ratio of water to ethanol is 10:90 to 90:10, and treat for 1 min to 30 min. The antisolvent exchanges solvent with NMP, causing PVP to undergo antisolvent-induced deposition, aggregation, or fixation on the inner pore walls of the polyphenylene sulfide nonwoven fabric, thereby forming an interface modification layer on the inner pore walls.
[0039] Step six involves washing, solvent replacement, drying, and / or heat treatment of the treated porous substrate to obtain an antisolvent-induced interface-modified porous substrate. The polyphenylene sulfide nonwoven fabric treated in step five is then washed sequentially with deionized water and ethanol to remove free modifying components and residual solvent, followed by drying at 60°C to 80°C to obtain the antisolvent-induced interface-modified polyphenylene sulfide nonwoven fabric.
[0040] The obtained antisolvent-induced interface-modified polyphenylene sulfide (PPS) nonwoven fabric was combined with a ZrO2 / polysulfone / NMP functional slurry to prepare a composite membrane. Cross-sectional observation showed that the mass increase of the interface modification layer on the inner wall of the pores was 0.05 wt% of the porous substrate mass, the pore blockage area ratio was less than 10%, the liquid permeability retention rate was not less than 90% of that before treatment, and the porosity retention rate was not less than 93% of that before treatment. The thickness of the interface modification layer on the inner wall of the pores was 20 nm, and the interface modification layer on the inner wall of the pores accounted for 20% of the pore volume of the porous substrate. The results showed that the NMP contact angle of the PPS nonwoven fabric was about 68° before treatment, which was reduced to about 24° after treatment in this example; the complete wetting time of the ZrO2 / polysulfone / NMP slurry was shortened from more than 90 s to about 10 s; the peel strength of the composite membrane increased from about 0.18 N / cm in the untreated sample to about 0.60 N / cm, and the bubble point pressure increased from about 0.31 MPa to about 0.51 MPa. Image analysis shows that the porosity retention rate of the treated polyphenylene sulfide nonwoven fabric is higher than 80%, and the average thickness of the interface modification layer on the inner wall of the pores is less than 10% of the average pore diameter.
[0041] Example 2: PPS / DMAc / polysulfone-ethanol antisolvent system Step 1: Provide a porous substrate. A polyphenylene sulfide (PPS) woven mesh is used as the porous substrate. It is cleaned with ethanol and deionized water, then dried for later use.
[0042] Step 2: Prepare the organic solvent modification solution. Prepare an N,N-dimethylacetamide (DMAc) modification solution, wherein the organic solvent modification solution comprises N,N-dimethylacetamide and polysulfone. The polysulfone serves as the interface modification component, with a mass fraction of 0.1 wt% to 3.0 wt%; the organic solvent modification solution has a viscosity of 120 mPa·s at 25 °C.
[0043] Step 3: Introduce the organic solvent modification solution into the pores of the porous substrate. Immerse the polyphenylene sulfide (PPS) woven mesh in the DMAc / polysulfone modification solution, and use pressure-assisted wetting or cyclic wetting methods to allow the organic solvent modification solution to enter the pores of the PPS woven mesh and contact the inner walls of the pores.
[0044] Step four: Perform liquid control treatment on the porous substrate treated with the organic solvent modification solution. Remove the polyphenylene sulfide woven mesh treated with the modification solution, and use a scraping and metering roller to remove free DMAc / polysulfone modification solution from the outer surface and orifices. This ensures that no continuous covering liquid film forms at the orifices, and that the thickness of the residual organic solvent modification solution film on the outer surface does not exceed 10 μm, with the area of the continuous organic solvent modification solution film on the outer surface accounting for less than 10% of the observed area.
[0045] Step 5: Contact the porous substrate after liquid control treatment with the antisolvent to fix the interface modification component on the inner wall of the pores of the porous substrate. Place the polyphenylene sulfide woven web after liquid control treatment in ethanol antisolvent for 10 minutes to allow DMAc to exchange solvent with ethanol, and cause non-solvent-induced phase separation and deposition of polysulfone at the inner wall of the polyphenylene sulfide pores, forming a thin layer, island layer, or semi-continuous pore inner wall interface modification layer.
[0046] Step six involves washing, solvent replacement, drying, and / or heat treatment of the treated porous substrate to obtain an antisolvent-induced interface-modified porous substrate. The polyphenylene sulfide (PPS) woven mesh treated in step five is then washed with ethanol and dried to obtain an PPS woven mesh with antisolvent-induced interface modification.
[0047] The modified woven web was then composited with a ZrO2 / polysulfone / NMP functional slurry. Cross-sectional observation showed that the mass increase of the pore inner wall interface modification layer was 2.5 wt% of the porous substrate mass, the pore blockage area ratio was less than 5%, the liquid flux retention rate was not less than 80% of that before treatment, and the porosity retention rate was not less than 93% of that before treatment. The thickness of the pore inner wall interface modification layer was 520 nm, and the pore inner wall interface modification layer accounted for 5% of the pore volume of the porous substrate. The results showed that the DMAc contact angle of the polyphenylene sulfide woven web decreased to approximately 21° after treatment; the peel strength of the composite membrane was approximately 0.66 N / cm, and the bubble point pressure was approximately 0.54 MPa.
[0048] Example 3: PTFE / DMF / dopamine-water antisolvent system Step 1: Provide a porous substrate. A polytetrafluoroethylene (PTFE) porous membrane is used as the porous substrate, and is prepared for use after being cleaned with ethanol and dried.
[0049] Step 2: Prepare the organic solvent modification solution. Prepare an N,N-dimethylformamide (DMF) modification solution, wherein the organic solvent modification solution comprises N,N-dimethylformamide and dopamine or dopamine hydrochloride. The dopamine or dopamine hydrochloride serves as the interface modification component, with a concentration of 0.1 wt% to 1 wt%; the organic solvent modification solution has a viscosity of 10 mPa·s at 25 °C.
[0050] Step 3: Introduce the organic solvent modification solution into the pores of the porous substrate. Immerse the polytetrafluoroethylene porous membrane in the DMF / dopamine modification solution and use ultrasonic-assisted wetting for 5 to 20 minutes to allow the organic solvent modification solution to enter the pores of the polytetrafluoroethylene porous membrane.
[0051] Step four involves controlling the liquid level of the porous substrate treated with the organic solvent modification solution. The polytetrafluoroethylene porous membrane treated with the modification solution is removed, and liquid level is controlled by negative pressure suction or filtration to reduce free DMF / dopamine modification solution on the outer surface and at the pores. The thickness of the residual organic solvent modification solution film on the outer surface should not exceed 10 μm, and the area of the continuous organic solvent modification solution film on the outer surface should be less than 10% of the observed area.
[0052] Step 5: Contact the porous substrate after controlled liquid treatment with the antisolvent to fix the interface modification component onto the inner pore wall of the porous substrate. Transfer the polytetrafluoroethylene porous membrane after controlled liquid treatment to an aqueous antisolvent for 15 min, allowing solvent exchange between DMF and water, and causing the dopamine component to undergo antisolvent-induced deposition, aggregation, and subsequent oxidative self-polymerization at the inner pore wall of the polytetrafluoroethylene, forming an interface modification layer containing catechol groups on the inner pore wall.
[0053] Step six involves washing, solvent replacement, drying, and / or heat treatment of the treated porous substrate to obtain an antisolvent-induced interface-modified porous substrate. The polytetrafluoroethylene porous membrane obtained in step five is then washed and dried to obtain an antisolvent-induced interface-modified polytetrafluoroethylene porous membrane.
[0054] Cross-sectional observation showed that the mass increase of the pore inner wall interface modification layer was 5 wt% of the porous substrate mass, the pore blockage area ratio was less than 8%, the liquid permeability retention rate was not less than 90% of that before treatment, and the porosity retention rate was not less than 97% of that before treatment. The thickness of the pore inner wall interface modification layer was 1000 nm, and the pore inner wall interface modification layer accounted for 150% of the pore volume of the porous substrate. The results showed that the DMF contact angle of the original polytetrafluoroethylene porous membrane was about 92°, which was reduced to about 39° after treatment in this embodiment; after composite with an organic solvent functional slurry containing inorganic particles, the peel strength increased from about 0.08 N / cm in the untreated sample to about 0.44 N / cm.
[0055] Example 4: PVDF / NMP / PAA-PVP-water / isopropanol antisolvent system Step 1: Provide a porous substrate. A polyvinylidene fluoride (PVDF) porous membrane is used as the porous substrate, cleaned with ethanol and deionized water, and then dried for later use.
[0056] Step 2: Prepare the organic solvent modification solution. The organic solvent modification solution comprises NMP, polyacrylic acid (PAA), and polyvinylpyrrolidone (PVP), with a total mass fraction of 0.1 wt% to 5.0 wt%; the organic solvent modification solution has a viscosity of 170 mPa·s at 25 °C.
[0057] Step 3: Introduce the organic solvent modification solution into the pores of the porous substrate. Use vacuum-assisted wetting for 10 to 30 minutes to allow the organic solvent modification solution to enter the pores of the porous substrate and contact the inner wall of the pores.
[0058] Step four involves controlling the liquid content of the porous substrate treated with the organic solvent modification solution. Free modification solution is removed from the outer surface and pore openings using air knife purging and negative pressure suction, ensuring that a continuous film of modification solution does not form at the pore openings, and that the thickness of the residual organic solvent modification solution film on the outer surface does not exceed 10 μm, with the area of the continuous organic solvent modification solution film on the outer surface accounting for less than 10% of the observed area.
[0059] Step 5: Contact the porous substrate after liquid control treatment with the antisolvent to fix the interface modification component onto the inner wall of the pores of the porous substrate. Then, contact the porous substrate after liquid control treatment with a water / isopropanol mixed antisolvent to induce the interface modification component to be fixed at the inner wall of the pores, forming an interface modification layer on the inner wall of the pores.
[0060] Step six involves washing, solvent replacement, drying, and / or heat treatment of the treated porous substrate to obtain an antisolvent-induced interface-modified porous substrate. The porous substrate treated in step five is then washed and dried to obtain the antisolvent-induced interface-modified porous substrate.
[0061] Cross-sectional observation showed that the mass increase of the pore inner wall interface modification layer was 5 wt% of the porous substrate mass, the pore blockage area ratio was less than 6%, the liquid flux retention rate was not less than 90% of that before treatment, and the porosity retention rate was not less than 77% of that before treatment. The thickness of the pore inner wall interface modification layer was 280 nm, and the pore inner wall interface modification layer accounted for 7% of the pore volume of the porous substrate. The results showed that the bubble point pressure increased from about 0.30 MPa in the untreated sample to about 0.48 MPa, and the defects inside the pores were reduced.
[0062] Example 5: PPS multi-stage antisolvent gradient fixation system Step 1: Provide a porous substrate. Polyphenylene sulfide nonwoven fabric is used as the porous substrate, cleaned with ethanol and deionized water, and then dried for later use.
[0063] Step 2: Prepare the organic solvent modification solution. The organic solvent modification solution includes NMP and PVP, with the PVP mass fraction ranging from 0.1 wt% to 5.0 wt%; the viscosity of the organic solvent modification solution at 25 °C is 900 mPa·s.
[0064] Step 3: Introduce the organic solvent modification solution into the pores of the porous substrate. A vacuum-assisted wetting method is used to allow the organic solvent modification solution to enter the pores of the porous substrate and contact the inner walls of the pores.
[0065] Step four: Perform liquid control treatment on the porous substrate treated with the organic solvent modification liquid. Use a roller pressing method to remove free modification liquid from the outer surface and orifices, so that no continuous covering modification liquid film forms at the orifices, and the thickness of the residual organic solvent modification liquid film on the outer surface is no more than 10 μm, and the area of the continuous organic solvent modification liquid film on the outer surface accounts for less than 10% of the observed area of the outer surface.
[0066] Step 5: Contact the porous substrate after controlled liquid treatment with the antisolvent to fix the interface modification component onto the inner pore wall of the porous substrate. The porous substrate after controlled liquid treatment is sequentially subjected to a mixture of NMP / ethanol at a volume ratio of 70 / 30, a mixture of NMP / ethanol at a volume ratio of 30 / 70, and an ethanol and water system, with each treatment lasting 1 to 10 minutes. This allows the interface modification component to be antisolvent-induced and fixed at the inner pore wall, forming an interface modification layer on the inner pore wall.
[0067] Step six involves washing, solvent replacement, drying, and / or heat treatment of the treated porous substrate to obtain an antisolvent-induced interface-modified porous substrate. The porous substrate treated in step five is then washed and dried to obtain the antisolvent-induced interface-modified porous substrate.
[0068] Cross-sectional observation showed that the mass increase of the pore inner wall interface modification layer was 0.5 wt% of the porous substrate mass, the pore blockage area ratio was less than 9%, the liquid permeability retention rate was not less than 90% of that before treatment, and the porosity retention rate was not less than 87% of that before treatment. The thickness of the pore inner wall interface modification layer was 80 nm, and the pore inner wall interface modification layer accounted for 2% of the pore volume of the porous substrate. The results showed that compared with a one-time water antisolvent treatment, pore blockage was reduced, pore wall modification was more uniform, and the peel strength of the composite membrane was approximately 0.69 N / cm.
[0069] Example 6: PPS / NMP / PEI-KOH aqueous solution antisolvent system Step 1: Provide a porous substrate. Polyphenylene sulfide nonwoven fabric is used as the porous substrate, cleaned with ethanol and deionized water, and then dried for later use.
[0070] Step 2: Prepare the organic solvent modification solution. The organic solvent modification solution comprises NMP and polyethyleneimine (PEI), with a polyethyleneimine mass fraction of 0.05 wt% to 3.0 wt%; the viscosity of the organic solvent modification solution at 25°C is 360 mPa·s.
[0071] Step 3: Introduce the organic solvent modification solution into the pores of the porous substrate. A vacuum-assisted wetting method is used to allow the organic solvent modification solution to enter the pores of the porous substrate and contact the inner walls of the pores.
[0072] Step four involves controlling the liquid level in the porous substrate treated with the organic solvent modification solution. Free modification solution is removed from the outer surface and pore openings using air knife purging and filtration to prevent the formation of a continuous modification solution film at the pore openings. The thickness of the residual organic solvent modification solution film on the outer surface should not exceed 10 μm, and the area of the continuous organic solvent modification solution film on the outer surface should be less than 10% of the observed area.
[0073] Step 5: Contact the porous substrate after liquid control treatment with an antisolvent to fix the interface modification component onto the inner pore wall of the porous substrate. Contact the porous substrate after liquid control treatment with a 0.1 mol / L to 6.0 mol / L KOH aqueous solution to induce antisolvent fixation of the interface modification component at the inner pore wall, forming an interface modification layer on the inner pore wall.
[0074] Step six involves washing, solvent replacement, drying, and / or heat treatment of the treated porous substrate to obtain an antisolvent-induced interface-modified porous substrate. The porous substrate treated in step five is then washed and dried to obtain the antisolvent-induced interface-modified porous substrate.
[0075] The results showed that, upon cross-sectional observation, the mass increase of the pore inner wall interface modification layer was 1.5 wt% of the porous substrate mass, the pore blockage area ratio was less than 4%, the liquid flux retention rate was not less than 90% of that before treatment, and the porosity retention rate was not less than 83% of that before treatment. The thickness of the pore inner wall interface modification layer was 170 nm, and the pore inner wall interface modification layer accounted for 4% of the pore volume of the porous substrate. The NMP contact angle could be reduced to approximately 25° to 32°, the peel strength was approximately 0.55 N / cm to 0.64 N / cm, and the bubble point pressure was approximately 0.47 MPa to 0.53 MPa.
[0076] Example 7: PPS / DMSO / PVA-salt solution antisolvent system Step 1: Provide a porous substrate. A polyphenylene sulfide (PPS) woven mesh is used as the porous substrate, cleaned with ethanol and deionized water, and then dried for later use.
[0077] Step 2: Prepare the organic solvent modification solution. The organic solvent modification solution comprises dimethyl sulfoxide (DMSO) and polyvinyl alcohol (PVA), with a PVA mass fraction of 0.1 wt% to 5.0 wt%; the organic solvent modification solution has a viscosity of 450 mPa·s at 25 °C.
[0078] Step 3: Introduce the organic solvent modification solution into the pores of the porous substrate. A circulating injection method is used to allow the organic solvent modification solution to enter the pores of the porous substrate and contact the inner walls of the pores.
[0079] Step four involves controlling the liquid flow of the porous substrate treated with the organic solvent modification solution. Free modification solution is removed from the outer surface and orifices using roller pressing and air knife blowing methods, ensuring that a continuous film of modification solution does not form at the orifices, and that the thickness of the residual organic solvent modification solution film on the outer surface does not exceed 10 μm, with the area of the continuous organic solvent modification solution film on the outer surface accounting for less than 10% of the observed area.
[0080] Step 5: Contact the porous substrate after liquid control treatment with the antisolvent to fix the interface modification component onto the inner wall of the pores of the porous substrate. Contact the porous substrate after liquid control treatment with an aqueous solution of sodium sulfate, sodium chloride, potassium sulfate, or a mixture thereof for 14 minutes to induce antisolvent-induced fixation of the interface modification component at the inner wall of the pores, forming an interface modification layer on the inner wall of the pores.
[0081] Step six involves washing, solvent replacement, drying, and / or heat treatment of the treated porous substrate to obtain an antisolvent-induced interface-modified porous substrate. The porous substrate treated in step five is then washed and dried to obtain the antisolvent-induced interface-modified porous substrate.
[0082] The results showed that, upon cross-sectional observation, the mass increase of the pore inner wall interface modification layer was 2.2 wt% of the porous substrate mass, the pore blockage area ratio was less than 8%, the liquid flux retention rate was not less than 60% of that before treatment, and the porosity retention rate was not less than 96% of that before treatment. The thickness of the pore inner wall interface modification layer was 310 nm, and the pore inner wall interface modification layer accounted for 13% of the pore volume of the porous substrate. The slurry penetration time was shortened from more than 90 s to about 15 s to 25 s, the peel strength was about 0.48 N / cm to 0.58 N / cm, and the bubble point pressure was about 0.44 MPa to 0.50 MPa.
[0083] Example 8: PEEK / NMP / PES-water / acetone antisolvent system Step 1: Provide a porous substrate. A polyetheretherketone (PEEK) porous membrane is used as the porous substrate, cleaned with ethanol and deionized water, and then dried for later use.
[0084] Step 2: Prepare the organic solvent modification solution. The organic solvent modification solution comprises NMP and polyethersulfone (PES), with a polyethersulfone mass fraction of 0.1 wt% to 4.0 wt%; the organic solvent modification solution has a viscosity of 450 mPa·s at 25 °C.
[0085] Step 3: Introduce the organic solvent modification solution into the pores of the porous substrate. Use pressure-assisted wetting for 10 to 30 minutes to allow the organic solvent modification solution to enter the pores of the porous substrate and contact the inner wall of the pores.
[0086] Step four involves controlling the liquid flow of the porous substrate treated with the organic solvent modification solution. Free modification solution is removed from the outer surface and orifices using negative pressure suction or a quantitative roller to prevent the formation of a continuous film of modification solution at the orifices. The thickness of the residual organic solvent modification solution film on the outer surface should not exceed 10 μm, and the area of the continuous organic solvent modification solution film on the outer surface should be less than 10% of the observed area.
[0087] Step 5: Contact the porous substrate after liquid control treatment with the antisolvent to fix the interface modification component onto the inner wall of the pores of the porous substrate. Contact the porous substrate after liquid control treatment with a water / acetone mixed antisolvent for 17 minutes to induce antisolvent fixation of the interface modification component at the inner wall of the pores, forming an interface modification layer on the inner wall of the pores.
[0088] Step six involves washing, solvent replacement, drying, and / or heat treatment of the treated porous substrate to obtain an antisolvent-induced interface-modified porous substrate. The porous substrate treated in step five is then washed and dried to obtain the antisolvent-induced interface-modified porous substrate.
[0089] Cross-sectional observation showed that the mass increase of the pore inner wall interface modification layer was 2.9 wt% of the porous substrate mass, the pore blockage area ratio was less than 10%, the liquid flux retention rate was not less than 70% of that before treatment, and the porosity retention rate was not less than 93% of that before treatment. The thickness of the pore inner wall interface modification layer was 320 nm, and the pore inner wall interface modification layer accounted for 10% of the pore volume of the porous substrate. The peel strength increased from about 0.12 N / cm to about 0.50 N / cm, and the bubble point pressure increased from about 0.28 MPa to about 0.46 MPa.
[0090] Example 9: PPS / NMP / PVP-PSF Composite Modified Component System Step 1: Provide a porous substrate. Polyphenylene sulfide (PPS) nonwoven fabric is used as the porous substrate, cleaned with ethanol and deionized water, and then dried for later use.
[0091] Step 2: Prepare the organic solvent modification solution. The organic solvent modification solution comprises NMP, polyvinylpyrrolidone (PVP), and polysulfone (PSF), wherein the mass fraction of PVP is 0.1 wt% to 3.0 wt%, and the mass fraction of PSF is 0.1 wt% to 3.0 wt%; the viscosity of the organic solvent modification solution at 25 °C is 150 mPa·s.
[0092] Step 3: Introduce the organic solvent modification solution into the pores of the porous substrate. A vacuum-assisted wetting method is used to allow the organic solvent modification solution to enter the pores of the porous substrate and contact the inner walls of the pores.
[0093] Step four involves controlling the liquid flow of the porous substrate treated with the organic solvent modification solution. Free modification solution is removed from the outer surface and orifices using roller pressing and air knife blowing methods, ensuring that a continuous film of modification solution does not form at the orifices, and that the thickness of the residual organic solvent modification solution film on the outer surface does not exceed 10 μm, with the area of the continuous organic solvent modification solution film on the outer surface accounting for less than 10% of the observed area.
[0094] Step 5: Contact the porous substrate after liquid control treatment with the antisolvent to fix the interface modification component onto the inner wall of the pores of the porous substrate. Contact the porous substrate after liquid control treatment with a water / ethanol mixed antisolvent for 17 minutes to induce antisolvent-induced fixation of the interface modification component at the inner wall of the pores, forming an interface modification layer on the inner wall of the pores.
[0095] Step six involves washing, solvent replacement, drying, and / or heat treatment of the treated porous substrate to obtain an antisolvent-induced interface-modified porous substrate. The porous substrate treated in step five is then washed and dried to obtain the antisolvent-induced interface-modified porous substrate.
[0096] The results showed that, upon cross-sectional observation, the mass increase of the pore inner wall interface modification layer was 1.5 wt% of the porous substrate mass; the pore blockage area ratio was less than 3%; the liquid flux retention rate was not less than 90% of that before treatment; the porosity retention rate was not less than 83% of that before treatment; the thickness of the pore inner wall interface modification layer was 200 nm; and the pore inner wall interface modification layer accounted for 5% of the pore volume of the porous substrate. The NMP contact angle decreased to approximately 20° to 26°; the slurry complete wetting time was approximately 6 s to 12 s; the peel strength was approximately 0.65 N / cm to 0.72 N / cm; and the bubble point pressure was approximately 0.50 MPa to 0.56 MPa.
[0097] Example 10: Antisolvent-induced interface modification treatment for continuous roll materials Step 1: Provide a porous substrate. A continuous polyphenylene sulfide (PPS) nonwoven fabric roll is used as the porous substrate, which is cleaned with ethanol and deionized water and then dried for later use.
[0098] Step 2: Prepare the organic solvent modification solution. The organic solvent modification solution includes an NMP / PVP modification solution or an NMP / PVP-PSF composite modification solution.
[0099] Step 3: Introduce the organic solvent modification solution into the pores of the porous substrate. Use a continuous unwinding-rewinding method with a roll speed of 0.1 m / min to 5 m / min and a modification solution wetting time of 5 s to 120 s to allow the organic solvent modification solution to enter the pores of the porous substrate and contact the inner walls of the pores.
[0100] Step four involves controlling the liquid flow of the porous substrate treated with the organic solvent modification solution. Free modification solution on the outer surface and orifices is removed using methods such as scraping, metering roller control, roller pressing, and / or air knife blowing, ensuring that a continuous film of modification solution does not form at the orifices, and that the thickness of the residual organic solvent modification solution film on the outer surface does not exceed 10 μm, with the area of the continuous organic solvent modification solution film on the outer surface accounting for less than 10% of the observed area.
[0101] Step 5: Contact the porous substrate after liquid control treatment with an antisolvent to fix the interface modification component onto the inner wall of the pores of the porous substrate. The porous substrate after liquid control treatment is contacted with water, ethanol, a water / ethanol mixture, or a KOH aqueous solution for an antisolvent-induced treatment time of 5 to 180 seconds, causing the interface modification component to be fixed at the inner wall of the pores by antisolvent induction, forming an interface modification layer on the inner wall of the pores.
[0102] Step six involves washing, solvent replacement, drying, and / or heat treatment of the treated porous substrate to obtain an antisolvent-induced interface-modified porous substrate. The porous substrate treated in step five is then washed and dried to obtain the antisolvent-induced interface-modified porous substrate.
[0103] The results showed that, according to cross-sectional observation, the mass increase of the pore inner wall interface modification layer was 1.0 wt% of the porous substrate mass, the pore blockage area ratio was less than 4%, the liquid permeability retention rate was not less than 81% of that before treatment, the porosity retention rate was not less than 90% of that before treatment, the thickness of the pore inner wall interface modification layer was 500 nm, the pore inner wall interface modification layer accounted for 7% of the pore volume of the porous substrate, the NMP contact angle at different positions of the roll material was stable in the range of about 22° to 30°, the slurry complete wetting time was about 8 s to 15 s, the peel strength was about 0.55 N / cm to 0.68 N / cm, and the bubble point pressure was about 0.48 MPa to 0.55 MPa.
[0104] Comparative Example 1: PPS porous substrate without pore wall interface modification The same polyphenylene sulfide (PPS) nonwoven fabric as in Example 1 was provided, but without organic solvent modification, liquid control, or anti-solvent treatment, and was directly composited with a ZrO2 / polysulfone / NMP functional slurry. Results showed that the NMP contact angle of the untreated PPS nonwoven fabric was approximately 68°, and the complete wetting time of the ZrO2 / polysulfone / NMP slurry was greater than 90 s. The peel strength of the composite diaphragm was approximately 0.18 N / cm, and the bubble point pressure was approximately 0.31 MPa.
[0105] Comparative Example 2: Wetting with only organic solvent-modified solution without antisolvent contact. The polyphenylene sulfide nonwoven fabric was treated according to steps one through three of Example 1, but the antisolvent contact treatment in step five was omitted, and the sample was directly washed and dried. The results showed that some interface modification components were carried out during the subsequent washing process, the fixation effect on the inner wall of the pores was weak, and the increase in peel strength and bubble point pressure of the composite membrane was small.
[0106] Comparative Example 3: Direct contact with the antisolvent without liquid control treatment The polyphenylene sulfide nonwoven fabric was treated according to steps one through three of Example 1, but step four, the liquid control treatment, was omitted. The impregnated polyphenylene sulfide nonwoven fabric was directly transferred to a water / ethanol mixed antisolvent. The results showed that the uncontrolled liquid sample exhibited significant accumulation of interface modification components at the pore openings and outer surface, with some pore openings being blocked, resulting in poor uniformity of subsequent functional slurry entering the deep pores.
[0107] Comparative Example 4: Treatment with high-concentration organic solvent modification solution Polyphenylene sulfide nonwoven fabric was treated according to the method in Example 1, except that the mass fraction of PVP in the NMP / PVP modification solution was increased to over 10 wt%. The results showed that the high-concentration modification solution, after antisolvent treatment, easily formed a thicker deposition layer at the pore openings and on the outer surface, resulting in a significant decrease in the porosity retention rate and blockage of some pores.
[0108] Comparative Example 5: Conventional Surface Coating Type Interface Treatment PVP or polysulfone solution was directly coated onto the surface of polyphenylene sulfide (PPS) nonwoven fabric, and after drying, a surface-coated modified PPS nonwoven fabric was obtained, which was then compounded with a ZrO2 / polysulfone / NMP functional slurry. The results showed that ordinary surface coating mainly forms a coating on the outer surface of the PPS nonwoven fabric, with insufficient modification of the inner walls of deep pores; when the coating is thick, pore openings are prone to blockage.
[0109] The composite membranes prepared in Examples 1-10 and Comparative Examples 1-5 were tested, and the results are shown in Tables 1-4.
[0110] Test methods Contact angle test: At 25 ℃, 3 μL of the organic solvent to be tested or the functional slurry containing the organic solvent is dropped onto the surface of the porous substrate, and the droplet image is acquired within 10 seconds. At least 5 locations are tested for each sample and the average value is taken.
[0111] Slurry complete wetting time test: 20 μL of functional slurry containing organic solvent is dropped onto the surface of a horizontally placed porous substrate. The endpoint is reached when the slurry completely enters the pores within the observation area and there are no obvious residual droplets on the surface. The time required is recorded. Each sample is tested at least 5 times and the average value is taken.
[0112] Peel strength test: The prepared composite diaphragm is cut into strips of a specified width, and the peel strength between the functional composite layer and the porous substrate is tested by 180° peel or T-shaped peel.
[0113] Bubble point pressure test: The composite diaphragm is pre-wetted and fixed in the bubble point pressure test device. The gas pressure is gradually increased on both sides of the membrane, and the pressure at which continuous bubbles appear is taken as the bubble point pressure.
[0114] Pore inner wall interface modification layer thickness test: The thickness of the interface modification layer on the pore inner wall was measured using a scanning electron microscope. Measurements were taken at no fewer than 10 locations, and the average value was recorded as the average thickness of the interface modification layer on the pore inner wall.
[0115] External surface residual liquid film thickness test: After liquid control treatment, samples were taken from different areas of the porous substrate, and the thickness of the residual organic solvent modification liquid film on the external surface was measured by scanning electron microscopy. At least 5 locations were tested for each sample, and the average value was taken.
[0116] Test of the proportion of continuous liquid film area on the outer surface: The proportion of the area covered by the continuous organic solvent-modified liquid film on the outer surface after liquid control to the observed area was statistically analyzed using optical microscopy.
[0117] Test on the increase in mass of the interface modification layer: The dry weight of the porous substrate before and after treatment was measured under the same drying conditions. The increase in mass was calculated as (m1-m0) / m0×100%, where m0 is the dry weight before treatment and m1 is the dry weight after anti-solvent-induced interface modification and drying.
[0118] Table 1 Summary of Implementation Results
[0119] Table 2 Results of antisolvent-induced pore wall interface modification examples
[0120] Table 3. Performance comparison of antisolvent-induced treated and untreated substrates
[0121] Note: The above data are representative results from the examples and comparative examples in the specification, and are used to support the ability of confined antisolvent-induced fixation in the pores after liquid control to simultaneously improve wetting, interface bonding and pore connectivity.
[0122] Table 4 Comparative verification of key steps in the antisolvent-induced method
[0123] Note: The above data are representative results from the examples and comparative examples in the specification, and are used to support the ability of confined antisolvent-induced fixation in the pores after liquid control to simultaneously improve wetting, interface bonding and pore connectivity.
[0124] As can be seen from the above embodiments and comparative examples, the interface-modified porous substrate provided by the present invention can improve the wettability, pore permeability and interfacial bonding stability of subsequent functional slurries containing organic solvents, while reducing the risk of pore blockage through liquid control treatment, making it suitable for the preparation of alkaline electrolytic water composite membranes.
[0125] Those skilled in the art, after considering the disclosure in this specification, can make various modifications, uses, or adaptations to this invention without departing from the inventive concept. The specification and embodiments are merely illustrative, and the scope of protection of this invention is determined by the claims.
Claims
1. A method for modifying the interface of pore walls induced by antisolvents, characterized in that, Includes the following steps: Step 1: Provide a porous substrate with communicating channels, wherein the communicating channels have an opening, an outer surface, and an inner wall of the pores; Step 2: Prepare an organic solvent modification solution, wherein the organic solvent modification solution includes an organic solvent and an interface modification component; Step 3: Introduce the organic solvent modification liquid into the interconnecting channels of the porous substrate, so that the organic solvent modification liquid contacts the inner wall of the pores, the edge of the channels and / or the fiber crossing area inside the pores; Step 4: Perform liquid control treatment on the porous substrate after treatment with the organic solvent modification liquid to remove excess organic solvent modification liquid from the outer surface, pore opening and / or outside of the pore channel of the porous substrate, so that the thickness of the residual organic solvent modification liquid film on the outer surface is not higher than 10 μm, and the area of the continuous organic solvent modification liquid film on the outer surface accounts for less than 10% of the observation area of the outer surface. Step 5: The porous substrate after liquid control treatment is brought into contact with the antisolvent, so that the interface modification component is deposited, precipitated, entangled or fixed in the inner wall of the pores, the edge of the pores and / or the fiber crossing area inside the pores, and forms an interface modification layer on the inner wall of the pores. Step 6: Wash, solvent-displace, dry and / or heat-treat the porous substrate with the pore inner wall interface modification layer to obtain the anti-solvent-induced interface modified porous substrate. After treatment, the mass increase of the pore inner wall interface modification layer is 0.05 wt% to 5 wt% of the porous substrate mass, the pore blockage area ratio is not higher than 10%, the liquid permeability retention rate is not lower than 70% of that before treatment, and the porosity retention rate is not lower than 80% of that before treatment.
2. The method according to claim 1, characterized in that, The porous substrate is an alkali-resistant inert porous substrate, and the porous substrate is selected from polyphenylene sulfide woven mesh, polyphenylene sulfide nonwoven fabric, polytetrafluoroethylene porous membrane, polyether ether ketone porous membrane, polyvinylidene fluoride porous membrane or composite porous substrate.
3. The method according to claim 1, characterized in that, The organic solvent is selected from N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, or a mixture thereof; the interface modification component is selected from polyvinylpyrrolidone, polysulfone, polyethersulfone, polyvinylidene fluoride, polyacrylic acid, polyvinyl alcohol, dopamine, polyethyleneimine, or a combination thereof; the mass fraction of the interface modification component in the organic solvent-modified liquid is 0.05 wt% to 5 wt%, and the viscosity of the organic solvent-modified liquid at 25 °C is 1 mPa·s to 1000 mPa·s.
4. The method according to claim 1, characterized in that, The organic solvent modification solution described in step three is introduced into the interconnecting channels of the porous substrate through dip coating, spraying, roller coating, blade coating, vacuum-assisted wetting, pressure-assisted wetting, circulating injection, ultrasonic-assisted wetting, or a combination thereof. And / or, the liquid control process described in step four includes methods such as scraping, roller pressing and squeezing, air knife blowing, centrifugal slinging, negative pressure suction, filtration and drainage, quantitative roller control, contact of liquid-absorbing materials, or combinations thereof.
5. The method according to claim 1, characterized in that, After the liquid control treatment in step four, the thickness of the residual organic solvent modification liquid film on the outer surface of the porous substrate is no more than 5 μm. And / or, the area of the continuous organic solvent-modified liquid film on the outer surface accounts for less than 5% of the observation area of the outer surface.
6. The method according to claim 1, characterized in that, The antisolvent in step five is selected from water, ethanol, isopropanol, acetone, water / ethanol mixture, water / isopropanol mixture, water / acetone mixture, alkaline aqueous solution, salt aqueous solution, or a combination thereof. The antisolvent contact method is single-sided contact, double-sided contact, immersion contact, spray contact, or gradient displacement. The antisolvent contact time is 5 s to 30 min.
7. The method according to claim 1, characterized in that, The pore inner wall interface modification layer mentioned in step five is a thin layer, a semi-continuous layer, an island layer, a dotted layer, a network layer, or a discontinuous interface layer, and does not constitute a continuous filling layer that fills the pores. And / or, the thickness of the pore inner wall interface modification layer is 5 nm to 1 μm, and the pore inner wall interface modification layer accounts for 2% to 15% of the pore volume of the porous substrate.
8. The method according to claim 1, characterized in that, The contact angle of the porous substrate to the corresponding organic solvent or functional slurry containing organic solvent after treatment is less than 40°; and / or, after the anti-solvent-induced interface-modified porous substrate is combined with the functional slurry containing organic solvent, the resulting composite membrane has a higher peel strength and a higher bubble point pressure than the composite membrane obtained from the untreated porous substrate.
9. A solvent-induced interface-modified porous substrate, characterized in that, It includes a porous substrate and a pore inner wall interface modification layer located on the inner wall of the pores of the porous substrate; the pore inner wall interface modification layer is formed by fixing an interface modification component through a confined antisolvent-induced process in any one of claims 1 to 8.
10. A composite diaphragm, characterized in that, The invention includes the antisolvent-induced interface-modified porous substrate as described in claim 9 and a functional composite layer bonded to the antisolvent-induced interface-modified porous substrate; the functional composite layer is formed from a functional slurry containing organic solvents, the functional slurry containing organic solvents including inorganic particles, polymer binders, dispersants and organic solvents, and at least partially enters the pores of the antisolvent-induced interface-modified porous substrate and forms a continuous intrapore bond structure with the interface modification layer on the inner wall of the pores.