A photochromic environmental adaptive camouflage fabric and its preparation method

By employing surface activation/interface anchoring and partition threshold control technologies, the problem of unstable light response threshold of photochromic materials on flexible fabrics has been solved, achieving stable differentiation and improved durability, making it suitable for military camouflage and special protection applications.

CN123108943APending Publication Date: 2026-11-17杭州智元研究院有限公司 +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611051672.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-15
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

When existing photochromic materials are applied to flexible fabrics, it is difficult to stably distinguish the light response thresholds of different pattern areas. Insufficient response levels or visual crosstalk are likely to occur between areas. Furthermore, the functional layer is not well bonded to the fabric interface, making it easy to fall off or become blurred, which affects durability and softness.

Method used

By surface activation/interface anchoring treatment, combined with partition threshold control and a transparent protective layer, the adhesion and stability of photochromic microcapsules are improved. By using differences in the type, amount, and shell structure of photochromic microcapsules in different regions, a stable photoresponse threshold is formed, and different color changes are exhibited under external light.

Benefits of technology

It achieves stable differentiation of light response levels on flexible fabrics, enhances the realism and resolution of environmentally adaptive camouflage, strengthens pattern boundary stability and durability, and maintains fabric softness and breathability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108943A_ABST
    Figure CN123108943A_ABST
Patent Text Reader

Abstract

This invention discloses a photochromic environmentally adaptive camouflage fabric and its preparation method, addressing the problems of existing photochromic camouflage fabrics, such as difficulty in stably distinguishing response thresholds under multi-regional differential response conditions, insufficient adhesion between the microcapsule functional layer and the substrate fabric, and easy distortion of pattern boundaries after friction and washing. The method includes: performing surface activation treatment on the substrate fabric, or further forming an interface anchoring layer; preparing two or more photochromic finishing liquids based on photochromic microcapsules, film-forming binders, and threshold control components; applying them to different regions to form partitioned photoresponse camouflage layers with different light response thresholds; and forming a transparent protective layer on the surface after drying and curing, followed by secondary curing. Through the synergistic effect of interface activation, differential threshold control, and the protective layer, the fabric's softness, breathability, and sewingability can be maintained while improving the response resolution of different pattern areas, pattern boundary stability, and resistance to friction, washing, and weathering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of functional textile materials technology, specifically relating to a photochromic environmental adaptive camouflage fabric and its preparation method. Background Technology

[0002] In complex and ever-changing field environments, the ability to autonomously achieve visual concealment based on external lighting conditions is a core requirement in military camouflage and special protection. Intelligent color-changing camouflage fabrics capable of responding to external stimuli and autonomously altering their appearance have demonstrated significant application potential and practical value. CN103126149A prepares a color-changing fabric that changes color with temperature by coating thermochromic microcapsules onto the fiber surface, suitable for fashion apparel and military camouflage scenarios. CN120868831A uses a screen printing method to apply thermochromic microcapsule dyes to a base fabric and composites it with a far-infrared coating to obtain a bistable thermochromic camouflage fabric that switches colors with temperature. CN109267361A produces a multi-functional color-changing camouflage equipment coating fabric with flame-retardant and infrared reconnaissance protection functions by combining a fixed camouflage pattern with a multi-layer functional coating, suitable for individual soldier camouflage in various terrains.

[0003] Lightweight, flexible, and directly applicable smart camouflage fabrics for equipment and clothing are crucial carriers for next-generation environmentally adaptive camouflage systems. While photochromic materials and zoned pattern concepts have been reported, their application in flexible fabrics faces several technical bottlenecks: First, the light response thresholds of different pattern areas are difficult to distinguish stably, leading to insufficient response levels or visual crosstalk between regions, making it difficult to create dynamic textures that closely resemble natural shadow changes. Second, when photochromic microcapsules are directly applied to the fabric surface, they often lack sufficient bonding with the fiber interface, easily detaching, migrating, or blurring their boundaries after bending, friction, and washing. Third, simply increasing the coating thickness to improve durability can result in a stiff feel and reduced breathability. Therefore, the core technical problem this invention aims to solve is not merely "zoned color change," but rather, while maintaining fabric softness and processability, achieving stable construction of light response thresholds for different pattern areas, and improving the bonding strength between the functional layer and the fabric interface, as well as the stability of pattern boundaries during long-term use. Summary of the Invention

[0004] To address the aforementioned issues, this invention proposes a technical approach of "surface activation / interface anchoring—regional threshold control—transparent protective sealing": by surface activation of the substrate fabric or the application of an interface anchoring layer, the adhesion and fixation of the microcapsule-containing functional layer on the fiber surface are improved; by adjusting the type, amount, shell structure, and type or content of threshold control components of photochromic microcapsules in different regions, stably distinguishable regional photoresponse thresholds are established; and combined with the coverage and secondary curing of the transparent protective layer, the stability of pattern boundaries, abrasion resistance, washability, and outdoor service life are improved without significantly sacrificing softness and breathability.

[0005] A photochromic environmental adaptive camouflage fabric has a multi-layer composite structure, including a base fabric layer, a partitioned light-responsive camouflage layer disposed on the base fabric layer, and a transparent protective layer covering the outside of the partitioned light-responsive camouflage layer; if necessary, a base color layer and / or an interface anchoring layer may also be disposed between the base fabric layer and the partitioned light-responsive camouflage layer. Different patterned areas in the partitioned light-responsive camouflage layer contain photochromic microcapsules coated and fixed by a film-forming binder. At least two adjacent patterned areas differ in at least one of the following: photochromic microcapsule type, amount added, particle size, shell structure, and type or content of threshold-regulating components, thereby causing each patterned area to exhibit different activation thresholds, color-changing depths, or color responses under the same external light irradiation; the transparent protective layer covers the outside of the camouflage layer to inhibit microcapsule migration, improve pattern boundary stability, and enhance durability.

[0006] A method for preparing photochromic environmental adaptive camouflage fabric includes: (1) Preparation of the base fabric layer: After desizing, degreasing and cleaning the fabric, a surface activation treatment is performed to obtain a clean and highly active base fabric layer. The base fabric can be woven fabric, knitted fabric or nonwoven fabric, and the material is selected from one or more composites of polyester, nylon, cotton, spandex and aramid. The surface activation treatment is preferably one or more of low-temperature plasma activation, corona activation, alkali reduction activation, silane coupling activation and dopamine primer activation; preferably, the low-temperature plasma activation power is 100~400W and the time is 10~120s, and / or the treatment is carried out with 0.5~3wt% aminosilane or epoxysilane hydrolysate for 30~300s to form an active interface on the fiber surface that is conducive to the adhesion of the film-forming binder.

[0007] Alternatively, an interface anchoring layer may be further formed on the surface of the base fabric. This interface anchoring layer is an interface layer formed from one or more of aminosilane, epoxysilane, dopamine, or waterborne polyurethane primer, with a sizing amount of 0.5~10 g / m². 2 This is to further enhance the adhesion of subsequent functional layers.

[0008] (2) Preparation of photochromic finishing solution: Photochromic microcapsules, film-forming binder, dispersant, leveling agent, stabilizing agent, and threshold-regulating component are mixed evenly to obtain a stable photochromic finishing solution. The finishing solution preferably comprises, by total mass: 5-35 wt% photochromic microcapsules, 10-40 wt% film-forming binder, 0.2-5 wt% dispersant, 0.1-3 wt% leveling agent, 0.1-5 wt% stabilizing agent, 0.5-10 wt% threshold-regulating component, and the balance being water or a mixture of organic solvent and water. The film-forming binder is preferably one or more of waterborne polyurethane, polyurethane-acrylate composite emulsion, or acrylate emulsion; the dispersant is preferably one or more of polycarboxylate dispersant or polyurethane dispersant; the leveling agent is preferably one or more of polyether-modified siloxane leveling agent or acrylate leveling agent; and the stabilizing agent is preferably one or more of antioxidant, UV stabilizer, anti-settling agent, and pH adjuster. The threshold-regulating component is one or more of the following: ultraviolet absorber, ultraviolet scattering particles, transparent filler, and diluting resin. The photoresponse threshold of different regions is achieved by adjusting the type or content of the threshold-regulating component, the amount of photochromic microcapsules added, the shell thickness, and / or the weight gain of the single-region coating. The organic solvent is typically one or more of ethanol, isopropanol, ethylene glycol monobutyl ether, and propylene glycol methyl ether, preferably mixed with water to form a mixed solvent, thereby improving the dispersion stability and application compatibility of the photochromic microcapsules, film-forming binder, and threshold-regulating component in the finishing solution.

[0009] (3) Preparation of a partitioned photoresponsive camouflage layer: According to the preset camouflage pattern, photochromic finishing liquids with different response thresholds or different color-changing colors are applied to different areas of the fabric to form a partitioned photoresponsive camouflage layer. The threshold difference between different areas can be achieved by adjusting the type, color, amount, particle size, shell structure of the photochromic microcapsules, and the type or content of the threshold-regulating components; if necessary, it can also be finely controlled by combining the weight gain difference of the single-area coating. The application method can be selected from one or more of partitioned coating, screen printing, digital inkjet printing, and padding-local fixation, and the weight gain of the single-area coating is preferably 5~40g / m². 2 .

[0010] (4) Drying and curing: The fabric to which the finishing liquid is applied is dried and cured to ensure that the partitioned photoresponsive camouflage layer is firmly bonded to the base fabric. The drying temperature is preferably 60~100℃ and the time is 1~8min, and the curing temperature is preferably 100~160℃ and the time is 1~10min. Through the above heat treatment, the film-forming binder can be continuously formed and the photochromic microcapsules can be stably fixed, thereby reducing the risk of migration and blurring of the multi-region pattern boundary during subsequent use.

[0011] (5) Transparent protective layer coating and secondary curing: A transparent polyurethane, siloxane elastomer, or fluorinated transparent resin protective layer is applied to the surface of the photoresponsive camouflage layer. The thickness of the protective layer is preferably 1~30μm, and then a secondary curing is performed to obtain the final fabric. The secondary curing temperature is preferably 80~140℃ and the time is 0.5~8min. This transparent protective layer can reduce the exposure and shedding of microcapsules during friction and washing, and can improve the stability of pattern boundaries and outdoor weather resistance while maintaining light transmittance.

[0012] Compared with the prior art, the beneficial effects of the present invention are at least as follows: (1) The core of this invention is not only about “zone color change”, but also about using a combination of surface activation / interface anchoring and zone threshold control to enable different pattern areas to form stable and distinguishable light response layers on flexible fabric, thereby improving the realism and resolution of environmental adaptive camouflage.

[0013] (2) By using photochromic microcapsules of different types, amounts or shell structures in different pattern areas, and combining them with threshold control components, adjacent areas can exhibit different activation thresholds and color change depths under the same lighting conditions, thus more closely resembling the light and dark gradients and shadow textures in natural backgrounds.

[0014] (3) Through the synergistic effect of surface activation / interface anchoring treatment, film-forming adhesive fixation and secondary curing of transparent protective layer, the bonding strength between functional layer and fabric interface can be improved, microcapsule migration and pattern boundary blurring can be inhibited, and friction resistance, washability and long-term service stability can be improved.

[0015] (4) The present invention can achieve stable fixation of the functional layer without the need for a thick rigid substrate. While maintaining the soft, breathable and sewnable properties of the fabric, it also takes into account the engineering application needs of camouflage clothing, equipment covers, outdoor tents and coverings. Attached Figure Description

[0016] Figure 1 A schematic diagram of the structure of a photochromic environment-adaptive camouflage fabric; Figure 2 A schematic diagram showing the setting of different light response thresholds for photochromic environment-adaptive camouflage fabrics in different pattern areas; Figure 3 A schematic diagram showing the apparent color change of a photochromic environment-adaptive camouflage fabric under low and high light conditions. Figure 4 Flowchart of a method for preparing photochromic environmental adaptive camouflage fabric. Detailed Implementation

[0017] The present invention will be described in detail below with reference to the accompanying drawings and preferred embodiments. The purpose and effects of the present invention will become clearer. It should be understood that the specific embodiments described herein are merely for explaining the present invention and are not intended to limit the present invention.

[0018] Example 1 A method for preparing a photochromic environmentally adaptive camouflage fabric, comprising the following steps: (1) Preparation of the base fabric layer: Polyester-cotton woven fabric was selected as the base fabric layer with a surface density of 120~220 g / m 2 After desizing, degreasing, and cleaning the base fabric in sequence, surface activation is performed using low-temperature plasma at a power of 200W for 60s. Subsequently, the fabric is padded with a 1.0wt% aminosilane hydrolysate for 30s and dried at 80°C for 2min to form an active interface on the fabric surface that is conducive to the subsequent fixation of functional layers, resulting in a clean polyester / cotton blended base fabric layer.

[0019] (2) Preparation of base color layer: A base color layer is formed on the surface of the base fabric layer. The base color layer is a composite base color of military green and yellowish brown. The base color layer can be prepared by conventional dyeing, printing or coating processes to provide a basic camouflage base color for subsequent photochromic pattern layers.

[0020] (3) Preparation of photochromic finishing solutions: Three photochromic finishing solutions with different color systems and different response thresholds were prepared respectively. The first finishing solution, by total mass, included: 18wt% green photochromic microcapsules, 22wt% aqueous polyurethane film-forming binder, 1.2wt% polycarboxylate dispersant, 0.4wt% polyether-modified siloxane leveling agent, 0.8wt% UV stabilizer, 0.6wt% antioxidant, 0.8wt% UV absorber, with the balance being deionized water; the second finishing solution, by total mass, included: 16wt% brown photochromic microcapsules, 22wt% aqueous polyurethane film-forming binder, 1.2wt% polycarboxylate dispersant, 0.6wt% UV stabilizer, 0.8wt% UV absorber, with the balance being deionized water; The first finishing solution contains 0.4 wt% polyether-modified siloxane leveling agent, 0.8 wt% UV stabilizer, 0.6 wt% antioxidant, and 1.6 wt% UV absorber, with the balance being deionized water. The second finishing solution, by total mass, comprises: 14 wt% gray-brown photochromic microcapsules, 22 wt% aqueous polyurethane film-forming binder, 1.2 wt% polycarboxylate dispersant, 0.4 wt% polyether-modified siloxane leveling agent, 0.8 wt% UV stabilizer, 0.6 wt% antioxidant, and 2.4 wt% UV absorber, with the balance being deionized water. The particle size of all three types of photochromic microcapsules is 1–8 μm. By adjusting the amount of microcapsules added and the content of the UV absorber, the three finishing solutions correspond to low, medium, and high photoresponse thresholds, respectively.

[0021] (4) Preparation of photochromic pattern layer: According to the preset camouflage pattern, the photochromic finishing liquids with different formulations are applied to the surface of the base color layer in sections by screen printing, so that green, brown and gray-brown color blocks are formed in different areas respectively, thereby constructing a photochromic pattern layer with differentiated light response characteristics on the fabric surface.

[0022] (5) Pre-drying and curing treatment: The printed fabric is pre-dried at 80°C for 3 minutes to remove moisture or solvent from the system; then it is cured at 130°C for 2 minutes to firmly bond the photochromic pattern layer with the base color layer and the base fabric layer to form a stable functional layer structure.

[0023] (6) Preparation of transparent protective layer: A transparent polyurethane thin layer with a thickness of about 8 μm is applied as a protective layer to the surface of the cured photochromic pattern layer, and then cured again at 110°C for 2 min to obtain the photochromic environmental adaptive camouflage fabric. The transparent protective layer is used to improve the abrasion resistance, washability and use stability of the fabric, while maintaining its light transmittance and flexibility.

[0024] Example 2 A method for preparing a photochromic environmentally adaptive camouflage fabric suitable for desert environments, comprising the following steps: (1) Preparation of the base fabric layer: Nylon spandex elastic fabric was selected as the base. After desizing, degreasing and cleaning of the fabric in sequence, it was activated by low-temperature plasma with a power of 150W and a time of 45s to improve the surface activity and bonding strength of the fabric and obtain a base fabric layer with good elasticity and stable adhesion.

[0025] (2) Preparation of base color layer: Apply sand yellow base color coating to the surface of the activated base fabric, and dry and cure to form a uniform sand yellow base color that matches the background characteristics of the desert environment.

[0026] (3) Preparation of photochromic finishing solution: Three photochromic finishing solutions of light brown, gray-yellow and brown were prepared respectively. Photochromic microcapsules of the corresponding color system were used as functional components, and waterborne polyurethane was used as film-forming binder. Different contents of threshold-regulating components and ultraviolet absorbers were introduced into the different finishing solutions. Specifically, the mass fractions of photochromic microcapsules in the three finishing solutions were 15wt%, 13wt% and 11wt% respectively, the mass fractions of ultraviolet absorbers were 0.6wt%, 1.4wt% and 2.2wt% respectively, the waterborne polyurethane film-forming binder was 22wt% in all three solutions, and 1.0wt% of polycarboxylate dispersant, 0.3wt% of leveling agent and 0.8wt% of ultraviolet stabilizer were added. The solutions were stirred and dispersed thoroughly to obtain three differentiated response finishing solutions.

[0027] (4) Preparation of partitioned photochromic pattern layer: According to the desert camouflage texture design, three photochromic finishing liquids are applied to different areas of the base color layer by printing or partition coating to form a multi-regional independent response photochromic pattern layer.

[0028] (5) Drying and curing: Dry (80℃ for 2 min) and cure (110℃ for 5 min) the fabric after applying the finishing liquid to make the photochromic pattern layer firmly bonded to the base fabric, ensuring that it is not easy to fall off and is resistant to friction during use.

[0029] (6) Application of protective layer and secondary curing: A transparent protective layer is applied to the surface of the photochromic pattern layer, and secondary curing at 100°C for 3 minutes further improves the weather resistance, washability and service life of the fabric. The fabric prepared by this method can adjust the differences in component and microcapsule content by different thresholds in different areas, so that each pattern area produces different degrees of color deepening effect after light exposure, forming a dynamic camouflage texture that is close to the shadow changes on the desert surface, and is suitable for use in desert environments.

[0030] Example 3 A method for preparing a photochromic environmental adaptive camouflage fabric suitable for equipment camouflage covers, comprising the following steps: (1) Preparation of the base fabric layer: High-strength polyester fiber fabric is selected as the base. After desizing, degreasing and deionized water cleaning of the fabric in sequence, it is then immersed in 1.5wt% epoxy silane hydrolysate for 60s and dried at 85℃ for 2min for surface activation treatment to improve the surface adhesion and coating uniformity of the fabric and obtain a base fabric layer with a firm structure and stable dimensions.

[0031] (2) Preparation of photochromic finishing solution: 18wt% of photochromic microcapsules, 24wt% of aqueous polyurethane film-forming binder, 1.0wt% of polycarboxylate dispersant, 0.4wt% of polyether modified siloxane leveling agent, 0.8wt% of UV stabilizer, 1.2wt% of threshold control component and the balance of deionized water are mixed in proportion and stirred thoroughly under high-speed dispersion conditions to obtain a stable photochromic finishing solution suitable for printing and coating.

[0032] (3) Preparation of photochromic pattern layer: The prepared photochromic finishing liquid is applied to the outside of the base fabric by coating or printing to form a uniform photochromic pattern layer with light-responsive color-changing ability, so that the fabric can change color and brightness when the external light changes.

[0033] (4) Drying and curing: The fabric with photochromic finishing liquid is dried (60℃ for 5 min) and cured (150℃ for 1 min) to fully bond the photochromic pattern layer with the base fabric, thereby improving the adhesion, abrasion resistance and outdoor stability of the functional layer.

[0034] (5) Coating and secondary curing of wear-resistant and waterproof protective layer: Apply a wear-resistant and waterproof transparent protective layer with a thickness of about 10μm evenly to the surface of the photochromic pattern layer. After secondary curing at 120℃ for 2min, the protective layer is tightly bonded to the fabric surface, improving the weather resistance, waterproofness and wear resistance during outdoor use.

[0035] The photochromic environmental adaptive camouflage fabric prepared by this method can automatically enhance the contrast between light and dark on the surface under long-term outdoor light conditions, effectively reducing the contrast between the target's appearance and the environmental background. It is suitable for use as outdoor protective and camouflage products such as equipment covers.

[0036] Example 4 Based on Example 1, an anti-UV aging agent, an antioxidant, and a softening agent are added to the photoresponsive camouflage layer. The preparation method for a photochromic environmentally adaptive camouflage fabric includes the following steps: (1) Preparation of base fabric layer and base color layer: Polyester-cotton woven fabric with a surface density of 120 to 220 g / m² was selected as the base. After desizing, degreasing and cleaning, the fabric was treated with low-temperature plasma activation and aminosilane coupling. The plasma power was 180W and the time was 50s. The mass fraction of aminosilane hydrolysate was 1.0wt% and the treatment time was 30s. Subsequently, a military green and yellow-brown composite base color layer was prepared on the fabric surface.

[0037] (2) Preparation of photochromic finishing solution: Three types of photochromic finishing solutions, namely green, brown and gray-brown, were prepared respectively. Photochromic microcapsules of the corresponding color with a particle size of 1 to 8 micrometers were used as functional components, and waterborne polyurethane was used as film-forming binder. Anti-ultraviolet aging agent, antioxidant and softening agent were added to the finishing solution, and dispersant, leveling agent and threshold regulating component ultraviolet absorber were added. The solution was stirred and dispersed to obtain three types of photochromic finishing solutions with anti-aging and softening properties. The mass fractions of photochromic microcapsules in the three finishing solutions were 17wt%, 15wt% and 13wt% respectively, the mass fractions of threshold regulating component were 0.8wt%, 1.5wt% and 2.2wt% respectively, and the contents of other components were the same.

[0038] (3) Preparation of the partitioned photochromic pattern layer: According to the preset camouflage pattern, three different formulations of photochromic finishing liquid are applied to different areas of the base color layer surface by screen printing to form a partitioned response photochromic pattern layer.

[0039] (4) Drying and curing treatment: The printed fabric is subjected to segmented heat treatment. First, it is pre-dried at 80 degrees Celsius for 3 minutes, and then cured at 130 degrees Celsius for 2 minutes to make the photochromic pattern layer firmly bonded to the base fabric.

[0040] (5) Transparent protective layer coating and secondary curing: A transparent polyurethane thin layer with a thickness of about 6 μm is applied to the surface of the photochromic pattern layer. After secondary curing at 100°C for 3 min, the photochromic environment-adaptive camouflage fabric is obtained. This preparation method introduces anti-UV aging agents, antioxidants and softening agents based on Example 1, which can further improve the anti-aging performance and hand comfort of the fabric, and help maintain good reversible color-changing performance and fabric hand feel under cyclic light exposure and repeated bending conditions.

[0041] Comparison and performance evaluation The sample prepared in Example 1 was used as the experimental group, and the following comparative examples were set up: Comparative Example 1 was to remove the surface activation / interface anchoring treatment while keeping the other conditions basically the same; Comparative Example 2 was to remove the transparent protective layer while keeping the other conditions basically the same; Comparative Example 3 was to use the same amount of microcapsule addition and the same threshold control component in each pattern area, without constructing differentiated photoresponse thresholds.

[0042] The light response activation illuminance or activation time, overall color difference change, surface integrity after dry and wet friction, pattern boundary retention after washing, and functional layer adhesion after repeated bending were tested on the experimental group and each comparative sample. The results showed that: compared with Comparative Example 1, the functional layer of the sample obtained in Example 1 had stronger adhesion and clearer pattern boundaries after washing and bending; compared with Comparative Example 2, the sample obtained in Example 1 had better abrasion resistance and washability; compared with Comparative Example 3, the sample obtained in Example 1 could form more obvious zonal response levels and a dynamic camouflage effect that more closely resembled the changes in natural background shadows under the same lighting conditions.

[0043] The above comparative examples illustrate that surface activation / interface anchoring, partition threshold control, and secondary curing of the transparent protective layer are the key technical means for achieving pattern boundary stability, durable service, and environmentally adaptive camouflage effects in this invention.

[0044] It will be understood by those skilled in the art that the above descriptions are merely preferred examples of the invention and are not intended to limit the invention. Although the invention has been described in detail with reference to the foregoing examples, those skilled in the art can still modify the technical solutions described in the foregoing examples or make equivalent substitutions for some of the technical features. All modifications and equivalent substitutions made within the spirit and principles of the invention should be included within the scope of protection of the invention.

Claims

1. A method for the production of a photochromic environmentally adaptive camouflage fabric, characterized in that, include: S1. After desizing, degreasing and cleaning the base fabric, a surface activation treatment is performed to improve the surface energy of the base fabric and the adhesion of the functional layer. Optionally, an interface anchoring layer is further formed on the surface of the base fabric. S2. Prepare two or more photochromic finishing solutions, wherein the photochromic finishing solution includes photochromic microcapsules, film-forming binder, dispersant, leveling agent, stabilizing agent, and threshold regulating component; the different photochromic finishing solutions differ in the type, color, amount added, particle size, shell structure of the photochromic microcapsules and / or the type and content of the threshold regulating component, thereby having different light response thresholds and / or different color change responses; S3. According to the preset camouflage pattern, apply different photochromic finishing liquids to different surface areas of the base fabric in sections, or first form a base color layer on the surface of the base fabric, and then apply different photochromic finishing liquids to different areas of the base color layer to form a partitioned light-response camouflage layer. S4. The fabric after applying the photochromic finishing liquid is dried and cured to ensure that the partitioned light-response camouflage layer is firmly bonded to the base fabric. S5. A transparent protective layer is covered on the surface of the partitioned light-response camouflage layer and then cured a second time to obtain the photochromic environment-adaptive camouflage fabric.

2. The production method according to claim 1, characterized by, The base fabric is a woven fabric, knitted fabric, or nonwoven fabric, and the material is selected from one or more composites of polyester, nylon, cotton, spandex, and aramid.

3. The preparation method according to claim 1, characterized in that, The surface activation treatment is one or more of the following: low-temperature plasma activation, corona activation, alkali reduction activation, silane coupling activation, and dopamine primer activation; preferably, the power of the low-temperature plasma activation is 100~400W and the treatment time is 10~120s, and / or the silane coupling activation is performed by treating with an aminosilane hydrolysate or an epoxysilane hydrolysate with a mass fraction of 0.5~3wt% for 30~300s.

4. The production method according to claim 1, characterized by, The interface anchoring layer is an interface layer formed by one or more of aminosilane, epoxysilane, dopamine, or waterborne polyurethane primer, with a coating amount of 0.5~10 g / m³. 2 .

5. The method of claim 1, wherein, The photochromic finishing solution comprises, by total mass: 5-35 wt% photochromic microcapsules, 10-40 wt% film-forming binder, 0.2-5 wt% dispersant, 0.1-3 wt% leveling agent, 0.1-5 wt% stabilizing agent, 0.5-10 wt% threshold regulating component, and the balance being water or a mixture of organic solvent and water.

6. The production method according to claim 5, wherein The film-forming binder is one or more of waterborne polyurethane, polyurethane-acrylate composite emulsion, and acrylate emulsion; the dispersant is one or more of polycarboxylate dispersant and polyurethane dispersant; the leveling agent is one or more of polyether-modified siloxane leveling agent and acrylate leveling agent; and the stabilizing agent is one or more of antioxidant, UV stabilizer, anti-settling agent, and pH adjuster.

7. The preparation method according to claim 5, characterized in that, The threshold control component is one or more of ultraviolet absorbers, ultraviolet scattering particles, transparent fillers, and diluents, and the photoresponse threshold of different regions is achieved by adjusting the type or content of the threshold control component, the amount of photochromic microcapsules added, the shell thickness, and / or the weight gain of the single-region coating.

8. The preparation method according to claim 1, characterized in that, The application mode is one or more of zoned coating, screen printing, digital jet printing, padding-local fixation; the single-zone coating weight is 5-40 g / m 2 .

9. The method of claim 1, wherein, The drying temperature is 60~100℃, and the drying time is 1~8min; the curing temperature is 100~160℃, and the curing time is 1~10min; the transparent protective layer is transparent polyurethane, siloxane elastomer, or fluorinated transparent resin, and the thickness of the protective layer is 1~30μm; the secondary curing temperature is 80~140℃, and the time is 0.5~8min.

10. A photochromic environmentally adaptive camouflage fabric, characterized in that, The system includes a base fabric layer, a partitioned photosensitive camouflage layer disposed on the base fabric layer, and a transparent protective layer covering the outside of the partitioned photosensitive camouflage layer. At least two adjacent patterned regions in the partitioned photosensitive camouflage layer each contain photochromic microcapsules fixed by a film-forming binder, and these microcapsules differ in at least one of the following: type, amount, shell structure, or type or content of threshold-regulating components, so that the two adjacent patterned regions have different photosensitive thresholds. A bonding interface formed by surface activation treatment and / or an interface anchoring layer is provided between the base fabric layer and the partitioned photosensitive camouflage layer to improve the stability of the partitioned pattern boundaries and the resistance to abrasion and washing.

Citation Information

Patent Citations

  • Fabric capable of color changing

    CN103126149A

  • Multifunctional color-changing camouflage device coating fabric

    CN109267361A

  • Bistable thermochromic fabric, preparation method thereof and cloak formed by bistable thermochromic fabric

    CN120868831A