An antibacterial and breathable functional fabric for sportswear and its preparation method
By using polyether-modified organosilicon and silica sol to synergistically modify mesoporous silica, combined with waterborne polyurethane emulsion and blocked isocyanate crosslinking agent, a stable functional finishing layer is constructed, which solves the problem of balancing antibacterial properties and breathability in sportswear fabrics and achieves excellent comprehensive performance.
Patent Information
- Application Number
- CN202611246470.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-17
- Publication Date
- 2026-11-17
AI Technical Summary
Existing functional fabrics for sportswear struggle to balance antibacterial and breathability properties, exhibit poor dispersion stability and interfacial compatibility of mesoporous silica, lack sufficient wash fastness of functional finishing layers, and are prone to functional degradation during long-term use.
Using polyester knitted fabric as the base material, a flexible film-forming system is constructed by combining mesoporous silica with polyether-modified organosilicon and silica sol for surface modification, along with water-based polyurethane emulsion and a blocked isocyanate crosslinking agent. The system is then continuously impregnated, dried, and baked to form a uniform and stable functional finishing layer.
It significantly improves the stability and durability of the functional finishing layer, enabling sportswear fabrics to simultaneously possess excellent antibacterial properties, breathability, moisture wicking properties, and wash fastness, meeting the comprehensive performance requirements of high-end sportswear.
Smart Images

Figure CN123108944A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of textile functional finishing materials technology, and in particular to an antibacterial and breathable sportswear functional fabric and its preparation method. Background Technology
[0002] With the popularization of the national fitness concept and the rapid development of the outdoor sports, competitive sports, and leisure sports industries, consumers have placed higher demands on the functionality of sportswear. Modern sportswear not only requires good softness, elasticity, and comfort, but also excellent breathability, moisture-wicking properties, antibacterial properties, and washability to meet the needs of the human body during exercise, such as heavy sweating, prolonged wear, and frequent washing. Therefore, developing functional fabrics with antibacterial, breathable, and durable properties has become an important research direction in the field of functional textiles.
[0003] Currently, the main technical approaches for functional sportswear fabrics are functional fiber blend spinning, fabric structure optimization, and post-processing functional finishing. Among these, post-processing has become the mainstream technology for the industrial production of functional sportswear fabrics due to its advantages such as low production cost, wide applicability to various fibers, and ease of integration with existing continuous production equipment. Existing post-processing systems often use functional materials such as silver ions, zinc oxide, titanium dioxide, chitosan, and silicone softeners to impart antibacterial or moisture-wicking properties to fabrics, but some shortcomings still exist.
[0004] On the one hand, while silver ions and nano-metal oxides offer good antibacterial effects, they suffer from high costs, easy agglomeration of nanoparticles, insufficient wash fastness, and significant functional degradation over long-term use. On the other hand, traditional silicone softening agents, while improving fabric softness and feel, offer limited improvement in breathability and moisture wicking. Furthermore, some agents exhibit poor compatibility with waterborne polyurethane systems, leading to uneven distribution of functional components on the fabric surface and affecting the stability of the finished layer. Moreover, most existing antibacterial finishing technologies primarily focus on antibacterial properties, with relatively insufficient research on the synergistic improvement of breathability, moisture wicking, and wash fastness, making it difficult to meet the comprehensive performance requirements of high-end sportswear.
[0005] In recent years, mesoporous silica has been increasingly used in the field of functional finishing materials due to its advantages such as large specific surface area, regular pore structure, high chemical stability, and ease of surface functionalization. However, unmodified mesoporous silica has high silanol activity on its surface, making it prone to particle aggregation and exhibiting poor compatibility with organic film-forming systems. This leads to problems such as insufficient dispersion stability, low adhesion, and decreased wash resistance during fabric finishing, thus limiting its further application in functional sportswear fabrics.
[0006] Therefore, developing an antibacterial and breathable functional fabric for sportswear that can improve the dispersion stability and interfacial compatibility of mesoporous silica while also taking into account antibacterial, breathable, moisture-wicking, and washable properties, and its preparation method, is of great practical significance for improving the overall performance of sportswear and meeting the needs of high-quality development of functional textiles. Summary of the Invention
[0007] To overcome the technical problems of existing sportswear functional fabrics, such as the difficulty in simultaneously achieving antibacterial and breathable properties, poor dispersion stability and interfacial compatibility of mesoporous silica, insufficient wash fastness of the functional finishing layer, and easy functional degradation during long-term use, the present invention aims to provide an antibacterial and breathable sportswear functional fabric and its preparation method. This invention uses polyester knitted fabric as the base material, and polyether-modified organosilicon and silica sol-synergistically surface-modified mesoporous silica as functional fillers. A flexible film-forming system is constructed using an aqueous polyurethane emulsion, and L-arginine and a blocked isocyanate crosslinking agent are introduced for synergistic finishing. Through continuous padding, drying, and baking setting processes, a uniform, stable, and durable functional finishing layer is formed on the fabric surface, thereby obtaining a sportswear functional fabric with excellent antibacterial, breathable, moisture-wicking, and wash-resistant properties.
[0008] Compared with existing technologies, this invention significantly improves the stability and durability of the functional finishing layer by constructing a mesoporous silica functional system synergistically modified with polyether-modified organosilicon and silica sol, and combining it with waterborne polyurethane film formation and closed isocyanate crosslinking technology. This results in a sportswear functional fabric that simultaneously possesses excellent antibacterial properties, breathability, moisture wicking properties, and wash fastness, and has good prospects for industrial application.
[0009] The objective of this invention can be achieved through the following technical solutions:
[0010] An antibacterial and breathable sportswear functional fabric comprises the following raw materials in parts by weight: 100 parts polyester knitted fabric; 5-18 parts synergistically modified mesoporous silica; 15-35 parts waterborne polyurethane emulsion; 0.2-2 parts L-arginine; 0.5-3 parts blocked isocyanate crosslinking agent; and 200-400 parts deionized water. The synergistically modified mesoporous silica is prepared by synergistically surface modifying mesoporous silica with polyether-modified organosilicon and silica sol.
[0011] Optionally, the synergistically modified mesoporous silica comprises the following raw materials in parts by weight: 100 parts mesoporous silica; 5-20 parts polyether-modified organosilicon; 10-30 parts tetraethyl orthosilicate; 80-200 parts anhydrous ethanol; and 20-80 parts deionized water.
[0012] Optionally, the method for preparing synergistically modified mesoporous silica includes the following steps:
[0013] (1) Mesoporous silica was dispersed in an ethanol-water mixture to obtain a mesoporous silica suspension;
[0014] (2) Add silica sol to the mesoporous silica suspension for coating treatment, and then add polyether modified organosilicon for synergistic modification to obtain a synergistically modified suspension;
[0015] (3) The synergistically modified suspension is filtered, washed and dried to obtain synergistically modified mesoporous silica.
[0016] Optionally, the reaction conditions in step (1) are as follows: the volume ratio of ethanol to deionized water is 3:1 to 5:1, mesoporous silica is added and ultrasonically dispersed for 20 to 40 minutes, followed by mechanical stirring for 30 to 60 minutes.
[0017] Optionally, the reaction conditions in step (2) are as follows: first add silica sol, stir and react at 25-40°C for 1-3 hours; then add polyether-modified organosilicon, and continue stirring and reacting at 50-70°C for 2-4 hours.
[0018] Optionally, the reaction conditions for step (3) are: after filtration, wash with anhydrous ethanol 2 to 3 times, vacuum dry at 60 to 80°C for 6 to 10 hours, and then pulverize and pass through a 200 to 400 mesh sieve.
[0019] Optionally, the blocked isocyanate crosslinking agent is prepared by mixing blocked hexamethylene diisocyanate trimer with deionized water at a mass ratio of 1:(0.8 to 1.5).
[0020] Optionally, a method for preparing an antibacterial and breathable sportswear functional fabric includes the following steps:
[0021] S1, add waterborne polyurethane emulsion to deionized water, stir evenly, then add synergistic modified mesoporous silica, L-arginine and blocked isocyanate crosslinking agent in sequence, and continue stirring to obtain finishing solution;
[0022] S2, the polyester knitted fabric is immersed in the finishing solution of the step, and the finished fabric is obtained after padding.
[0023] S3 involves pre-drying, baking, and cooling the finished fabric in sequence to obtain an antibacterial and breathable sportswear functional fabric.
[0024] Optionally, the reaction conditions in step S1 are: a stirring speed of 300-600 r / min, a stirring time of 30-60 min, and the finishing solution is adjusted to a solid content of 5-12 wt%.
[0025] Optionally, the reaction conditions for steps S2 and S3 are as follows: the rolling process is a two-dip two-roll process with a rolling rate of 70% to 85%; the pre-drying temperature is 80 to 100°C and the pre-drying time is 2 to 5 minutes; the baking temperature is 140 to 160°C and the baking time is 1 to 3 minutes, followed by cooling to room temperature.
[0026] The beneficial effects of this invention are:
[0027] This invention employs polyether-modified organosilicon and silica sol to synergistically modify the surface of mesoporous silica. The polyether-modified organosilicon forms flexible hydrophilic segments on the surface of the mesoporous silica, reducing interparticle surface energy and improving its dispersion stability and interfacial compatibility in waterborne polyurethane finishing systems. The silica sol forms a continuous and stable silica-oxygen network coating layer on the surface of the mesoporous silica, enhancing particle structural stability and improving the bonding strength between the functional filler and the film-forming system. The synergistic effect of these two components not only effectively inhibits the aggregation and sedimentation of mesoporous silica in the finishing solution but also further improves the uniformity and wash fastness of the functional finishing layer on the fabric surface. This allows the abundant mesoporous structure of the mesoporous silica to continuously perform its functions of water vapor transport and air exchange, thereby achieving a simultaneous improvement in air permeability and moisture wicking properties.
[0028] Meanwhile, the synergistically modified mesoporous silica can form a stable organic-inorganic composite finishing layer with waterborne polyurethane emulsion. Under the action of a closed isocyanate crosslinking agent, a dense and flexible three-dimensional crosslinking network is further constructed, which makes the functional filler more firmly fixed on the surface of the polyester knitted fabric, significantly reducing the loss of functional components during washing and friction, and improving the durability and stability of the functional finishing layer. L-arginine molecules are uniformly dispersed in the composite finishing layer, which can further improve the hydrophilicity of the fabric surface, promote the rapid spread and diffusion of sweat, and have a synergistic effect with the transport channels formed by the mesoporous silica, enabling the fabric to complete the sweat absorption, diffusion and evaporation process more quickly, thereby effectively improving the wearing comfort during exercise.
[0029] Because a stable synergistic interface structure is formed between polyether-modified organosilicon, silica sol, and mesoporous silica, the problems of easy agglomeration, easy shedding, and poor washability of traditional mesoporous silica during functional finishing are solved. This allows the functional filler to play a stable role for a long time, while taking into account antibacterial, breathable, moisture-wicking, and durable properties. It avoids the problem in existing technologies where improved antibacterial performance is often accompanied by decreased breathability, or improved breathability but insufficient washability. It achieves synergistic optimization of multiple functions, with significant technical effects and good industrial application value. Attached Figure Description
[0030] The invention will now be further described with reference to the accompanying drawings.
[0031] Figure 1 This is a comparison chart of the antibacterial performance test results for samples with different formulation ratios. Detailed Implementation
[0032] The present invention will be further described below with reference to specific embodiments. However, the present invention is not limited to the following embodiments. Equivalent adjustments made without departing from the spirit and essence of the present invention should also be considered to fall within the protection scope of the present invention.
[0033] Example 1: This example uses the lower limit of the raw material composition and process parameters within the scope of the claims to prepare antibacterial and breathable sportswear functional fabric, in order to verify that the technical solution of the present invention can still obtain stable synergistic modified mesoporous silica under low functional component addition and low process conditions, and ensure that the finishing liquid has good dispersion stability and finishing performance, providing a basic control for subsequent examples.
[0034] S1, Preparation of Synergistically Modified Mesoporous Silica
[0035] 100 parts of mesoporous silica were weighed and added to an ethanol-water mixture prepared with 80 parts of anhydrous ethanol and 20 parts of deionized water. The mixture was ultrasonically dispersed for 20 minutes, followed by stirring at a constant speed for 30 minutes using a mechanical stirrer to obtain a uniform mesoporous silica suspension. 10 parts of tetraethyl orthosilicate were added to the suspension, and the mixture was stirred continuously at 25°C for 1 hour to form a uniform coating layer of tetraethyl orthosilicate on the surface of the mesoporous silica. Subsequently, 5 parts of polyether-modified organosilicon were added, and the mixture was stirred continuously at 50°C for 2 hours to allow the polyether-modified organosilicon to be uniformly adsorbed and fixed on the surface of the mesoporous silica, completing the synergistic surface modification. After the reaction, the resulting suspension was filtered, washed twice with anhydrous ethanol, and vacuum dried at 60°C for 6 hours. After drying, the suspension was pulverized and passed through a 200-mesh sieve to obtain the synergistically modified mesoporous silica for later use.
[0036] S2, Preparation of finishing solution
[0037] Weigh out 5 parts of the synergistically modified mesoporous silica, 15 parts of the aqueous polyurethane emulsion, 0.2 parts of L-arginine, and 0.5 parts of the blocked isocyanate crosslinking agent. The blocked isocyanate crosslinking agent is prepared by pre-mixing blocked hexamethylene diisocyanate trimer and deionized water at a mass ratio of 1:0.8. Add the aqueous polyurethane emulsion to 200 parts of deionized water and stir at 300 r / min for 10 min using a mechanical stirrer to ensure thorough dispersion. Then, add the synergistically modified mesoporous silica, L-arginine, and blocked isocyanate crosslinking agent in sequence, and continue stirring at 300 r / min for 30 min. Simultaneously, adjust the solid content of the finishing liquid to 5 wt% to obtain a uniform and stable functional finishing liquid.
[0038] S3. Preparation of functional fabrics for sportswear
[0039] One hundred parts of polyester knitted fabric were completely immersed in the finishing solution obtained in step S2 and finished using a two-dip two-padding process, with the padding rate controlled at 70%. The padded fabric was first pre-dried in an 80℃ hot air oven for 2 minutes to remove most of the moisture. Then it was transferred to a 140℃ hot air setting machine for baking for 1 minute, so that the closed isocyanate crosslinking agent was gradually de-blocked and formed a crosslinking network with the water-based polyurethane emulsion, while the modified mesoporous silica was firmly bonded to the surface of the polyester knitted fabric. After baking, the fabric was cooled to room temperature to obtain an antibacterial and breathable sportswear functional fabric.
[0040] Example 2: This example uses the median of the raw material composition and process parameters within the scope of the claims to prepare an antibacterial and breathable sportswear functional fabric. This further improves the surface modification effect of the synergistically modified mesoporous silica and its dispersion stability in the finishing solution, enhances the bonding strength between the functional finishing layer and the polyester knitted fabric, and achieves synergistic optimization of antibacterial properties, breathability, moisture absorption and wicking properties, and washability. This example is the preferred embodiment of the present invention.
[0041] S1, Preparation of Synergistically Modified Mesoporous Silica
[0042] 100 parts of mesoporous silica were weighed and added to an ethanol-water mixture prepared with 140 parts of anhydrous ethanol and 50 parts of deionized water. The mixture was ultrasonically dispersed for 30 minutes, followed by continuous stirring with a mechanical stirrer for 45 minutes to obtain a uniformly dispersed mesoporous silica suspension. 20 parts of tetraethyl orthosilicate were added to the suspension, and the mixture was stirred at 32°C for 2 hours to form a uniform and continuous silica-oxygen coating layer on the surface of the mesoporous silica. Subsequently, 12.5 parts of polyether-modified organosilicon were added, and the mixture was stirred at 60°C for 3 hours to allow the polyether-modified organosilicon to be fully adsorbed and fixed on the surface of the mesoporous silica, forming a stable organic-inorganic synergistic interface structure. After the reaction, the resulting suspension was filtered, washed three times with anhydrous ethanol, and vacuum dried at 70°C for 8 hours. After drying, the suspension was pulverized and passed through a 300-mesh sieve to obtain synergistically modified mesoporous silica for later use.
[0043] S2, Preparation of finishing solution
[0044] Weigh out 11.5 parts of the synergistically modified mesoporous silica obtained in step S1, 25 parts of the aqueous polyurethane emulsion, 1.1 parts of L-arginine, and 1.75 parts of the blocked isocyanate crosslinking agent; the blocked isocyanate crosslinking agent is prepared by pre-mixing blocked hexamethylene diisocyanate trimer and deionized water at a mass ratio of 1:1.15; add the aqueous polyurethane emulsion to 300 parts of deionized water, and stir at 450 r / min for 15 min under the action of a mechanical stirrer to form a uniform and stable emulsion system; then add the synergistically modified mesoporous silica, L-arginine, and blocked isocyanate crosslinking agent in sequence, continue stirring at 450 r / min for 45 min, and adjust the solid content of the finishing liquid to 8.5 wt% to obtain a stable and uniform functional finishing liquid;
[0045] S3. Preparation of functional fabrics for sportswear
[0046] One hundred parts of polyester knitted fabric were immersed in the finishing solution obtained in step S2 and finished using a two-dip, two-padding process, with the padding rate controlled at 78%. After padding, the fabric was first pre-dried in a 90℃ hot air oven for 3.5 minutes to allow the finishing solution to penetrate evenly and remove some moisture. Then, it was placed in a 150℃ hot air setting machine for 2 minutes to allow the blocked isocyanate crosslinking agent to fully deblock and react with the water-based polyurethane emulsion, while promoting the synergistic modification of mesoporous silica to firmly bond to the surface of the polyester knitted fabric, forming a continuous, dense, and uniform functional finishing layer. After baking, the fabric was cooled to room temperature to obtain an antibacterial and breathable sportswear functional fabric.
[0047] Example 3: In this example, an antibacterial and breathable sportswear functional fabric was prepared using the upper limit of the raw material composition and process parameters within the scope of the claims. The modification effect of synergistic modification of mesoporous silica and the formation of the finishing layer under the conditions of higher functional component addition and higher process parameters were investigated. This further verifies that the technical solution of the present invention still has good process stability and repeatability under high addition conditions.
[0048] S1, Preparation of Synergistically Modified Mesoporous Silica
[0049] 100 parts of mesoporous silica were weighed and added to an ethanol-water mixture prepared with 200 parts of anhydrous ethanol and 80 parts of deionized water. The mixture was ultrasonically dispersed for 40 minutes, followed by continuous stirring with a mechanical stirrer for 60 minutes to obtain a uniform and stable mesoporous silica suspension. 30 parts of tetraethyl orthosilicate were added to the suspension and stirred at 40°C for 3 hours to allow the tetraethyl orthosilicate to fully coat the surface of the mesoporous silica and form a continuous silicon-oxygen network. Subsequently, 20 parts of polyether-modified organosilicon were added and stirred at 70°C for 4 hours to further adsorb and fix the polyether-modified organosilicon onto the surface of the mesoporous silica, forming a stable synergistic modification layer. After the reaction, the resulting suspension was filtered, washed three times with anhydrous ethanol, and vacuum dried at 80°C for 10 hours. After drying, the suspension was pulverized and passed through a 400-mesh sieve to obtain synergistically modified mesoporous silica for later use.
[0050] S2, Preparation of finishing solution
[0051] Weigh out 18 parts of the synergistically modified mesoporous silica obtained in step S1, 35 parts of the aqueous polyurethane emulsion, 2 parts of L-arginine, and 3 parts of the blocked isocyanate crosslinking agent; the blocked isocyanate crosslinking agent is prepared by pre-mixing blocked hexamethylene diisocyanate trimer and deionized water at a mass ratio of 1:1.5; add the aqueous polyurethane emulsion to 400 parts of deionized water, and stir at 600 r / min for 20 min under the action of a mechanical stirrer to form a uniform and stable emulsion system; then add the synergistically modified mesoporous silica, L-arginine, and blocked isocyanate crosslinking agent in sequence, continue stirring at 600 r / min for 60 min, and adjust the solid content of the finishing liquid to 12 wt% to obtain a stable and uniform functional finishing liquid;
[0052] S3. Preparation of functional fabrics for sportswear
[0053] One hundred parts of polyester knitted fabric were immersed in the finishing solution obtained in step S2 and finished using a two-dip, two-padding process, with the padding rate controlled at 85%. The padded fabric was first pre-dried in a 100℃ hot air oven for 5 minutes to allow the finishing solution to fully penetrate and complete the initial film formation. Then, it was baked in a 160℃ hot air setting machine for 3 minutes to allow the closed isocyanate crosslinking agent to fully de-block and form a denser crosslinking network with the water-based polyurethane emulsion. At the same time, it promoted the synergistic modification of mesoporous silica to firmly bond to the surface of the polyester knitted fabric, forming a complete functional finishing layer. After baking, the fabric was naturally cooled to room temperature to obtain an antibacterial and breathable sportswear functional fabric.
[0054] Comparative Example 1: This comparative example aims to verify the effect of synergistically modified mesoporous silica on the overall performance of sportswear functional fabrics compared to unmodified mesoporous silica.
[0055] This comparative example is basically the same as Example 2, except that in step S1, polyether-modified organosilicon and silica sol are not used to modify the surface of mesoporous silica, but unmodified mesoporous silica is used directly. The composition, ratio and process conditions of the other raw materials are the same as those in Example 2.
[0056] S1, Treatment of mesoporous silica
[0057] 100 parts of mesoporous silica were weighed and added to an ethanol-water mixed solution prepared by 140 parts of anhydrous ethanol and 50 parts of deionized water. The solution was ultrasonically dispersed for 30 min, then mechanically stirred for 45 min. After filtration, the solution was washed three times with anhydrous ethanol, dried under vacuum at 70℃ for 8 h, pulverized and passed through a 300-mesh sieve to obtain unmodified mesoporous silica.
[0058] S2, Preparation of finishing solution
[0059] Weigh 11.5 parts of the above-mentioned unmodified mesoporous silica, 25 parts of aqueous polyurethane emulsion, 1.1 parts of L-arginine, 1.75 parts of blocked isocyanate crosslinking agent and 300 parts of deionized water, and prepare the finishing solution according to the method in S2 of Example 2.
[0060] S3. Preparation of functional fabrics for sportswear
[0061] Following the method in S3 of Example 2, the fabric undergoes two dips and two rolls, pre-drying, baking, and cooling to obtain a functional fabric for sportswear.
[0062] Comparative Example 2: This comparative example aims to verify the effect of synergistic surface modification of polyether-modified organosilicon and silica sol on the comprehensive performance of functional sportswear fabrics compared to single polyether-modified organosilicon modification.
[0063] This comparative example is basically the same as Example 2, except that in step S1, only polyether-modified organosilicon is used to modify the surface of mesoporous silica, and no silica sol is added. The composition, ratio and process conditions of the other raw materials are the same as those in Example 2.
[0064] S1, Preparation of polyether-modified mesoporous silica
[0065] 100 parts of mesoporous silica were weighed and added to an ethanol-water mixture prepared with 140 parts of anhydrous ethanol and 50 parts of deionized water. The mixture was ultrasonically dispersed for 30 min, followed by mechanical stirring for 45 min to obtain a uniform mesoporous silica suspension. 12.5 parts of polyether-modified organosilicon were added to the suspension and stirred at 60°C for 3 h to allow the polyether-modified organosilicon to adsorb onto the surface of the mesoporous silica. After the reaction was completed, the resulting suspension was filtered, washed three times with anhydrous ethanol, vacuum dried at 70°C for 8 h, pulverized, and passed through a 300-mesh sieve to obtain polyether-modified mesoporous silica.
[0066] S2, Preparation of finishing solution
[0067] Weigh 11.5 parts of the above-mentioned polyether-modified mesoporous silica, 25 parts of waterborne polyurethane emulsion, 1.1 parts of L-arginine, 1.75 parts of blocked isocyanate crosslinking agent and 300 parts of deionized water, and prepare the finishing solution according to the method in S2 of Example 2.
[0068] S3. Preparation of functional fabrics for sportswear
[0069] Following the method in S3 of Example 2, the fabric undergoes two dips and two rolls, pre-drying, baking, and cooling to obtain a functional fabric for sportswear.
[0070] Performance testing:
[0071] 1. Antibacterial performance test
[0072] The antimicrobial properties of the sportswear functional fabrics prepared in each example and comparative example were tested according to GB / T20944.3—2008 "Evaluation of antimicrobial properties of textiles - Part 3: Shaking method". Staphylococcus aureus and Escherichia coli were used as test bacteria. The cut samples were co-cultured with a certain concentration of bacterial solution for 18–24 hours with shaking. After incubation, the number of viable bacteria in the culture solution was measured, and the inhibition rate (%) of the samples against the bacteria was calculated. Each group of samples was tested in triplicate, and the average value was taken as the final test result.
[0073] 2. Breathability test
[0074] The air permeability of the sportswear functional fabrics prepared in each example and comparative example was tested according to GB / T5453—1997 "Textiles - Determination of Air Permeability of Fabrics". After conditioning the samples in a standard temperature and humidity environment for 24 hours, the air flow rate through a unit area of fabric per unit time was measured using a fabric air permeability tester under a pressure difference of 100 Pa. The air permeability of the fabric was expressed as air permeability (mm / s). Five different locations were tested for each group of samples, and the average value was taken as the final test result.
[0075] 3. Moisture absorption and wicking performance test
[0076] The moisture absorption and wicking properties of the sportswear functional fabrics prepared in each example and comparative example were tested according to GB / T21655.2—2019 "Evaluation of moisture absorption and quick-drying properties of textiles - Part 2: Dynamic moisture transfer method". The unidirectional moisture transfer index and overall liquid moisture management capacity (OMMC value) of the samples were determined using a dynamic liquid moisture management tester, with the overall liquid moisture management capacity used as the evaluation index. Each group of samples was tested repeatedly five times, and the average value was taken as the final test result. The higher the OMMC value, the better the fabric's moisture absorption, diffusion, and wicking properties.
[0077] 4. Antibacterial retention rate test after washing
[0078] The sportswear functional fabrics prepared in each example and comparative example were washed 20 times continuously according to GB / T8629—2017 "Home Washing and Drying Procedures for Textiles". After washing, the inhibition rate of Staphylococcus aureus was determined again according to GB / T20944.3—2008, and the antibacterial retention rate (%) was calculated based on the retention of antibacterial rate before and after washing to evaluate the durability stability of the finishing layer after repeated washing. Each group of samples was tested in parallel 3 times, and the average value was taken as the final test result.
[0079] Table 1 Performance test results of different embodiments and comparative examples
[0080] sample Antibacterial rate (%) Air permeability (mm / s) OMMC value Antibacterial retention rate after washing (%) Example 1 94.6 302 0.79 90.5 Example 2 97.8 315 0.88 96.2 Example 3 96.9 309 0.84 94.7 Comparative Example 1 83.8 282 0.57 73.8 Comparative Example 2 90.4 295 0.70 84.6
[0081] As shown in Table 1, the antibacterial and breathable sportswear functional fabrics prepared in different embodiments and comparative examples exhibit significant differences in antibacterial rate, breathability, moisture absorption and wicking properties, and antibacterial retention rate after washing. Among these, the embodiments are all superior to the comparative examples, with Example 2 showing the best overall performance. This indicates that the technical solution of the present invention, which uses polyether-modified organosilicon and silica sol to synergistically modify the surface of mesoporous silica, can effectively improve the stability of the functional finishing layer and fully leverage the synergistic effect between the components, thereby significantly improving the overall performance of the sportswear functional fabric.
[0082] In terms of antibacterial performance, the antibacterial rates of Examples 1, 2, and 3 reached 94.6%, 97.8%, and 96.9%, respectively, all significantly higher than those of Comparative Examples 1 and 2. Comparative Example 1, using unmodified mesoporous silica, had an antibacterial rate of only 83.8%, indicating that unmodified mesoporous silica is prone to aggregation in the finishing solution and has poor interfacial compatibility with the aqueous polyurethane system, resulting in uneven distribution of the functional finishing layer and difficulty in fully realizing its functional role. Comparative Example 2, using polyether-modified organosilicon to modify mesoporous silica alone, increased the antibacterial rate to 90.4%, indicating that single modification can improve the dispersion performance of mesoporous silica. However, due to the lack of a stable silica-oxygen network formed by silica sol, its surface modification effect still has certain limitations. Example 2, using polyether-modified organosilicon and silica sol for synergistic surface modification, further improved the dispersion stability of mesoporous silica in the finishing solution and its binding ability with the film-forming system, making the functional finishing layer more uniform and stable, thus achieving the best antibacterial performance.
[0083] In terms of air permeability, Example 2 achieved an air permeability of 315 mm / s, higher than Example 1's 302 mm / s and Example 3's 309 mm / s, and also significantly better than Comparative Examples 1 and 2. This indicates that the synergistically modified mesoporous silica can fully maintain the integrity of the mesoporous structure while improving its uniform distribution on the fabric surface, ensuring that the finishing layer does not significantly block the fabric pores while maintaining functionality, thus maintaining high air circulation capacity. Although Example 3 had a higher amount of functional filler, the increased thickness of the finishing layer caused some coverage of the fabric pores, resulting in slightly lower air permeability than Example 2. Example 1, with its lower amount of functional components, had a relatively limited effect on optimizing the fabric pore structure, and therefore its air permeability was also slightly lower than Example 2.
[0084] In terms of moisture absorption and wicking performance, Example 2 achieved the highest OMMC value of 0.88 among all samples, indicating its superior liquid moisture transfer capability. This is mainly due to the hydrophilic flexible segments provided by the polyether-modified silicone, which enhances the wetting ability of the fabric surface. Meanwhile, the synergistically modified mesoporous silica retains a rich mesoporous structure, forming continuous moisture transport channels. Both work together to promote the rapid absorption, diffusion, and evaporation of sweat in the fabric. In contrast, Comparative Example 1, being unmodified, exhibited a high OMMC value of only 0.57 due to the tendency of its mesoporous silica to aggregate. Although Comparative Example 2 underwent single polyether-modified silicone treatment, the lack of a stable interface structure synergistically constructed with silica sol resulted in lower moisture wicking performance compared to the Example 2.
[0085] In terms of antibacterial retention rate after washing, Examples 1, 2, and 3 reached 90.5%, 96.2%, and 94.7% respectively, all significantly higher than Comparative Example 1 (73.8%) and Comparative Example 2 (84.6%). This indicates that the present invention, through the synergistic modification of polyether-modified organosilicon and silica sol, can form a stable organic-inorganic composite interface on the surface of mesoporous silica. Furthermore, under the combined action of a blocked isocyanate crosslinking agent and an aqueous polyurethane emulsion, a dense crosslinking network is constructed, allowing the functional filler to be more firmly bonded to the surface of the polyester knitted fabric. This effectively reduces the shedding of functional components during washing, thus exhibiting excellent wash resistance and durability. While Example 3 has a high wash resistance retention rate, its thicker finishing layer somewhat affects the fabric's breathability and moisture wicking properties, resulting in slightly lower overall performance compared to Example 2.
[0086] In summary, this invention employs a synergistic surface modification of mesoporous silica using polyether-modified organosilicon and silica sol, combined with an aqueous polyurethane emulsion, L-arginine, and a blocked isocyanate crosslinking agent to construct a stable functional finishing system. This significantly improves the dispersion stability and interfacial compatibility of mesoporous silica, enhances the bonding strength between the functional finishing layer and the fabric, and results in sportswear functional fabrics that simultaneously possess excellent antibacterial properties, breathability, moisture absorption and wicking properties, and washability and durability. Example 2, using a median formulation, achieves optimal synergistic balance among the components, thus exhibiting the best overall performance, fully demonstrating the significant technical effects and good application value of this invention.
Claims
1. An antibacterial and breathable functional fabric for sportswear, characterized in that, The raw materials include the following parts by weight: 100 parts polyester knitted fabric; 5-18 parts synergistically modified mesoporous silica; 15-35 parts aqueous polyurethane emulsion; 0.2-2 parts L-arginine; 0.5-3 parts blocked isocyanate crosslinking agent; and 200-400 parts deionized water. The synergistically modified mesoporous silica is prepared by synergistically surface modifying mesoporous silica with polyether-modified organosilicon and silica sol.
2. The antibacterial and breathable sportswear functional fabric according to claim 1, characterized in that, The synergistically modified mesoporous silica comprises the following raw materials in parts by weight: 100 parts mesoporous silica; 5-20 parts polyether-modified organosilicon; 10-30 parts tetraethyl orthosilicate; 80-200 parts anhydrous ethanol; and 20-80 parts deionized water.
3. The antibacterial and breathable sportswear functional fabric according to claim 1 or 2, characterized in that, The method for preparing the synergistically modified mesoporous silica includes the following steps: (1) Mesoporous silica was dispersed in an ethanol-water mixture to obtain a mesoporous silica suspension; (2) Add silica sol to the mesoporous silica suspension for coating treatment, and then add polyether modified organosilicon for synergistic modification to obtain a synergistically modified suspension; (3) The synergistically modified suspension is filtered, washed and dried to obtain synergistically modified mesoporous silica.
4. The antibacterial and breathable sportswear functional fabric according to claim 3, characterized in that, The reaction conditions for step (1) are as follows: the volume ratio of ethanol to deionized water is 3:1 to 5:1; after adding mesoporous silica, it is ultrasonically dispersed for 20 to 40 minutes, followed by mechanical stirring for 30 to 60 minutes.
5. The antibacterial and breathable sportswear functional fabric according to claim 3, characterized in that, The reaction conditions for step (2) are as follows: first, add silica sol and stir the reaction at 25-40°C for 1-3 hours; then add polyether-modified organosilicon and continue stirring the reaction at 50-70°C for 2-4 hours.
6. The antibacterial and breathable sportswear functional fabric according to claim 3, characterized in that, The reaction conditions for step (3) are as follows: after filtration, the material is washed 2-3 times with anhydrous ethanol, dried under vacuum at 60-80℃ for 6-10 hours, pulverized, and then passed through a 200-400 mesh sieve.
7. The antibacterial and breathable sportswear functional fabric according to claim 1, characterized in that, The blocked isocyanate crosslinking agent is formed by mixing blocked hexamethylene diisocyanate trimer with deionized water at a mass ratio of 1:(0.8-1.5).
8. A method for preparing an antibacterial and breathable functional fabric for sportswear, characterized in that, The preparation method includes the following steps: S1, add waterborne polyurethane emulsion to deionized water, stir evenly, then add synergistic modified mesoporous silica, L-arginine and blocked isocyanate crosslinking agent in sequence, and continue stirring to obtain finishing solution; S2, the polyester knitted fabric is immersed in the finishing solution of the step, and the finished fabric is obtained after padding. S3 involves pre-drying, baking, and cooling the finished fabric in sequence to obtain an antibacterial and breathable sportswear functional fabric.
9. The method for preparing an antibacterial and breathable sportswear functional fabric according to claim 8, characterized in that, The reaction conditions for step S1 are: a stirring speed of 300-600 r / min, a stirring time of 30-60 min, and the finishing solution is adjusted to a solid content of 5-12 wt%.
10. The method for preparing an antibacterial and breathable sportswear functional fabric according to claim 8, characterized in that, The reaction conditions for steps S2 and S3 are as follows: the rolling process is a two-dip two-roll process with a rolling rate of 70% to 85%; the pre-drying temperature is 80 to 100°C and the pre-drying time is 2 to 5 minutes; the baking temperature is 140 to 160°C and the baking time is 1 to 3 minutes, followed by cooling to room temperature.