A special ink for acetate textiles and its preparation method
By employing a three-stage composite dispersion stabilization system and pH buffering technology, the problems of low dyeing rate and poor color fastness of acetate fiber textiles have been solved, achieving efficient dyeing and excellent color fastness, improving wetting and printing continuity, and enhancing the overall performance of the ink.
Patent Information
- Application Number
- CN202611092104.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-22
- Publication Date
- 2026-11-17
AI Technical Summary
Existing digital printing inks are not suitable for acetate fiber textiles, and have problems such as low dyeing rate, poor color fastness, fiber damage due to pH mismatch, printing defects due to poor wetting properties, and easy nozzle clogging.
A three-stage composite dispersion and stabilization system is adopted, including sodium lignosulfonate, sodium naphthalenesulfonic acid-formaldehyde condensate and sodium polycarboxylate, combined with hydrophobically modified nano-silica and light stabilizers. Stabilization is achieved through hydrogen bonding and electrostatic repulsion. Combined with a pH buffer system, the pH value of the ink is precisely controlled, improving the dyeing rate and color fastness. Furthermore, the dye particle size and adhesion are improved through ultrafine dispersion and mechanical sand milling technology.
It significantly improves the dye uptake, rubbing fastness, and light fastness on acetate fibers, enhances wettability and printing continuity, and ensures fiber stability and environmental friendliness.
Smart Images

Figure CN123108964A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of ink preparation technology, and in particular to an ink for acetate textiles and its preparation method. Background Technology
[0002] Cellulose acetate fiber (hereinafter referred to as cellulose acetate fiber) is a semi-synthetic fiber made from cellulose through acetylation reaction. Its macromolecular chain contains abundant acetyl groups (ester groups), which endow the fiber with excellent silk-like luster, soft hand feel, good drape and moderate moisture absorption. It is widely used in high-end clothing fabrics, linings, ties, scarves and decorative textiles. In recent years, digital inkjet printing technology has gradually replaced traditional printing processes due to its advantages such as plateless printing, on-demand printing, high pattern precision, and low wastewater consumption. However, existing digital printing inks are mainly designed for cotton, polyester, and silk fibers, and their applicability to acetate fiber textiles is significantly insufficient. Acetate fibers have a glass transition temperature of approximately 180-190℃, making them quite sensitive to heat. Furthermore, their ester groups are prone to hydrolysis under alkaline conditions, leading to a decrease in fiber strength. Simultaneously, acetate fibers have a smooth surface and a low critical surface tension (approximately 35-40 mN / m), resulting in poor ink wettability and defects such as droplet retraction, edge smudging, and uneven penetration. Conventional disperse dye inks for polyester achieve only 50%-65% dye uptake on acetate fibers, and their lightfastness and rubbing fastness are generally low, with insufficient nozzle anti-skinning performance, making it difficult to meet the requirements of industrial production.
[0003] Existing technologies suffer from problems such as low dye uptake, poor color fastness, fiber damage due to pH mismatch, printing defects due to poor wettability, and easy nozzle clogging. To address these issues, we propose a special ink for acetate textiles and its preparation method. Summary of the Invention
[0004] The purpose of this invention is to address the shortcomings of existing technologies, such as low dyeing rate, poor color fastness, fiber damage due to pH mismatch, printing defects due to poor wettability, and easy nozzle clogging. Therefore, this invention proposes a special ink for acetate textiles and its preparation method.
[0005] This application provides a special ink for acetate textiles and its preparation method, which adopts the following technical solution: An ink for acetate textiles, comprising raw materials, wherein the raw materials include the following components in parts by weight: 3-12 parts disperse dye, 3-8 parts diethylene glycol, 2-8 parts glycerin, 2-6 parts sodium lignosulfonate, 2-6 parts butanediol, 1-5 parts polyethylene glycol, 1-5 parts sodium naphthalenesulfonic acid-formaldehyde condensate, 0.5-3 parts sodium polycarboxylate, 0.5-2 parts alkyl glycoside, 0.5-2 parts hydrophobically modified nano-silica, and light stabilizer. 0.3-1.5 parts of agent, 0.1-0.8 parts of fatty alcohol polyoxyethylene ether, 0.1-0.5 parts of sodium citrate, 0.1-0.5 parts of hydroxyethyl cellulose, 0.1-0.5 parts of polyether-modified polydimethylsiloxane, 0.1-0.5 parts of antioxidant, 0.05-0.3 parts of citric acid, 0.05-0.2 parts of disodium ethylenediaminetetraacetate, 0.02-0.1 parts of isothiazolinone, and deionized water to make up to 100 parts.
[0006] Further, the raw material comprises the following components in parts by weight: 4-10 parts disperse dye, 4-7 parts diethylene glycol, 3-7 parts glycerin, 3-5 parts sodium lignosulfonate, 3-5 parts butanediol, 2-4 parts polyethylene glycol, 2-4 parts sodium naphthalenesulfonic acid-formaldehyde condensate, 1-2.5 parts sodium polycarboxylate, 0.8-1.5 parts alkyl glycoside, 0.8-1.5 parts hydrophobically modified nano-silica, and 0 parts light stabilizer. 0.5-1 parts, fatty alcohol polyoxyethylene ether 0.2-0.6 parts, sodium citrate 0.2-0.4 parts, hydroxyethyl cellulose 0.2-0.4 parts, polyether modified polydimethylsiloxane 0.2-0.4 parts, antioxidant 0.2-0.4 parts, citric acid 0.1-0.2 parts, disodium ethylenediaminetetraacetate 0.1-0.15 parts, isothiazolinone 0.05-0.08 parts, deionized water to make up to 100 parts.
[0007] Further, the raw materials comprise the following components in parts by weight: 8 parts disperse dye, 6 parts diethylene glycol, 5 parts glycerin, 4 parts sodium lignosulfonate, 4 parts butanediol, 3 parts polyethylene glycol, 3 parts sodium naphthalenesulfonic acid-formaldehyde condensate, 2 parts sodium polycarboxylate, 1 part alkyl glycoside, 1 part hydrophobically modified nano silica, 0.8 parts light stabilizer, 0.4 parts fatty alcohol polyoxyethylene ether, 0.3 parts sodium citrate, 0.3 parts hydroxyethyl cellulose, 0.3 parts polyether-modified polydimethylsiloxane, 0.3 parts antioxidant, 0.15 parts citric acid, 0.12 parts disodium ethylenediaminetetraacetate, 0.06 parts isothiazolinone, and deionized water to make up to 100 parts.
[0008] This invention also proposes a method for preparing an acetate textile-specific ink, wherein the acetate textile-specific ink is the aforementioned acetate textile-specific ink, comprising the following steps: S1: Add deionized water to the pre-dispersion tank, and add chelating dispersant, preservative and pH buffer in sequence while stirring. Stir until completely dissolved to form a basic solution. S2: Add three dispersants in sequence, disperse evenly, then add alkyl glycosides, followed by four polyol humectants and dual penetration enhancers, and stir until uniform and transparent; S3: After ultrasonically pre-dispersing hydrophobically modified nano-silica in glycerol, add it to the system, and then add defoamer; S4: Add disperse dye, mix thoroughly, and then mechanically mill to initially reduce the dye particle size; S5: After preparing hydroxyethyl cellulose into an aqueous solution, slowly add it to the system and adjust the ink to the appropriate rheological properties; S6: Filter and ultrafine homogenize the obtained ink to obtain the finished special ink product.
[0009] Further, in step S1, the prescribed amount of deionized water is added to a pre-dispersion tank, and under stirring conditions of 200-400 rpm, disodium ethylenediaminetetraacetate, isothiazolinone, citric acid and sodium citrate are added in sequence, and stirring is continued until completely dissolved to form a uniform and transparent base solution.
[0010] Further, in step S2, sodium lignosulfonate, sodium naphthalenesulfonic acid-formaldehyde condensate, and sodium polycarboxylate are added sequentially under stirring, and the mixture is stirred and dispersed for 20-40 minutes to allow the dispersant to fully dissolve and self-polymerize to form a stable micelle structure; then alkyl glycosides are added, and stirring is continued for 10-20 minutes until homogeneous; subsequently, diethylene glycol, butanediol, polyethylene glycol, and glycerol are added sequentially, and the mixture is stirred until homogeneous and transparent; then fatty alcohol polyoxyethylene ether, light stabilizer, and antioxidant are added, and the mixture is stirred until completely dissolved. Sodium lignosulfonate, sodium naphthalenesulfonic acid-formaldehyde condensate, and sodium polycarboxylate are all sodium salt-type anionic surfactants / polymer dispersants that dissociate in water. Sodium lignosulfonate (R-SO3Na): ; Sodium naphthalenesulfonic acid-formaldehyde condensate (NNO, structural diagram): ; Sodium polycarboxylate (comb-like polymer, -COONa side chain): ; The three dispersant molecules contain a hydrophobic skeleton (aromatic ring / carbon chain) and a hydrophilic group (-SO3). - -COO - (e.g., phenolic hydroxyl groups), in aqueous solutions, when the concentration exceeds the critical micelle concentration (CMC), molecules spontaneously aggregate through hydrophobic interactions: Hydrophobic framework aggregates inward (avoiding polar water molecules) + hydrophilic groups face outward (extending towards the aqueous phase) → forming spherical or rod-shaped micelles; The disperse dye particles are encapsulated in the hydrophobic core of micelles, and the dye surface adsorbs a negatively charged dispersant layer, achieving electrostatic repulsion stability and steric hindrance stability. Diethylene glycol, butanediol, polyethylene glycol, glycerol, and water molecules form a complex solvent network through hydrogen bonds. ; Alkyl glycosides are nonionic surfactants that do not ionize in aqueous solutions. They rely on their hydrophilic glycosylation heads (multiple -OH groups) and hydrophobic alkyl tails (C8-C14 carbon chains) to adsorb onto the surface of dye particles through hydrophobic interactions, thus aiding in wetting and dispersion.
[0011] Further, in step S3, the hydrophobic modified nano-silica of the formulation amount is pre-dispersed in an equal mass of glycerol and ultrasonically treated at a frequency of 20-40kHz and a power of 200-400W for 10-20 minutes to ensure uniform dispersion; then it is added to the system and stirred to mix evenly; subsequently, polyether modified polydimethylsiloxane defoamer is added.
[0012] Further, in step S4, the formulated amount of disperse dye is added under stirring, and the mixture is stirred and mixed thoroughly for 30-60 minutes. Then, it is mechanically milled 3-5 times, with zirconium oxide beads as the milling medium each time, with a particle size of 0.3-0.6 mm and a milling time of 1-2 hours each time, so that the dye particle size is initially reduced to below 500 nm.
[0013] Further, in step S5, hydroxyethyl cellulose is pre-prepared into an aqueous solution with a mass concentration of 2%, swollen for 4-6 hours, and then slowly added to the system under stirring, and stirring is continued for 20-30 minutes until homogeneous.
[0014] Further, in step S6, the ink obtained in step S5 is initially filtered through a 200-300 mesh stainless steel filter, and then subjected to ultra-fine dispersion homogenization 2-3 times in a 100-150MPa ultra-high pressure homogenizer, with the feed temperature controlled at 25-35℃, so that the dye particle size reaches 80-200nm; then it is finely filtered through a 0.22μm nanometer membrane, and the finished product of acetate textile special ink is obtained.
[0015] In summary, this application includes at least one of the following beneficial technical effects: 1. This solution utilizes a three-tiered composite dispersion and stabilization system—anionic-polymer-comb-like—composed of sodium lignosulfonate, sodium naphthalenesulfonic acid-formaldehyde condensate, and sodium polycarboxylate. Combined with the dispersing aid of alkyl glycosides, this system ensures uniform dispersion of disperse dye particles to the nanoscale (80-200 nm), achieving deep penetration into acetate fibers. Furthermore, low-energy disperse dyes (molecular weight 250-450) are selected, exhibiting high diffusion coefficients in the amorphous regions of acetate fibers, enabling efficient dyeing at relatively low temperatures (100-130℃). The synergistic effect of these components results in a dyeing rate of 88%-95%, a 30-40 percentage point improvement compared to conventional polyester disperse dye inks (55%-68%). 2. This method utilizes hydrophobically modified nano-silica (particle size 15~50nm, surface grafted with methyl hydrogen-containing siloxane groups) to form hydrogen bonds (bond energy approximately 15~25kJ / mol) with the ester groups on the surface of cellulose acetate fibers, constructing a nanoscale anchoring point network on the fiber surface, significantly improving ink adhesion and rubbing fastness; light stabilizer (2-(2H-benzotriazol-2-yl)-4,6-di-tert-pentylphenol) and antioxidant (2,6-di-tert-butylphenol) are also used. (p-cresol) forms a “UV shielding-free radical scavenging” synergistic protection system in a mass ratio of (3~5):1. The former absorbs 280~350nm UV light through an intramolecular excited-state proton transfer mechanism and converts it into heat energy. The latter blocks the auto-oxidation chain reaction of dye molecules by capturing free radicals. The double protection improves the light fastness by 1~2 grades. The synergistic effect of the two makes the rubbing fastness reach 4~5 grades, the washing fastness reach 4 grades, and the light fastness reach 4~5 grades. 3. This solution uses citric acid and sodium citrate to form a pH buffer system, precisely controlling the ink pH value within the range of 4.5~5.5, matching the ester group stability window (pH 3~6) of cellulose acetate fibers. This effectively avoids the hydrolytic degradation of ester groups under alkaline conditions, ensuring that the hand feel, luster, and strength of textiles do not diminish after printing. At the same time, the weakly acidic environment is conducive to the fixation of disperse dyes on cellulose acetate fibers. Combined with the three-stage composite dispersion system, it further improves the dyeing rate and color fastness.
[0016] This invention significantly improves dye dispersibility and dyeing rate through a three-stage composite dispersion system, and significantly enhances color fastness by combining nano-anchoring and anti-UV and anti-oxidation synergistic protection. The pH buffer system is precisely adapted to the characteristics of acetate fiber to avoid fiber damage. At the same time, the polyol gradient moisturizing and dual penetration promote and improve printing continuity and wetting spreadability. Furthermore, the chelation stabilization, anti-corrosion and antibacterial and defoaming functions enhance storage stability. While achieving excellent comprehensive performance, it reduces the emission of harmful substances and is green and environmentally friendly. Attached Figure Description
[0017] Figure 1 This is a flowchart illustrating a method for preparing an acetate textile ink according to the present invention. Detailed Implementation
[0018] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.
[0019] Example 1: Refer to Figure 1 An ink for acetate textiles, comprising raw materials, wherein the raw materials consist of the following components in parts by weight: 3 parts disperse dye, 3 parts diethylene glycol, 2 parts glycerin, 2 parts sodium lignosulfonate, 2 parts butanediol, 1 part polyethylene glycol, 1 part sodium naphthalenesulfonic acid-formaldehyde condensate, 0.5 parts sodium polycarboxylate, 0.5 parts alkyl glycoside, 0.5 parts hydrophobically modified nano silica, 0.3 parts light stabilizer, 0.1 parts fatty alcohol polyoxyethylene ether, 0.1 parts sodium citrate, 0.1 parts hydroxyethyl cellulose, 0.1 parts polyether-modified polydimethylsiloxane, 0.1 parts antioxidant, 0.05 parts citric acid, 0.05 parts disodium ethylenediaminetetraacetate, 0.02 parts isothiazolinone, and deionized water to make up to 100 parts.
[0020] This embodiment also proposes a method for preparing an acetate textile-specific ink, which is the above-mentioned acetate textile-specific ink, including the following steps: S1: Add deionized water to the pre-dispersion tank, and add chelating dispersant, preservative and pH buffer in sequence while stirring. Stir until completely dissolved to form a base solution. Add the formula amount of deionized water to the pre-dispersion tank, and add disodium ethylenediaminetetraacetate, isothiazolinone, citric acid and sodium citrate in sequence while stirring at 200 rpm. Continue stirring until completely dissolved to form a uniform and transparent base solution. S2: Add three dispersants sequentially, and after uniform dispersion, add alkyl glycosides, followed by four polyol humectants and a dual-penetration promoter. Stir until uniform and transparent. While stirring, add sodium lignosulfonate, sodium naphthalenesulfonic acid-formaldehyde condensate, and sodium polycarboxylate sequentially, and stir for 20 minutes to allow the dispersants to fully dissolve and self-polymerize to form a stable micelle structure. Then add alkyl glycosides and continue stirring for 10 minutes until uniform. Then add diethylene glycol, butanediol, polyethylene glycol, and glycerin sequentially, and stir until uniform and transparent. Finally, add fatty alcohol polyoxyethylene ether, light stabilizer, and antioxidant, and stir until completely dissolved. Sodium lignosulfonate, sodium naphthalenesulfonic acid-formaldehyde condensate, and sodium polycarboxylate are all sodium salt-type anionic surfactants / polymer dispersants that dissociate in water. Sodium lignosulfonate (R-SO3Na): ; Sodium naphthalenesulfonic acid-formaldehyde condensate (NNO, structural diagram): ; Sodium polycarboxylate (comb-like polymer, -COONa side chain): ; The three dispersant molecules contain a hydrophobic skeleton (aromatic ring / carbon chain) and a hydrophilic group (-SO3). - -COO - (e.g., phenolic hydroxyl groups), in aqueous solutions, when the concentration exceeds the critical micelle concentration (CMC), molecules spontaneously aggregate through hydrophobic interactions: Hydrophobic framework aggregates inward (avoiding polar water molecules) + hydrophilic groups face outward (extending towards the aqueous phase) → forming spherical or rod-shaped micelles; The disperse dye particles are encapsulated in the hydrophobic core of micelles, and the dye surface adsorbs a negatively charged dispersant layer, achieving electrostatic repulsion stability and steric hindrance stability. Diethylene glycol, butanediol, polyethylene glycol, glycerol, and water molecules form a complex solvent network through hydrogen bonds. ; Alkyl glycosides are nonionic surfactants that do not ionize in aqueous solutions. They adsorb onto the surface of dye particles through hydrophobic interactions by relying on their hydrophilic glycosyl heads (multiple -OH groups) and hydrophobic alkyl tails (C8-C14 carbon chains), thus aiding in wetting and dispersion. S3: After ultrasonically pre-dispersing the hydrophobic modified nano-silica in glycerol, add it to the system, then add the defoamer. The prescribed amount of hydrophobic modified nano-silica is pre-dispersed in an equal mass of glycerol and ultrasonically treated at 20kHz frequency and 200W power for 10 minutes to ensure uniform dispersion. Then add it to the system and stir to mix evenly. Subsequently, add the polyether modified polydimethylsiloxane defoamer. S4: Add disperse dye, mix thoroughly and then mechanically mill to initially reduce the dye particle size. Add the amount of disperse dye in the formula while stirring, mix thoroughly for 30 minutes, and then mechanically mill 4 times. Each time, the milling medium is zirconia beads with a particle size of 0.5 mm and each milling time is 1 hour to initially reduce the dye particle size to below 500 nm. S5: After preparing hydroxyethyl cellulose into an aqueous solution, slowly add it to the system and adjust the ink to the appropriate rheological properties. Prepare hydroxyethyl cellulose into an aqueous solution with a mass concentration of 2% in advance, swell for 4 hours, and then slowly add it to the system under stirring. Continue stirring for 20 minutes until uniform. S6: The obtained ink is filtered and ultra-fine homogenized to obtain the finished special ink. The ink obtained in S5 is initially filtered through a 200-mesh stainless steel filter, and then ultra-finely dispersed and homogenized three times in a 100MPa ultra-high pressure homogenizer. The feed temperature is controlled at 25℃ to make the dye particle size reach 80nm. Then it is finely filtered through a 0.22μm nanometer membrane and discharged to obtain the finished special ink for acetate textiles.
[0021] Example 2: Refer to Figure 1 An ink for acetate textiles, comprising raw materials, wherein the raw materials consist of the following components in parts by weight: 5 parts disperse dye, 4 parts diethylene glycol, 3 parts glycerin, 3 parts sodium lignosulfonate, 3 parts butanediol, 2 parts polyethylene glycol, 2 parts sodium naphthalenesulfonic acid-formaldehyde condensate, 1 part sodium polycarboxylate, 0.8 parts alkyl glycoside, 0.8 parts hydrophobically modified nano silica, 0.8 parts light stabilizer, 0.3 parts fatty alcohol polyoxyethylene ether, 0.2 parts sodium citrate, 0.2 parts hydroxyethyl cellulose, 0.2 parts polyether-modified polydimethylsiloxane, 0.2 parts antioxidant, 0.1 parts citric acid, 0.08 parts disodium ethylenediaminetetraacetate, 0.04 parts isothiazolinone, and deionized water to make up to 100 parts.
[0022] This embodiment also proposes a method for preparing an acetate textile-specific ink, which is the above-mentioned acetate textile-specific ink, including the following steps: S1: Add deionized water to the pre-dispersion tank, and add chelating dispersant, preservative and pH buffer in sequence while stirring. Stir until completely dissolved to form a basic solution. Add the formula amount of deionized water to the pre-dispersion tank, and add disodium ethylenediaminetetraacetate, isothiazolinone, citric acid and sodium citrate in sequence while stirring at 250 rpm. Continue stirring until completely dissolved to form a uniform and transparent basic solution. S2: Add three dispersants sequentially, and after uniform dispersion, add alkyl glycosides, followed by four polyol humectants and a dual-penetration promoter. Stir until uniform and transparent. While stirring, add sodium lignosulfonate, sodium naphthalenesulfonic acid-formaldehyde condensate, and sodium polycarboxylate sequentially, and stir for 25 minutes to allow the dispersants to fully dissolve and self-polymerize to form a stable micelle structure. Then add alkyl glycosides and continue stirring for 12 minutes until uniform. Then add diethylene glycol, butanediol, polyethylene glycol, and glycerin sequentially, and stir until uniform and transparent. Finally, add fatty alcohol polyoxyethylene ether, light stabilizer, and antioxidant, and stir until completely dissolved. Sodium lignosulfonate, sodium naphthalenesulfonic acid-formaldehyde condensate, and sodium polycarboxylate are all sodium salt-type anionic surfactants / polymer dispersants that dissociate in water. Sodium lignosulfonate (R-SO3Na): ; Sodium naphthalenesulfonic acid-formaldehyde condensate (NNO, structural diagram): ; Sodium polycarboxylate (comb-like polymer, -COONa side chain): ; The three dispersant molecules contain a hydrophobic skeleton (aromatic ring / carbon chain) and a hydrophilic group (-SO3). - -COO - (e.g., phenolic hydroxyl groups), in aqueous solutions, when the concentration exceeds the critical micelle concentration (CMC), molecules spontaneously aggregate through hydrophobic interactions: Hydrophobic framework aggregates inward (avoiding polar water molecules) + hydrophilic groups face outward (extending towards the aqueous phase) → forming spherical or rod-shaped micelles; The disperse dye particles are encapsulated in the hydrophobic core of micelles, and the dye surface adsorbs a negatively charged dispersant layer, achieving electrostatic repulsion stability and steric hindrance stability. Diethylene glycol, butanediol, polyethylene glycol, glycerol, and water molecules form a complex solvent network through hydrogen bonds. ; Alkyl glycosides are nonionic surfactants that do not ionize in aqueous solutions. They adsorb onto the surface of dye particles through hydrophobic interactions by relying on their hydrophilic glycosyl heads (multiple -OH groups) and hydrophobic alkyl tails (C8-C14 carbon chains), thus aiding in wetting and dispersion. S3: After ultrasonically pre-dispersing the hydrophobic modified nano-silica in glycerol, add it to the system, then add the defoamer. The prescribed amount of hydrophobic modified nano-silica is pre-dispersed in an equal mass of glycerol and ultrasonically treated at 25kHz frequency and 250W power for 12 minutes to ensure uniform dispersion. Then add it to the system and stir to mix evenly. Subsequently, add the polyether modified polydimethylsiloxane defoamer. S4: Add disperse dye, mix thoroughly, and then mechanically mill to initially reduce the dye particle size. Add the amount of disperse dye in the formula while stirring, mix thoroughly for 35 minutes, and then mechanically mill 4 times. Each time, the milling medium is zirconia beads with a particle size of 0.5 mm, and each milling time is 1.2 hours, so that the dye particle size is initially reduced to below 500 nm. S5: After preparing hydroxyethyl cellulose into an aqueous solution, slowly add it to the system and adjust the ink to the appropriate rheological properties. Prepare hydroxyethyl cellulose into an aqueous solution with a mass concentration of 2% and allow it to swell for 4.5 hours. Then, slowly add it to the system while stirring and continue stirring for 22 minutes until homogeneous. S6: The obtained ink is filtered and ultra-fine homogenized to obtain the finished special ink. The ink obtained in S5 is initially filtered through a 220-mesh stainless steel filter, and then ultra-finely dispersed and homogenized three times in a 110MPa ultra-high pressure homogenizer. The feed temperature is controlled at 28℃ to make the dye particle size reach 100nm. Then it is finely filtered through a 0.22μm nanometer membrane and discharged to obtain the finished special ink for acetate textiles.
[0023] Example 3: Refer to Figure 1 An ink for acetate textiles, comprising raw materials, the raw materials being composed of the following components in parts by weight: 8 parts disperse dye, 5 parts diethylene glycol, 4 parts glycerin, 4 parts sodium lignosulfonate, 4 parts butanediol, 3 parts polyethylene glycol, 3 parts sodium naphthalenesulfonic acid-formaldehyde condensate, 1.5 parts sodium polycarboxylate, 1 part alkyl glycoside, 1 part hydrophobically modified nano silica, 1 part light stabilizer, 0.5 parts fatty alcohol polyoxyethylene ether, 0.3 parts sodium citrate, 0.3 parts hydroxyethyl cellulose, 0.3 parts polyether-modified polydimethylsiloxane, 0.1-0.5 parts antioxidant, 0.15 parts citric acid, 0.1 parts disodium ethylenediaminetetraacetate, 0.06 parts isothiazolinone, and deionized water to make up to 100 parts.
[0024] This embodiment also proposes a method for preparing an acetate textile-specific ink, which is the above-mentioned acetate textile-specific ink, including the following steps: S1: Add deionized water to the pre-dispersion tank, and add chelating dispersant, preservative and pH buffer in sequence while stirring. Stir until completely dissolved to form a basic solution. Add the formula amount of deionized water to the pre-dispersion tank, and add disodium ethylenediaminetetraacetate, isothiazolinone, citric acid and sodium citrate in sequence while stirring at 300 rpm. Continue stirring until completely dissolved to form a uniform and transparent basic solution. S2: Add three dispersants sequentially, and after uniform dispersion, add alkyl glycosides, followed by four polyol humectants and a dual-penetration promoter. Stir until uniform and transparent. While stirring, add sodium lignosulfonate, sodium naphthalenesulfonic acid-formaldehyde condensate, and sodium polycarboxylate sequentially, and stir for 30 minutes to allow the dispersants to fully dissolve and self-polymerize to form a stable micelle structure. Then add alkyl glycosides and continue stirring for 14 minutes until uniform. Then add diethylene glycol, butanediol, polyethylene glycol, and glycerin sequentially, and stir until uniform and transparent. Finally, add fatty alcohol polyoxyethylene ether, light stabilizer, and antioxidant, and stir until completely dissolved. Sodium lignosulfonate, sodium naphthalenesulfonic acid-formaldehyde condensate, and sodium polycarboxylate are all sodium salt-type anionic surfactants / polymer dispersants that dissociate in water. Sodium lignosulfonate (R-SO3Na): ; Sodium naphthalenesulfonic acid-formaldehyde condensate (NNO, structural diagram): ; Sodium polycarboxylate (comb-like polymer, -COONa side chain): ; The three dispersant molecules contain a hydrophobic skeleton (aromatic ring / carbon chain) and a hydrophilic group (-SO3). - -COO - (e.g., phenolic hydroxyl groups), in aqueous solutions, when the concentration exceeds the critical micelle concentration (CMC), molecules spontaneously aggregate through hydrophobic interactions: Hydrophobic framework aggregates inward (avoiding polar water molecules) + hydrophilic groups face outward (extending towards the aqueous phase) → forming spherical or rod-shaped micelles; The disperse dye particles are encapsulated in the hydrophobic core of micelles, and the dye surface adsorbs a negatively charged dispersant layer, achieving electrostatic repulsion stability and steric hindrance stability. Diethylene glycol, butanediol, polyethylene glycol, glycerol, and water molecules form a complex solvent network through hydrogen bonds. ; Alkyl glycosides are nonionic surfactants that do not ionize in aqueous solutions. They adsorb onto the surface of dye particles through hydrophobic interactions by relying on their hydrophilic glycosyl heads (multiple -OH groups) and hydrophobic alkyl tails (C8-C14 carbon chains), thus aiding in wetting and dispersion. S3: After ultrasonically pre-dispersing the hydrophobic modified nano-silica in glycerol, add it to the system, then add the defoamer. The prescribed amount of hydrophobic modified nano-silica is pre-dispersed in an equal mass of glycerol and ultrasonically treated at 30kHz frequency and 300W power for 14 minutes to ensure uniform dispersion. Then add it to the system and stir to mix evenly. Subsequently, add the polyether modified polydimethylsiloxane defoamer. S4: Add disperse dye, mix thoroughly, and then mechanically mill to initially reduce the dye particle size. Add the amount of disperse dye in the formula while stirring, mix thoroughly for 40 minutes, and then mechanically mill 4 times. Each time, the milling medium is zirconia beads with a particle size of 0.5 mm, and each milling time is 1.5 h, so that the dye particle size is initially reduced to below 500 nm. S5: After preparing hydroxyethyl cellulose into an aqueous solution, slowly add it to the system and adjust the ink to the appropriate rheological properties. Prepare hydroxyethyl cellulose into an aqueous solution with a mass concentration of 2% and let it swell for 5 hours. Then, slowly add it to the system while stirring and continue stirring for 25 minutes until uniform. S6: The obtained ink is filtered and ultra-fine homogenized to obtain the finished special ink. The ink obtained in S5 is initially filtered through a 250-mesh stainless steel filter, and then ultra-finely dispersed and homogenized three times in a 120MPa ultra-high pressure homogenizer. The feed temperature is controlled at 30℃ to make the dye particle size reach 130nm. Then it is finely filtered through a 0.22μm nanometer membrane and discharged to obtain the finished special ink for acetate textiles.
[0025] Example 4: Refer to Figure 1 An ink for acetate textiles, comprising raw materials, the raw materials being composed of the following components in parts by weight: 10 parts disperse dye, 7 parts diethylene glycol, 7 parts glycerin, 5 parts sodium lignosulfonate, 5 parts butanediol, 4 parts polyethylene glycol, 4 parts sodium naphthalenesulfonic acid-formaldehyde condensate, 2 parts sodium polycarboxylate, 1.5 parts alkyl glycoside, 1.5 parts hydrophobically modified nano silica, 1.2 parts light stabilizer, 0.7 parts fatty alcohol polyoxyethylene ether, 0.4 parts sodium citrate, 0.4 parts hydroxyethyl cellulose, 0.4 parts polyether-modified polydimethylsiloxane, 0.4 parts antioxidant, 0.2 parts citric acid, 0.15 parts disodium ethylenediaminetetraacetate, 0.08 parts isothiazolinone, and deionized water to make up to 100 parts.
[0026] This embodiment also proposes a method for preparing an acetate textile-specific ink, which is the above-mentioned acetate textile-specific ink, including the following steps: S1: Add deionized water to the pre-dispersion tank, and add chelating dispersant, preservative and pH buffer in sequence while stirring. Stir until completely dissolved to form a basic solution. Add the formula amount of deionized water to the pre-dispersion tank, and add disodium ethylenediaminetetraacetate, isothiazolinone, citric acid and sodium citrate in sequence while stirring at 350 rpm. Continue stirring until completely dissolved to form a uniform and transparent basic solution. S2: Add three dispersants sequentially, and after uniform dispersion, add alkyl glycosides, followed by four polyol humectants and a dual-penetration promoter. Stir until uniform and transparent. While stirring, add sodium lignosulfonate, sodium naphthalenesulfonic acid-formaldehyde condensate, and sodium polycarboxylate sequentially, and stir for 35 minutes to allow the dispersants to fully dissolve and self-polymerize to form a stable micelle structure. Then add alkyl glycosides and continue stirring for 18 minutes until uniform. Then add diethylene glycol, butanediol, polyethylene glycol, and glycerin sequentially, and stir until uniform and transparent. Finally, add fatty alcohol polyoxyethylene ether, light stabilizer, and antioxidant, and stir until completely dissolved. Sodium lignosulfonate, sodium naphthalenesulfonic acid-formaldehyde condensate, and sodium polycarboxylate are all sodium salt-type anionic surfactants / polymer dispersants that dissociate in water. Sodium lignosulfonate (R-SO3Na): ; Sodium naphthalenesulfonic acid-formaldehyde condensate (NNO, structural diagram): ; Sodium polycarboxylate (comb-like polymer, -COONa side chain): ; The three dispersant molecules contain a hydrophobic skeleton (aromatic ring / carbon chain) and a hydrophilic group (-SO3). - -COO - (e.g., phenolic hydroxyl groups), in aqueous solutions, when the concentration exceeds the critical micelle concentration (CMC), molecules spontaneously aggregate through hydrophobic interactions: Hydrophobic framework aggregates inward (avoiding polar water molecules) + hydrophilic groups face outward (extending towards the aqueous phase) → forming spherical or rod-shaped micelles; The disperse dye particles are encapsulated in the hydrophobic core of micelles, and the dye surface adsorbs a negatively charged dispersant layer, achieving electrostatic repulsion stability and steric hindrance stability. Diethylene glycol, butanediol, polyethylene glycol, glycerol, and water molecules form a complex solvent network through hydrogen bonds. ; Alkyl glycosides are nonionic surfactants that do not ionize in aqueous solutions. They adsorb onto the surface of dye particles through hydrophobic interactions by relying on their hydrophilic glycosyl heads (multiple -OH groups) and hydrophobic alkyl tails (C8-C14 carbon chains), thus aiding in wetting and dispersion. S3: After ultrasonically pre-dispersing the hydrophobic modified nano-silica in glycerol, add it to the system, then add the defoamer. The prescribed amount of hydrophobic modified nano-silica is pre-dispersed in an equal mass of glycerol and ultrasonically treated at 35kHz frequency and 350W power for 18 minutes to ensure uniform dispersion. Then add it to the system and stir to mix evenly. Subsequently, add the polyether modified polydimethylsiloxane defoamer. S4: Add disperse dye, mix thoroughly, and then mechanically mill to initially reduce the dye particle size. Add the amount of disperse dye in the formula while stirring, mix thoroughly for 50 minutes, and then mechanically mill 4 times. Each time, the milling medium is zirconia beads with a particle size of 0.5 mm, and each milling time is 1.8 h, so that the dye particle size is initially reduced to below 500 nm. S5: After preparing hydroxyethyl cellulose into an aqueous solution, slowly add it to the system and adjust the ink to the appropriate rheological properties. Prepare hydroxyethyl cellulose into an aqueous solution with a mass concentration of 2% and allow it to swell for 5.5 hours. Then, slowly add it to the system while stirring and continue stirring for 28 minutes until homogeneous. S6: The obtained ink is filtered and ultra-fine homogenized to obtain the finished special ink. The ink obtained in S5 is initially filtered through a 280-mesh stainless steel filter, and then ultra-finely dispersed and homogenized three times in a 140MPa ultra-high pressure homogenizer. The feed temperature is controlled at 32℃ to make the dye particle size reach 180nm. Then it is finely filtered through a 0.22μm nanometer membrane and discharged to obtain the finished special ink for acetate textiles.
[0027] Example 5: Refer to Figure 1 An ink for acetate textiles, comprising raw materials, wherein the raw materials consist of the following components in parts by weight: 12 parts disperse dye, 8 parts diethylene glycol, 8 parts glycerin, 6 parts sodium lignosulfonate, 6 parts butanediol, 5 parts polyethylene glycol, 5 parts sodium naphthalenesulfonic acid-formaldehyde condensate, 3 parts sodium polycarboxylate, 2 parts alkyl glycoside, 2 parts hydrophobically modified nano silica, 1.5 parts light stabilizer, 0.8 parts fatty alcohol polyoxyethylene ether, 0.5 parts sodium citrate, 0.5 parts hydroxyethyl cellulose, 0.5 parts polyether-modified polydimethylsiloxane, 0.5 parts antioxidant, 0.3 parts citric acid, 0.2 parts disodium ethylenediaminetetraacetate, 0.1 parts isothiazolinone, and deionized water to make up to 100 parts.
[0028] This embodiment also proposes a method for preparing an acetate textile-specific ink, which is the above-mentioned acetate textile-specific ink, including the following steps: S1: Add deionized water to the pre-dispersion tank, and add chelating dispersant, preservative and pH buffer in sequence while stirring. Stir until completely dissolved to form a basic solution. Add the formula amount of deionized water to the pre-dispersion tank, and add disodium ethylenediaminetetraacetate, isothiazolinone, citric acid and sodium citrate in sequence while stirring at 400 rpm. Continue stirring until completely dissolved to form a uniform and transparent basic solution. S2: Add three dispersants sequentially, and after uniform dispersion, add alkyl glycosides, followed by four polyol humectants and a dual-penetration promoter. Stir until uniform and transparent. While stirring, add sodium lignosulfonate, sodium naphthalenesulfonic acid-formaldehyde condensate, and sodium polycarboxylate sequentially, and stir for 40 minutes to allow the dispersants to fully dissolve and self-polymerize to form a stable micelle structure. Then add alkyl glycosides and continue stirring for 20 minutes until uniform. Then add diethylene glycol, butanediol, polyethylene glycol, and glycerin sequentially, and stir until uniform and transparent. Finally, add fatty alcohol polyoxyethylene ether, light stabilizer, and antioxidant, and stir until completely dissolved. Sodium lignosulfonate, sodium naphthalenesulfonic acid-formaldehyde condensate, and sodium polycarboxylate are all sodium salt-type anionic surfactants / polymer dispersants that dissociate in water. Sodium lignosulfonate (R-SO3Na): ; Sodium naphthalenesulfonic acid-formaldehyde condensate (NNO, structural diagram): ; Sodium polycarboxylate (comb-like polymer, -COONa side chain): ; The three dispersant molecules contain a hydrophobic skeleton (aromatic ring / carbon chain) and a hydrophilic group (-SO3). - -COO - (e.g., phenolic hydroxyl groups), in aqueous solutions, when the concentration exceeds the critical micelle concentration (CMC), molecules spontaneously aggregate through hydrophobic interactions: Hydrophobic framework aggregates inward (avoiding polar water molecules) + hydrophilic groups face outward (extending towards the aqueous phase) → forming spherical or rod-shaped micelles; The disperse dye particles are encapsulated in the hydrophobic core of micelles, and the dye surface adsorbs a negatively charged dispersant layer, achieving electrostatic repulsion stability and steric hindrance stability. Diethylene glycol, butanediol, polyethylene glycol, glycerol, and water molecules form a complex solvent network through hydrogen bonds. ; Alkyl glycosides are nonionic surfactants that do not ionize in aqueous solutions. They adsorb onto the surface of dye particles through hydrophobic interactions by relying on their hydrophilic glycosyl heads (multiple -OH groups) and hydrophobic alkyl tails (C8-C14 carbon chains), thus aiding in wetting and dispersion. S3: After ultrasonically pre-dispersing the hydrophobic modified nano-silica in glycerol, add it to the system, then add the defoamer. The prescribed amount of hydrophobic modified nano-silica is pre-dispersed in an equal mass of glycerol and ultrasonically treated at 40kHz frequency and 400W power for 20 minutes to ensure uniform dispersion. Then add it to the system and stir to mix evenly. Subsequently, add the polyether modified polydimethylsiloxane defoamer. S4: Add disperse dye, mix thoroughly and then mechanically mill to initially reduce the dye particle size. Add the amount of disperse dye in the formula while stirring, mix thoroughly for 60 minutes, and then mechanically mill 4 times. Each time, the milling medium is zirconia beads with a particle size of 0.5 mm and each milling time is 2 hours to initially reduce the dye particle size to below 500 nm. S5: After preparing hydroxyethyl cellulose into an aqueous solution, slowly add it to the system and adjust the ink to the appropriate rheological properties. Prepare hydroxyethyl cellulose into an aqueous solution with a mass concentration of 2% and allow it to swell for 6 hours. Then, slowly add it to the system while stirring and continue stirring for 30 minutes until homogeneous. S6: The obtained ink is filtered and ultra-fine homogenized to obtain the finished special ink. The ink obtained in S5 is initially filtered through a 2300-mesh stainless steel filter, and then ultra-finely dispersed and homogenized three times in a 150MPa ultra-high pressure homogenizer. The feed temperature is controlled at 35℃ to make the dye particle size reach 200nm. Then it is finely filtered through a 0.22μm nanometer membrane and discharged to obtain the finished special ink for acetate textiles.
[0029] Comparative Example 1 (without nano-silica anchoring reinforcement) Referring to Example 1, the difference is that hydrophobically modified nano-silica is not added, while the other components and their contents remain unchanged.
[0030] Comparative Example 2 (Synthetic System without UV Protection and Antioxidant) Referring to Example 1, the difference is that no light stabilizer and antioxidant are added, while the other components and their contents remain unchanged.
[0031] Comparative Example 3 (Single dispersant replacing a three-stage composite dispersion system) Referring to Example 1, the difference is that sodium lignosulfonate, sodium naphthalenesulfonic acid-formaldehyde condensate, and sodium polycarboxylate are replaced with an equal amount of dispersant MF, and alkyl glycosides are removed, while the remaining components and their contents remain unchanged. Experimental Example I. Experimental Objective To verify the synergistic effect of the various functional modules of the present invention, the effects of removing hydrophobically modified nano-silica (Comparative Example 1), removing the anti-UV and antioxidant system (Comparative Example 2), and replacing the three-level composite dispersion system with a single dispersant (Comparative Example 3) on the overall performance of the ink were investigated, based on the ink prepared in Example 1.
[0032] II. Experiment Setup Four inks prepared in Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3 were used as test samples. Dyeing rate, rubbing fastness, washing fastness, light fastness, contact angle, nozzle clogging rate, and storage stability were tested under the same conditions. All tests were performed according to the corresponding national standards, and each test group was repeated three times, with the average value taken.
[0033] III. Test Results
[0034] IV. Test Report Comparative Example 1 (without nano-SiO2) showed a decrease in rubbing fastness from grade 4-5 to grade 3-4, an increase in contact angle from 24° to 42°, and an increase in nozzle clogging rate from 2.1% to 8.5%. This demonstrates that hydrophobic modified nano-silica significantly enhances color fastness through hydrogen bond anchoring, while also contributing to ink dispersion stability and printing smoothness. The light fastness of Comparative Example 2 (without UV antioxidant) decreased from level 4-5 to level 3, a decrease of 1.5 levels, proving that the "UV shielding-free radical scavenging" synergistic protection system composed of light stabilizer and antioxidant plays a decisive role in improving the light fastness of dyes; The dye uptake rate of Comparative Example 3 (single dispersant) decreased from 91.2% to 76.8%, the nozzle clogging rate increased from 2.1% to 15.8%, and the 90-day particle size change rate increased from 4.2% to 18.6%, demonstrating that the three-stage composite dispersion system composed of sodium lignosulfonate, sodium naphthalenesulfonic acid-formaldehyde condensate, sodium polycarboxylate, and alkyl glycoside has an irreplaceable synergistic effect on dye dispersion stability and dye uptake rate. In summary, the functional modules of this invention exhibit a significant synergistic effect. The absence of any module leads to a significant decrease in multiple performance indicators, with the decrease exceeding the mass percentage of that component in the system. This demonstrates that the overall technical solution of this invention has a non-obvious technical effect.
[0035] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A textile special ink for acetic acid, comprising raw materials, characterized in that: The raw materials consist of the following components in parts by weight: disperse dye 3-12 parts, diethylene glycol 3-8 parts, glycerin 2-8 parts, sodium lignosulfonate 2-6 parts, butanediol 2-6 parts, polyethylene glycol 1-5 parts, sodium naphthalenesulfonic acid-formaldehyde condensate 1-5 parts, sodium polycarboxylate 0.5-3 parts, alkyl glycoside 0.5-2 parts, hydrophobically modified nano-silica 0.5-2 parts, and light stabilizer 0.3-1.5 parts. 0.1-0.8 parts of fatty alcohol polyoxyethylene ether, 0.1-0.5 parts of sodium citrate, 0.1-0.5 parts of hydroxyethyl cellulose, 0.1-0.5 parts of polyether-modified polydimethylsiloxane, 0.1-0.5 parts of antioxidant, 0.05-0.3 parts of citric acid, 0.05-0.2 parts of disodium ethylenediaminetetraacetate, 0.02-0.1 parts of isothiazolinone, and deionized water to make up to 100 parts.
2. The acetate textile ink according to claim 1, characterized in that: The raw materials consist of the following components in parts by weight: disperse dye 4-10 parts, diethylene glycol 4-7 parts, glycerin 3-7 parts, sodium lignosulfonate 3-5 parts, butanediol 3-5 parts, polyethylene glycol 2-4 parts, sodium naphthalenesulfonic acid-formaldehyde condensate 2-4 parts, sodium polycarboxylate 1-2.5 parts, alkyl glycoside 0.8-1.5 parts, hydrophobically modified nano-silica 0.8-1.5 parts, and light stabilizer 0.5- 1 part, fatty alcohol polyoxyethylene ether 0.2-0.6 parts, sodium citrate 0.2-0.4 parts, hydroxyethyl cellulose 0.2-0.4 parts, polyether modified polydimethylsiloxane 0.2-0.4 parts, antioxidant 0.2-0.4 parts, citric acid 0.1-0.2 parts, disodium ethylenediaminetetraacetate 0.1-0.15 parts, isothiazolinone 0.05-0.08 parts, deionized water to make up to 100 parts.
3. The acetate textile ink according to claim 2, characterized in that: The raw materials consist of the following components in parts by weight: 8 parts disperse dye, 6 parts diethylene glycol, 5 parts glycerin, 4 parts sodium lignosulfonate, 4 parts butanediol, 3 parts polyethylene glycol, 3 parts sodium naphthalenesulfonic acid-formaldehyde condensate, 2 parts sodium polycarboxylate, 1 part alkyl glycoside, 1 part hydrophobically modified nano silica, 0.8 parts light stabilizer, 0.4 parts fatty alcohol polyoxyethylene ether, 0.3 parts sodium citrate, 0.3 parts hydroxyethyl cellulose, 0.3 parts polyether-modified polydimethylsiloxane, 0.3 parts antioxidant, 0.15 parts citric acid, 0.12 parts disodium ethylenediaminetetraacetate, 0.06 parts isothiazolinone, and deionized water to make up to 100 parts.
4. A method for preparing an acetate textile ink, wherein the acetate textile ink is the acetate textile ink according to any one of claims 1-3, characterized in that: Includes the following steps: S1: Add deionized water to the pre-dispersion tank, and add chelating dispersant, preservative and pH buffer in sequence while stirring. Stir until completely dissolved to form a basic solution. S2: Add three dispersants in sequence, disperse evenly, then add alkyl glycosides, followed by four polyol humectants and dual penetration enhancers, and stir until uniform and transparent; S3: After ultrasonically pre-dispersing hydrophobically modified nano-silica in glycerol, add it to the system, and then add defoamer; S4: Add disperse dye, mix thoroughly, and then mechanically mill to initially reduce the dye particle size; S5: After preparing hydroxyethyl cellulose into an aqueous solution, slowly add it to the system and adjust the ink to the appropriate rheological properties; S6: Filter and ultrafine homogenize the obtained ink to obtain the finished special ink product.
5. The method for preparing an acetate textile ink according to claim 4, characterized in that: In step S1, the prescribed amount of deionized water is added to a pre-dispersion tank, and under stirring conditions of 200-400 rpm, disodium ethylenediaminetetraacetate, isothiazolinone, citric acid and sodium citrate are added in sequence, and stirring is continued until completely dissolved to form a uniform and transparent base solution.
6. The method for preparing an acetate textile ink according to claim 5, characterized in that: In step S2, sodium lignosulfonate, sodium naphthalenesulfonic acid-formaldehyde condensate, and sodium polycarboxylate are added sequentially under stirring. The mixture is stirred and dispersed for 20-40 minutes to allow the dispersant to fully dissolve and self-polymerize to form a stable micelle structure. Then, alkyl glycosides are added, and stirring is continued for 10-20 minutes until homogeneous. Subsequently, diethylene glycol, butanediol, polyethylene glycol, and glycerol are added sequentially, and the mixture is stirred until homogeneous and transparent. Finally, fatty alcohol polyoxyethylene ether, light stabilizer, and antioxidant are added, and the mixture is stirred until completely dissolved. Sodium lignosulfonate, sodium naphthalenesulfonic acid-formaldehyde condensate, and sodium polycarboxylate are all sodium salt-type anionic surfactants / polymer dispersants that dissociate in water. Sodium lignosulfonate: ; Sodium salt of naphthalenesulfonic acid-formaldehyde condensate: ; Sodium polycarboxylate: ; The three dispersant molecules contain a hydrophobic framework and hydrophilic groups. In aqueous solution, when the concentration exceeds the critical micelle concentration, the molecules spontaneously aggregate through hydrophobic interactions. Hydrophobic framework aggregates inward + hydrophilic groups face outward → forming spherical or rod-shaped micelles; The disperse dye particles are encapsulated in the hydrophobic core of micelles, and the dye surface adsorbs a negatively charged dispersant layer, achieving electrostatic repulsion stability and steric hindrance stability. Diethylene glycol, butanediol, polyethylene glycol, glycerol, and water molecules form a complex solvent network through hydrogen bonds. ; Alkyl glycosides are nonionic surfactants that do not ionize in aqueous solutions. They adsorb onto the surface of dye particles through hydrophobic interactions, relying on their hydrophilic glycosylation head and hydrophobic alkyl tail, thus aiding in wetting and dispersion.
7. The method for preparing an acetate textile ink according to claim 6, characterized in that: In step S3, the hydrophobic modified nano silica of the formulation amount is pre-dispersed in an equal mass of glycerol and ultrasonically treated for 10-20 minutes at a frequency of 20-40kHz and a power of 200-400W to ensure uniform dispersion; then it is added to the system and stirred until uniformly mixed; subsequently, polyether modified polydimethylsiloxane defoamer is added.
8. The method for preparing an acetate textile ink according to claim 7, characterized in that: In step S4, the formulated amount of disperse dye is added under stirring, and the mixture is stirred and mixed thoroughly for 30-60 minutes. Then, it is mechanically milled 3-5 times, with zirconium oxide beads as the milling medium each time, with a particle size of 0.3-0.6 mm and a milling time of 1-2 hours each time, so that the dye particle size is initially reduced to below 500 nm.
9. The method for preparing an acetate textile ink according to claim 8, characterized in that: In step S5, hydroxyethyl cellulose is pre-prepared into an aqueous solution with a mass concentration of 2%, and after swelling for 4-6 hours, it is slowly added to the system under stirring, and stirring is continued for 20-30 minutes until homogeneous.
10. The method for preparing an acetate textile ink according to claim 9, characterized in that: In step S6, the ink obtained in step S5 is initially filtered through a 200-300 mesh stainless steel filter, and then subjected to ultra-fine dispersion homogenization 2-3 times in a 100-150MPa ultra-high pressure homogenizer, with the feed temperature controlled at 25-35℃, so that the dye particle size reaches 80-200nm; then it is finely filtered through a 0.22μm nanometer membrane, and the finished product of acetate textile special ink is obtained.