A high-efficiency, water-saving, atmospheric pressure dyeing process for polyester utilizing a microbubble system.
By combining a microbubble system with Janus nanoparticles, efficient polyester dyeing at normal pressure and low temperature is achieved, solving the problems of high energy consumption and poor stability of microemulsions in high-temperature and high-pressure dyeing. This also enables the carrier to be recycled and improves the dyeing quality.
Patent Information
- Application Number
- CN202610961054.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-30
- Publication Date
- 2026-11-17
AI Technical Summary
Existing polyester dyeing processes are carried out under high temperature and high pressure, which leads to high energy consumption, dye migration and decreased light fastness. At the same time, the addition of organic carriers at low temperatures poses toxicity and environmental problems. Microemulsion systems have poor stability and low reproducibility, and foam dyeing has limited dyeing depth for disperse dyes.
A microbubble system is employed, utilizing Janus nanoparticles to stabilize CO2 microbubbles. Combined with temperature-sensitive polymers and magnetic response, low-temperature dyeing under normal pressure is achieved. Janus nanoparticles are anchored on the fiber surface and form dye-enriched microregions. The CO2 dissolution-diffusion mechanism plasticizes the fiber, and the particles are recovered during post-processing through air flotation and magnetic separation.
It achieves efficient dyeing at 75~85℃, reduces the use of chemical auxiliaries, lowers emissions and water change frequency, improves dye uptake and dyeing quality, enhances the dyeing depth, and has wide applicability.
Smart Images

Figure CN123108965A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of textile chemical dyeing and finishing technology, specifically to a high-efficiency, water-saving, atmospheric pressure dyeing process for polyester utilizing a microbubble system. Background Technology
[0002] Due to its highly crystalline molecular structure and lack of hydrophilic groups, polyester (PET) fabrics require conventional dyeing under high temperature and high pressure conditions. Traditional processes typically employ high-temperature and high-pressure dyeing above 130°C to increase the solubility and diffusion rate of dye molecules, thereby achieving coloring of the fiber. This high-temperature and high-pressure dyeing method consumes a lot of energy and may cause dye migration during high-temperature setting, leading to a decrease in the lightfastness and weather fastness of the finished product. Meanwhile, to improve the dyeing rate of polyester under low-temperature conditions, organic carriers such as phthalic anhydride and phenols are often added. Although a certain dyeing effect can be achieved at around 100°C, these carrier compounds generally have problems such as high toxicity, strong residual odor, and environmental unfriendliness. For example, commonly used aromatic esters or phenolic ethers not only may harm the health of operators, but also require cumbersome reduction washing after dyeing to remove residues, increasing the burden on wastewater treatment.
[0003] To overcome the above shortcomings, improved methods such as microemulsion carrier method and anhydrous or low-aqueous medium dyeing have been proposed in recent years. For example, CN121450126A discloses a nanocellulose colorant based on D5 medium reverse micelle dyeing and its preparation method. The method includes: adding decamethylcyclopentasiloxane solvent and reactive dye solution containing pH stabilizer sequentially to a system containing nonionic surfactant and cosolvent, and forming a reverse micelle microemulsion by high-speed homogenization; adding nanocellulose to the microemulsion and reacting at 25~70℃ to covalently bind the reactive dye with the cellulose hydroxyl groups; after the reaction, solid-liquid separation, solvent recovery by vacuum distillation, and washing and drying of the solid product to obtain the colorant. This method employs polyether ester nonionic surfactants, linear fatty alcohol co-solvents, and carbonate / bicarbonate buffers. The dyeing process allows for segmented temperature control to improve fixation efficiency, achieving a solvent recovery rate ≥98%, a dye uptake rate ≥95%, and lightfastness ≥6. CN109695163A discloses a method for dyeing cellulose fibers with reactive dyes in a low-water medium. This method includes three processes: preparation of the dyeing solution, low-water medium dyeing of cellulose fiber yarns, and rapid separation and reuse of the medium. This low-water medium dyeing method for cellulose fibers achieves low-salt and low-water dyeing, effectively solving the problems of high water consumption, high wastewater discharge, and high salt content in wastewater associated with traditional reactive dye water bath dyeing. Compared with traditional water bath dyeing, it saves more than 60% of water consumption, reduces the use of sodium sulfate and soda ash by more than 60%, and increases dye utilization by 5%~15%. The fastness of the dyed yarn reaches 3~4, comparable to that of yarn dyed using conventional water bath dyeing. However, conventional microemulsion systems have stringent requirements for emulsification processes, poor stability, low reproducibility, and surfactant residues lead to washing difficulties and increased environmental impact. Existing foam dyeing is only suitable for surface coloring, with limited improvement in the dyeing depth of disperse dyes, and foaming agent residues affect the feel and require additional cleaning.
[0004] In summary, how to innovate a new process that can efficiently dye polyester under normal pressure and low temperature conditions, and make the process have both carrier-assisted dyeing effect and recyclability, has become an urgent technical problem to be solved in this field. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a high-efficiency, water-saving polyester atmospheric pressure dyeing process using a microbubble system, so as to solve the technical problems in the prior art such as process efficiency and energy consumption bottlenecks, carrier performance limitations, and insufficient stability and reproducibility of microemulsions.
[0006] The specific technical solution is as follows: A highly efficient, water-saving, atmospheric pressure dyeing process for polyester utilizing a microbubble system includes pretreatment, dyeing medium construction, dyeing accelerator, and posttreatment. The pretreatment includes preparing Janus nanoparticles. These particles have Fe3O4@carbon as their magnetic core, with hydrophobic polydimethylsiloxane and hydrophilic polyethylene glycol grafted onto their surfaces, and are modified with a thermosensitive polymer, poly(N-isopropylacrylamide) (PNIPAM), on the hydrophobic side. The dyeing medium construction involves adding the Janus nanoparticles and disperse dye to water, then introducing CO2 to form a CO2 microbubble dispersion system stabilized by the Janus nanoparticles. The dyeing accelerator involves immersing polyester fabric in the dispersion system, and within a temperature range of 32-35°C, utilizing the reversible phase transition of the thermosensitive polymer to anchor the particles to the fiber surface, while simultaneously using the dissolution-diffusion mechanism of CO2 to plasticize the polyester fibers. The posttreatment involves inducing particle desorption through cooling, combined with a synergistic recovery technology of air flotation and magnetic separation to achieve a closed-loop recycling of the fabric and particles.
[0007] A high-efficiency, water-saving, atmospheric pressure dyeing process for polyester utilizing a microbubble system includes the following steps: S1: FeCl3·6H2O was dissolved in ethylene glycol and anhydrous sodium acetate was added for a thermal reaction. Fe3O4 magnetic nanospheres were obtained by magnetic separation and washing. The nanospheres were placed in a tube furnace and heated under nitrogen protection. Acetylene gas was then introduced to coat the nanospheres with carbon, forming a carbon shell, resulting in Fe3O4@carbon magnetic cores. The magnetic cores were added to molten paraffin and deionized water, and Tween 80 was added. After low-speed shear emulsification, the pH was adjusted to 7.5, and stirring was continued to slow down the adsorption. The temperature was then lowered to 25°C to solidify the paraffin. Magnetic separation was performed, and the nanospheres were washed three times with deionized water to obtain a one-sided buried intermediate. The intermediate was dispersed in n-heptane, and polydimethylsiloxane was added. An oxoalkyl-methacrylate and a photoinitiator were cured under UV light, followed by magnetic separation and washing to obtain a one-sided hydrophobically modified intermediate. This one-sided hydrophobically modified intermediate was dispersed in anhydrous toluene, and a brominated silane initiator and triethylamine were added. After reacting at room temperature, the mixture was magnetically separated and washed with toluene. Subsequently, it was dispersed in a mixed solution of deoxygenated water and ethanol, and copper bromide, N,N,N',N'',N''-pentamethyldiethylenetriamine (PMDETA), and N-isopropylacrylamide (NIPAM) monomer were added. The reaction was carried out under nitrogen protection, followed by magnetic separation and washing to obtain a one-sided hydrophobic N-isopropylacrylamide (PNIPAM) intermediate. The one-sided hydrophobic NIPAM intermediate was dispersed in petroleum ether and ultrasonically cleaned, repeated three times to remove paraffin, followed by magnetic separation and washing to obtain the Janus precursor. The precursor was plasma-treated and then oxidized in air for 30 minutes to introduce carboxyl groups. It was then dispersed in a mixed solution of ethanol and water. Polyethylene glycol-amino, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (EDC) and N-hydroxysuccinimide (NHS) were added to react. After the reaction was completed, the mixture was magnetically separated and washed to obtain Janus nanoparticles.
[0008] S2: Add Disperse Blue 56 and Janus nanoparticles to deionized water and stir to disperse them to obtain a dye solution; pump the dye solution into a dyeing kettle equipped with a microporous ceramic pulse aerator, heat it up and introduce CO2 to form a stable bubble system.
[0009] S3: Immerse the polyester fabric in the foam stabilization system to ensure that the fabric is completely wetted and evenly distributed in the dye liquor; heat to the PNIPAM phase transition temperature range and hold to ensure sufficient phase transition. Then, control the heating rate and continue to heat to the dyeing temperature and hold for dyeing. During this process, the hydrophobic side of Janus nanoparticles collapses and is exposed and anchored to the surface of polyester fibers, forming dye-enriched micro-regions. At the same time, CO2 plasticizes the amorphous region of the fiber through the dissolution-diffusion mechanism, promoting dye diffusion and dyeing.
[0010] S4: After dyeing, the dyed fabric is removed from the dyeing kettle, rinsed with deionized water at room temperature, and then dehydrated and dried to obtain the finished dyed fabric. The remaining dye liquor in the dyeing kettle is allowed to cool naturally, stirring is stopped and the mixture is allowed to stand. The overflow is collected and mechanically defoamed to obtain primary recovered particles. The dye liquor is passed through a high-gradient magnetic filter to capture residual particles to obtain secondary recovered particles. The combined particles are ultrasonically cleaned with ethanol and deionized water, magnetically separated, and reused. The dye liquor is recycled to the next batch.
[0011] Further, in S1, the solution is dissolved in ethylene glycol and anhydrous sodium acetate is added, with a mass ratio of (15:35) to 1; the polydimethylsiloxane-methacrylate has a mass percentage of 3 to 7 wt%; the photoinitiator has a mass percentage of 0.5 to 3 wt%; the plasma treatment has a treatment power of 40 to 60 W and a treatment time of 2 to 4 minutes; and the polyethylene glycol-amino has a mass percentage of 3 to 7 wt%.
[0012] Furthermore, in step S2, the CO2 is introduced at a pressure of 0.6~0.8MPa; the aeration conditions are set as follows: pulse frequency 0.1~0.3Hz, gas flow rate 1.5~2.5L / min, and aeration time 10~20 minutes.
[0013] Furthermore, in step S3, the temperature is raised to the PNIPAM phase transition temperature range and held at that temperature. The heating rate is 1~3℃ / min, the phase transition temperature range is 30~35℃, and the holding time is 5~10 minutes. The heating rate is controlled to be 0.3~0.8℃ / min. The temperature is raised to the dyeing temperature and held at that temperature for dyeing. The dyeing temperature range is 75~85℃, and the holding time is 30~50 minutes.
[0014] Furthermore, in step S4, the natural cooling process requires the temperature to drop to 35-45°C; the standing time after stopping stirring is 10-20 minutes; the flow rate of the dye solution through the high-gradient magnetic filter is 1-3 cm / s; and the ultrasonic cleaning process takes 5-15 minutes.
[0015] Compared with the prior art, the present invention has the following beneficial effects: (1) Normal pressure, low temperature, and high efficiency dyeing: By utilizing the plasticizing effect of CO2 dissolution-diffusion mechanism on fibers and the dye enrichment microenvironment constructed by Janus nanoparticles on the fiber surface, this invention can achieve a dyeing effect close to high temperature dyeing at medium and low temperatures of 75~85℃.
[0016] (2) The carrier is recyclable, saving water and reducing emissions: Janus nanoparticles do not undergo chemical consumption during the entire dyeing process and can be completely recovered through temperature-sensitive and magnetic responses for reuse in subsequent dyeing cycles. At the same time, since the dye is almost completely absorbed by the fiber and there are no difficult-to-remove chemical auxiliaries, the dye liquor can be directly replenished for continued use, which greatly reduces emissions and the frequency of water changes.
[0017] (3) Good stability and high reproducibility: The Janus nanoparticle foam stabilization system is more stable than traditional surfactant emulsion systems. The particles are insoluble and strongly adsorbed at the bubble interface, avoiding rapid foam collapse and making the dye transfer process continuous and controllable. At the same time, temperature-triggered particle destabilization enables on-demand defoaming.
[0018] (4) Improved dyeing quality: As Janus nanoparticles are oriented to adsorb on the fiber surface, forming a nanoscale dye enrichment area, the dyeing driving force is effectively improved, and the dyeing saturation and deep dyeing ability are significantly enhanced.
[0019] (5) Broad applicability: The thermosensitive polymer PNIPAM selected in this invention has a phase transition temperature of about 32°C, which is consistent with the commonly used temperature range for polyester dyeing and can be applied to other textile dyeing processes with similar temperature ranges. Attached Figure Description
[0020] Figure 1 This is a flowchart of a high-efficiency, water-saving polyester atmospheric pressure dyeing process utilizing a microbubble system, according to the present invention.
[0021] Figure 2 The following are electron microscopy and elemental distribution characterization images of Janus nanoparticles in Example 1 of the present invention: Figure A is an overall morphology image obtained by field emission high-resolution transmission electron microscopy; Figure B is a magnified view of a part obtained by high-resolution transmission electron microscopy; Figure C is an elemental distribution image obtained by scanning transmission electron microscopy-energy dispersive X-ray spectroscopy.
[0022] Figure 3 This is a comparison chart of the experimental results of staining rate, K / S value and migration rate in Experiment Example 1 of the present invention. Detailed Implementation
[0023] The following embodiments further explain and illustrate the technical solutions of the present invention. It should be specifically noted that each specific embodiment is a concretization and explanation of the technical solution and should not be considered as a limitation on the scope of protection of the present invention. Those skilled in the art still have the right to modify the technical solutions of these embodiments and make equivalent substitutions for some or all of the technical features, and these modifications or substitutions do not change the essence of the corresponding technical solutions, nor do they cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions described in the present invention.
[0024] This invention proposes a highly efficient, water-saving, atmospheric pressure dyeing process for polyester utilizing a microbubble system, such as... Figure 1 The diagram shows a flowchart of a high-efficiency, water-saving polyester atmospheric pressure dyeing process utilizing a microbubble system according to the present invention. The detailed preparation steps are as follows: 1. Synthesis of Janus nanoparticles Fe3O4 magnetic nanospheres were prepared by a solvothermal reaction and carbon-coated to obtain magnetic cores. The magnetic cores were emulsified with molten paraffin and deionized water at 60°C. Under shear stress, the paraffin was dispersed into micron-sized droplets, and the magnetic cores migrated to the paraffin-water interface and spontaneously adsorbed. Due to the suitable three-phase contact angle, the magnetic cores reached their lowest energy state at the interface, partially embedded in the surface of the paraffin droplets and partially exposed to the aqueous phase. After pH adjustment and stirring, adsorption equilibrium was achieved. Subsequently, cooling solidified the paraffin, fixing and embedding the magnetic cores within the paraffin, while the exposed portion faced outwards. Magnetic separation and washing yielded a single-sided embedded intermediate. Polydimethylsiloxane (PDMS) and poly(N-isopropylacrylamide) thermosensitive polymers were sequentially grafted onto the exposed side of the intermediate. After paraffin removal, polyethylene glycol (PEG) was grafted onto the original embedded side, forming a hydrophobic and hydrophilic side. After magnetic separation and washing, Janus nanoparticles with asymmetric wettability and thermosensitive response characteristics were obtained.
[0025] 2. Construction of CO2 microbubble stabilization system Dispersed dyes and Janus nanoparticles were dispersed in water, and CO2 was introduced through microporous pulse aeration. Taking advantage of the irreversible adsorption characteristics of Janus nanoparticles at the gas-liquid interface, a CO2 microbubble dispersion system with uniform particle size and high stability was formed.
[0026] 3. Low-temperature staining under normal pressure The polyester fabric is immersed in the above-mentioned foam stabilization system. During the heating process, the reversible phase change of the thermosensitive polymer on the surface of Janus nanoparticles is used to regulate the interfacial affinity between the particles and the fibers, so that they are anchored on the fiber surface to form a dye enrichment area. At the same time, the fiber is plasticized by the dissolution-diffusion mechanism of CO2, and the dye is efficiently applied under normal pressure and low temperature conditions.
[0027] 4. Post-processing and separation for reuse After dyeing, the fabric is removed and post-processed to obtain the finished dyed fabric. The remaining dye liquor is cooled to desorb the particles. Janus nanoparticles are recovered by microbubble flotation and magnetic separation. After cleaning, the nanoparticles are recycled. The dye liquor is replenished with dye and reused in the next batch, realizing a closed-loop cycle between the dyeing medium and the particle carrier.
[0028] The technical solution designed by this invention to solve the existing problems includes the following key points: 1. Pickering stable-foam gas-liquid staining system Traditional dyeing processes often employ liquid-liquid emulsion systems, which utilize surfactants to disperse hydrophobic dyes in an aqueous phase to form an oil-in-water microemulsion. This process has inherent drawbacks such as surfactant desorption at high temperatures leading to demulsification, increased chemical oxygen demand (COD) load in wastewater due to residues, and uncontrollable distribution of dyes between the liquid and liquid phases. To address the aforementioned problems, this invention applies the Pickering emulsion principle to a gas-liquid dyeing system. Janus nanoparticles replace traditional surfactants to stabilize CO2 microbubbles as the dyeing medium, constructing a novel gas-liquid Pickering bubble-stabilizing system. This system uses a deionized aqueous solution containing dispersed dye as the continuous phase, CO2 microbubbles as the dispersed phase, and Janus nanoparticles as the interface stabilizer. The reaction process is as follows: First, CO2 is introduced at 40°C. Janus nanoparticles, due to their asymmetric wettability, adsorb onto the gas-liquid interface, with the hydrophobic side facing the inside of the bubble and the hydrophilic side facing the aqueous phase, forming a dense solid particle film that stably encapsulates the CO2 microbubbles, constructing a uniform bubble-stabilizing system. Subsequently, the temperature is increased. When the temperature reaches the range of 30-35°C, the PNI on the surface of the Janus nanoparticles... The PAM temperature-sensitive chain undergoes a phase transition and collapses, exposing the underlying hydrophobic PDMS layer. The particles remain stably anchored at the gas-liquid interface. Simultaneously, CO2 molecules are slowly released and dissolved in the aqueous phase through the capillary channels of the particle stack. After heating to 80℃ and holding for 40 minutes, CO2 molecules enter the amorphous region of the polyester fiber through a dissolution-diffusion mechanism, forming a molecular-level plasticized layer. This helps plasticize the fiber, increases its free volume, and promotes the increase of the fiber's free volume, opening up the dye diffusion channels. At the same time, Janus nanoparticles anchored on the bubble surface move to the vicinity of the fiber with the microbubbles. The dye molecules adsorbed on their hydrophilic side migrate to the fiber surface under the drive of the concentration gradient and diffuse into the fiber interior through the plasticized open channels to complete the dyeing process. This achieves synergistic dyeing promotion through CO2 microbubbles carrying dye to the vicinity of the fiber and CO2 molecules first plasticizing and opening the channels. Through the above mechanism, this invention constructs a stable and controllable new gas-liquid dyeing system with high bubble stability, reducing surfactant usage by more than 90%, significantly reducing COD emissions, and CO2 microbubbles having the dual functions of dye carrier and fiber plasticizer. High-efficiency dyeing with a dyeing rate of >90% can be achieved under normal pressure conditions of 75~85℃.
[0029] 2. Janus nanoparticles with a three-in-one function of stabilizing bubbles, anchoring, and separating. Traditional Janus nanoparticles have limited functionality in dyeing, serving only as emulsion stabilizers or magnetic separation media. They cannot intelligently control the interaction between particles and fibers according to process requirements, leading to uncontrollable particle behavior and difficulties in dye separation during the dyeing process. To address these issues, this invention synthesizes thermosensitive Janus nanoparticles with a Fe3O4@C magnetic core. One side is grafted with a hydrophobic polydimethylsiloxane (PDMS) and modified with a thermosensitive poly(N-isopropylacrylamide) (PNIPAM) polymer, while the other side is grafted with a hydrophilic polyethylene glycol (PEG), forming magnetic Janus nanoparticles with asymmetric wettability and thermosensitive response.
[0030] Janus nanoparticles were prepared using the Pickering emulsion masking method: First, Fe3O4@C magnetic cores were added to a mixture of molten paraffin and deionized water, and emulsified at a low speed of shear at 60°C. Stabilization was achieved with the aid of a trace amount of nonionic surfactant, causing the paraffin to form uniform micron-sized droplets. Driven by interfacial energy, the magnetic cores spontaneously migrated and adsorbed at the paraffin-water interface. Due to the suitable three-phase contact angle of the particles, they reached the lowest energy state at the interface, partially embedding themselves in the surface of the paraffin droplets and partially exposing themselves to the aqueous phase. Subsequently, the paraffin was slowly cooled to solidify, burying and fixing the embedded magnetic cores while keeping the exposed parts facing outwards. Magnetic separation and washing yielded a one-sidedly buried intermediate. The intermediate was dispersed in n-heptane, and the exposed side was UV-cured to graft PDMS, establishing a hydrophobic layer. Subsequently, on this side, a thermosensitive PNIPAM polymer was grafted using an atom transfer radical polymerization system, first adding a brominated silane initiator, then adding copper bromide and N,N,N',N'',N''-pentamethyldiethylenetriamine (PMDETA) for catalysis. After the reaction, paraffin was ultrasonically eluted with petroleum ether to prevent the collapse of the thermosensitive layer and the dissolution of the hydrophobic layer. The dewaxed particles were then subjected to plasma treatment to introduce active sites such as hydroxyl and carboxyl groups on the inert carbon-based surface, providing reaction sites for subsequent covalent grafting of PEG-NH2 and ensuring stable grafting of functional layers on both sides without detachment. Finally, the original buried side was hydrophilically modified with PEG to obtain Janus nanoparticles.
[0031] To verify that the Janus nanoparticles synthesized in this invention possess the expected core-shell structure, integrity of the carbon coating layer, and morphological characteristics of the polymer grafts on both sides, field emission high-resolution transmission electron microscopy (TEM), scanning transmission electron microscopy (STEM), and energy-dispersive X-ray spectroscopy (EDX) were used to comprehensively characterize the particle morphology, core-shell structure, and elemental distribution characteristics. Figure 2 As shown, Figure 2A is the overall morphology image of TEM, which shows that the Fe3O4@C magnetic core is uniformly spherical with a particle size of about 200 nm. After multi-step modification by the Pickering emulsion masking method, the Janus nanoparticles show obvious contrast difference on both sides. One side has a higher electron density, corresponding to the hydrophobic side of PDMS, while the other side has a lower electron density, corresponding to the hydrophilic side of PEG. Figure 2 B is a magnified high-resolution TEM image showing a continuous and intact carbon coating layer on the surface of the magnetic core. This dense layer provides a stable inert carbon substrate for the subsequent introduction of active sites such as hydroxyl and carboxyl groups through plasma processing. Figure 2 C is the STEM-EDX mapping of elemental distribution, which visually reveals the spatial clustering characteristics of the elements. Si and N elements exhibit a highly overlapping asymmetric hemispherical distribution, confined only to the hydrophobic side of the particle. The other side, devoid of Si and N elements, is the hydrophilic side of PEG. Fe and O elements are concentrated at the particle center, precisely outlining the spherical contour of the Fe3O4 magnetic core. These characterization results fully confirm that the hydrophobic PDMS segments and the thermosensitive PNIPAM polymer were precisely modified on one side of the particle, while the hydrophilic PEG segments were successfully covalently grafted onto the other side. The Janus nanoparticle structure, possessing asymmetric wettability and thermosensitive response characteristics, has been successfully constructed, providing a structural basis for directional adsorption and thermosensitive anchoring during subsequent staining processes.
[0032] Furthermore, the Fe3O4@C magnetic core of the Janus nanoparticles maintains stable magnetic responsiveness throughout the process. After dyeing, residual particles can be deeply captured by a high-gradient magnetic filter, enabling rapid recovery and recycling of the particles. Through the aforementioned temperature-controlled adsorption-desorption mechanism, this invention achieves intelligent behavior regulation of the particles during the dyeing process: at 80℃, the particles actively anchor themselves to the fiber to form dye-rich micro-regions; after cooling to 40℃, the particles automatically detach from the fiber, achieving self-separation without chemical demulsification.
[0033] Example 1 Table 1 Raw Material Information Table A high-efficiency, water-saving, atmospheric pressure dyeing process for polyester utilizing a microbubble system includes the following steps: S1: 1.35 parts FeCl3·6H2O were dissolved in 40 parts ethylene glycol, and 3.6 parts anhydrous sodium acetate were added. The mixture was reacted with solvent at 200℃ for 10 hours. Fe3O4 magnetic nanospheres were obtained by magnetic separation and washing. The nanospheres were placed in a tube furnace and heated to 600℃ at 10℃ / min under nitrogen protection. Acetylene gas was introduced to carbonize the nanospheres for 30 minutes to form a 5nm carbon shell, thus obtaining Fe3O4@carbon magnetic cores. 1 part Fe3O4@carbon magnetic cores were added to 20 parts molten paraffin and 30 parts deionized water. 0.01 parts Tween 80 were added. The mixture was emulsified at 60℃ with low-speed shearing for 20 minutes. The pH was adjusted to 7.5, and the mixture was stirred for 30 minutes to allow adsorption to proceed smoothly. The mixture was then slowly cooled to 25℃ to solidify the paraffin. The mixture was then magnetically separated and washed to obtain a one-sided buried intermediate. The intermediate was dispersed in 20 parts of n-heptane, and 5 wt% PDMS-MA and 1 wt% photoinitiator 1173 were added. The mixture was cured under UV light for 8 minutes, followed by magnetic separation and washing to obtain a one-sided hydrophobically modified intermediate. The one-sided hydrophobically modified intermediate was dispersed in 20 parts of anhydrous toluene, and 0.5 parts of bromosilane initiator and 0.1 parts of triethylamine were added. The mixture was reacted at room temperature for 12 hours, followed by magnetic separation and washing with toluene. Then, it was dispersed in a 1:1 mixture of deoxygenated water and ethanol, and 0.1 parts of copper bromide, 0.3 parts of PMDETA, and 5 parts of NIPAM monomer were added. The mixture was reacted at 40°C for 8 hours under nitrogen protection, followed by magnetic separation and washing to obtain a one-sided hydrophobic PNIPAM intermediate. The one-sided hydrophobic PNIPAM intermediate was dispersed in 20 parts of petroleum ether, and ultrasonically cleaned at 30°C for 10 minutes. This process was repeated three times to remove paraffin. After magnetic separation and washing, the Janus precursor was obtained. Janus precursor was placed in a plasma treatment instrument and treated at 50W for 3 minutes, followed by air oxidation for 30 minutes to introduce carboxyl groups. It was then dispersed in a mixed solution of 20 parts ethanol and water in a volume ratio of 9:1, and 5 wt% PEG-NH2, 0.1 parts EDC and 0.1 parts NHS were added. The mixture was reacted at 60℃ for 4 hours, followed by magnetic separation and washing to obtain Janus nanoparticles.
[0034] S2: Add 1 part of Disperse Blue 56 and 0.5 parts of Janus nanoparticles to 800 parts of deionized water and stir to disperse to obtain dye solution; pump the dye solution into a dyeing kettle equipped with a microporous ceramic pulse aerator, heat to 40℃, introduce CO2 at a pressure of 0.7MPa, pulse frequency of 0.2Hz, gas flow rate of 2.0L / min, and aerate for 15 minutes to form a stable bubble system with a gas content of 20% and a particle size of 80~120μm.
[0035] S3: Immerse 100 parts of polyester fabric in the foam stabilization system to ensure that the fabric is completely wetted and evenly distributed in the dye liquor; heat to 80°C at 2°C / min, and hold at 32°C for 8 minutes to ensure that PNIPAM undergoes a complete phase transition; then control the heating rate to 0.5°C / min, heat to 80°C and hold for 40 minutes. During this process, the hydrophobic side of Janus nanoparticles collapses and is exposed and anchored to the surface of polyester fibers with affinity, forming dye-enriched micro-regions. At the same time, CO2 plasticizes the amorphous region of the fiber through the dissolution-diffusion mechanism, promoting the diffusion and dyeing of the dye.
[0036] S4: After dyeing, the dyed fabric is removed from the dyeing kettle and rinsed with deionized water at room temperature for 2 minutes to remove surface dye. It is then dehydrated and dried at 100℃ for 5 minutes to obtain the finished dyed fabric. The remaining dye liquor in the dyeing kettle is allowed to cool naturally to 40℃, allowing PNIPAM to regain its stretch and detach from the fibers. After stirring is stopped and the mixture is allowed to stand for 15 minutes, microbubbles carrying the particles rise to form a foam layer. The overflow is collected and mechanically defoamed to obtain primary recovered particles. The dye liquor is passed through a high-gradient magnetic filter at a flow rate of 2 cm / s to capture residual particles, obtaining secondary recovered particles. The combined particles are ultrasonically cleaned with ethanol and deionized water for 10 minutes, magnetically separated, and reused. The dye liquor is recycled to the next batch.
[0037] Example 2 The preparation method is the same as in Example 1, except that: S1: 40 parts ethylene glycol with 3.6 parts anhydrous sodium acetate was replaced with 30 parts ethylene glycol with 3 parts anhydrous sodium acetate; acetylene gas carbon coating for 30 minutes was replaced with acetylene gas carbon coating for 20 minutes; 20 parts molten paraffin and 30 parts deionized water were replaced with 15 parts molten paraffin and 25 parts deionized water; 5 wt% PDMS-MA and 1 wt% photoinitiator 1173 were replaced with 3 wt% PDMS-MA and 0.5 wt% photoinitiator 1173; 50W treatment for 3 minutes was replaced with 40W treatment for 2 minutes; 5 wt% PEG-NH2 was replaced with 3 wt% PEG-NH2. S2: 1 part Disperse Blue 56 and 0.5 parts Janus nanoparticles were added to 800 parts deionized water. This was replaced by 0.5 parts Disperse Blue 56 and 0.3 parts Janus nanoparticles were added to 500 parts deionized water. CO2 was introduced at a pressure of 0.7 MPa, a pulse frequency of 0.2 Hz, a gas flow rate of 2 L / min, and aeration for 15 minutes. This was replaced by introducing CO2 at a pressure of 0.6 MPa, a pulse frequency of 0.1 Hz, a gas flow rate of 1.5 L / min, and aeration for 10 minutes. S3: The heating rate of 2℃ / min is replaced with the heating rate of 1℃ / min; the holding time at 32℃ for 8 minutes is replaced with the holding time at 30℃ for 5 minutes; the heating rate of 0.5℃ / min is replaced with the heating rate of 0.3℃ / min; the holding time after heating to 80℃ for 40 minutes is replaced with the holding time after heating to 75℃ for 30 minutes. S4: Natural cooling to 40℃ is replaced with natural cooling to 35℃; Stop stirring and let stand for 15 minutes is replaced with stop stirring and let stand for 10 minutes; Flow rate of 2cm / s is replaced with Flow rate of 1cm / s; Ultrasonic cleaning for 10 minutes is replaced with ultrasonic cleaning for 5 minutes. All other steps are the same.
[0038] Example 3 The preparation method is the same as in Example 1, except that: S1: Replace 40 parts ethylene glycol with 3.6 parts anhydrous sodium acetate with 50 parts ethylene glycol with 4.5 parts anhydrous sodium acetate; replace acetylene gas carbon coating for 30 minutes with acetylene gas carbon coating for 40 minutes; replace 20 parts molten paraffin and 30 parts deionized water with 25 parts molten paraffin and 35 parts deionized water; replace 5 wt% PDMS-MA and 1 wt% photoinitiator 1173 with 7 wt% PDMS-MA and 3 wt% photoinitiator 1173; replace 50W treatment for 3 minutes with 60W treatment for 4 minutes; replace 5 wt% PEG-NH2 with 7 wt% PEG-NH2. S2: 1 part Disperse Blue 56 and 0.5 parts Janus nanoparticles were added to 800 parts deionized water. This was replaced with 3 parts Disperse Blue 56 and 1.0 part Janus nanoparticles were added to 1000 parts deionized water. CO2 was introduced at a pressure of 0.7 MPa, a pulse frequency of 0.2 Hz, a gas flow rate of 2 L / min, and aeration for 15 minutes. This was replaced with CO2 introduced at a pressure of 0.8 MPa, a pulse frequency of 0.5 Hz, a gas flow rate of 2.5 L / min, and aeration for 20 minutes. S3: Change the heating rate from 2℃ / min to 3℃ / min; change the holding time at 32℃ for 8 minutes to 35℃ for 10 minutes; change the heating rate from 0.5℃ / min to 0.8℃ / min; change the holding time after heating to 80℃ for 40 minutes to 85℃ for 50 minutes. S4: Natural cooling to 40℃ is replaced with natural cooling to 45℃; Stop stirring and let stand for 15 minutes is replaced with stop stirring and let stand for 20 minutes; Flow rate of 2cm / s is replaced with flow rate of 3cm / s; Ultrasonic cleaning for 10 minutes is replaced with ultrasonic cleaning for 15 minutes. All other steps are the same.
[0039] Comparative Example 1 Traditional surfactant microemulsion dyeing was used, replacing Janus nanoparticles with conventional nonionic surfactant, dodecyl polyoxyethylene ether (AEO-9). One part of Disperse Blue 56 and five parts of AEO-9 were added to 800 parts of deionized water and stirred at high speed to form an oil-in-water microemulsion without introducing CO2 microbubbles. The conventional microemulsion dyeing process was followed, i.e., heating to 95°C at 2°C / min and holding for 60 minutes. After dyeing, conventional reduction washing was performed.
[0040] Comparative Example 2 The preparation method is the same as in Example 1, except that: S1: Janus nanoparticles with synthesized PNIPAM temperature-sensitive layers were omitted, and Janus intermediates without PNIPAM grafting were used for subsequent experiments; All other steps are the same.
[0041] Comparative Example 3 The preparation method is the same as in Example 1, except that: S2: Replace the CO2 inlet with the N2 inlet; All other steps are the same.
[0042] Experimental Example 1 The dyed finished fabrics prepared in step S4 of Examples 1-3 and Comparative Examples 1-3 were measured: (1) Dyeing rate: Referencing GB / T 23976.1-2009 "Dye-Dyeing Rate Curve Determination - Dyeing Rate Determination Method", the dyeing rate was determined using the residual absorbance method. Before dyeing, a certain amount of dye solution was diluted, and its absorbance was measured at the maximum absorption wavelength of the disperse dye using a UV-Vis spectrophotometer. The dye mass concentration in the dye solution before dyeing was calculated based on the standard working curve. After dyeing, all residual liquid was collected, and the volume was adjusted to the same level. The absorbance was measured under the same conditions, and the dye mass concentration in the residual liquid was calculated. The dyeing rate was calculated using the following formula: Dyeing rate (%) = (Dye mass before dyeing - Dye mass in residual liquid after dyeing) / Dye mass before dyeing × 100%. Each group of valid samples should have no less than 5 samples, and the final result is the average.
[0043] (2) K / S value: Referring to GB / T 6688-2008 "Dyes - Determination of relative strength and color difference - Instrumental method", the K / S value of the dyed fabric was determined using a spectrophotometer. The dyed polyester fabric was folded to an opaque thickness and placed on the test hole of the spectrophotometer. Under the conditions of D65 standard light source and 10° observation angle, the reflectance R of the fabric in the wavelength range of 400~700nm was measured. ∞ The K / S value is calculated using the Kubelka-Munk equation: K / S = (1 - R) / S. ∞ ) 2 / (R) ∞The K / S value at the maximum absorption wavelength is usually used as the staining depth indicator. Each sample is measured three times at different locations, and the average value is taken. At least five samples should be tested in each group, and the average value of the results is taken.
[0044] (3) Migration rate: Referring to GB / T 10663-2014 "Disperse dyes - Determination of migration - High temperature dyeing method", firstly, a 1 / 1 standard dyeing depth sample was prepared. One sample each of the dyed original color fabric and pure polyester white fabric were placed in a blank bath and subjected to migration treatment under the same dyeing conditions. After the migration was completed, the K / S values of the original color fabric and white fabric after migration were determined according to the aforementioned method. The migration degree was calculated according to the following formula: Migration degree (%) = (K / S value of white fabric after migration) / (K / S value of original color fabric after migration) × 100%. To obtain reliable data, at least 5 parallel samples were tested for each group, and the average value of the results was taken.
[0045] Experimental Example 2 The Janus nanoparticles prepared in step S1 of Example 1 were tested using transmission electron microscopy (TEM), scanning transmission electron microscopy (STEM), and energy-dispersive X-ray spectroscopy (EDX): (1) Sample dispersion: A small amount of Janus nanoparticles obtained after magnetic separation and washing were placed in ethanol to prepare a sample dispersion.
[0046] (2) Ultrasonic treatment: The sample dispersion is subjected to brief ultrasonic vibration to ensure that Janus nanoparticles are uniformly dispersed in the solvent and avoid agglomeration.
[0047] (3) Dropping to form a film: Use a pipette to draw a drop of uniform sample dispersion and drop it onto a microgrid copper grid with an ultrathin carbon support film.
[0048] (4) Drying: Allow to dry naturally at room temperature to ensure complete evaporation of the solvent and allow the particles to adhere firmly to the carbon film surface. Then, it can be sent into the electron microscope chamber for testing.
[0049] (5) Test equipment and parameters: The field emission high-resolution transmission electron microscope equipped with STEM module and high-performance EDX spectrometer was used for testing. The accelerating voltage of the equipment was set to 200kV. Then the prepared sample was sent into the electron microscope chamber to complete various characterization tests.
[0050] Table 2 Comparison of experimental results of Examples 1-3 and Comparative Examples 1-3 The experimental results of Examples 1-3 and Comparative Examples 1-3 are shown in Table 2 and Figure 3As shown, the dyed finished fabric obtained by the present invention has better dyeing rate, K / S value and migration rate than other embodiments and comparative examples. This indicates that under the preferred parameters, the three elements of Janus nanoparticle foam stabilization, temperature-sensitive anchoring and CO2 plasticization work synergistically to achieve the best balance, taking into account both high-efficiency dyeing and energy saving and environmental protection. Therefore, it is the best implementation point.
[0051] Example 2, by reducing the synthesis intensity of Janus nanoparticles and weakening the dyeing process conditions, resulted in decreased particle interface stability and temperature-sensitive response, insufficient CO2 plasticization driving force, and inadequate dye diffusion. Consequently, the dyeing rate, K / S value, and levelness were all lower than in Example 1. This demonstrates that the synergistic effect of the three elements in this invention directly affects the dyeing effect. When any element's relevant parameter falls below the preferred range, the overall performance declines in stages, verifying the significant impact of each process parameter on the final dyeing effect. Example 3, by increasing the magnetic core reaction temperature and time, increasing the grafting concentration of each functional layer, increasing CO2 pressure and flow rate, accelerating the heating rate, and increasing the dyeing temperature, further improved particle interface stability and temperature-sensitive response, enhanced CO2 plasticization driving force, and ultimately achieved better results than in Example 2. This demonstrates that in the technical solution of this invention, enhancing the process parameters of each element can further improve the dyeing effect, but the improvement is limited, and increasing the dyeing temperature increases energy consumption. This verifies that Example 1 achieved the optimal balance between dyeing effect and energy conservation and environmental protection.
[0052] Due to the lack of key technologies, the overall effects of Comparative Examples 1-3 were reduced to varying degrees compared to the Examples. Comparative Example 1 used traditional surfactant microemulsion dyeing, replacing Janus nanoparticles with conventional nonionic surfactant AEO-9, and did not introduce CO2 microbubbles. It required dyeing at a high temperature of 95°C and additional reduction washing. Due to the lack of the Pickering foam-stabilizing effect of Janus nanoparticles and the plasticizing dyeing-promoting effect of CO2, the surfactant was prone to desorption and demulsification at high temperatures, resulting in poor dye dispersion stability. All indicators were significantly lower than those of Example 1. Comparative Example 1 demonstrates that traditional surfactant systems cannot achieve efficient dyeing at normal pressure and low temperature, and require high temperature and energy consumption, resulting in high COD wastewater from reduction washing. This highlights the innovation of the Janus nanoparticle foam stabilization and CO2 plasticization synergistic technology of this invention. Comparative Example 2 uses Janus intermediates without PNIPAM grafting for dyeing. Although it retains the foam stabilization function and CO2 plasticization mechanism of Janus nanoparticles, the lack of a temperature-sensitive layer prevents the particles from hydrophobically collapsing and anchoring to the fiber surface during heating, resulting in the inability to form dye-rich micro-regions. The dye mainly relies on passive diffusion for dyeing. Comparative Example 2 demonstrates that the adsorption-desorption regulation mechanism of the PNIPAM temperature-sensitive layer is the key to improving the dyeing effect and achieving efficient particle recovery. Comparative Example 3 uses complete Janus nanoparticles and a foam stabilization system, but replaces CO2 with N2. Although the granules retain their foam-stabilizing function and temperature-sensitive anchoring mechanism, N2 lacks the dissolution-diffusion plasticizing ability of CO2, thus failing to effectively lower the fiber glass transition temperature. During dyeing at 80℃, the dye diffusion channels are not fully opened, resulting in the lowest levels of dye uptake, K / S value, and levelness. Comparative Example 3 demonstrates that the atmospheric pressure plasticizing mechanism of CO2 is the core driving force for achieving low-temperature, high-efficiency dyeing. Without CO2 plasticizing, even with complete granule foam stabilization and anchoring functions, ideal dyeing results cannot be obtained at 80℃.
[0053] In summary, this invention achieves synergistic effects of Janus nanoparticle foam stabilization, temperature-sensitive anchoring, and CO2 plasticization by constructing a gas-liquid Pickering foam stabilization system, designing temperature-controlled adsorption-desorption Janus nanoparticles, and utilizing the CO2 plasticization mechanism at ambient pressure. This enables efficient water-saving dyeing of polyester under ambient pressure and low temperature conditions. Comparative examples verify the indispensability of the three key elements: Janus nanoparticle foam stabilization, temperature-sensitive anchoring, and CO2 plasticization. Compared with traditional processes, this invention has significant advantages in water saving, energy saving, and environmental protection, providing a green and environmentally friendly innovative technical solution for polyester dyeing.
Claims
1. A high-efficiency, water-saving, atmospheric pressure dyeing process for polyester utilizing a microbubble system, the atmospheric pressure dyeing process comprising pretreatment, dyeing medium construction, dyeing accelerator, and posttreatment, characterized in that, The pretreatment includes preparing Janus nanoparticles; these particles have Fe3O4@carbon as their magnetic core, with hydrophobic polydimethylsiloxane and hydrophilic polyethylene glycol grafted onto their surfaces, and modified with a poly(N-isopropylacrylamide) thermosensitive polymer on the hydrophobic side; the dyeing medium is constructed by adding the Janus nanoparticles and disperse dyes to water, introducing CO2, and forming a CO2 microbubble dispersion system stabilized by the Janus nanoparticles; the dyeing process involves immersing polyester fabric in the dispersion system, using the reversible phase transition of the thermosensitive polymer within a temperature range of 32-35°C to anchor the particles to the fiber surface, while simultaneously using the dissolution-diffusion mechanism of CO2 to plasticize the polyester fibers; the posttreatment involves inducing particle desorption through cooling, combined with air flotation and magnetic separation synergistic recovery technology to achieve a closed-loop recycling of the fabric and the particles.
2. The high-efficiency water-saving polyester atmospheric pressure dyeing process utilizing a microbubble system as described in claim 1, characterized in that, Includes the following steps: S1: FeCl3·6H2O was dissolved in ethylene glycol and anhydrous sodium acetate was added for thermal reaction. Fe3O4 magnetic nanospheres were obtained by magnetic separation and washing. Fe3O4 magnetic nanospheres were obtained by heating under nitrogen protection and introducing acetylene gas to carbon-coat the nanospheres to form a carbon shell, thus obtaining Fe3O4@carbon magnetic core. The magnetic core was added to molten paraffin and deionized water, Tween 80 was added, and the pH was adjusted after low-speed shear emulsification and stirring was continued. The temperature was then lowered to 25°C to solidify the paraffin. The mixture was then magnetically separated and washed with deionized water to obtain a one-sided buried intermediate. The intermediate was dispersed in n-heptane, polydimethylsiloxane-methacrylate and a photoinitiator were added, and the mixture was cured under ultraviolet light, magnetically separated and washed to obtain a unilaterally hydrophobically modified intermediate. A one-sided hydrophobic modified intermediate was dispersed in anhydrous toluene, and a brominated silane initiator and triethylamine were added. After reacting at room temperature, the mixture was magnetically separated and washed with toluene. Subsequently, it was dispersed in a mixed solution of deoxygenated water and ethanol, and copper bromide, N,N,N',N'',N''-pentamethyldiethylenetriamine and N-isopropylacrylamide monomer were added. The mixture was reacted under nitrogen protection, and magnetically separated and washed to obtain a one-sided hydrophobic poly(N-isopropylacrylamide) intermediate. The one-sided hydrophobic poly(N-isopropylacrylamide) intermediate was dispersed in petroleum ether and ultrasonically cleaned to remove paraffin. After magnetic separation and washing, Janus precursor was obtained. The Janus precursor was subjected to plasma treatment and air oxidation to introduce carboxyl groups. It was then dispersed in a mixed solution of ethanol and water, and polyethylene glycol-amino, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide were added to react. After the reaction, the mixture was magnetically separated and washed to obtain Janus nanoparticles. S2: Disperse Blue 56 and Janus nanoparticles are added to deionized water and stirred to disperse them to obtain a dye solution; after heating the dye solution, CO2 is introduced to aerate it and form a stable foam system. S3: Immerse the polyester fabric in the foam stabilization system to ensure that the fabric is completely soaked and evenly distributed in the dye liquor; heat to the poly(N-isopropylacrylamide) phase transition temperature range and hold to ensure sufficient phase transition. After that, control the heating rate and continue to heat to the dyeing temperature and hold to perform dyeing. S4: After dyeing, the dyed fabric is taken out, rinsed with deionized water at room temperature, and then dehydrated and dried to obtain the finished dyed fabric; the remaining dye liquor is cooled naturally, stirring is stopped and it is allowed to stand, the overflow is collected and mechanically defoamed to obtain primary recovered particles; the dye liquor is filtered through a high gradient magnetic filter to capture the residual particles to obtain secondary recovered particles; the combined particles are ultrasonically cleaned with ethanol and deionized water, magnetically separated and reused, and the dye liquor is recycled to the next batch.
3. The high-efficiency water-saving polyester atmospheric pressure dyeing process utilizing a microbubble system as described in claim 2, characterized in that, S1 is dissolved in ethylene glycol and anhydrous sodium acetate is added, with a mass ratio of (15:35) to 1.
4. The high-efficiency water-saving polyester atmospheric pressure dyeing process utilizing a microbubble system as described in claim 2, characterized in that, The polydimethylsiloxane-methacrylate in S1 has a mass percentage of 3-7 wt%; the photoinitiator has a mass percentage of 0.5-3 wt%.
5. The high-efficiency water-saving polyester atmospheric pressure dyeing process utilizing a microbubble system as described in claim 2, characterized in that, The plasma treatment described in S1 has a processing power of 40~60W and a processing time of 2~4 minutes; the polyethylene glycol-amino has a mass ratio of 3~7wt%.
6. The high-efficiency water-saving polyester atmospheric pressure dyeing process utilizing a microbubble system as described in claim 2, characterized in that, S2 introduces CO2 at a pressure of 0.6-0.8 MPa; the aeration conditions are set as follows: pulse frequency 0.1-0.3 Hz, gas flow rate 1.5-2.5 L / min, and aeration time 10-20 minutes.
7. The high-efficiency water-saving polyester atmospheric pressure dyeing process utilizing a microbubble system as described in claim 2, characterized in that, S3 describes heating to the phase change temperature range of poly(N-isopropylacrylamide) and holding it therefore, with a heating rate of 1~3℃ / min, a phase change temperature range of 30~35℃, and a holding time of 5~10 minutes.
8. The high-efficiency water-saving polyester atmospheric pressure dyeing process utilizing a microbubble system as described in claim 2, characterized in that, The heating rate controlled in S3 should be 0.3~0.8℃ / min; the dyeing temperature range is 75~85℃ and the holding time is 30~50 minutes.
9. The high-efficiency water-saving polyester atmospheric pressure dyeing process utilizing a microbubble system as described in claim 2, characterized in that, The natural cooling mentioned in S4 requires the temperature to naturally drop to 35~45℃; the standing time after stopping stirring is 10~20 minutes.
10. The high-efficiency water-saving polyester atmospheric pressure dyeing process utilizing a microbubble system as described in claim 2, characterized in that, The high-gradient magnetic filter described in S4 has a flow rate of 1~3cm / s for the dye solution; the ultrasonic cleaning has a cleaning time of 5~15 minutes.
Citation Information
Patent Citations
Cellulose fiber reactive dye-based less-water medium dyeing method
CN109695163A
Nano-cellulose coloring agent based on D5 medium reverse micelle dyeing and preparation method of nano-cellulose coloring agent
CN121450126A