A type of crepe paper base paper, its preparation method and application
By adding polyamide polyamine-epoxychloropropane resin in stages to improve the distribution of cellulose pulp, crepe paper base paper is prepared, which solves the problems of complex electrical performance improvement and weak fiber bonding in the existing technology, and achieves higher electrical performance and stability.
Patent Information
- Application Number
- CN202611539649.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-17
AI Technical Summary
Existing methods for improving the electrical properties of crepe paper base paper are complex and difficult, and the weak fiber bonding force makes it prone to fiber shedding and insufficient electrical properties in humid and hot environments.
A method of adding polyamide polyamine-epoxychloropropane resin in stages is used to premix it into a portion of the cellulose pulp, and then mix it with the remaining resin to form a modified mixed pulp. The crepe paper base is then prepared by wet papermaking.
It improves the electrical properties of cellulose-based paper, especially the DC breakdown field strength and volume resistivity, while reducing the power frequency dielectric constant and dielectric loss, making it suitable for insulation treatment of electrical components.
Smart Images

Figure CN123108984A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of insulating materials technology, and in particular to a crepe paper base paper, its preparation method, and its application. Background Technology
[0002] Crepe paper is a special electrical insulation material. A special crepe process creates continuous or discontinuous micro-wrinkles on the surface of the base paper. Compared to ordinary flat insulation paper, this crepe structure gives the paper a higher longitudinal elongation, providing excellent stretchability under tension. It also enhances its flexibility and bending adaptability, enabling crepe paper to effectively adapt to conductor bending, tight winding, and frequent mechanical vibrations during equipment operation. Through the micro-deformation and recovery mechanism of the crepe structure, it effectively buffers and disperses local stress, improving the reliability and service life of electrical equipment during long-term operation.
[0003] Cellulose insulating paper possesses excellent electrical insulation properties, mechanical strength, oil impregnation compatibility, flexibility, and processing adaptability, making it an important solid insulating material in high-voltage electrical equipment and a significant source of paper base for crepe paper. Existing crepe paper bases are typically made from high-purity cellulose insulating pulp through pulping, mixing, wet forming, pressing, and drying. To achieve high longitudinal elongation and softness, the creping process requires longitudinal shrinkage and localized fiber network deformation. However, when the fiber bond in crepe paper bases is weak, the paper is prone to fiber shedding, wrinkle damage, decreased wet strength, and paper breakage during creping, winding, oil impregnation, and in humid and hot environments.
[0004] PAAE resin is a water-soluble cationic thermosetting resin that can adsorb onto the surface of negatively charged cellulose fibers and form a cross-linked structure during drying and heating. Currently, it is mainly used as a wet strength agent to improve paper strength. Adding it to cellulose insulating pulp for co-forming can enhance fiber bonding through the cross-linked network, improving the dry and wet mechanical strength of cellulose paper. Simultaneously, the PAAE cross-linked structure can also improve its volume resistivity and dielectric properties to some extent, but the improvement has not yet fully reached the expected level to meet the needs of most practical engineering applications, and its electrical properties still need further improvement.
[0005] Existing technologies primarily improve the electrical properties of crepe paper through methods such as fiber microstructure regulation, chemical grafting modification, and nanomaterial composites. Among these, optimizing the fiber microstructure to improve the paper's pore structure is an effective way to enhance breakdown strength, such as adding highly finely fiberized softwood pulp to improve DC breakdown strength. Chemical grafting modification optimizes the insulation properties of cellulose at the molecular level, introducing long methylene chains or benzene rings into the cellulose system through grafting technology to improve insulation. Nanomaterial composites are a breakthrough direction in recent years, such as uniformly doping nano-silica particles into the pulp to reduce dielectric loss. While these methods can effectively improve electrical properties, they still have significant shortcomings. Among these, the microstructure control of fibers places stringent requirements on equipment precision and operational control, increasing production complexity and cost; chemical grafting modification usually involves multi-step organic synthesis reactions, with long process routes, difficult-to-control reaction conditions, and the potential introduction of by-products or residual reagents, affecting the purity and long-term stability of insulating paper; and nanomaterial composites face inherent problems such as the difficulty in dispersing nanoparticle agglomeration and weak interfacial bonding with cellulose fibers, requiring the addition of dispersants or surface modification, further increasing the difficulty of formulation design and homogenization processes. Summary of the Invention
[0006] This invention aims to at least solve one of the aforementioned technical problems existing in the prior art. Therefore, one objective of this invention is to provide a method for preparing crepe paper base paper. A second objective of this invention is to provide a crepe paper base paper obtained by the preparation method described in the first aspect. A third objective of this invention is to provide an application of the crepe paper base paper described in the second aspect.
[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A first aspect of the present invention is to provide a method for preparing crepe paper base paper, comprising the following steps: (1) Provide cellulose pulp and polyamide polyamine-epoxychloropropane resin; (2) A portion of the cellulose slurry is premixed with a portion of the polyamide polyamine-epoxychloropropane resin to obtain a premixed slurry; (3) Add the remaining amount of the cellulose slurry and the remaining amount of the polyamide polyamine-epoxychloropropane resin to the premixed slurry and mix to obtain a mixed slurry; (4) The mixed slurry is wet-processed to obtain crepe paper base paper.
[0008] In some preferred embodiments, the total solids addition of the polyamide polyamine-epoxychloropropane resin in step (1) is in the mass ratio of the oven-dry fibers of the cellulose slurry to (0.5-1.5):100; more preferably (0.8-1.2):100.
[0009] In some preferred embodiments, the mixed slurry comprises, by oven-dry weight, 80-100 parts of high-purity coniferous wood insulating slurry, 0-20 parts of auxiliary fibers, and 0.5-1.5 parts of polyamide polyamine-epoxychloropropane resin.
[0010] The high-purity coniferous wood insulating pulp of this invention refers to the high-grade product that meets the requirements of GB / T 13505-2025 "High-purity Insulating Wood Pulp", namely, α-cellulose content ≥95% and ash content ≤0.25%.
[0011] In some preferred embodiments, the auxiliary fiber includes one or more of cotton pulp fiber, hardwood insulating pulp fiber, hemp pulp fiber, or nanocellulose.
[0012] In some preferred embodiments, the cellulose slurry premixed in step (2) accounts for 10-40% of the total mass of the cellulose slurry, based on oven-dry fiber; for example, it can be any value of 10%, 15%, 20%, 25%, 30%, 35%, 40%, or any range between two.
[0013] In some preferred embodiments, the total solids content of the premixed polyamide polyamine-epoxychloropropane resin in step (2) accounts for 20-60% of the total mass of the resin; for example, it can be any value among 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60% or any range between two.
[0014] In some preferred embodiments, the pH value of the premixed solution in step (2) is 4.5-6.5; more preferably 5-5.5.
[0015] In some preferred embodiments, the temperature of the premixing in step (2) is 15-45°C; more preferably 20-30°C.
[0016] In some preferred embodiments, the stirring rate of the premixing in step (2) is 100-800 r / min; more preferably 400-600 r / min.
[0017] In some preferred embodiments, the premixing time in step (2) is 5-40 min; more preferably 10-20 min.
[0018] In some preferred embodiments, the cellulose pulp has a freeness of 25-45°SR; more preferably 30-40°SR; and even more preferably 30-35°SR.
[0019] In some preferred embodiments, the mixing speed in step (3) is 100-800 r / min; more preferably 400-500 r / min.
[0020] In some preferred embodiments, the mixing time in step (3) is 5-30 min; more preferably 10-15 min.
[0021] In some preferred embodiments, the wet papermaking process in step (4) includes the following steps: After adjusting the solid content of the mixed pulp, wet forming is carried out to obtain wet paper sheets, which are then pressed, dried and heat-cured to obtain crepe paper base paper.
[0022] In some preferred embodiments, the solid content of the mixed slurry is adjusted to 0.1-1.0 wt% before wet forming; more preferably, it is 0.3-0.7 wt%.
[0023] In some preferred embodiments, the pressing pressure is 0.2-0.6 MPa; more preferably 0.3-0.5 MPa.
[0024] In some preferred embodiments, the pressing time is 1-10 minutes; more preferably 3-7 minutes.
[0025] In some preferred embodiments, the moisture content of the pressed wet paper sheet is 20-45%; more preferably 30-40%.
[0026] In some preferred embodiments, the moisture content of the dried paper is 2-8%; more preferably 4-6%.
[0027] In some preferred embodiments, the thermosetting temperature is 85-90°C.
[0028] In some preferred embodiments, the thermosetting time is 10-15 minutes.
[0029] A second aspect of the present invention is to provide a crepe paper base paper, which is prepared by the preparation method described in the first aspect.
[0030] In some preferred embodiments, the thickness of the crepe paper base is 0.05-0.13 mm; for example, it can be any value or a range between 0.05 mm, 0.06 mm, 0.07 mm, 0.08 mm, 0.09 mm, 0.10 mm, 0.11 mm, and 0.12 mm.
[0031] A third aspect of the present invention is to provide an application of the crepe paper base paper described in the second aspect, specifically in the insulation of electrical components.
[0032] In some preferred embodiments, the crepe paper base paper is wrinkled to form crepe paper for application.
[0033] In some preferred embodiments, the application includes the covering, lead covering, or interlayer insulation of winding conductors in oil-immersed transformers, reactors, motors, instrument transformers, power capacitors, or other electrical equipment.
[0034] The beneficial effects of this invention are: (1) In view of the problems of low electrical properties of cellulose-based paper and the complexity and difficulty of improving the electrical properties of crepe paper in the prior art, the present invention provides a method for preparing crepe paper base paper. Polyamide polyamine-epoxychloropropane resin is introduced into cellulose-based paper by adding it in stages. The polyamide polyamine-epoxychloropropane resin is first pre-adsorbed in part of the cellulose pulp and then mixed with the remaining pulp and resin. This helps to improve the distribution of resin in the fiber network, reduce local enrichment and the resulting structural defects and polarization losses, and effectively improve the electrical properties of cellulose-based paper. Compared with one-time addition, the staged addition method of the present invention has obvious advantages in electrical performance. At the same time, the preparation method of the present invention is simple and easy to implement, requiring no special equipment, reagents or processes. It can be fully integrated with existing wet papermaking and drying cylinder creping processes, and has excellent prospects for industrial application.
[0035] (2) In this invention, polyamide polyamine-epoxychloropropane resin is added in stages to effectively improve the electrical properties of cellulose-based paper, thereby obtaining higher DC breakdown field strength and volume resistivity, while reducing power frequency dielectric constant and dielectric loss.
[0036] (3) Based on the good electrical properties of the crepe paper base paper described in this invention, it can be used for insulation treatment of electrical components, especially suitable for the covering of winding wires, lead wire covering or interlayer insulation in oil-immersed transformers, reactors, motors, instrument transformers, power capacitors or other electrical equipment. Attached Figure Description
[0037] Figure 1 This is a schematic diagram illustrating the preparation process of the crepe paper base paper in this embodiment; Figure 2 A histogram comparing the average volume resistivity of the crepe paper base paper prepared in Examples 1-3 and Comparative Examples 1-4. Figure 3 The graph shows a comparison of the DC breakdown field strength of the crepe paper base paper prepared in Examples 1-3 and Comparative Examples 1-4. Figure 4 This is a bar chart comparing the relative permittivity of the crepe paper base paper prepared in Examples 1-3 and Comparative Examples 1-4. Figure 5 This is a comparative graph of the dielectric loss angle tangent of the crepe paper base paper prepared in Examples 1-3 and Comparative Examples 1-4. Detailed Implementation
[0038] The present invention will be further described in detail below through specific embodiments.
[0039] Embodiments of the present invention relate to a crepe paper base paper, as shown in the attached drawing. Figure 1 A schematic diagram of the preparation process, the preparation method of which includes the following steps: S1. Add high-purity cellulose insulating paste to deionized water to loosen and pulp, so that the pulping degree reaches 25-45°SR.
[0040] S2. Take out 10%-40% of the dry fiber mass from the slurry obtained in step S1 as the pre-adsorption slurry. Add 20%-60% of the total solid mass of polyamide polyamine-epoxychloropropane resin to the pre-adsorption slurry, adjust the pH to 4.5-6.5, and stir at 15-45℃ for 5-40 min.
[0041] S3. Mix the pre-adsorbed slurry with the remaining slurry, add the remaining polyamide polyamine-epoxychloropropane resin under stirring conditions, and continue stirring for 5-30 min to obtain the modified mixed slurry.
[0042] S4. Dilute the modified mixed pulp to a mass concentration of 0.1%-1.0%, and use a cylinder wire, long wire, inclined wire or paper forming device for wet forming and pressing to obtain a wet paper sheet.
[0043] S5. Adjust the moisture content of the wet paper sheet to 20%-45% and attach it to the surface of the heated drying cylinder.
[0044] S6. Dry the paper to a moisture content of 2%-8%, and then heat-cure it at 85-90℃ for 10-15 minutes to obtain the crepe paper base paper.
[0045] In some specific embodiments, the total solids content of polyamide polyamine-epoxychloropropane resin is in a mass ratio of (0.5-1.5):100 to the dry fiber content of cellulose insulating paste.
[0046] In some specific implementations, the cellulose insulating paste is desized and beaten to a freeness of 30-40°SR.
[0047] In some specific implementations, the pressing pressure is 0.2-0.6 MPa, the pressing time is 1-10 min, and the moisture content of the wet paper sheet after pressing is 20-45%.
[0048] The invention will now be described in further detail through some more specific embodiments.
[0049] Unless otherwise specified, the raw materials, reagents, or apparatus used in the following examples and comparative examples are all available from conventional commercial sources or can be obtained by existing technical methods. Unless otherwise specified, the test or experimental methods are conventional methods in the art.
[0050] Polyamide-polyamine-epichlorohydrin resin (PAAE) is referred to as PAAE resin in the following text. Unless otherwise stated, the amount of PAAE resin added refers to the percentage of PAAE resin solids by weight to the weight of oven-dry fibers.
[0051] Example 1 This embodiment relates to a crepe paper base paper, comprising cellulose fibers and PAAE resin, and its preparation method specifically includes the following steps: (1) Weigh 1000g of high-purity coniferous sulfate insulating slurry and 5g of PAAE resin. The coniferous sulfate insulating slurry is added to deionized water for dissolution and pulping until the pulping degree is 30°SR to obtain coniferous slurry. The PAAE resin is dissolved in deionized water and diluted to a mass percentage concentration of 2.0% to obtain PAAE resin solution.
[0052] (2) Mix 20% softwood pulp with 40% PAAE resin solution, adjust the pH of the mixture to 5.5 with acetic acid aqueous solution, and stir for 15 min at 25℃ and 500r / min to obtain premixed pulp.
[0053] (3) Mix the remaining 80% softwood pulp, 60% PAAE resin solution and premixed pulp, and continue stirring and mixing for 10 minutes at 400 r / min to obtain mixed pulp.
[0054] (4) Dilute the mixed pulp with deionized water to a solid content of 0.5wt%, use a paper forming machine for wet forming, press at 0.4MPa for 5min, adjust the moisture content to 35%, obtain wet paper, attach the wet paper to the surface of the heating drying cylinder, dry to a moisture content of 5%, and then heat cure at 85℃ for 10min to obtain crepe paper base paper.
[0055] The thickness of the paper was measured using a Japanese Sanryu paper thickness gauge according to GB / T 451.3-2002 "Determination of the thickness of paper and paperboard". The test environment was 23±1℃ and 50±2% RH, and the unit of thickness was mm. The results showed that the thickness of the crepe paper base obtained in this example was 0.09-0.12 mm, with an average thickness of 0.103-0.115 mm, a standard deviation ≤0.008 mm, a range ≤0.014 mm, and a coefficient of variation (CV) ≤6.4%, indicating uniform thickness distribution and good process stability.
[0056] Example 2 This embodiment relates to a crepe paper base paper, which differs from Embodiment 1 only in that the amount of PAAE resin used in step (1) is 10g, and the rest is the same as in Embodiment 1.
[0057] Example 3 This embodiment relates to a crepe paper base paper, which differs from Embodiment 1 only in that the amount of PAAE resin used in step (1) is 15g, and the rest is the same as in Embodiment 1.
[0058] Example 4 This embodiment relates to a crepe paper base paper. The only difference from embodiment 2 is that in step (2), the amount of softwood pulp is 10% and the amount of PAAE resin solution is 20%. The remaining 90% of the softwood pulp and 80% of the PAAE resin solution are added in step (3), and the rest is the same as in embodiment 2.
[0059] Example 5 This embodiment relates to a crepe paper base paper. The only difference from embodiment 2 is that in step (2), the amount of softwood pulp is 40% and the amount of PAAE resin solution is 60%. The remaining 60% of softwood pulp and 40% of PAAE resin solution are added in step (3), and the rest is the same as in embodiment 2.
[0060] Comparative Example 1 This comparative example relates to a crepe paper base paper, which differs from Example 1 only in that it does not contain PAAE resin; otherwise, it is the same as Example 1.
[0061] Comparative Example 2 This comparative example relates to a crepe paper base paper, which differs from Example 2 only in that the softwood pulp and PAAE resin solution are mixed together in one go to form a mixed pulp instead of adding it in steps (2)-(3) in stages. The rest is the same as Example 2.
[0062] Comparative Example 3 This comparative example relates to a crepe paper base paper, which differs from Example 1 only in that the softwood pulp and PAAE resin solution are mixed together in one go to form a mixed pulp instead of adding it in steps (2)-(3) in stages. The rest is the same as Example 1.
[0063] Comparative Example 4 This comparative example relates to a crepe paper base paper, which differs from Example 3 only in that the softwood pulp and PAAE resin solution are mixed together in one go to form a mixed pulp instead of adding it in steps (2)-(3) in stages. The rest is the same as Example 3.
[0064] The electrical properties of the crepe paper bases prepared in Examples 1-5 and Comparative Examples 1-4 were tested. The volume resistivity was determined by drying the crepe paper base samples at 105°C for 24 hours, cooling them in the dry environment, and then testing their volume resistivity using a flat plate electrode at a voltage of 100V. The DC breakdown field strength was determined by vacuum immersing the dried crepe paper base samples in mineral insulating oil, and then testing their breakdown voltage using a DC breakdown test at a rate of 0.5kV / s, an ambient temperature of 25°C, and a relative humidity of 30%. The power frequency relative permittivity and power frequency dielectric loss were determined using a dielectric spectrum testing system at an AC voltage of 1.0Vrms, measuring the real part (ε′) of the power frequency relative permittivity and the power frequency dielectric loss tangent (tanδ) at a frequency of 50Hz.
[0065] To compare the effects of PAAE resin addition amount and addition method on the electrical properties of crepe paper base paper, the volume resistivity, DC breakdown field strength, power frequency relative permittivity, and power frequency dielectric loss of the crepe paper base paper prepared in Examples 1-3 and Comparative Examples 1-4 were measured. The test results were taken as the average of three parallel tests. The test results are shown in Table 1 and Appendix. Figure 2-5 .
[0066] Table 1. Electrical performance test results of the crepe paper base paper prepared in Examples 1-3 and Comparative Examples 1-4
[0067] According to the test results in Table 1, both the amount and method of adding PAAE resin affect the DC breakdown field strength, volume resistivity, and power frequency dielectric properties of the crepe paper base. Specifically: The DC breakdown field strength test results show that the average DC breakdown field strength of the base paper without added PAAE resin is 21.71 kV / mm, and the field strength is further improved by adding 0.5%, 1.0%, and 1.5% PAAE resin in stages. After adding PAAE resin, the average DC breakdown field strength of the base paper increased to 34.72, 35.43, and 34.45 kV / mm, respectively, which were approximately 59.9%, 63.2%, and 58.7% higher than the 21.71 kV / mm without PAAE resin. After adding 0.5%, 1.0%, and 1.5% PAAE resin at one time, the average DC breakdown field strength of the base paper increased to 33.54, 34.86, and 33.09 kV / mm, respectively. When the PAAE resin addition was 1.0%, the DC breakdown field strength of the base paper obtained by adding it in stages was approximately 1.64% higher than that obtained by adding it in one stage. The above results indicate that the addition of PAAE resin can improve the DC breakdown resistance of cellulose base paper, and under the same PAAE resin addition conditions, the staged addition has better DC breakdown performance than the single addition.
[0068] The volume resistivity test results showed that the average volume resistivity of the base paper without added PAAE resin was 96.37 GΩ·cm. After adding 0.5%, 1.0%, and 1.5% PAAE resin in stages, the average volume resistivity of the base paper increased to 142.00, 224.00, and 164.67 GΩ·cm, respectively. After adding 0.5%, 1.0%, and 1.5% PAAE resin in one go, the average volume resistivity of the base paper increased to 114.96, 192.71, and 137.59 GΩ·cm, respectively. When the amount of PAAE resin added was 1.0%, the volume resistivity of the base paper obtained by adding it in stages was about 16.24% higher than that obtained by adding it in one go. These results indicate that the addition of PAAE resin can improve the volume resistivity of cellulose base paper, and under the same amount of PAAE resin added, adding it in stages has better insulation performance than adding it in one go.
[0069] The power frequency dielectric property test results show that the relative permittivity of the base paper without added PAAE resin is 3.8580, and the dielectric loss tangent is 0.2020. After adding 0.5%, 1.0%, and 1.5% PAAE resin in stages, the relative permittivity of the base paper decreases to 3.7525, 3.3126, and 3.6329, respectively, and the dielectric loss tangent decreases to 0.1840, 0.1641, and 0.1799, respectively. Adding 0.5%, 1.0%, and 1.5% PAAE resin in a single step further reduces the relative permittivity. After the addition of PAAE resin, the relative permittivity of the base paper decreased to 3.8063, 3.5788, and 3.7294, respectively, and the dielectric loss tangent decreased to 0.1952, 0.1908, and 0.1937, respectively. When the amount of PAAE resin added was 1.0%, the relative permittivity of the base paper prepared by adding it in stages decreased by about 7.44% and the dielectric loss tangent decreased by about 13.99% compared with the single addition. The above results indicate that the addition of PAAE resin can reduce the relative permittivity and dielectric loss tangent of cellulose base paper. Under the same PAAE resin addition conditions, the staged addition has better dielectric properties than the single addition, which is more conducive to reducing the power frequency polarization and dielectric loss of the base paper.
[0070] According to the appendix Figure 2-5 Comparing the bar charts, when PAAE was added in stages, as the addition amount increased from 0.5% to 1.5%, the overall electrical properties of the crepe paper base paper showed a trend of first improving and then slightly declining. The optimal overall electrical properties were observed when the PAAE resin addition amount was 1.0% of the oven-dry fiber mass of the pulp. For the same addition amount, the crepe paper base paper prepared by adding PAAE in stages exhibited better electrical properties compared to sequential addition.
[0071] To compare the effect of the resin / slurry premixing ratio on the electrical insulation properties of crepe paper base paper, the volume resistivity and DC breakdown field strength of the crepe paper base paper prepared in Examples 4-5 were tested. The test results were taken as the average of three parallel tests. The test results are shown in Table 2 and compared with Example 2 and Comparative Example 2.
[0072] Table 2. Test results of electrical insulation properties of the crepe paper base paper of Examples 2, 4-5 and Comparative Example 2.
[0073] According to the test results in Table 2, under the same resin addition amount, the premixing ratio of resin and slurry can affect the electrical insulation performance of crepe paper base paper. With the increase of both slurry and resin premixing ratios, the electrical insulation performance of crepe paper base paper generally shows a trend of first improving and then slightly declining, with the best electrical insulation performance observed when the slurry and resin premixing ratios were 20% and 40%, respectively. Furthermore, under the same resin addition amount, compared to the single addition in Comparative Example 2, the base paper prepared by adding resin in stages with different premixing ratios all exhibited superior electrical insulation performance, showing promising application prospects in electrical component insulation.
[0074] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.
Claims
1. A method for preparing crepe paper base paper, characterized in that, Includes the following steps: (1) Provide cellulose pulp and polyamide polyamine-epoxychloropropane resin; (2) A portion of the cellulose slurry is premixed with a portion of the polyamide polyamine-epoxychloropropane resin to obtain a premixed slurry; (3) Add the remaining amount of the cellulose slurry and the remaining amount of the polyamide polyamine-epoxychloropropane resin to the premixed slurry and mix to obtain a mixed slurry; (4) The mixed slurry is wet-processed to obtain crepe paper base paper.
2. The method for preparing a crepe paper base paper according to claim 1, characterized in that, The total solids content of the polyamide polyamine-epoxychloropropane resin in step (1) is in the mass ratio of the oven-dry fibers of the cellulose pulp to (0.5-1.5):
100.
3. The method for preparing a crepe paper base paper according to claim 1, characterized in that, Based on oven-dry fiber, the cellulose slurry premixed in step (2) accounts for 10-40% of the total mass of the cellulose slurry; and / or, the total solids addition of the polyamide polyamine-epoxychloropropane resin premixed in step (2) accounts for 20-60% of the total mass of the resin.
4. The method for preparing a crepe paper base paper according to claim 1, characterized in that, The premixing in step (2) satisfies one or more of the following characteristics: The premixed pH value is 4.5-6.5; The premixing temperature is 15-45℃; The stirring rate for premixing is 100-800 r / min; The premixing time is 5-40 minutes.
5. The method for preparing a crepe paper base paper according to claim 1, characterized in that, The beating degree of the cellulose pulp is 25-45°SR.
6. The method for preparing a crepe paper base paper according to claim 1, characterized in that, Step (4) of the wet papermaking process includes the following steps: The mixed pulp is wet-formed to obtain wet paper sheets, which are then pressed, dried and heat-cured to obtain crepe paper base paper.
7. A crepe paper base paper, characterized in that, It is prepared by the preparation method described in any one of claims 1-6.
8. The crepe paper base paper according to claim 7, characterized in that, The thickness of the crepe paper base is 0.05-0.13 mm.
9. A type of crepe paper, characterized in that, It is obtained by wrinkling the crepe paper base paper as described in claim 7 or 8.
10. The use of the crepe paper base paper of claim 7 or 8, or the crepe paper of claim 9, in the insulation of electrical components.