A reverse gradient UV-resistant co-extruded PET light diffusion film
The PET light diffusion film with UV absorbers distributed in reverse gradient in a multilayer film structure solves the problems of insufficient UV light blocking and weather resistance in the existing technology, and achieves a balance between high UV blocking, visible light transmission and haze, improves processing stability and UV absorber utilization rate, and has excellent mechanical properties and environmental protection characteristics.
Patent Information
- Application Number
- CN202611560506.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-10
- Publication Date
- 2026-11-17
AI Technical Summary
Existing PET light diffusion films have shortcomings in terms of ultraviolet light blocking and weather resistance, especially in outdoor or semi-outdoor lighting applications, where ultraviolet radiation has a significant impact on the PET matrix and diffusion particles. Furthermore, the existing methods of adding UV absorbers have issues with processing stability and compatibility.
The film employs a multilayer film structure, with UV absorber pre-dispersed masterbatch distributed in a reverse gradient along the film thickness direction. It is formed in one step through co-extrusion and biaxial stretching. The incident layer, intermediate layer, and light-emitting layer contain UV absorbers and diffusion masterbatch, with the intermediate layer having the highest content of diffusion masterbatch. The UV absorber content gradually decreases in the incident layer and light-emitting layer, forming a reverse gradient UV-resistant co-extruded PET light diffusion film.
It achieves a balance between high UV blocking rate, visible light transmittance, and haze, improves processing stability and weather resistance, reduces the amount of UV absorber used, improves the effective utilization rate of UV absorbers, and requires no additional coating layer, possessing excellent mechanical properties and environmental characteristics.
Smart Images

Figure CN123113064A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of light diffusion film technology, specifically to a reverse gradient anti-UV co-extruded PET light diffusion film. Background Technology
[0002] PET light diffusion film is one of the core optical components of a backlight module (BLU), and its main function is to convert point or line light sources such as LEDs into uniform surface light sources. Currently, commercially available PET light diffusion films mainly adopt three technical solutions: single-layer homogeneous structure (light diffusion masterbatch is uniformly mixed into the PET substrate, and the haze is usually in the range of 80-92%), three-layer co-extrusion structure (ABA type, with a low concentration of diffusion masterbatch on the surface layer and a high concentration of diffusion masterbatch in the core layer, representative patents such as CN102096129B, CN109130422A, CN118876548A, etc.), and coating type (a resin layer containing diffusion particles is coated on the surface of the PET base film, representative patents such as CN102768374A, CN110161601A, etc.).
[0003] The aforementioned existing technologies still have room for further improvement. First, some existing PET light diffusion films primarily focus on light diffusion performance, with insufficient attention paid to the long-term blocking and weather resistance synergy of UVA (320-400 nm) and UVB (280-320 nm). In outdoor or semi-outdoor lighting and display applications, the PET substrate, diffusion particles, and adjacent optical components may still be affected by ultraviolet radiation. Second, when using surface coating to impart UV resistance, the different compositions and interface states between the coating and the PET substrate may lead to issues such as adhesion stability, additional solvent / curing processes, and compatibility with subsequent melt recycling. Third, existing multilayer co-extrusion light diffusion schemes mainly focus on the interlayer configuration of diffusion particles; there is still room for optimization regarding the synergistic spatial configuration of UV absorbers and diffusion particles in different film layers.
[0004] Studies have found that when some small-molecule UV absorbers are directly added to PET melt, they may volatilize, thermally degrade, locally accumulate, or be lost through filtration during high-temperature melting, shearing, and residence. Simultaneously, there may be insufficient matching between the solubility parameters and molecular scale of the small-molecule UV absorbers and the PET matrix, potentially leading to migration, precipitation, or crystal formation at higher addition levels or under longer thermal histories. When UV absorbers coexist with diffusing particles such as PMMA, it is also necessary to consider visible light transmission, scattering environment, and system compatibility.
[0005] Therefore, it is necessary to develop a PET light diffusion film that can be formed in one step through co-extrusion and biaxial stretching, and that coordinates UV absorption and light diffusion functions in the film thickness direction, so as to take into account UV blocking, visible light transmission, haze, weather resistance and processing stability. Summary of the Invention
[0006] The purpose of this invention is to achieve a balance between high UV blocking, high visible light transmittance, and high haze in PET light diffusion films, while reducing the processing and compatibility risks that may arise from direct blending of UV absorbers and high loading of a single film layer.
[0007] To achieve the above objectives, this invention discloses a reverse gradient UV-resistant co-extruded PET light diffusion film. The technical solution employed is a multilayer film structure, including an incident layer, an intermediate layer, and a light-emitting layer. The intermediate layer has one or more film structures. At least two layers of the incident layer, intermediate layer, and light-emitting layer contain UV absorber pre-dispersion masterbatch and diffusion masterbatch. The content of the UV absorber pre-dispersion masterbatch gradually decreases from the incident layer to the light-emitting layer until it contains no UV absorber pre-dispersion masterbatch. The diffusion masterbatch content in the intermediate layer is higher than that in the incident layer and the light-emitting layer. Furthermore, at least one layer within the incident layer contains diffusion masterbatch but does not contain UV absorber pre-dispersion masterbatch. The reverse gradient UV-resistant co-extruded PET light diffusion film has a UV blocking rate greater than 99%, a visible light transmittance greater than 85%, and a haze greater than 90%.
[0008] As a preferred embodiment of the present invention, the intermediate layer is the main scattering layer, and the thickness proportions of the three-layer structure in the entire reverse gradient anti-UV co-extruded PET light diffusion film are 15~30%, 50~70%, and 15~30%, respectively.
[0009] As a preferred embodiment of the present invention, the components of the incident layer include 90-96 parts of PET substrate, 3-8 parts of UV absorber pre-dispersion masterbatch, 0.5-2 parts of diffusion masterbatch, and 0.1-0.3 parts of antioxidant by weight; the incident layer primarily functions to preferentially weaken incident ultraviolet radiation while also taking into account primary light diffusion. The main scattering layer comprises, by weight, 78-88 parts of PET substrate, 10-18 parts of diffusion masterbatch, 0.5-2 parts of UV absorber pre-dispersion masterbatch, and 0.1-0.3 parts of antioxidant. The main scattering layer primarily functions to diffuse light and supplements the absorption of residual UV rays that have passed through the incident layer with a lower content of UV absorber. The components of the light-emitting layer by weight include 94-99 parts of PET substrate, 0.5-2 parts of diffusion masterbatch, 0.3-1 parts of anti-blocking masterbatch, and 0.1-0.3 parts of antioxidant.
[0010] The incident layer primarily resists UV radiation, with diffusion as a secondary function; the main scattering layer primarily diffuses UV radiation, with residual UV absorption as a secondary function; the light-emitting layer serves the functions of light emission, surface protection, and anti-adhesion.
[0011] As a preferred embodiment of the present invention, the UV absorber pre-dispersed masterbatch uses PET as the carrier resin, and the mass fraction of the effective UV absorber component in the masterbatch is 20-40%. The thermal decomposition temperature of the effective UV absorber component is not lower than 300℃, and it has heat resistance suitable for PET melt processing.
[0012] As a preferred embodiment of the present invention, the UV absorber pre-dispersion masterbatch in the incident layer comprises benzotriazole UV absorbers and / or triazine UV absorbers; the UV absorber pre-dispersion masterbatch in the main scattering layer comprises triazine UV absorbers.
[0013] In a preferred embodiment of the present invention, both the diffusion masterbatch and the anti-blocking masterbatch are PMMA microspheres. The average particle size of the diffusion masterbatch is 3 μm, and the average particle size of the anti-blocking masterbatch is 6 μm. The term "masterbatch" refers to granules formed from a carrier resin and functional microspheres, and is not equivalent to the PMMA microspheres themselves.
[0014] As a preferred technical solution of the present invention, a UV absorber pre-dispersion masterbatch is first prepared, and then the UV absorber pre-dispersion masterbatch is separately formulated, mixed and dried with other raw materials of each layer, followed by three-layer co-extrusion casting, longitudinal stretching, transverse stretching, heat setting and annealing, and post-treatment molding.
[0015] As a preferred technical solution of the present invention, the raw materials are dried after mixing to a moisture content of ≤50 ppm; during the three-layer co-extrusion casting, the extrusion temperature is below 290℃, the melt extruded from the three-layer co-extrusion die adheres closely to the quench roll, the quench roll temperature is 30-40℃, the rotation speed is 8-15 m / min, and a three-layer composite casting is obtained; the melt pressure of the co-extrusion die is 12-18 MPa, and the residence time of the UV absorber in the molten state is <5 min.
[0016] As a preferred technical solution of the present invention, the casting stretching includes longitudinal stretching and transverse stretching, wherein the transverse stretching temperature is higher than that of the longitudinal stretching temperature and the transverse stretching temperature does not exceed 120°C.
[0017] As a preferred embodiment of the present invention, during the annealing process, the annealing temperature is 220-240℃, the annealing time is 10-30 seconds, and a longitudinal tension of 5-15 N / m is applied simultaneously.
[0018] The preparation method of the above-mentioned UV-resistant co-extruded PET light diffusion film includes the following steps: S1: Preparation of UV absorber predispersed masterbatch UV absorber (Tinuvin 326 or Tinuvin 1577), dispersant (PET-g-GMA), and carrier PET (intrinsic viscosity 0.75-0.85 dL / g) are mixed in a certain proportion. Hindered phenolic antioxidant (Irganox 1010 or Irganox 1076, 0.3-0.8%) is added. The mixture is then melt-extruded at 250-270℃ using a twin-screw extruder, water-cooled, and pelletized to obtain UV absorber pre-dispersion masterbatch. The UV absorber content in the masterbatch is 20-40%. S2: Raw material pretreatment Each of the three raw materials was added to a high-speed mixer for dry mixing at a speed of 800-1200 r / min for 10-20 min. After dry mixing, the mixture was sent to a vacuum drying oven and dried at 140-160℃ for 4-6 h, with the moisture content of the raw materials controlled to be ≤50ppm, to obtain the premix of each layer.
[0019] S3: Three-layer co-extruded sheet The three-layer premix was fed into three twin-screw extruders, with the extrusion temperature window precisely controlled below 290℃ to prevent thermal degradation of the UV absorber caused by excessive temperature. The melt from each extruder was filtered and degassed before being extruded through a three-layer co-extrusion die to achieve composite extrusion. The melt adhered tightly to the quench roll, which was maintained at 30-40℃ and rotated at 8-15 m / min, to produce a three-layer composite casting. The melt pressure at the co-extrusion die was 12-18 MPa, and the residence time of the UV absorber in the molten state was <5 min (to avoid thermal degradation). S4: Longitudinal Stretch (MDO) The composite casting is fed into the longitudinal stretching unit through guide rollers and heated to 80-100℃ (the stretching temperature does not exceed 100℃, in order to take into account the PET chain segment movement ability, stretching stability and longitudinal orientation structure formation). The stretching ratio is 3.0-3.5 times and the preheating time is 15-25 seconds. S5: Lateral Stretch (TDO) After longitudinal stretching, the film enters a tenter frame for transverse stretching at a temperature of 100-120℃ (slightly higher than the longitudinal stretching temperature) and a stretching ratio of 3.2-4.0 times. This is matched with the longitudinal stretching parameters to achieve isotropic film. During the stretching process, excessively fast stretching can cause microcracks, while excessively slow stretching can lead to excessive crystallinity. S6: Heat setting and annealing treatment The biaxially stretched film is sent to an annealing furnace for heat setting at a temperature of 220-240℃ (higher than the operating temperature but lower than the film melting point) for 10-30 seconds to eliminate internal stress. At the same time, a longitudinal tension of 5-15 N / m is applied to prevent orientation loss caused by thermal relaxation. The annealing process locks in the film structure, reduces thermal shrinkage, and increases the heat distortion temperature. S7: Post-processing molding The heat-set film is cooled and forced to <50℃ before being wound up; then corona treatment is performed (power 5-10 kW, processing speed 10-15 m / min) to improve the adhesion of the film surface; finally, the edges are trimmed and wound up to obtain the finished UV-resistant co-extruded PET light diffusion film.
[0020] Compared with existing technologies, the beneficial effects of this invention are as follows: By employing a UV absorber pre-dispersed masterbatch with a reverse concentration gradient in the multilayer film structure, this invention enables the PET light diffusion film to achieve long-term UV blocking and weather resistance synergistically, reducing the impact of UV irradiation on the PET matrix, diffusion particles, and adjacent optical components. By using a high heat-resistant UV absorber, combined with the pre-dispersed masterbatch, the UV absorber can be integrally formed into the film structure during the melt co-extrusion of the light diffusion film, endowing the light diffusion film with UV resistance while achieving higher stability. Furthermore, the preparation process is simple and facilitates subsequent melt recovery. The reverse concentration gradient arrangement of the UV absorber pre-dispersed masterbatch enables an effective utilization rate of 98.2%, superior to 71.5% with uniform content distribution and 48.7% with positive concentration gradient arrangement, thus reducing the amount of UV absorber used by 30% under the same UV blocking conditions. Furthermore, by making the diffusion masterbatch content in the intermediate layer higher than that in the incident layer and the light-emitting layer, and by ensuring that at least one layer in the film structure within the incident layer contains diffusion masterbatch but not UV absorber pre-dispersed masterbatch, the interference of UV absorber absorption on visible light is effectively avoided, enabling the visible light transmittance of the overall film structure to reach over 85%. The UV absorber arranged in a reverse gradient can reduce the encapsulation of diffusion masterbatch by UV absorber in the intermediate layer and the light-emitting layer, thereby enabling the haze of the overall film structure to reach over 90%, which is superior to that of existing light diffusion films (80~88%).
[0021] Furthermore, the light diffusion film prepared by this invention has a tensile strength greater than 140 MPa, an elongation at break greater than 80%, and a thermal shrinkage rate of less than 1.0% at 180℃ / 30 min, exhibiting excellent mechanical properties.
[0022] Furthermore, the light diffusion film of the present invention only requires one co-extrusion molding during preparation, without the need for subsequent coating; it is made of 100% PET material (UV absorber is introduced through physical blending of pre-dispersed masterbatch without changing the PET molecular chain structure), and can be directly melted and granulated, with a recycling rate of more than 95%; it is free of organic solvent pollution and is green and environmentally friendly.
[0023] Furthermore, this invention employs co-extrusion and biaxial stretching processes to integrate UV protection and light diffusion functions, eliminating the need for an additional UV functional coating layer. The film uses PET as the main resin, and the UV absorber is introduced through blending via pre-dispersed masterbatch, eliminating the need to directly introduce UV-absorbing groups into the PET backbone via copolymerization. Moreover, the light diffusion film simultaneously achieves high UV blocking rate, visible light transmittance, and haze, while exhibiting good QUV aging stability. Attached Figure Description
[0024] Figure 1 This is a schematic diagram of the three-layer membrane structure and the functional allocation of each layer of the present invention; Figure 2 A schematic diagram illustrating the concept of interlayer distribution of three types of UV absorbers: reverse gradient, equal concentration, and positive gradient. Figure 3 This is a schematic diagram of the preparation process of the present invention. Detailed Implementation
[0025] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0026] The performance testing and data processing methods involved in the embodiments and comparative examples are as follows: 1. UV blocking rate: The UV transmittance in the 280-400nm band was measured using a UV-Vis spectrophotometer. UV blocking rate = 1 - UV transmittance. 2. Visible light transmittance and haze: Tested according to GB / T 2410-2008 Test methods for light transmittance and haze of transparent plastics; 3. Mechanical properties (tensile strength, elongation at break): Tested according to GB / T 13022-1991 Test method for tensile properties of plastic films. The specimen is a strip with a length of 150 mm and a width of (15±0.1) mm. The distance between the clamps is 100 mm. The test speed is (250±25) mm / min. 4. Heat shrinkage rate: Tested according to GB / T 12027-2004 Test method for dimensional change rate of plastic film, test conditions 150℃ / 30min; 5. QUV aging performance: QUV accelerated aging test was conducted according to ASTM G154. Test conditions: UVA-340 lamp, 0.89 W / m² / nm@340nm, 60℃ / 4h UV + 50℃ / 4h condensation cycle. 6. Surface crystal points: observed visually and microscopically, unit: points / m²; 7. Effective utilization rate of UV absorber: The proportion of UV light absorbed by UV absorber during the propagation of UV light within the membrane was calculated using Monte Carlo ray tracing simulation (TracePro software).
[0027] In the following examples and comparative examples, the concepts of reverse gradient, equal gradient, and positive gradient UV absorber interlayer distribution mentioned are as follows: Figure 2 As shown, this represents the arrangement of concentration gradients. However, it should be noted that... Figure 2 The values in the text only represent relative distribution and do not represent specific concentration values.
[0028] Example 1 This invention discloses a reverse gradient UV-resistant co-extruded PET light diffusion film. The technical solution adopted is a three-layer film structure comprising an incident layer (layer A), a main scattering layer (layer B), and a light emitting layer (layer C). The raw material composition of each layer is as follows: Layer A (by weight): 92.8 parts PET, 6 parts UV absorber predispersed masterbatch (containing Tinuvin 326, UV absorber content in the masterbatch is 30%), 1 part diffusion masterbatch (PMMA microspheres, average particle size 3μm), 0.2 parts antioxidant 1076; the effective UV absorber mass fraction of Layer A is 6.0 × 30% = 1.80%.
[0029] Layer B (by weight): 82.6 parts PET, 16 parts diffusion masterbatch (PMMA microspheres, average particle size 3μm), 1.2 parts UV absorber predispersant masterbatch (containing Tinuvin 1577, UV absorber content in the masterbatch is 25%), 0.2 parts antioxidant 1076; the effective UV absorber mass fraction in layer B is 1.2 × 25% = 0.30%.
[0030] Layer C (parts by weight): 98.3 parts PET, 1 part diffusion masterbatch (PMMA microspheres, average particle size 3μm), 0.5 parts anti-blocking masterbatch (PMMA microspheres, particle size 6μm), 0.2 parts antioxidant 1076; no UV absorber pre-dispersion masterbatch is added to reduce the potential impact of UV absorbers on visible light transmission.
[0031] Layer thickness ratio: A:B:C=20:60:20, total film thickness 188μm. This results in an inverse gradient distribution of effective UV absorber from 1.80% to 0.30% to 0, while the diffusion masterbatch exhibits a "low-high-low" stratified configuration from 1.0 part to 16.0 parts to 1.0 part.
[0032] In this embodiment, the UV absorber predispersed masterbatch contains a single-component UV absorber.
[0033] Functional allocation of each layer of the membrane structure as follows Figure 1 As shown.
[0034] The preparation method of the above-mentioned reverse gradient UV-resistant co-extruded PET light diffusion film is as follows: Figure 3 As shown, specifically: Step 1, Preparation of UV absorber pre-dispersion masterbatch: Tinuvin 326, PET-g-GMA dispersant (8% of Tinuvin 326), carrier PET (intrinsic viscosity 0.80 dL / g), and antioxidant Irganox 1076 (0.5% of Tinuvin 326) are mixed in proportion, melt-extruded at 260℃ using a twin-screw extruder, and then water-cooled and pelletized to obtain UV absorber pre-dispersion masterbatch (UV absorber content in the masterbatch is 30%); Tinuvin 1577 masterbatch is prepared in the same way (content 25%). Step 2, raw material pretreatment: each layer of raw material is added to a high-speed mixer for dry mixing at a speed of 1000 r / min for 15 min; after dry mixing, it is sent to a vacuum drying oven and vacuum dried at 160℃ for 5 h, with the moisture content controlled to be ≤50ppm, to obtain the premix of each layer. Step 3, Three-layer co-extrusion casting: The premixed materials of layers A, B, and C are respectively added to three twin-screw extruders. The extrusion temperature of layer A is 272℃, layer B is 278℃, and layer C is 283℃ to avoid thermal degradation of the UV absorber due to excessive temperature. After filtration and degassing, the melt from each extruder is compounded through the ABC three-layer co-extrusion die. The melt pressure of the co-extrusion die is 14 MPa, the residence time is 4.5 min, and the melt is tightly attached to the quench roll. The quench roll temperature is 35℃ and the rotation speed is 12 m / min to obtain the three-layer composite casting. Step 4, longitudinal stretching: The composite casting is fed into the longitudinal stretching unit through guide rollers, heated to 90°C, with a stretching ratio of 3.2 times and a preheating time of 20 seconds; Step 5, Lateral stretching: The longitudinally stretched film is fed into a tenter frame for lateral stretching at a temperature of 115℃ and a stretching ratio of 3.6 times, matching the longitudinal stretching parameters to achieve isotropic film. During the stretching process, excessively fast stretching can cause microcracks, while excessively slow stretching can lead to excessive crystallinity. Step 6, Heat setting annealing: The biaxially stretched film is sent into an annealing furnace for heat setting treatment at a temperature of 230℃ (higher than the operating temperature but lower than the film melting point) for 15 seconds to eliminate internal stress; at the same time, a longitudinal tension of 10 N / m is applied to prevent orientation loss caused by thermal relaxation; the annealing process locks in the film structure, reduces thermal shrinkage, and increases the heat distortion temperature. Step 7, Post-processing: Cool the heat-set film to <50℃ and then roll it up; then perform corona treatment (power 7 kW, processing speed 12 m / min) to improve the adhesion of the film surface; finally trim the edges and roll it up to obtain the finished UV-resistant co-extruded PET light diffusion film.
[0035] In Example 1, UV light is incident from layer A. In layer A (containing 6 parts of pre-dispersed masterbatch, corresponding to a UV absorber concentration of approximately 3.6%), the UV light is efficiently absorbed (absorption rate of approximately 91%), with intensity attenuating to approximately 9%. After entering layer B (containing 1.2 parts of pre-dispersed masterbatch, with a UV absorber concentration of approximately 0.7%), the residual UV light is further absorbed by approximately 9%, resulting in a cumulative blocking rate of approximately 99.6%. By the time UV light reaches layer C, it has been almost completely absorbed, eliminating the need for a UV absorber. The high concentration of UV absorber in layer A corresponds to the absorption requirements when UV light is at its strongest, while the absence of UV absorber in layer C avoids interference from UV absorber absorption on visible light, thus maintaining a high visible light transmittance of 87.2%. Meanwhile, the UV absorbers are concentrated in layers A and B, with layer B having a low UV absorber content. Combined with layer C having no UV absorbers, this maintains a haze of 92.5%. The high UV absorber load in layer A is used to preferentially attenuate incident ultraviolet radiation, the low load in layer B is used to supplement the absorption of residual UV, and layer C has no UV absorbers to reduce the potential impact on visible light transmission.
[0036] This embodiment employs different interlayer spatial configurations of UV absorbers and diffusing particles, enabling each film layer to perform different functions: the incident layer contains a higher concentration of effective UV absorbers to preferentially attenuate incident UV radiation; the main scattering layer contains a higher concentration of diffusing particles and a lower concentration of UV absorbers to form the main light diffusion and further process residual UV; the light-emitting layer contains no UV absorbers to reduce the potential impact of UV absorbers on visible light transmission. The interlayer advantages of this embodiment are not solely determined by Beer-Lambert's law in an ideal, homogeneous, non-scattering medium, but also by the combined effects of UV absorption, multiple refractions / scattering caused by diffusing particles, actual optical path length, visible light loss, additive compatibility, and photoaging stability.
[0037] Example 2 The difference between this embodiment and Example 1 is that in the raw material ratio, layer A (parts by weight): 93.8 parts PET, 5 parts UV absorber pre-dispersion masterbatch (containing 3.3 parts Tinuvin 326 + 1.7 parts Tinuvin 1577), 1 part diffusion masterbatch, and 0.2 parts antioxidant; the effective UV absorber mass fraction in layer A is 3.3 × 30% + 1.7 × 25% = 1.415%, approximately 1.42%. Layer B (parts by weight): 82.8 parts PET, 16 parts diffusion masterbatch, 1 part UV absorber predispersion masterbatch (containing 0.7 parts Tinuvin 326 + 0.3 parts Tinuvin 1577), 0.2 parts antioxidant; the effective UV absorber mass fraction in Layer B is 0.7 × 30% + 0.3 × 25% = 0.285%, approximately 0.29%; Layer C: Same as in Example 1.
[0038] This structure forms an effective UV absorber inverse gradient of approximately 1.42% → 0.29% → 0.
[0039] The layer thickness ratio and total film thickness are the same as in Example 1.
[0040] In this embodiment, the UV absorber predispersed masterbatch contains a multi-component UV absorber. Preparation process: Same as in Example 1, except that the UV absorber predispersed masterbatch needs to be prepared separately with Tinuvin 326 masterbatch (content 30%) and Tinuvin 1577 masterbatch (content 25%), premixed at a mass ratio of 2:1 and then added to the A layer material.
[0041] Example 3 The difference between this embodiment and Example 1 is that in the raw material ratio, layer A (parts by weight): 93.8 parts PET, 5 parts UV absorber pre-dispersion masterbatch (containing Tinuvin 326), 1 part diffusion masterbatch, and 0.2 parts antioxidant. Layers B and C: same as in Example 1. The layer thickness ratio A:B:C = 30:50:20, the UV absorber content in layer A is 5%, and the total film thickness is 188 μm.
[0042] This embodiment compensates for the reduced concentration of UV absorber in layer A by increasing the thickness ratio of layer A, and is used to examine the synergistic effect of "concentration-layer thickness".
[0043] Preparation process: Same as in Example 1.
[0044] Example 4 The difference between this embodiment and Embodiment 1 is that, in the raw material ratio, Layer A (parts by weight): 90.8 parts PET, 8 parts UV absorber pre-dispersion masterbatch (containing Tinuvin 326), 1 part diffusion masterbatch, and 0.2 parts antioxidant; the effective UV absorber mass fraction of Layer A is 2.40%. Layers B and C: Same as in Example 1. Layer thickness ratio A:B:C = 15:65:20, UV absorber content in layer A is 8%, and total film thickness is 188 μm.
[0045] This embodiment is used to examine the optical and processing performance when the UV load of layer A is increased while the thickness of layer A is reduced.
[0046] Preparation process: Same as in Example 1.
[0047] Example 5 The difference between this embodiment and Embodiment 1 is that: Layer A: 92.4 parts by weight of PET substrate, 4.0 parts by weight of UV absorber predispersant masterbatch containing Tinuvin 326, 2.4 parts by weight of UV absorber predispersant masterbatch containing Tinuvin 1577, 1.0 part by weight of diffusion masterbatch, and 0.2 parts by weight of antioxidant 1076, totaling 100 parts by weight. The effective UV absorber mass fraction of Layer A is 1.80%.
[0048] Layer B: 82.73 parts by weight of PET substrate, 16.0 parts by weight of diffusion masterbatch, 0.67 parts by weight of UV absorber pre-dispersion masterbatch containing Tinuvin 326, 0.40 parts by weight of UV absorber pre-dispersion masterbatch containing Tinuvin 1577, and 0.20 parts by weight of antioxidant 1076, totaling 100 parts by weight. The effective UV absorber mass fraction of Layer B is approximately 0.30%.
[0049] Layer C is the same as in Example 1, but without the addition of UV absorbers.
[0050] The layer thickness ratio of A:B:C is 20:60:20, and the total film thickness is 188 μm. Weighted by the layer thickness ratio, the relative amount of effective UV absorber in the entire film is 1.80%×20%+0.30%×60%=0.54%.
[0051] This embodiment serves as a strict comparison with Comparative Examples 1 and 7 to determine the spatial distribution of the UV absorber. All three samples maintained the same total effective UV absorbed dose, total effective amount of Tinuvin 326 / Tinuvin 1577, diffusion system, layer-to-thickness ratio, total film thickness, and processing technology; only the spatial distribution of the UV absorber in layers A, B, and C was changed.
[0052] Example 6 The difference between this embodiment and Embodiment 1 is that the total film thickness is adjusted to 170 μm, corresponding to theoretical thicknesses of layers A, B, and C of approximately 34 μm, 102 μm, and 34 μm, respectively.
[0053] This embodiment is used to verify UV blocking rate, visible light transmittance, haze, mechanical properties and thermal shrinkage properties at a lower total film thickness.
[0054] Example 7 The difference between this embodiment and Embodiment 1 is that the total film thickness is adjusted to 220 μm, corresponding to theoretical thicknesses of layers A, B, and C of approximately 44 μm, 132 μm, and 44 μm, respectively.
[0055] This embodiment is used to verify UV blocking rate, visible light transmittance, haze, mechanical properties and thermal shrinkage properties at a higher total film thickness.
[0056] Comparative Example 1 The difference between this comparative example and Example 5 lies in the proportions of the raw materials. Layer A: 98.0 parts by weight of PET substrate, 0.5 parts by weight of UV absorber predispersed masterbatch containing Tinuvin 326, 0.3 parts by weight of UV absorber predispersed masterbatch containing Tinuvin 1577, 1.0 part by weight of diffusion masterbatch, and 0.2 parts by weight of antioxidant, totaling 100 parts by weight; the effective UV absorber mass fraction is 0.225%.
[0057] Layer B: 82.2 parts by weight of PET substrate, 16.0 parts by weight of diffusion masterbatch, 1.0 part by weight of UV absorber predispersant masterbatch containing Tinuvin 326, 0.6 parts by weight of UV absorber predispersant masterbatch containing Tinuvin 1577, and 0.2 parts by weight of antioxidant, totaling 100 parts by weight; the effective UV absorber mass fraction is 0.45%.
[0058] Layer C: 94.3 parts by weight of PET substrate, 1.0 part by weight of diffusion masterbatch, 0.5 parts by weight of anti-blocking masterbatch, 2.5 parts by weight of UV absorber pre-dispersion masterbatch containing Tinuvin 326, 1.5 parts by weight of UV absorber pre-dispersion masterbatch containing Tinuvin 1577, and 0.2 parts by weight of antioxidant, totaling 100 parts by weight; the effective UV absorber mass fraction is 1.125%.
[0059] The relative amount of effective UV absorber in the whole film, weighted by layer thickness, is 0.225%×20%+0.45%×60%+1.125%×20%=0.54%.
[0060] In this comparative example, the UV absorber concentration is arranged in a positive gradient structure that gradually increases from the incident side to the light-emitting side.
[0061] Comparative Example 2 The difference between this comparative example and Example 1 is that all the UV absorber predispersed masterbatch in the raw material ratio is replaced with Tinuvin 326 powder. Specifically, the content of Tinuvin 326 powder in layer A is 1.8 parts, the content of Tinuvin 1577 powder in layer B is 0.3 parts, and layer C does not contain Tinuvin 326 powder.
[0062] The reduction in the total mass of raw materials due to the replacement of UV absorbers is made up with PET substrate.
[0063] In the preparation process, the UV absorber pre-dispersion masterbatch preparation (step 1) is no longer performed. Instead, step 2 is performed directly, in which Tinuvin 326 powder is directly added to the high-speed mixer as one of the raw materials.
[0064] This comparative example uses direct powder blending to verify the role of pre-dispersed masterbatch technology.
[0065] Comparative Example 3 The difference between this comparative example and Example 1 is that the raw material ratio is as follows: Layer A (parts by weight): 98.8 parts PET, 1.0 part diffusion masterbatch, 0.2 parts antioxidant; Layer B (parts by weight): 83.8 parts PET, 16 parts diffusion masterbatch, 0.2 parts antioxidant; Layer C (parts by weight): Same as in Example 1.
[0066] The raw materials do not contain UV absorber pre-dispersed masterbatch, and step 1 is omitted from the preparation method.
[0067] This comparative example uses a method without UV absorbers to verify the effect of UV absorbers. Comparative Example 4 First, a PET light-diffusing base film is prepared. The dry components of the base film, per 100 parts by weight, consist of: 97.8 parts by weight of PET substrate, 2.0 parts by weight of diffusion masterbatch, and 0.2 parts by weight of antioxidant. After biaxial stretching, a UV functional coating is prepared on the surface of the base film. The dry coating solids, per 100 parts by weight, consist of 92 parts by weight of acrylate resin and 8 parts by weight of Tinuvin 326, with a dry coating thickness of approximately 3 μm. Organic solvents used in application are not included in the 100 parts by weight of the dry coating.
[0068] This comparative example is used to compare the differences between the surface-coated structure and the integrated co-extrusion structure of Example 1 in terms of UV barrier properties, QUV stability, coating integrity, and process complexity. Comparative Example 5 The difference between this comparative example and Example 1 is that the UV absorber predispersed masterbatch content in layer A is 0.5 parts; the reduction in the total mass of raw materials due to the decrease in the UV absorber predispersed masterbatch content is made up with PET substrate.
[0069] This comparative example is used to verify the change in UV blocking performance when the amount of pre-dispersed masterbatch of the incident layer UV absorber is too low, and to help determine the lower boundary of the A-layer formulation. Comparative Example 6 This comparative example simulates the window film scheme of Chinese patent CN104842608A: the UV absorber is located in the core layer (intermediate layer), introduced by PET copolymer modification (chemical bonding), and has no diffusion function.
[0070] Raw material ratio: The core layer is benzotriazole modified PET copolymer (containing UV absorber) and PET homopolymer, with a mass ratio of 40:60; the upper and lower surface layers are nano-inorganic modified PET copolymer and PET homopolymer, with a mass ratio of 30:70; the layer thickness ratio is upper:core:lower = 2:26:2, the total film thickness is 30μm, and there is no diffusion masterbatch.
[0071] Preparation process: Refer to the process described in Chinese patent CN104842608A: melt extrusion at 260-285℃, rapid cooling casting, longitudinal stretching (80-90℃, 3.0-3.6 times), transverse stretching (100-140℃, 3.4-4.4 times), heat setting (220-250℃).
[0072] Because the material system, total film thickness, and functional objectives of this scheme differ from those of this invention, it is only used as a technical route reference and not as a strictly univariate quantitative comparative example. Comparative Example 7 This comparative example simulates the scheme of Chinese patent CN109817739A: the UV absorber is set at the same concentration (0.5-3% by mass) in layers A and B, and there is no UV absorber in layer C. Since the specific concentration is not fully specified in the patent, this comparative example uses a UV absorber mass fraction of 0.675% as the UV absorber concentration in layers A and B. The total amount of UV absorber in layers A and B is the same as that in Example 5, which is consistent with the 0.5-3% range in CN109817739A.
[0073] Raw material ratio: Layer A (parts by weight): 96.4 parts PET, 1.5 parts UV absorber predispersant masterbatch containing Tinuvin 326, 0.9 parts UV absorber predispersant masterbatch containing Tinuvin 1577, 1 part diffusion masterbatch, 0.2 parts antioxidant; the effective UV absorber mass fraction of Layer A is 0.675%; Layer B (parts by weight): 81.4 parts PET, 16 parts diffusion masterbatch, 1.5 parts UV absorber predispersant masterbatch containing Tinuvin 326, 0.9 parts UV absorber predispersant masterbatch containing Tinuvin 1577, and 0.2 parts antioxidant; the effective UV absorber mass fraction in Layer B is also 0.675%. Layer C (parts by weight): Same as in Example 1.
[0074] The layer thickness ratio A:B:C = 20:60:20, and the total film thickness is 188 μm.
[0075] The relative amount of effective UV absorber in the whole film is 0.675%×20%+0.675%×60%=0.54%, the same as in Example 5.
[0076] Preparation process: Same as in Example 1.
[0077] The test results are detailed in Tables 1 and 2.
[0078] Table 1 Table 2 Data Analysis Based on the data listed in Tables 1 and 2, a preliminary comparison can be made of the performance changes under different interlayer structures, UV absorber formulations, and film thickness conditions. 1. Influence of Spatial Distribution of UV Absorbers. Examples 5, 7, and 1 maintained essentially the same total effective UV absorbed dose, total effective amount of Tinuvin 326 / Tinuvin 1577, diffusion system, A:B:C layer thickness ratio, and total film thickness, mainly altering the interlayer spatial distribution of the UV absorbers. Optical testing results showed that Example 5 achieved a UV blocking rate of 99.62%, 79.24%, and 18.31%, respectively. The corresponding residual UV transmittances were approximately 0.38%, 0.76%, and 1.69%. Based on the predicted values, with the same total effective UV absorber amount, the reverse gradient structure reduces residual UV transmittance by approximately 50% compared to the equal concentration structure, and by approximately 77% compared to the positive gradient structure. These results indicate that the interlayer spatial configuration of the UV absorbers significantly affects the final UV shielding efficiency; a configuration with a high concentration in the incident layer, a low concentration in the main scattering layer, and no UV absorber in the emitting layer exhibits better blocking effects.
[0079] 2. Synergistic effect of UV absorber concentration and layer thickness. A comparison of Examples 1, 3, and 4 shows that UV blocking performance does not simply increase monotonically with a simple increase in the effective UV absorber mass fraction in layer A. In Example 3, the effective UV absorber mass fraction in layer A was 1.50%, and the layer thickness increased to 30%, achieving a UV blocking rate of 99.80%, but the visible light transmittance decreased to 85%. In Example 4, the effective UV absorber mass fraction in layer A increased to 2.40%, while the layer thickness decreased to 15%, maintaining a UV blocking rate of 99.60%, while the visible light transmittance increased to 88.00%, and the haze was 93.00%. This trend indicates that the overall performance of the membrane material depends on the combined effect of UV absorber concentration, functional layer thickness, and interlayer position, rather than simply relying on increasing the amount of UV absorber used.
[0080] 3. Effect of Total Film Thickness on Optical Performance. Under the same formulation and thickness ratio for each layer, the total film thicknesses of Examples 6, 1, and 7 were 170 μm, 188 μm, and 220 μm, respectively. This corresponded to an increase in UV blocking efficiency from 99.32% to 99.60% and 99.84%, an increase in haze from 90.39% to 92.50% and 95.17%, and a decrease in visible light transmittance from 88.35% to 87.20% and 85.19%. Therefore, under the established model conditions, increasing the film thickness is beneficial for improving UV blocking efficiency and haze, but it also leads to a decrease in visible light transmittance. 170–220 μm can be considered as the preferred film thickness range for subsequent experiments, with the area around 188 μm exhibiting a relatively balanced performance in terms of UV blocking, transmittance, and diffusion; the final determination of this range should still be based on actual sample preparation results.
[0081] 4. Effect of Composite UV Absorption System. Example 2 used a composite predispersed masterbatch of Tinuvin 326 and Tinuvin 1577, with effective UV absorber mass fractions of approximately 1.42% and 0.29% in layers A and B, respectively. The UV blocking rate was 99.70%, the visible light transmittance was 86.80%, and the haze was 92.30%. These results indicate that even with a reduction in the total effective UV absorber concentration in layer A, it is still possible to achieve high UV blocking by using composite configurations of different types of UV absorbers.
[0082] 5. Necessity of UV Absorber. In Comparative Example 3, without adding a UV absorber, the UV blocking rate was only 28.0%, while the visible light transmittance and haze remained at 88.5% and 91.8%, respectively. In Comparative Example 5, after reducing the effective UV absorber in layer A to 0.15%, the UV blocking rate reached 86.84%. Therefore, it can be preliminarily concluded that the high UV blocking capability mainly stems from a specially formulated UV absorption system, and when the UV absorber content in the incident layer is too low, relying solely on the low concentration of supplementary absorption in layer B is insufficient to achieve a blocking target greater than 99%.
[0083] 6. Comparison of pre-dispersed masterbatch and direct powder blending. Example 1 and Comparative Example 2 maintained consistency in terms of UV absorber type, effective addition amount, and interlayer configuration. The main difference was that the former used pre-dispersed masterbatch, while the latter used direct blending of UV absorber powder. Test results showed that pre-dispersion treatment can improve the effective retention, dispersion uniformity, and film surface defects of UV absorbers during high-temperature co-extrusion, and further enhance UV blocking and weather resistance.
[0084] 7. Comparison of different technical routes. Comparative Examples 4 and 6 represent surface-coated UV functional films and core-layer copolymer UV absorption structures, respectively. Because their material systems, total film thickness, processing methods, or functional objectives differ significantly from those of this invention, they are mainly used to illustrate the structural and functional differences between different technical routes and are not suitable for rigorous univariate quantitative attribution to the inverse gradient structure of Example 5.
[0085] 8. Comprehensive Analysis. Based on the above results, under the established formulation and model conditions, configuring the UV absorber along the light propagation direction into an inverse gradient structure of "high incident layer – low main scattering layer – none emitting layer," while concentrating the diffusion component primarily in the main scattering layer, facilitates the spatial division of labor between UV absorption and light diffusion functions. The results also show a clear interdependent relationship between UV blocking rate, visible light transmittance, and haze. By synergistically adjusting the UV absorber concentration, functional layer thickness, and total film thickness, a better balance can be achieved between high UV blocking, high haze, and relatively high visible light transmittance.
[0086] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A reverse gradient UV-resistant co-extruded PET light-diffusing film, characterized in that: It has a multilayer film structure, including an incident layer, an intermediate layer, and a light-emitting layer, wherein the intermediate layer has one or more film structures; at least two of the incident layer, intermediate layer, and light-emitting layer contain UV absorber pre-dispersion masterbatch and diffusion masterbatch, the content of the UV absorber pre-dispersion masterbatch gradually decreases from the incident layer to the light-emitting layer, until it contains no UV absorber pre-dispersion masterbatch; the diffusion masterbatch content of the intermediate layer is higher than that of the incident layer and the light-emitting layer, and at least one layer of the film structure within the incident layer contains diffusion masterbatch but does not contain UV absorber pre-dispersion masterbatch; the UV blocking rate of the reverse gradient anti-UV co-extruded PET light diffusion film is greater than 99%, the visible light transmittance is greater than 85%, and the haze is greater than 90%.
2. The inverse gradient UV-resistant co-extruded PET light diffusion film according to claim 1, characterized in that: The intermediate layer is the main scattering layer, and the thickness proportions of the three-layer structure in the entire reverse gradient anti-UV co-extruded PET light diffusion film are 15~30%, 50~70%, and 15~30%, respectively.
3. The inverse gradient UV-resistant co-extruded PET light diffusion film according to claim 2, characterized in that: The components of the incident layer, by weight, include 90-96 parts of PET substrate, 3-8 parts of UV absorber pre-dispersion masterbatch, 0.5-2 parts of diffusion masterbatch, and 0.1-0.3 parts of antioxidant; The main scattering layer comprises, by weight, 78-88 parts of PET substrate, 10-18 parts of diffusion masterbatch, 0.5-2 parts of UV absorber pre-dispersion masterbatch, and 0.1-0.3 parts of antioxidant; The components of the light-emitting layer by weight include 94-99 parts of PET substrate, 0.5-2 parts of diffusion masterbatch, 0.3-1 parts of anti-blocking masterbatch, and 0.1-0.3 parts of antioxidant.
4. The inverse gradient UV-resistant co-extruded PET light diffusion film according to claim 3, characterized in that: The UV absorber pre-dispersed masterbatch uses PET as the carrier resin, and the mass fraction of the effective UV absorber component in the masterbatch is 20-40%, and the thermal decomposition temperature of the effective UV absorber component is not lower than 300℃.
5. The inverse gradient UV-resistant co-extruded PET light diffusion film according to claim 4, characterized in that: The UV absorber pre-dispersion masterbatch in the incident layer includes benzotriazole UV absorbers and / or triazine UV absorbers; the UV absorber pre-dispersion masterbatch in the main scattering layer includes triazine UV absorbers.
6. The inverse gradient UV-resistant co-extruded PET light diffusion film according to claim 3, characterized in that: Both the diffusion masterbatch and the anti-blocking masterbatch are PMMA microspheres, with the average particle size of the diffusion masterbatch being 3 μm and the average particle size of the anti-blocking masterbatch being 6 μm.
7. The inverse gradient UV-resistant co-extruded PET light diffusion film according to claim 3, characterized in that: First, UV absorber pre-dispersion masterbatch is prepared. Then, the UV absorber pre-dispersion masterbatch is separately formulated, mixed and dried with other raw materials in each layer. Subsequently, three-layer co-extrusion casting, longitudinal stretching, transverse stretching, heat setting and annealing, and post-treatment molding are carried out.
8. The inverse gradient UV-resistant co-extruded PET light diffusion film according to claim 7, characterized in that: After mixing, the raw materials are dried to a moisture content of ≤50 ppm. During the three-layer co-extrusion casting, the extrusion temperature is below 290℃. The melt extruded from the three-layer co-extrusion die adheres closely to the quench roll. The quench roll temperature is 30-40℃, and the rotation speed is 8-15 m / min, thus obtaining a three-layer composite casting. The melt pressure of the co-extrusion die is 12-18 MPa, and the residence time of the UV absorber in the molten state is <5 min.
9. The reverse gradient UV-resistant co-extruded PET light diffusion film according to claim 7, characterized in that: Casting stretching includes longitudinal stretching and transverse stretching. The transverse stretching temperature is higher than the longitudinal stretching temperature, and the transverse stretching temperature does not exceed 120℃.
10. The inverse gradient UV-resistant co-extruded PET light diffusion film according to claim 7, characterized in that: During annealing, the annealing temperature is 220-240℃, the annealing time is 10-30 seconds, and a longitudinal tension of 5-15 N / m is applied simultaneously.
Citation Information
Patent Citations
Three-layer compound antistatic high-performance optical diffusion membrane and preparation method thereof
CN102096129B
Optical-grade coating PET (Polyethylene terephthalate) film and preparation method thereof
CN102768374A
Uvioresistant polyester film for window film and preparation method therefor
CN104842608A
Matte bidirectional stretch polyester film and preparation method thereof
CN109130422A
Polyester film for solar cell backboard
CN109817739A