Solder resist composition, solder resist dry film and solder resist layer
By using a photo-thermal dual-curing system and a compound resin system, the problems of rapid and complete curing and high performance of solder resist dry film at low temperatures have been solved, achieving high crosslinking density, high adhesion and excellent optical performance, making it suitable for solder resist dry film applications in a variety of scenarios.
Patent Information
- Application Number
- CN202611432731.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-17
AI Technical Summary
Existing dry resist films are difficult to cure quickly and completely at low temperatures, and it is difficult to achieve high crosslinking density, high adhesion, high hardness and excellent optical properties at the same time. This results in high risk of thermal damage, high energy consumption and cost, low production efficiency and poor process compatibility during high-temperature curing.
A photo-thermal dual-curing system is adopted, which combines photocationic curing and low-temperature latent thermal curing. This system is combined with a compound resin system of glycidyl methacrylate grafted polyester polyol, epoxy resin and alicyclic epoxy acrylate polymer to achieve rapid and complete curing at low temperature. Fillers, photosensitive monomers and latent curing agents are added to improve crosslinking density and adhesion.
It achieves rapid and complete curing at low temperatures, with a pencil hardness of ≥3H, a cross-cut adhesion of 5B grade, a light transmittance of ≥90% at 550nm wavelength, a haze of ≤1.5%, and a performance degradation of ≤5% after immersion in water and alcohol for 24 hours. It is suitable for flexible substrates, thin substrates, photovoltaic modules, and other scenarios, and is compatible with existing production line processes without the need for additional equipment investment.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of solder resist dry film technology, and more specifically, to a solder resist layer composition, a solder resist dry film, and a solder resist layer. Background Technology
[0002] Solder resist dry film is a core material in the manufacturing processes of printed circuit boards, photovoltaic modules, and semiconductor packaging. Its main functions are to protect the circuit board, prevent solder bridging, and improve the weather resistance and lifespan of components. Currently, the curing process of solder resist dry film typically requires more than 60 minutes at a high temperature of 150~180℃. However, this high-temperature curing process has the following problems:
[0003] 1) High risk of thermal damage: High-temperature curing easily leads to lamination deformation of multilayer boards and warping of thin substrates. It also causes irreversible thermal damage to heat-sensitive components, low-temperature sintered ceramic substrates, and biodegradable substrates, thus limiting the application of advanced packaging structures and new substrates. 2) High energy consumption: Prolonged high-temperature baking requires a large amount of electricity, increasing energy costs and carbon emissions. 3) Low production efficiency: Long-term high-temperature curing becomes a bottleneck in the entire production line, severely restricting capacity expansion. 4) Poor process compatibility: It cannot adapt to temperature-sensitive flexible substrates and roll-to-roll continuous production processes, limiting application scenarios.
[0004] To address the challenges of high-temperature curing, photopolymerization technology has been gradually introduced into the field of solder resist dry films. However, photopolymerization alone has the following performance limitations: 1) Insufficient crosslinking density: Photopolymerization alone cannot achieve the same crosslinking density as thermopolymerization, resulting in a film pencil hardness typically ≤2H, and insufficient abrasion resistance and chemical resistance. 2) Poor substrate adhesion: The interfacial bonding between UV-cured films and polyethylene terephthalate (PET) and copper foil substrates is weak, achieving only 3B~4B grade in cross-cut adhesion tests, leading to easy peeling and delamination with long-term use. 3) Insufficient durability: Alcohol resistance rapidly declines with long-term use, with performance decreasing by 20~30% after 24 hours of solvent immersion. 4) Poor curing uniformity: Extremely sensitive to film thickness; when film thickness >30μm, incomplete curing of the bottom layer and over-curing of the surface layer are prone to occur, requiring specialized high-precision UV curing equipment, resulting in high equipment investment costs.
[0005] Therefore, there is an urgent need to develop a photosensitive solder resist dry film that can be rapidly and completely cured at low temperatures, while also taking into account high crosslinking density, high adhesion, high hardness and excellent optical properties. Summary of the Invention
[0006] The main objective of this invention is to provide a solder resist composition, a solder resist dry film, and a solder resist layer to solve the problems in the prior art where solder resist dry films are difficult to cure quickly and completely at low temperatures, and at the same time, it is difficult to achieve high crosslinking density, high adhesion, high hardness, and excellent optical properties.
[0007] To achieve the above objectives, according to one aspect of the present invention, a solder resist composition is provided, comprising, by weight parts: 55-75 parts of a matrix resin, 10-50 parts of a filler, 0.5-5 parts of a thermal initiator, 2-8 parts of a cationic photoinitiator, 15-25 parts of a photosensitive monomer, 10-18 parts of a latent curing system, and 5-10 parts of a low-temperature activating agent; the matrix resin comprises glycidyl methacrylate grafted polyester polyol; the matrix resin further comprises epoxy resin and / or an acrylate polymer containing alicyclic epoxy.
[0008] The base resin of this application uses glycidyl methacrylate-grafted polyester polyol as the core, combined with epoxy resin and acrylate polymers containing alicyclic epoxy to form a composite resin system, enabling the solder resist composition to achieve both photosensitivity and low-temperature curing activity. The carbon-carbon double bond of the methacryloyloxy group in the glycidyl methacrylate-grafted polyester polyol, combined with the highly reactive epoxy groups in the epoxy resin, can both match the photocuring system for exposure imaging and undergo cross-linking reactions with the thermocuring system at low temperatures, thus solving the problem of insufficient low-temperature reactivity of traditional resins. The flexible polyester polyol segments of the glycidyl methacrylate-grafted polyester polyol can also improve the adhesion and flexibility of the cured film, preventing brittleness in the low-temperature cured film. The composite epoxy resin and acrylate polymers containing alicyclic epoxy can further improve the cross-linking density and heat and chemical resistance of the system, thereby achieving a balance between low-temperature curing properties and overall performance.
[0009] This application employs a photo-thermal dual-curing system to achieve rapid and complete low-temperature curing. By constructing a dual-curing system of photocationic curing and low-temperature latent thermal curing, photocuring is first achieved through exposure to set the shape and complete patterning imaging, followed by low-temperature thermal curing to achieve deep cross-linking. The cationic photoinitiator can achieve efficient excitation in the 400nm~500nm ultraviolet band, and with the addition of a sensitizer, it can be extended to the 400nm~500nm visible light band, thus better adapting to industry-standard exposure equipment and achieving uniform curing even in thick films. The thermal initiator, combined with the latent curing system and low-temperature activating agent, can rapidly trigger the cross-linking reaction at 80~120℃, shortening the curing time to less than 30 minutes, with a gel content ≥95%, completely solving the problems of incomplete reaction and low curing efficiency in traditional low-temperature curing systems. The latent curing system exhibits excellent storage stability at room temperature, preventing premature gelation. Adding fillers provides necessary insulation and dimensional stability while improving light utilization. Adding photosensitive monomers improves the photosensitivity and cross-linking rate of the solder resist composition.
[0010] In summary, by controlling the components and weight proportions of the solder resist composition within the aforementioned range, this application comprehensively improves overall performance and adapts to various application scenarios. After curing, the solder resist composition of this application achieves a pencil hardness ≥3H, a cross-cut adhesion test grade of 5B, a light transmittance ≥90% at 550nm wavelength, a haze ≤1.5%, and a performance degradation of ≤5% after 24 hours of water and alcohol immersion. It also exhibits excellent anti-yellowing properties and weather resistance. Therefore, the solder resist composition of this application solves the problems of thermal damage and high energy consumption associated with high-temperature curing, while also overcoming the shortcomings of insufficient cross-linking density and poor durability associated with pure photocuring. It is suitable for various scenarios such as flexible substrates, thin substrates, thermal component encapsulation, and photovoltaic modules, while also being compatible with existing production line processes without additional equipment investment, thus possessing extremely high industrial application value.
[0011] Further, the epoxy resin is a bisphenol A type epoxy resin and / or an alicyclic epoxy resin; the alicyclic epoxy resin includes hydrogenated bisphenol A type epoxy resin; the epoxy equivalent of the epoxy resin is 180 g / eq to 500 g / eq; and / or, the weight-average molecular weight of the acrylate polymer containing alicyclic epoxy is 5000 g / mol to 20000 g / mol; and / or, the raw materials for preparing glycidyl methacrylate grafted polyester polyol include glycidyl methacrylate and polycaprolactone diol, and glycidyl methacrylate... The mass ratio of glycidyl methacrylate to polycaprolactone diol is 100:(20~50); and / or, the epoxy value of glycidyl methacrylate-grafted polyester polyol is 0.85mol / 100g~1.2mol / 100g; and / or, the content of carbon-carbon double bonds of methacryloyloxy groups in glycidyl methacrylate-grafted polyester polyol is 0.6mol / 100g~1.0mol / 100g; preferably, the mass percentage of glycidyl methacrylate-grafted polyester polyol in the matrix resin is 30%~40%.
[0012] Preferably selecting epoxy resins with epoxy equivalents within the aforementioned ranges facilitates the introduction of highly reactive epoxy groups. This, combined with glycidyl methacrylate-grafted polyesters, achieves synergistic effects of photocuring and thermocuring, further enhancing the system's crosslinking density and its heat and chemical resistance. Preferably, the weight-average molecular weight of the alicyclic epoxy-containing acrylate polymers is within the aforementioned range, which promotes better miscibility and crosslinking with other resins. Alicyclic epoxy-containing acrylate polymers combine the high adhesion and chemical resistance of epoxy resins with the rapid photo / thermal curing capabilities of acrylates; alicyclic epoxides exhibit higher reactivity and lower curing shrinkage than traditional bisphenol A epoxy resins, making them more suitable for low-temperature reactions.
[0013] The polyester segments of glycidyl methacrylate-grafted polyester polyols provide flexibility and reduce the coefficient of thermal expansion (CTE) to 20 ppm / °C, matching the PET substrate. Their aliphatic structure helps reduce chromophores, thereby improving the light transmittance of the solder resist dry film. Preferably, the content of carbon-carbon double bonds of methacryloyloxy groups in the glycidyl methacrylate-grafted polyester polyol is within the above-mentioned range, which helps to coordinate with highly reactive epoxy groups, balancing exposure imaging capability and low-temperature crosslinking reactivity. Preferably, the mass percentage of glycidyl methacrylate-grafted polyester polyol in the matrix resin is within the above-mentioned range, which helps to better synergize with epoxy resins and acrylate polymers containing alicyclic epoxy resins, balancing the photosensitivity and low-temperature curing activity of the solder resist composition.
[0014] Further, the thermal initiator is selected from any one or more of dicyclohexyl peroxide dicarbonate, microencapsulated imidazole thermal initiators, boron trifluoride amine complexes, and α-salt thermal initiators; and / or, the cationic photoinitiator is an aryl sulfonium salt and / or an aryl iodonium salt; wherein the aryl sulfonium salt is bis(triarylsulfonium)hexafluoroantimonate; and the aryl iodonium salt is (4-dodecyloxyphenyl)[4-(pentadecafluorodecyloxy)phenyl]iodonium hexafluoroantimonate and / or (4-methyl... The photoinitiator is selected from (4-(2-methylpropyl)phenyl)iodonium hexafluorophosphate; and / or, the mass ratio of glycidyl methacrylate-grafted polyester polyol and cationic photoinitiator is (4~10):1; the mass ratio of thermal initiator and cationic photoinitiator is 1:(1.5~5); and / or, the photosensitive monomer is selected from any one or more of trimethylolpropane triacrylate, pentaerythritol tetraacrylate and ethoxylated trimethylolpropane triacrylate.
[0015] Preferring thermal initiators within the aforementioned range helps improve the triggering efficiency and crosslinking rate of thermosetting. Preferring cationic photoinitiators within the aforementioned range helps achieve efficient excitation at wavelengths of 400-500 nm, improving curing uniformity in thick films. Cationic photoinitiators generate strong acids under ultraviolet light, initiating cationic and free radical polymerization of the matrix resin and photosensitive monomers, forming a preliminary crosslinking pattern, which is beneficial for the subsequent depth of low-temperature thermosetting. Preferring a mass ratio of glycidyl methacrylate-grafted polyester polyol and cationic photoinitiator, and of thermal initiator and cationic photoinitiator, within the aforementioned range, helps to form a synergistic effect of photo-thermal dual curing, thereby further improving low-temperature curing efficiency and curing completeness.
[0016] Further, the latent curing system includes a phosphine-based latent catalyst and a microencapsulated anhydride curing agent; preferably, the mass ratio of the phosphine-based latent catalyst to the microencapsulated anhydride curing agent is 4~8:6~10; preferably, the phosphine-based latent catalyst is a triphenylphosphine complex and / or microencapsulated triphenylphosphine; preferably, the microencapsulated anhydride curing agent includes a capsule shell, the capsule shell forming a closed cavity, and the cavity is filled with anhydride curing agent; preferably, the anhydride curing agent is methyltetrahydrophthalic anhydride; preferably, the capsule shell material is polyurea, and the thickness of the capsule shell is 0.2μm~0.5μm; preferably, the particle size of the microencapsulated anhydride curing agent is 3μm~5μm.
[0017] The latent curing system, through the synergistic design of a phosphine-based latent catalyst and a microencapsulated anhydride curing agent, controls their mass ratio within the aforementioned range, achieving highly efficient crosslinking at 80–120°C, a 40–70°C reduction in curing temperature compared to traditional curing systems. The aforementioned phosphine-based latent catalyst triggers the epoxy-anhydride nucleophilic catalytic reaction at temperature; the microcapsule shell ruptures at a set temperature to release the anhydride curing agent, and the two work synergistically to complete the epoxy-anhydride crosslinking. The microencapsulated anhydride curing agent, through the controlled-release design of the polyurea shell, remains stable below 80°C, ensuring the system's shelf life; at 100–120°C, the shell ruptures to release the anhydride curing agent, achieving controlled-release crosslinking.
[0018] Furthermore, the low-temperature activation aid includes ortho-hydroxyl-substituted phenolic resin; the ortho-hydroxyl-substituted phenolic resin is selected from any one or more of phenolic resin of the phenol type, o-cresol phenolic resin and bisphenol A phenolic resin; and / or, the weight average molecular weight of the low-temperature activation aid is 800 g / mol to 2500 g / mol; and / or, the mass ratio of the low-temperature activation aid to the thermal initiator is 2 to 10:1.
[0019] The preferred low-temperature activating agent is selected from the above-mentioned range in terms of type and dosage ratio, so that it can react with the trace acid generated by the pyrolysis of the cationic photoinitiator or the trace water in the system at 100~120℃, thereby reducing the activation energy of epoxy ring-opening polymerization and promoting the efficient decomposition of the thermal initiator at low temperature, generating free radicals to further crosslink the matrix resin. This results in the solder resist composition obtaining a high crosslinking density at low temperature, with performance far superior to a single latent curing agent system.
[0020] Furthermore, the solder resist composition further includes 2 to 10 parts of an active diluent; the active diluent is an epoxy-based active diluent, wherein the number of epoxy groups in the epoxy-based active diluent is ≥2, preferably 2 to 4; preferably, the epoxy-based active diluent is 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarbamate and / or 1,4-butanediol diglycidyl ether.
[0021] Adding the above-mentioned parts by weight and types of reactive diluent helps to regulate the polymerization rate of the system, balance the gel time and curing depth, shorten the curing time under the premise of full curing, and improve production efficiency.
[0022] Further, the filler is a silane-modified filler; preferably, the filler is selected from any one or more of silane-modified nano-silica, silane-modified nano-titanium dioxide, and silane-modified barium sulfate; and / or, the average particle size of the filler is 50 nm to 150 nm; preferably, when the filler is a combination of silane-modified nano-titanium dioxide and silane-modified barium sulfate, the mass ratio of silane-modified nano-titanium dioxide to silane-modified barium sulfate is (6 to 8): (2 to 4); preferably, the solder resist composition further includes 0.1 to 20 parts of additives; the additives are selected from any one or more of anti-yellowing agents, leveling agents, defoamers, pigments, sensitizers, and adhesion promoters.
[0023] Silane-modified nano-silica provides essential insulation and dimensional stability. Its surface hydroxyl groups can interact with low-temperature activating agents and matrix resins to enhance the low-temperature crosslinking network and improve the rheological properties of the film in the low-temperature molten state, thereby improving leveling and coverage. A composite filler using silane-modified nano-titanium dioxide and silane-modified barium sulfate helps to further improve the light reflectivity in the 450–700 nm wavelength range. Adding different types of additives can meet the performance requirements of various scenarios: anti-yellowing agents reduce oxidation and discoloration at high temperatures; leveling agents reduce surface tension and improve film uniformity; defoamers eliminate coating bubbles and reduce pinhole defects; pigments achieve different appearance colors; sensitizers broaden the photoinitiated response wavelength range; and adhesion promoters improve the adhesion between the film and the substrate.
[0024] According to another aspect of the present invention, a solder resist dry film is provided, comprising a support layer and a solder resist layer stacked thereon, the solder resist layer being obtained by mixing and drying the aforementioned solder resist layer composition.
[0025] The solder resist dry film, including the aforementioned solder resist layer, combines high cross-linking density, high adhesion, high hardness, and excellent optical properties.
[0026] The solder resist dry film may include a support layer, a photosensitive solder resist layer, and a cover film arranged sequentially; the support layer is a PET film with a thickness of 25~50μm, and one side is treated with an anti-stick coating; the cover film is a PE film with a thickness of 20~40μm. The thickness of the photosensitive solder resist layer is 15~50μm, preferably 20~30μm.
[0027] According to another aspect of the present invention, a solder resist layer is provided, which is obtained by photocuring and thermocuring the above-described solder resist layer composition.
[0028] The solder resist layer including the above-mentioned solder resist layer composition can achieve low-temperature rapid and complete curing, and also has high cross-linking density, high adhesion, high hardness and excellent optical properties.
[0029] Furthermore, the heat curing temperature is 100℃~120℃, and the heat curing time is 15min~30min.
[0030] The above solder resist composition can also achieve complete and rapid curing at the lower temperature and shorter curing time.
[0031] Applying the technical solution of this invention, the matrix resin of this application uses glycidyl methacrylate grafted polyester polyol as the core matrix resin, combined with epoxy resin and acrylate polymers containing alicyclic epoxy to form a composite resin system, enabling the solder resist composition to balance photosensitivity and low-temperature curing activity. The carbon-carbon double bond of the methacryloyloxy group in the glycidyl methacrylate grafted polyester polyol, combined with the highly reactive epoxy groups in the epoxy resin, can both match the photocuring system to achieve exposure imaging and undergo cross-linking reactions with the thermocuring system at low temperatures, thus solving the problem of insufficient low-temperature reactivity of traditional resins. The flexible polyester polyol segments of the glycidyl methacrylate grafted polyester polyol can also improve the adhesion and flexibility of the cured film, preventing brittleness of the low-temperature cured film. The composite epoxy resin and acrylate polymers containing alicyclic epoxy can further improve the cross-linking density and heat and chemical resistance of the system, thereby achieving a balance between low-temperature curing properties and overall performance. This application employs a photo-thermal dual-curing system to achieve rapid and complete low-temperature curing. By constructing a dual-curing system of photocationic curing and low-temperature latent thermal curing, photocuring and shaping are first achieved through exposure, completing patterning and imaging, followed by low-temperature thermal curing for deep cross-linking. The cationic photoinitiator can achieve efficient excitation in the 400nm~500nm ultraviolet band, and with the addition of a sensitizer, this can be extended to the 400nm~500nm visible light band, thus better adapting to industry-standard exposure equipment and achieving uniform curing even in thick films. The thermal initiator, combined with the latent curing system and low-temperature activating agent, can rapidly trigger the cross-linking reaction at 80~120℃, shortening the curing time to less than 30 minutes, with a gel content ≥95%, completely solving the problems of incomplete reaction and low curing efficiency in traditional low-temperature curing systems. The latent curing system exhibits excellent storage stability at room temperature, preventing premature gelation. Adding fillers provides necessary insulation and dimensional stability, as well as improving light utilization. Adding photosensitive monomers improves the photosensitivity of the solder resist composition. In summary, by controlling the components and weight proportions of the solder resist composition within the aforementioned range, this application comprehensively improves overall performance and adapts to various application scenarios. After curing, the solder resist composition of this application achieves a pencil hardness ≥3H, a cross-cut adhesion test grade of 5B, a light transmittance ≥90% at 550nm wavelength, a haze ≤1.5%, and a performance degradation of ≤5% after 24 hours of water and alcohol immersion. It also exhibits excellent anti-yellowing properties and weather resistance. Therefore, the solder resist composition of this application solves the problems of thermal damage and high energy consumption associated with high-temperature curing, and overcomes the shortcomings of insufficient cross-linking density and poor durability associated with pure photocuring. This allows it to be adapted to various scenarios such as flexible substrates, thin substrates, thermal component encapsulation, and photovoltaic modules, while remaining compatible with existing production line processes without additional equipment investment, thus possessing extremely high industrial application value. Detailed Implementation
[0032] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. The present invention will now be described in detail with reference to the embodiments.
[0033] As analyzed in the background section of this application, existing solder resist dry films have the problem of being difficult to cure quickly and completely at low temperatures, and at the same time, it is difficult to achieve high crosslinking density, high adhesion, high hardness and excellent optical performance. In order to solve the above problems, this application provides a solder resist composition, a solder resist dry film and a solder resist layer.
[0034] In a typical embodiment of this application, a solder resist composition is provided, comprising, by weight: 55-75 parts of a matrix resin, 10-50 parts of a filler, 0.5-5 parts of a thermal initiator, 2-8 parts of a cationic photoinitiator, 15-25 parts of a photosensitive monomer, 10-18 parts of a latent curing system, and 5-10 parts of a low-temperature activating agent; the matrix resin comprises glycidyl methacrylate grafted polyester polyol; the matrix resin further comprises epoxy resin and / or acrylate polymer containing alicyclic epoxy.
[0035] The matrix resin of this application uses glycidyl methacrylate-grafted polyester polyol as the core matrix resin, combined with epoxy resin and acrylate polymers containing alicyclic epoxy resins to form a composite resin system. This allows the solder resist composition to achieve both photosensitivity and low-temperature curing activity. The carbon-carbon double bond of the methacryloyloxy group in the glycidyl methacrylate-grafted polyester polyol, combined with the highly reactive epoxy groups in the epoxy resin, can both match the photocuring system to achieve exposure imaging and undergo cross-linking reactions with the thermocuring system at low temperatures, thus solving the problem of insufficient low-temperature reactivity of traditional resins. The flexible polyester polyol segments of the glycidyl methacrylate-grafted polyester polyol can also improve the adhesion and flexibility of the cured film, preventing brittleness of the low-temperature cured film. The composite epoxy resin and acrylate polymers containing alicyclic epoxy resins can further improve the cross-linking density and heat and chemical resistance of the system, thereby achieving a balance between low-temperature curing properties and overall performance. This application employs a photo-thermal dual-curing system to achieve rapid and complete low-temperature curing. By constructing a dual-curing system of photocationic curing and low-temperature latent thermal curing, photocuring and shaping are first achieved through exposure, completing patterning and imaging, followed by low-temperature thermal curing for deep cross-linking. The cationic photoinitiator can achieve efficient excitation in the 400nm~500nm ultraviolet band, and with the addition of a sensitizer, this can be extended to the 400nm~500nm visible light band, thus better adapting to industry-standard exposure equipment and achieving uniform curing even in thick films. The thermal initiator, combined with the latent curing system and low-temperature activating agent, can rapidly trigger the cross-linking reaction at 80~120℃, shortening the curing time to less than 30 minutes, with a gel content ≥95%, completely solving the problems of incomplete reaction and low curing efficiency in traditional low-temperature curing systems. The latent curing system exhibits excellent storage stability at room temperature, preventing premature gelation. Adding fillers provides necessary insulation and dimensional stability, as well as improving light utilization. Adding photosensitive monomers improves the photosensitivity of the solder resist composition. In summary, by controlling the components and weight proportions of the solder resist composition within the aforementioned range, this application comprehensively improves overall performance and adapts to various application scenarios. After curing, the solder resist composition of this application achieves a pencil hardness ≥3H, a cross-cut adhesion test grade of 5B, a light transmittance ≥90% at 550nm wavelength, a haze ≤1.5%, and a performance degradation of ≤5% after 24 hours of water and alcohol immersion. It also exhibits excellent anti-yellowing properties and weather resistance. Therefore, the solder resist composition of this application solves the problems of thermal damage and high energy consumption associated with high-temperature curing, and overcomes the shortcomings of insufficient cross-linking density and poor durability associated with pure photocuring. This allows it to be adapted to various scenarios such as flexible substrates, thin substrates, thermal component encapsulation, and photovoltaic modules, while remaining compatible with existing production line processes without additional equipment investment, thus possessing extremely high industrial application value.
[0036] In addition, the total weight parts of the matrix resin are the sum of the parts of glycidyl methacrylate grafted polyester polyol, epoxy resin and / or acrylate polymer containing alicyclic epoxy.
[0037] In one embodiment of this application, the epoxy resin is a bisphenol A type epoxy resin and / or an alicyclic epoxy resin; the alicyclic epoxy resin includes hydrogenated bisphenol A type epoxy resin; the epoxy equivalent of the epoxy resin is 180 g / eq to 500 g / eq; and / or, the weight-average molecular weight of the acrylate polymer containing alicyclic epoxy is 5000 g / mol to 20000 g / mol; and / or, the raw materials for preparing glycidyl methacrylate grafted polyester polyol include glycidyl methacrylate and polycaprolactone diol, methacrylate... The mass ratio of glycidyl methacrylate to polycaprolactone diol is 100:(20~50); and / or, the epoxy value of the glycidyl methacrylate-grafted polyester polyol is 0.85mol / 100g~1.2mol / 100g, and the carbon-carbon double bond content of the methacryloyloxy group in the glycidyl methacrylate-grafted polyester polyol is 0.6mol / 100g~1.0mol / 100g; preferably, the mass percentage of glycidyl methacrylate-grafted polyester polyol in the matrix resin is 30~40%.
[0038] Preferably selecting the type of epoxy resin and having an epoxy equivalent within the aforementioned range helps introduce highly reactive epoxy groups, thereby enabling photocuring and thermocuring in combination with glycidyl methacrylate-grafted polyesters. This further enhances the crosslinking density and heat and chemical resistance of the system. Preferably, the weight-average molecular weight of the acrylate polymer containing alicyclic epoxy is within the aforementioned range, which facilitates better crosslinking with other resins. The acrylate polymer containing alicyclic epoxy combines the high adhesion and chemical resistance of alicyclic epoxy resins with the rapid photo / thermal curing ability of acrylates. Alicyclic epoxy has higher reactivity and lower curing shrinkage than traditional bisphenol A epoxy resins, thus being more conducive to low-temperature reactions.
[0039] The weight percentage of glycidyl methacrylate-grafted polyester polyol can be 20-25 parts. A preferred preparation process for the glycidyl methacrylate-grafted polyester polyol includes: a transesterification reaction of glycidyl methacrylate (GMA) and polycaprolactone diol (PCL) in the above-mentioned mass ratio at 90-120°C for 2-6 hours under the catalysis of dibutyltin dilaurate, to obtain a glycidyl methacrylate-grafted polyester polyol with the above-mentioned epoxy content, and a grafting rate of 70-80%.
[0040] The polyester segments of glycidyl methacrylate-grafted polyester polyols provide flexibility and reduce the coefficient of thermal expansion (CTE) to 20 ppm / °C, matching that of PET (18 ppm / °C). Its aliphatic structure helps reduce chromophores, thereby improving the light transmittance of the solder resist dry film.
[0041] The preferred content of carbon-carbon double bonds of methacryloyloxy groups in glycidyl methacrylate-grafted polyester polyols is within the above-mentioned range, which helps to coordinate with highly active epoxy groups, thereby enabling both exposure imaging and cross-linking reaction with thermosetting systems at low temperatures, thus improving the low-temperature reactivity of the matrix resin.
[0042] The preferred matrix resin has a glycidyl methacrylate-grafted polyester polyol content within the above range, which helps it to better cooperate with epoxy resin and acrylate polymers containing alicyclic epoxy resin, thereby improving the photosensitivity and low-temperature curing activity of the solder resist composition.
[0043] When the matrix resin is a combination of epoxy resin and glycidyl methacrylate grafted polyester polyol, the mass ratio of epoxy resin to glycidyl methacrylate grafted polyester polyol is (1.5~2):1; when the matrix resin is a combination of acrylate polymer containing alicyclic epoxy and glycidyl methacrylate grafted polyester polyol, the mass ratio of acrylate polymer containing alicyclic epoxy and glycidyl methacrylate grafted polyester polyol is (1.5~2):1.
[0044] In one embodiment of this application, the thermal initiator is selected from any one or more of dicyclohexyl peroxide dicarbonate, microencapsulated imidazole thermal initiators, boron trifluoride amine complexes, and α-salt thermal initiators; and / or, the cationic photoinitiator is an aryl sulfonium salt and / or an aryl iodonium salt; wherein the aryl sulfonium salt is bis(triarylsulfonium)hexafluoroantimonate; and the aryl iodonium salt is (4-dodecyloxyphenyl)[4-(pentadecafluorodecyloxy)phenyl]iodonium hexafluoroantimonate and / or (4-Methylphenyl)[4-(2-Methylpropyl)phenyl]iodonium hexafluorophosphate; and / or, the mass ratio of glycidyl methacrylate-grafted polyester polyol to cationic photoinitiator is (4~10):1; the mass ratio of thermal initiator to cationic photoinitiator is 1:(1.5~5); and / or, the photosensitive monomer is selected from any one or more of trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and ethoxylated trimethylolpropane triacrylate.
[0045] Preferring thermal initiators within the aforementioned range helps improve thermosetting efficiency. Preferring cationic photoinitiators within the aforementioned range facilitates efficient excitation at wavelengths of 400-500 nm, improving curing uniformity in thick films. Cationic photoinitiators generate strong acids under ultraviolet light, initiating cationic and free radical polymerization of the matrix resin and photosensitive monomers, forming a preliminary cross-linking pattern, which is beneficial for subsequent low-temperature thermosetting.
[0046] The preferred mass ratio of glycidyl methacrylate-grafted polyester polyol and cationic photoinitiator, thermal initiator and cationic photoinitiator within the above range helps to form a synergistic effect of photo-thermal dual curing, thereby further improving the low-temperature curing efficiency and curing completeness.
[0047] In one embodiment of this application, the latent curing system comprises a phosphine-based latent catalyst and a microencapsulated anhydride curing agent; preferably, the mass ratio of the phosphine-based latent catalyst to the microencapsulated anhydride curing agent is 4~8:6~10; preferably, the phosphine-based latent catalyst is a triphenylphosphine complex and / or microencapsulated triphenylphosphine; preferably, the microencapsulated anhydride curing agent comprises a capsule shell, the capsule shell forming a closed cavity, the cavity being filled with anhydride curing agent; preferably, the anhydride curing agent is methyltetrahydrophthalic anhydride; preferably, the capsule shell is made of polyurea, and the thickness of the capsule shell is 0.2~0.5 μm; preferably, the particle size of the microencapsulated anhydride curing agent is 3~5 μm.
[0048] The latent curing system, through the synergistic design of "phosphine-based latent catalyst and microencapsulated anhydride curing agent", controls the mass ratio of the two within the above range, which helps to improve the synergistic effect of the two, thereby achieving efficient crosslinking at 80~120℃, reducing the curing temperature by 40~70℃ compared with the curing temperature of traditional curing systems.
[0049] The aforementioned types of phosphine latent catalysts can undergo thermal decomposition above 80°C, generating basic active centers that promote the catalytic epoxy-anhydride reaction. Microencapsulated triphenylphosphine comprises a capsule shell forming a closed cavity filled with triphenylphosphine. The capsule shell is made of polyurea with a thickness of 0.2–0.5 μm, and the microencapsulated triphenylphosphine has a particle size of 3–5 μm.
[0050] Microencapsulated anhydride curing agents, through the design of microcapsules, control the thickness and material of the capsule shell within the aforementioned range, achieving stable existence below 80°C and reducing cross-linking during storage; at 100~120°C, the shell ruptures, releasing the anhydride curing agent, thereby achieving controlled-release cross-linking.
[0051] In one embodiment of this application, the low-temperature activation aid is an ortho-hydroxy-substituted phenolic resin; the ortho-hydroxy-substituted phenolic resin is selected from any one or more of phenolic resin of the phenol type, o-cresol phenolic resin and bisphenol A phenolic resin; and / or, the weight average molecular weight of the low-temperature activation aid is 800 g / mol to 2500 g / mol; and / or, the mass ratio of the low-temperature activation aid to the thermal initiator is 2 to 10:1.
[0052] The preferred types of low-temperature activating agents are within the above-mentioned range, and the mass ratio of low-temperature activating agents to thermal initiators is controlled within the above-mentioned range. This helps them to react with the trace acid generated by the pyrolysis of cationic photoinitiators or the trace water in the system at 100~120℃, thereby reducing the activation energy of epoxy ring-opening polymerization and promoting the efficient decomposition of thermal initiators at low temperatures. This generates free radicals to further crosslink the matrix resin, thereby enabling the solder resist composition to obtain a high crosslinking density at low temperatures, which is far superior to a single latent curing agent system.
[0053] Ortho-hydroxyl-substituted phenolic resins refer to phenolic resins in which the benzene ring containing the phenolic hydroxyl group has at least one reactive hydrogen atom or a substituted group at the ortho position of the phenolic hydroxyl group. Specifically, for phenolic resins of the phenol type, both ortho positions of the phenolic hydroxyl group in the phenol monomer contain hydrogen atoms, which can be substituted with hydroxymethyl groups; for o-cresol resins, one ortho position of the phenolic hydroxyl group in the cresol monomer is substituted with a methyl group, and the other ortho position contains a hydrogen atom, which can be substituted with hydroxymethyl groups; for bisphenol A resins, the ortho position of the phenolic hydroxyl group in the bisphenol A monomer contains a hydrogen atom, which can be substituted with hydroxymethyl groups.
[0054] In one embodiment of this application, the solder mask composition further includes 2 to 10 parts of an active diluent; the active diluent is an epoxy-based active diluent, wherein the number of epoxy groups in the epoxy-based active diluent is ≥2, preferably 2 to 4; preferably, the epoxy-based active diluent is 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarbamate and / or 1,4-butanediol diglycidyl ether.
[0055] Adding the above-mentioned proportions and types of reactive diluents by weight helps to regulate the polymerization rate of the system, balance the gel time and the curing depth, thereby shortening the curing time and improving production efficiency while ensuring full curing.
[0056] In one embodiment of this application, the filler is a silane-modified filler; preferably, the filler is selected from any one or more of silane-modified nano-silica, silane-modified nano-titanium dioxide, and silane-modified barium sulfate; and / or, the average particle size of the filler is 50 nm to 150 nm; preferably, when the filler is a combination of silane-modified nano-titanium dioxide and silane-modified barium sulfate, the mass ratio of silane-modified nano-titanium dioxide to silane-modified barium sulfate is (6 to 8): (2 to 4); preferably, the solder resist composition further includes 0.1 to 20 parts of additives; the additives are selected from any one or more of anti-yellowing agents, leveling agents, defoamers, pigments, sensitizers, and adhesion promoters.
[0057] Silane-modified nano-silica provides essential insulation and dimensional stability. Its surface hydroxyl groups can interact with low-temperature activating agents and matrix resins, thereby enhancing the low-temperature crosslinking network and improving the rheological properties of the film in the low-temperature molten state, thus improving leveling and coverage. The use of a composite filler of silane-modified nano-titanium dioxide and silane-modified barium sulfate helps to further improve the light reflectivity in the 450–700 nm wavelength range.
[0058] Adding the above-mentioned additives can achieve the performance required for different scenarios. The anti-yellowing agent is 0.5 to 1.5 parts by weight, and the anti-yellowing agent is a benzotriazole ultraviolet absorber and / or a hindered amine light stabilizer. The anti-yellowing agent helps reduce oxidative discoloration at high temperatures.
[0059] The leveling agent is present in a weight ratio of 0.2 to 2 parts, and is a fluorosilicone-modified polyacrylate and / or a polyether-modified polydimethylsiloxane nonionic surfactant. The leveling agent helps to reduce the surface tension to below 25 mN / m, thereby improving the uniformity of the film layer.
[0060] The defoamer is present in a concentration of 0.1 to 1 part by weight, and is a polyether-modified silicone oil. The defoamer helps eliminate coating bubbles and reduce pinhole defects.
[0061] The pigment is present in 5 to 10 parts by weight, and is selected from one or more of carbon black, titanium dioxide, cadmium red, and iron blue. The pigment can achieve different appearance colors.
[0062] The sensitizer is present in an amount of 0.5 to 2 parts by weight, and the sensitizer is an anthracene compound and / or a thioxanthone compound. The sensitizer helps to broaden the wavelength range of the photoinitiated response, thereby improving the photosensitivity of the solder mask composition.
[0063] The adhesion promoter is present in parts by weight of 1 to 4 parts, and is an epoxy silane coupling agent and / or a mercaptosilane coupling agent. The adhesion promoter helps improve the adhesion and reliability of the solder resist composition.
[0064] In another typical embodiment of this application, a solder resist dry film is provided, comprising a support layer and a solder resist layer stacked thereon, wherein the solder resist layer is obtained by mixing and drying the aforementioned solder resist layer composition.
[0065] The solder resist dry film, including the aforementioned solder resist layer, combines high cross-linking density, high adhesion, high hardness, and excellent optical properties.
[0066] The solder resist dry film may include a support layer, a photosensitive solder resist layer, and a cover film arranged sequentially; the support layer is a PET film with a thickness of 25~50μm, and one side is treated with an anti-stick coating; the cover film is a PE film with a thickness of 20~40μm. The thickness of the photosensitive solder resist layer is 15~50μm, preferably 20~30μm.
[0067] In another typical embodiment of this application, a solder resist layer is provided, which is obtained by photocuring and thermocuring the above-mentioned solder resist layer composition.
[0068] The solder resist layer including the above-mentioned solder resist layer composition can achieve low-temperature rapid and complete curing, and also has high cross-linking density, high adhesion, high hardness and excellent optical properties.
[0069] In one embodiment of this application, the thermosetting temperature is 100~120℃ and the thermosetting time is 15~30min.
[0070] The solder resist composition of this application can also achieve complete and rapid curing at the aforementioned lower temperature and shorter thermosetting time.
[0071] Solder resist compositions can be applied at exposure energy of 50~200mJ / cm 2 Patterning was achieved at 365 nm, with the developing solution being a 1-3 wt% sodium carbonate aqueous solution and the developing time being 30-90 s.
[0072] Preparation method of solder resist dry film:
[0073] The raw materials corresponding to the solder resist composition are mixed, and the resulting mixture is uniformly coated onto the surface of the support layer by extrusion coating or doctor blade coating. After drying at 80~100℃ for 5~10 minutes, a solder resist layer is formed. A cover film is laminated onto the surface of the solder resist layer, and the mixture is wound up to form a finished dry film.
[0074] Furthermore, the curing process for the solder resist dry film includes:
[0075] 1) Film application: The finished dry film is applied to the clean substrate surface using a hot press roller at a pressure of 0.2~0.5MPa and a temperature of 60~80℃;
[0076] 2) Exposure: UV exposure is performed using a photomask at an energy of 50~200mJ / cm². 2;
[0077] 3) Development: The unexposed areas are removed by spraying developing solution.
[0078] 4) Low-temperature post-curing: Heat at 100~120℃ for 15~30 minutes to complete the final cross-linking and curing.
[0079] The beneficial effects of this application will be further illustrated below with reference to the embodiments.
[0080] Example 1
[0081] Preparation of microencapsulated acid anhydride curing agent: 100g of methyltetrahydrophthalic anhydride was dispersed in an aqueous phase containing 1wt.% Span 80, 30g of isophorone diisocyanate (IPDI) and 15g of diethylenetriamine (DETA) were added, and the mixture was reacted at 50℃ for 2h to form a polyurea shell. The microencapsulated acid anhydride curing agent was obtained by spray drying, with an encapsulation rate ≥90%, a capsule shell thickness of 0.3μm, and an average particle size of 4μm.
[0082] Preparation of glycidyl methacrylate grafted polyester polyol: 100g of glycidyl methacrylate (GMA) was mixed with polycaprolactone diol (PCL, Mn=1000), and dibutyltin dilaurate (0.5wt% of the total mass of raw materials) was added as a catalyst. The transesterification reaction was carried out at 110℃ for 4h to obtain glycidyl methacrylate grafted polyester polyol.
[0083] Preparation of silane-modified nanofillers: The nanofillers were dispersed in an ethanol-water solution with a volume ratio of 1:1, and silane coupling agent KH-560 (2% of the filler mass) was added. The surface modification was carried out at 80℃ for 60 min. After centrifugation, washing and vacuum drying, the silane-modified nanofillers were obtained.
[0084] The solder resist composition comprises, by weight, the following components: 40 parts of matrix resin, bisphenol A type epoxy resin (E-44, epoxy equivalent 210~240 g / eq), 22 parts of glycidyl methacrylate grafted polyester polyol (GMA and PCL mass ratio 100:30, epoxy value 0.95 mol / 100 g, methacryloyloxy carbon-carbon double bond content 0.6 mol / 100 g); 3 parts of thermal initiator, microencapsulated 2-methylimidazole (shell layer same as the aforementioned microencapsulated anhydride curing agent polyurea shell, core material 2-methylimidazole content 40 wt%, average particle size 5 μm, release temperature 95℃); 5 parts of cationic photoinitiator, bis(triarylsulfonium)hexafluoroantimonate; and 40 parts of photosensitive monomer. Main component: 20 parts of trimethylolpropane triacrylate; Latent curing system: 6 parts of triphenylphosphine complex, 8 parts of microencapsulated anhydride curing agent; Low-temperature activation aid: 7 parts of o-cresol phenolic resin (weight average molecular weight of 1500 g / mol); Reactive diluent: 5 parts of 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate (ECC); Filler: 15 parts of silane-modified nano silica with an average particle size of 100 nm; Additives: 1 part of leveling agent (EFKA-3030), 0.5 parts of defoamer (TEGO-901W), 1 part of anti-yellowing agent (Tinuvin 1130 and Chimassorb 119 in a mass ratio of 1:1), 2 parts of adhesion promoter (KH-560).
[0085] Preparation and Curing Process: Weigh each component according to the above weight proportions, add a mixed solvent (propylene glycol methyl ether acetate and cyclohexanone in a volume ratio of 7:3) to prepare a 65% solid content adhesive solution, stir in the dark for 2 hours, and degas under vacuum to obtain the solder resist composition. Coat it onto a 38μm thick PET film, dry at 80℃ for 5 minutes to form a 25μm thick solder resist layer. Lay a 30μm thick PE protective film on the surface of the solder resist layer away from the PET film to obtain a dry film. Apply the dry film to the surface of a clean copper-clad laminate substrate using a hot press roller at a pressure of 0.3MPa and a temperature of 70℃. Perform UV exposure using a photomask under the following conditions: 365nm, 80mJ / cm². 2 Unexposed areas were removed by spraying with a 2wt% sodium carbonate aqueous solution, followed by low-temperature thermal curing at 100℃ for 30 minutes to obtain a dry solder resist film.
[0086] Example 2
[0087] The difference from Example 1 is that, by weight, the components of the solder resist composition are as follows: Matrix resin: 45 parts of an acrylate polymer containing alicyclic epoxy (weight average molecular weight of 10000 g / mol) and 25 parts of glycidyl methacrylate grafted polyester polyol; Thermal initiator: 2 parts of dicyclohexyl peroxide dicarbonate; Photoinitiator: 6 parts of (4-methylphenyl)[4-(2-methylpropyl)phenyl]iodonium hexafluorophosphate; Photosensitive monomer: 18 parts of pentaerythritol tetraacrylate; Latent curing system: microencapsulated triphenylphosphine (shell layer as described above for microencapsulated anhydride curing). The agent consists of 5 parts of a polyurea shell (with an average particle size of 4 μm) and 7 parts of a microencapsulated anhydride curing agent; 8 parts of a low-temperature activation agent: bisphenol A type phenolic resin (weight average molecular weight of 2000 g / mol); 4 parts of an reactive diluent: 1,4-butanediol diglycidyl ether (BDDGE); 28 parts of silane-modified nano-titanium dioxide with an average particle size of 50 nm and 12 parts of silane-modified barium sulfate with an average particle size of 150 nm; and 0.5 parts of a leveling agent, 0.3 parts of a defoamer, 8 parts of titanium dioxide, 1 part of a sensitizer, and 3 parts of an adhesion promoter, ultimately yielding a dry solder resist film.
[0088] Example 3
[0089] The difference from Example 1 is that, by weight, the composition of the solder resist layer is as follows: Matrix resin: 35 parts hydrogenated bisphenol A type epoxy resin (epoxy equivalent of 220~260 g / eq), 20 parts glycidyl methacrylate grafted polyester polyol; Thermal initiator: 1 part boron trifluoride amine complex; Photoinitiator: 3 parts bis(triarylsulfonium)hexafluoroantimonate; Photosensitive monomer: 15 parts ethoxylated trimethylolpropane triacrylate; Latent... Curing system: 4 parts of triphenylphosphine complex and 6 parts of microencapsulated anhydride curing agent with a particle size of 3 μm (capsule shell thickness of 0.2 μm); low temperature activation aid: 5 parts of phenolic resin (weight average molecular weight of 1000 g / mol); reactive diluent: 2 parts of ECC; filler: 10 parts of silane-modified nano silica; additives: 0.2 parts of leveling agent, 0.1 parts of defoamer, and 0.5 parts of anti-yellowing agent, finally obtaining a dry solder resist film.
[0090] Example 4
[0091] The difference from Example 1 is that, by weight, the composition of the solder resist layer is as follows: Matrix resin: 50 parts of bisphenol A type epoxy resin (epoxy equivalent of 180~220 g / eq), 25 parts of glycidyl methacrylate grafted polyester polyol; Thermal initiator: 5 parts of aryl thioonium salt (bis(triarylsulfonium)hexafluoroantimonate); Cationic photoinitiator: 8 parts of (4-dodecyloxyphenyl)[4-(pentadecafluorodecyloxy)phenyl]iodonium hexafluoroantimonate; Photosensitive monomer: 25 parts of trimethylolpropane triacrylate; Latex The curing system consists of 8 parts of triphenylphosphine complex and 10 parts of microencapsulated anhydride curing agent with a particle size of 5 μm (capsule shell thickness of 0.5 μm); low-temperature activation aid: 10 parts of o-cresol phenolic resin; reactive diluent: 10 parts of ECC; filler: 40 parts of silane-modified nano-titanium dioxide with an average particle size of 100 nm and 10 parts of silane-modified barium sulfate with an average particle size of 100 nm; additives: 2 parts of leveling agent, 1 part of defoamer, 10 parts of carbon black, 2 parts of sensitizer, and 4 parts of adhesion promoter, ultimately yielding a dry solder resist film.
[0092] Example 5
[0093] The difference from Example 1 lies in the preparation of glycidyl methacrylate grafted polyester polyol: 100g of glycidyl methacrylate (GMA) and 20g of polycaprolactone diol (PCL, Mn=1000) were subjected to transesterification reaction at 110°C for 4h under the catalysis of dibutyltin dilaurate (0.5wt%). The epoxy value was 0.85mol / 100g, the carbon-carbon double bond content of methacryloyloxy group was 0.8mol / 100g, and the total weight parts of epoxy resin and glycidyl methacrylate grafted polyester polyol were 62 parts, with a mass ratio of 1.5:1, finally yielding a solder resist dry film.
[0094] Example 6
[0095] The difference from Example 1 lies in the preparation of glycidyl methacrylate grafted polyester polyol: 100g of glycidyl methacrylate (GMA) and 50g of polycaprolactone diol (PCL, Mn=1000) were subjected to transesterification reaction at 110°C for 4h under the catalysis of dibutyltin dilaurate (0.5wt%). The epoxy value was 1.2mol / 100g, the carbon-carbon double bond content of methacryloyloxy group was 1.0mol / 100g, and the total weight parts of epoxy resin and glycidyl methacrylate grafted polyester polyol were 62 parts, with a mass ratio of 2:1, finally yielding a solder resist dry film.
[0096] Example 7
[0097] The difference from Example 1 lies in the preparation of glycidyl methacrylate grafted polyester polyol: 100g of glycidyl methacrylate (GMA) and 10g of polycaprolactone diol (PCL, Mn=1000) were subjected to transesterification reaction at 110°C for 4h under the catalysis of dibutyltin dilaurate (0.5wt%). The epoxy value was 0.6mol / 100g, the carbon-carbon double bond content of methacryloyloxy group was 0.3mol / 100g, and the total weight parts of epoxy resin and glycidyl methacrylate grafted polyester polyol were 62 parts, with a mass ratio of 3:1, finally yielding a solder resist dry film.
[0098] Example 8
[0099] The difference from Example 1 is that the total weight of glycidyl methacrylate-grafted polyester polyol and cationic photoinitiator is 27 parts, and the mass ratio of the two is 10:1, resulting in a solder resist dry film.
[0100] Example 9
[0101] The difference from Example 1 is that the total weight of glycidyl methacrylate-grafted polyester polyol and cationic photoinitiator is 27 parts, and the mass ratio of the two is 2.5:1, resulting in a solder resist dry film.
[0102] Example 10
[0103] The difference from Example 1 is that the total weight of the thermal initiator and the cationic photoinitiator is 8 parts, and the mass ratio of the two is 1:5, resulting in a solder resist dry film.
[0104] Example 11
[0105] The difference from Example 1 is that the total weight of the thermal initiator and the cationic photoinitiator is 8 parts, and the mass ratio of the two is 1:0.6, resulting in a solder resist dry film.
[0106] Example 12
[0107] The difference from Example 1 is that the total weight of the triphenylphosphine complex and the microencapsulated anhydride curing agent in the latent curing system is 14 parts, the mass ratio of the two is 4:10, the thickness of the capsule shell of the microencapsulated anhydride curing agent (particle size of 5 μm) is 0.5 μm, and the final solder resist dry film is obtained.
[0108] Example 13
[0109] The difference from Example 1 is that the total weight of the triphenylphosphine complex and the microencapsulated anhydride curing agent in the latent curing system is 14 parts, the mass ratio of the two is 9:5, the thickness of the capsule shell of the microencapsulated anhydride curing agent (particle size of 2 μm) is 0.1 μm, and the final solder resist dry film is obtained.
[0110] Example 14
[0111] The difference from Example 1 is that the total weight of the low-temperature activating agent and the thermal initiator is 10 parts, and the mass ratio of the two is 10:1, resulting in a solder resist dry film.
[0112] Example 15
[0113] The difference from Example 1 is that the total weight of the low-temperature activating agent and the thermal initiator is 10 parts, and the mass ratio of the two is 1:1, resulting in a solder resist dry film.
[0114] Example 16
[0115] The difference from Example 1 is that the filler is silane-modified nano-titanium dioxide with an average particle size of 100 nm and silane-modified barium sulfate with an average particle size of 100 nm, with a total weight of 15 parts and a mass ratio of 7:3, and finally a solder resist dry film is obtained.
[0116] Example 17
[0117] The difference from Example 1 is that the filler is silane-modified nano-titanium dioxide with an average particle size of 100 nm and silane-modified barium sulfate with an average particle size of 100 nm, with a total weight of 15 parts and a mass ratio of 1:1, and finally a solder resist dry film is obtained.
[0118] Comparative Example 1
[0119] The difference from Example 1 is that the solder resist composition does not contain glycidyl methacrylate grafted polyester polyol, photoinitiator and low temperature activator, the total weight of the matrix resin remains unchanged, the weight of the thermal initiator is 8 parts, the weight of the latent curing system is 21 parts, and the curing conditions are 160℃ / 60min, finally obtaining a solder resist dry film.
[0120] Comparative Example 2
[0121] The difference from Example 1 is that no thermal initiator, latent curing system and low temperature activating agent are added to the solder resist composition. The photoinitiator is 8 parts by weight. Only UV curing is used and no thermal curing is performed to finally obtain a dry solder resist film.
[0122] Comparative Example 3
[0123] The difference from Example 1 is that glycidyl methacrylate-grafted polyester polyols are not added to the solder resist composition, and a solder resist dry film is finally obtained.
[0124] Comparative Example 4
[0125] The difference from Example 1 is that, by weight, the composition of the solder resist layer is as follows: Base resin: 40 parts bisphenol A type epoxy resin, 10 parts glycidyl methacrylate grafted polyester polyol; Thermal initiator: 6 parts microencapsulated imidazole; Photoinitiator: 1 part bis(triarylsulfonium)hexafluoroantimonate; Photosensitive monomer: 10 parts trimethylolpropane triacrylate; Latent curing system: 8 parts triphenylphosphine complex, 12 parts microencapsulated anhydride curing agent; Low-temperature activation aid: 2 parts o-cresol type phenolic resin; Reactive diluent: 12 parts ECC; Filler: 5 parts silane-modified nano silica; Additives: 1 part leveling agent, 0.5 parts defoamer, 1 part anti-yellowing agent, 0.5 parts adhesion promoter. The curing conditions are the same as in Example 1.
[0126] Test method:
[0127] Gel content test: Cut the cured solder resist dry film into fragments, accurately weigh the mass m1, use acetone as solvent, reflux extract in Soxhlet extractor for 24h, take out the insoluble matter and vacuum dry at 80℃ to constant weight, weigh the mass m2, gel content = m2 / m1×100%.
[0128] Pencil hardness test: According to GB / T6739-2006 standard, a pencil hardness tester with a load of 750g was used to test the pencil hardness of the cured film surface.
[0129] Cross-cut adhesion test: According to GB / T9286-1998 standard, draw 10×10 squares on the surface of the solder resist dry film, use 3M 600 tape to pull vertically, observe the squares falling off, and evaluate the adhesion level (0B~5B, 5B is the best).
[0130] Transmittance and haze testing: In accordance with GB / T2410-2008 standard, the transmittance and haze of the solder resist dry film at a wavelength of 550nm were tested using a haze meter.
[0131] Ethanol attenuation rate test: Immerse the solder resist dry film in anhydrous ethanol, seal and place at room temperature for 24 hours, remove and wipe dry, test pencil hardness, calculate hardness retention rate, attenuation rate = (initial hardness value - hardness value after immersion) / initial hardness value × 100% (hardness is assigned according to grade: 4H=4, 3H=3, 2H=2, and so on).
[0132] Storage stability test: After sealing the solder resist composition adhesive, store it in a 25℃ constant temperature chamber for 30 days. Observe whether the adhesive exhibits gelation, layering, or precipitation. If there are no abnormalities, it is considered qualified; if abnormalities occur, it is considered unqualified.
[0133] The test results are shown in Table 1.
[0134] Table 1
[0135]
[0136] As can be seen from the above, 1) Examples 1 to 4, 5 to 6, 8, 10, 12, 14 and 16 of this application all achieved excellent comprehensive performance under the low temperature short time curing conditions of 100℃ and 30min, with a gel content of ≥95%, pencil hardness of ≥3H, cross-cut adhesion of 5B, light transmittance of ≥90% at 550nm wavelength, haze of ≤1.5% and ethanol decay rate of ≤5%, and qualified storage stability, thereby solving the problems of incomplete low temperature curing, poor performance and large sacrifice of optical performance in the prior art.
[0137] 2) When the ratio of the solder resist composition deviates from the preferred range of this application (such as Examples 7, 9, 11, 13, 15, and 17), the performance decreases to varying degrees, but is still better than the comparative examples. When the ratio of the solder resist composition deviates significantly (such as Comparative Example 4), it leads to incomplete curing, significant performance degradation, and failure of storage stability, proving that the composition ratio range of the solder resist composition of this application is the key to achieving excellent performance.
[0138] 3) Compared with the traditional high-temperature curing system (Comparative Example 1), this application has better adhesion, optical properties and solvent resistance, and significantly reduced energy consumption and thermal damage, provided that the curing temperature is reduced by 60°C and the curing time is halved.
[0139] 4) Compared with the pure photocuring system (Comparative Example 2), the crosslinking density, hardness, adhesion and durability of the present invention are significantly improved, solving the core defects of pure photocuring.
[0140] 5) The system without glycidyl methacrylate grafted polyester polyol (Comparative Example 3) showed severe incomplete curing at low temperature, and its performance and storage stability were greatly reduced, proving that the core resin is the key to achieving low-temperature high-activity curing.
[0141] As can be seen from the above description, the embodiments of the present invention achieve the following technical effects:
[0142] The matrix resin of this application uses glycidyl methacrylate-grafted polyester polyol as the core matrix resin, combined with epoxy resin and acrylate polymers containing alicyclic epoxy resins to form a composite resin system. This allows the solder resist composition to achieve both photosensitivity and low-temperature curing activity. The carbon-carbon double bond of the methacryloyloxy group in the glycidyl methacrylate-grafted polyester polyol, combined with the highly reactive epoxy groups in the epoxy resin, can both match the photocuring system to achieve exposure imaging and undergo cross-linking reactions with the thermocuring system at low temperatures, thus solving the problem of insufficient low-temperature reactivity of traditional resins. The flexible polyester polyol segments of the glycidyl methacrylate-grafted polyester polyol can also improve the adhesion and flexibility of the cured film, preventing brittleness of the low-temperature cured film. The composite epoxy resin and acrylate polymers containing alicyclic epoxy resins can further improve the cross-linking density and heat and chemical resistance of the system, thereby achieving a balance between low-temperature curing properties and overall performance. This application employs a photo-thermal dual-curing system to achieve rapid and complete low-temperature curing. By constructing a dual-curing system of photocationic curing and low-temperature latent thermal curing, photocuring and shaping are first achieved through exposure, completing patterning and imaging, followed by low-temperature thermal curing for deep cross-linking. The cationic photoinitiator can achieve efficient excitation in the 400nm~500nm ultraviolet band, and with the addition of a sensitizer, this can be extended to the 400nm~500nm visible light band, thus better adapting to industry-standard exposure equipment and achieving uniform curing even in thick films. The thermal initiator, combined with the latent curing system and low-temperature activating agent, can rapidly trigger the cross-linking reaction at 80~120℃, shortening the curing time to less than 30 minutes, with a gel content ≥95%, completely solving the problems of incomplete reaction and low curing efficiency in traditional low-temperature curing systems. The latent curing system exhibits excellent storage stability at room temperature, preventing premature gelation. Adding fillers provides necessary insulation and dimensional stability, as well as improving light utilization. Adding photosensitive monomers improves the photosensitivity of the solder resist composition. In summary, by controlling the components and weight proportions of the solder resist composition within the aforementioned range, this application comprehensively improves overall performance and adapts to various application scenarios. After curing, the solder resist composition of this application achieves a pencil hardness ≥3H, a cross-cut adhesion test grade of 5B, a light transmittance ≥90% at 550nm wavelength, a haze ≤1.5%, and a performance degradation of ≤5% after 24 hours of water and alcohol immersion. It also exhibits excellent anti-yellowing properties and weather resistance. Therefore, the solder resist composition of this application solves the problems of thermal damage and high energy consumption associated with high-temperature curing, and overcomes the shortcomings of insufficient cross-linking density and poor durability associated with pure photocuring. This allows it to be adapted to various scenarios such as flexible substrates, thin substrates, thermal component encapsulation, and photovoltaic modules, while remaining compatible with existing production line processes without additional equipment investment, thus possessing extremely high industrial application value.
[0143] The above are merely embodiments of the present invention and are not intended to limit the invention. Those skilled in the art will recognize that the present invention can have various modifications and variations. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A solder resist composition, characterized in that, By weight, the solder resist composition comprises: 55-75 parts of a base resin, 10-50 parts of a filler, 0.5-5 parts of a thermal initiator, 2-8 parts of a cationic photoinitiator, 15-25 parts of a photosensitive monomer, 10-18 parts of a latent curing system, and 5-10 parts of a low-temperature activating agent; the base resin comprises glycidyl methacrylate grafted polyester polyol; the base resin further comprises epoxy resin and / or acrylate polymer containing alicyclic epoxy.
2. The solder resist composition according to claim 1, characterized in that, The epoxy resin is a bisphenol A type epoxy resin and / or an alicyclic epoxy resin; the alicyclic epoxy resin includes hydrogenated bisphenol A type epoxy resin; the epoxy equivalent of the epoxy resin is 180 g / eq to 500 g / eq. And / or, the weight-average molecular weight of the acrylate polymer containing alicyclic epoxy is 5000 g / mol to 20000 g / mol; And / or, the raw materials for preparing the glycidyl methacrylate-grafted polyester polyol include glycidyl methacrylate and polycaprolactone diol, wherein the mass ratio of glycidyl methacrylate to polycaprolactone diol is 100:(20~50); and / or, the epoxy value of the glycidyl methacrylate-grafted polyester polyol is 0.85mol / 100g~1.2mol / 100g; and / or, the content of carbon-carbon double bonds of methacryloyloxy groups in the glycidyl methacrylate-grafted polyester polyol is 0.6mol / 100g~1.0mol / 100g; And / or, the mass percentage of the glycidyl methacrylate-grafted polyester polyol in the matrix resin is 30% to 40%.
3. The solder resist composition according to claim 1, characterized in that, The thermal initiator is selected from any one or more of dicyclohexyl peroxide dicarbonate, microcapsule-encapsulated imidazole thermal initiators, boron trifluoride amine complexes, and α-salt thermal initiators; And / or, the cationic photoinitiator is an aryl sulfonium salt and / or an aryl iodonium salt; wherein, the aryl sulfonium salt is bis(triarylsulfonium)hexafluoroantimonate; the aryl iodonium salt is (4-dodecoxyphenyl)[4-(pentadecafluorodecoxy)phenyl]iodonium hexafluoroantimonate and / or (4-methylphenyl)[4-(2-methylpropyl)phenyl]iodonium hexafluorophosphate; And / or, the mass ratio of the glycidyl methacrylate-grafted polyester polyol to the cationic photoinitiator is (4~10):1; the mass ratio of the thermal initiator to the cationic photoinitiator is 1:(1.5~5). And / or, the photosensitive monomer is selected from any one or more of trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and ethoxylated trimethylolpropane triacrylate.
4. The solder resist composition according to any one of claims 1 to 3, characterized in that, The latent curing system includes a phosphine-based latent catalyst and a microencapsulated acid anhydride curing agent; Preferably, the mass ratio of the phosphine-based latent catalyst to the microencapsulated anhydride curing agent is (4~8):(6~10). Preferably, the phosphine-based latent catalyst is a triphenylphosphine complex and / or microencapsulated triphenylphosphine; Preferably, the microencapsulated anhydride curing agent includes a capsule shell, the capsule shell forming a closed cavity, and the cavity is filled with an anhydride curing agent; preferably, the anhydride curing agent is methyltetrahydrophthalic anhydride; preferably, the capsule shell is made of polyurea, and the thickness of the capsule shell is 0.2~0.5μm; preferably, the particle size of the microencapsulated anhydride curing agent is 3~5μm.
5. The solder resist composition according to claim 1, characterized in that, The low-temperature activation aid is an ortho-hydroxy-substituted phenolic resin; the ortho-hydroxy-substituted phenolic resin is selected from any one or more of phenolic resins, o-cresol phenolic resins, and bisphenol A phenolic resins. And / or, the weight-average molecular weight of the low-temperature activation aid is 800 g / mol to 2500 g / mol; And / or, the mass ratio of the low-temperature activating agent to the thermal initiator is (2~10):
1.
6. The solder resist composition according to any one of claims 1 to 5, characterized in that, The solder resist composition further includes 2 to 10 parts of reactive diluent; the reactive diluent is an epoxy reactive diluent, and the number of epoxy groups in the epoxy reactive diluent is ≥2, preferably 2 to 4; Preferably, the epoxy reactive diluent is 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarbamate and / or 1,4-butanediol diglycidyl ether.
7. The solder resist composition according to any one of claims 1 to 6, characterized in that, The filler is a silane-modified filler; preferably, the filler is selected from any one or more of silane-modified nano-silica, silane-modified nano-titanium dioxide and silane-modified barium sulfate; and / or, the average particle size of the filler is 50nm~150nm; Preferably, when the filler is a combination of silane-modified nano-titanium dioxide and silane-modified barium sulfate, the mass ratio of the silane-modified nano-titanium dioxide to the silane-modified barium sulfate is (6~8):(2~4). Preferably, the solder resist composition further includes 0.1 to 20 parts of an additive: the additive is selected from any one or more of anti-yellowing agents, leveling agents, defoamers, pigments, sensitizers and adhesion promoters.
8. A solder resist dry film, comprising a support layer and a solder resist layer stacked thereon, characterized in that, The solder resist layer is obtained by mixing and drying the solder resist layer composition according to any one of claims 1 to 7.
9. A solder resist layer, characterized in that, The solder resist composition according to any one of claims 1 to 7 is obtained by photocuring and thermocuring.