A Method and System for Predicting the Aging Life of Conductive Silicone Rubber Based on Multi-Characteristic Coupling

By employing a multi-characterization coupling method, combining dynamic mechanical properties, crosslinking density, and surface elemental tests, a multi-dimensional dataset is generated. By applying a first-order reaction kinetic model and the Arrhenius equation, the problem of multiple environmental factors in the aging prediction of conductive silicone rubber is solved, achieving accurate lifetime prediction and engineering applications.

CN123115653APending Publication Date: 2026-11-17SOUTHWEST TECHNICAL ENGINEERING RESEARCH INSTITUTE OF CHINA SOUTH IND GROUP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611255554.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing methods for predicting the aging life of conductive silicone rubber mostly use a single performance index, which makes it difficult to fully reflect the complex aging behavior under multiple environmental factors. Furthermore, they lack unified quantitative methods for multi-dimensional data, resulting in low prediction accuracy and the inability to form a standardized life assessment process.

Method used

A multi-characterization coupling method is adopted to generate a multi-dimensional characterization dataset through dynamic mechanical property testing, crosslinking density testing, and surface element content testing. After normalization, the aging degree and environmental acceleration factor are calculated by combining the first-order reaction kinetic model and the Arrhenius equation, and the service life at room temperature is extrapolated.

Benefits of technology

It achieves unified quantification and accurate extrapolation of the aging state of conductive silicone rubber, improves the prediction accuracy of service life at room temperature, and has practical engineering value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123115653A_ABST
    Figure CN123115653A_ABST
Patent Text Reader

Abstract

This invention discloses a method and system for predicting the aging life of conductive silicone rubber based on multi-characterization coupling. The method involves applying various environmental accelerated aging test stresses to conductive silicone rubber samples to obtain a series of samples under different aging environments. Dynamic mechanical property tests, crosslinking density tests, and surface element content tests are then performed on these samples to generate a multi-dimensional characterization dataset. Key indicators in the multi-dimensional characterization data are normalized to generate a normalized aging degree sequence. Based on the normalized aging degree sequence, a first-order reaction kinetic model combined with the Arrhenius equation is used for parameter fitting to generate a multi-environment kinetic parameter set. Based on the multi-environment kinetic parameter set and a preset material failure aging degree threshold, a predicted remaining life value for the conductive silicone rubber is generated. Using this invention, the aging state of conductive silicone rubber can be uniformly quantified and accurately extrapolated, improving the prediction accuracy of its service life at room temperature and enhancing its engineering practical value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of silicone rubber life prediction technology, and in particular to a method and system for predicting the aging life of conductive silicone rubber based on multi-characterization coupling. Background Technology

[0002] Conductive silicone rubber, due to its excellent conductivity and flexibility, is widely used in critical fields such as aerospace sealing, electronic shielding, and new energy battery connections. During actual service, conductive silicone rubber is simultaneously subjected to the coupled effects of multiple environmental factors, including heat, oxygen, humid heat, and electrical stress. Irreversible aging phenomena occur within the material, such as the destruction of cross-linked structures, oxidation of conductive fillers, and interface degradation, leading to a gradual deterioration of conductivity and mechanical properties, ultimately causing system failure. Accurately predicting its service life is crucial for ensuring equipment reliability. However, most existing aging life prediction methods use a single performance index (such as tensile strength or volume resistivity) as a degradation criterion, which is insufficient to comprehensively reflect the complex aging behavior of conductive silicone rubber under multiple environmental factors. Furthermore, traditional accelerated aging models often ignore the inherent coupling relationships between different characterization dimensions, resulting in low extrapolation prediction accuracy. They also lack a unified quantitative method for quantifying aging from multi-dimensional data to normalized aging degree, making it impossible to establish a standardized life assessment process. Summary of the Invention

[0003] The purpose of this invention is to provide a method and system for predicting the aging life of conductive silicone rubber based on multi-characterization coupling, so as to overcome the shortcomings of the prior art, realize the unified quantification and accurate extrapolation of the aging state of conductive silicone rubber, and improve the prediction accuracy and engineering practical value of the service life at room temperature.

[0004] One embodiment of this application provides a method for predicting the aging lifetime of conductive silicone rubber based on multi-characterization coupling, the method comprising: Various environmental accelerated aging test stresses were applied to conductive silicone rubber samples, and samples were taken at preset time intervals to obtain a series of samples under various aging environments. Dynamic mechanical properties, crosslinking density, and surface element content were tested on the series of samples to extract multi-dimensional characterization data and generate a multi-dimensional characterization dataset. The key indicators in the multi-dimensional characterization data are normalized to calculate a uniform aging degree between 0 and 1, and a normalized aging degree sequence is generated. Based on the normalized aging degree sequence, a first-order reaction kinetic model combined with the Arrhenius equation is used to fit the parameters, solve the reaction rate constant and environmental acceleration factor under each aging environment, and generate a multi-environment kinetic parameter set. Based on the set of multiple environmental dynamic parameters and the preset material failure aging threshold, the service life prediction formula after correction by the environmental acceleration factor is substituted into the formula, and the service life at room temperature is extrapolated to generate the remaining service life prediction value of conductive silicone rubber.

[0005] Another embodiment of this application provides a system for predicting the aging life of conductive silicone rubber based on multi-characterization coupling, the system comprising: The sampling module is used to apply various environmental accelerated aging test stresses to conductive silicone rubber samples and take samples at preset time intervals to obtain a series of samples under various aging environments. The extraction module is used to perform dynamic mechanical property testing, crosslinking density testing, and surface element content testing on the series of samples, extract multi-dimensional characterization data, and generate a multi-dimensional characterization dataset. The processing module is used to normalize the key indicators in the multi-dimensional characterization data, calculate the uniform aging degree between 0 and 1, and generate a normalized aging degree sequence. The fitting module is used to perform parameter fitting based on the normalized aging degree sequence, using a first-order reaction kinetic model combined with the Arrhenius equation, to solve the reaction rate constant and environmental acceleration factor under each aging environment, and generate a multi-environment kinetic parameter set. The generation module is used to extrapolate and calculate the service life prediction formula after environmental acceleration factor correction based on the set of multiple environmental dynamic parameters and the preset material failure aging threshold, and generate the remaining service life prediction value of conductive silicone rubber.

[0006] Another embodiment of this application provides a storage medium storing a computer program, wherein the computer program is configured to execute the method described in any of the preceding claims when running.

[0007] Another embodiment of this application provides an electronic device including a memory and a processor, wherein the memory stores a computer program and the processor is configured to run the computer program to perform the method described in any of the preceding claims.

[0008] This invention enables unified quantification and accurate extrapolation of the aging state of conductive silicone rubber, improving the accuracy of predicting service life at room temperature and its practical engineering value. Attached Figure Description

[0009] Figure 1 A hardware structure block diagram of a computer terminal for predicting the aging lifetime of conductive silicone rubber based on multi-characterization coupling, provided for an embodiment of the present invention. Figure 2 A flowchart illustrating a method for predicting the aging life of conductive silicone rubber based on multi-characterization coupling, provided in an embodiment of the present invention; Figure 3 This is a schematic diagram of a conductive silicone rubber aging life prediction system based on multi-characterization coupling, provided in an embodiment of the present invention. Detailed Implementation

[0010] The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.

[0011] Rubber materials, due to their excellent extensibility, strength, abrasion resistance, chemical resistance, and durability, are widely used as sealing materials and vibration damping materials in aerospace, military equipment, automotive, and transportation fields. However, during use, they inevitably age due to environmental factors such as temperature, humidity, ultraviolet radiation, and corrosion, causing changes in their performance and making them unable to meet usage requirements. In particular, rubber products that serve in extreme and harsh environments and suffer multiple environmental damages have a service life far shorter than expected.

[0012] During long-term use or natural storage, silicone rubber is affected by environmental factors such as heat and oxygen, as well as compressive stress present in the service environment, resulting in significant changes in certain macroscopic properties. This process is known as silicone rubber aging. Rubber aging is the result of the combined effects of the material's own molecular structure and external environmental factors. The main environmental factors that promote aging include temperature, humidity, ozone, radiation, irradiation, mechanical stress, chemical corrosion, and biodegradation.

[0013] Thermal oxidation is a typical aging process. Chain breaking and cross-linking reactions can change the molecular structure of rubber, leading to its performance degradation. These two reactions play a core role in the thermal oxidation mechanism.

[0014] Moist heat aging is one of the more common aging phenomena of silicone rubber materials. Moist heat aging is a coupled damage effect of thermal oxidation and hydrolysis. In thermal oxidation aging, the chain breakage reaction and cross-linking reaction compete, with the cross-linking reaction playing a dominant role in most rubber materials, showing an increasing trend in cross-linking density and leading to increased material hardness. Hydrolytic aging is mainly caused by the breakage of a large number of polymer chains, resulting in a decrease in cross-linking density and softening of the material. Compared with hydrolysis, water absorption decreases during moist heat aging; therefore, the moist heat aging process mainly has two effects: increased cross-linking reaction and decreased chain breakage reaction.

[0015] In recent years, in-depth research has been conducted on the aging mechanisms of rubber materials, including damp heat, hydrolysis, thermal oxidation, and ozone decomposition. Among these, based on the universality of environmental factors, damp heat, hydrolysis, and thermal oxidation are the most serious mechanisms affecting the aging of rubber materials. Researchers have conducted accelerated aging tests to simulate the real service environment of rubber. Studies have shown that the competitive mechanism of chain scission and crosslinking in thermal oxidation, the reduction of chain scission and crosslinking in hydrolysis, and the coupled damage from thermal oxidation and hydrolysis in damp heat aging are the main causes of the degradation of the physical, chemical, and mechanical properties of rubber materials. However, due to the complexity of the environmental factors experienced by rubber materials during use, research on the multi-factor coupled damage mechanism is insufficient, with most studies simply focusing on changes in performance and aging time. The aging of silver-plated aluminum powder conductive silicone rubber under heat, damp heat, and salt spray environments involves multiple mechanisms such as matrix crosslinking, hydrolysis, and filler corrosion, resulting in complex performance evolution. Existing aging evaluation methods generally have the following shortcomings: (1) Using only a single performance index (such as hardness or electrical resistance) cannot reflect the intrinsic relationship between the internal changes and surface chemical evolution of silicone rubber; (2) No unified kinetic model for the evolution of DMA, crosslinking density, and XPS elements has been established; (3) The acceleration factors in multiple environments (heat / humid heat / salt spray) are unclear, and the lifetime extrapolation error is large; (4) The lack of an engineerable life prediction model makes it difficult to guide material selection and reliability design under actual working conditions.

[0016] In practical applications, rubber is subjected to complex environmental factors. Research on the transmission mechanism of damage from various environmental factors between the micro, meso, and macro levels is still at the logical level, and the solution method for the dynamic model parameters of rubber products in complex environments still needs to be explored.

[0017] The thermodynamic and kinetic behaviors of rubber materials under the coupled effects of multiple environmental factors are the fundamental cause of their environmental damage. Revealing the essence of the coupled effects of multiple environmental factors from a thermodynamic perspective and studying the interaction process of these factors on rubber materials from a kinetic perspective are essential requirements for scientifically predicting lifespan and mitigating environmental impacts. Therefore, constructing a multi-dimensional, multi-environmentally applicable aging kinetic model to achieve accurate lifespan prediction has significant scientific and engineering application value.

[0018] The present invention first provides a method for predicting the aging life of conductive silicone rubber based on multi-characterization coupling. This method can be applied to electronic devices, such as computer terminals, specifically ordinary computers.

[0019] The following detailed explanation uses a computer terminal as an example. Figure 1 This is a hardware structure block diagram of a computer terminal for predicting the aging life of conductive silicone rubber based on multi-characterization coupling, provided as an embodiment of the present invention. Figure 1As shown, the computer device includes a processor, memory, and network interface connected via a system bus, wherein the memory may include non-volatile storage media and internal memory.

[0020] See Figure 2 The present invention provides a method for predicting the aging lifetime of conductive silicone rubber based on multi-characterization coupling, which may include the following steps: S201, apply various environmental accelerated aging test stresses to conductive silicone rubber samples and take samples at preset time intervals to obtain a series of samples under various aging environments; Specifically, standard dumbbell-shaped samples of conductive silicone rubber with silver-plated aluminum powder can be prepared, and the samples can be randomly divided into three groups and labeled as the thermo-oxidative aging group, the damp heat aging group, and the acidic salt spray aging group. The core of this step is to complete the standardized preparation and equal grouping of test samples, reduce the test errors caused by individual differences from the source of the samples, establish the sample basis for three types of accelerated aging tests, and ensure the comparability and validity of test data under different aging conditions. The specific implementation method is as follows: Silver-plated aluminum conductive silicone rubber is a polymer functional material composed of silicone rubber as the matrix and silver-plated aluminum powder as the conductive filler. It retains the excellent elasticity, weather resistance, and deformation resistance of silicone rubber while possessing stable conductivity. It is commonly used as a sealing and vibration-damping conductive component in various industrial applications and is the core object of this multi-environment aging study. The dumbbell shape is a standard sample shape commonly used in polymer aging, mechanical, and physicochemical testing. This shape effectively avoids stress concentration problems during testing and aging, ensuring that the aging effect is uniformly applied to the main body of the sample. During the sample preparation stage, the entire process of raw material mixing, high-temperature vulcanization, isothermal shaping, and precise cutting was strictly followed to control the uniformity of all sample dimensions, keeping the overall dimensional deviation within a minimal range. Simultaneously, the silver-plated aluminum filler was ensured to be uniformly dispersed within the silicone rubber matrix, avoiding localized filler enrichment or deficiency that could affect the aging evolution. Sufficient standard dumbbell-shaped samples were prepared for this experiment, with the overall quantity sufficient to meet all requirements for sampling at multiple time points, parallel testing, and replacement of abnormal samples.

[0021] After sample preparation, all samples were placed in a dry environment at room temperature for a sufficient period of time to allow the internal stress of the material to be fully released and return to a stable initial state. Then, random grouping was performed. Random grouping avoids minor individual differences that may occur during the molding and cutting processes, preventing systematic errors from being superimposed on the results of subsequent aging tests. All samples were divided into three evenly distributed groups, with multiple parallel samples reserved within each group for subsequent data verification. The three groups of samples were clearly marked according to the predetermined test direction, defined as the thermo-oxidative aging group, the damp-heat aging group, and the acidic salt spray aging group, respectively, corresponding to the three typical aging environments. Marking was performed only on the edges and corners of the samples, using a marking method that would not chemically react with the silicone rubber matrix or metal fillers, and would not scratch the sample surface or damage the original structure and properties of the material. After grouping, the three groups of samples were placed separately, awaiting transfer to the corresponding aging test equipment for accelerated aging treatment.

[0022] The thermo-oxidative aging group samples were placed in constant temperature aging chambers at four temperature points: 90℃, 100℃, 110℃, and 120℃. The damp heat aging group samples were placed in damp heat aging chambers at 70℃+90%RH and 90℃+90%RH. The acidic salt spray aging group samples were placed in a salt spray test chamber. All aging test devices were started. The core of this step is to establish gradient and differentiated accelerated aging conditions using specialized testing equipment, artificially reproducing three types of real service damage environments: thermo-oxidative, humid-heat, and acidic salt spray. This allows the samples to undergo molecular structure changes and filler corrosion reactions according to the corresponding aging mechanisms. The specific implementation method is as follows: Thermo-oxidative aging is the most basic form of aging for silicone rubber. The combined effect of ambient temperature and oxygen in the air triggers both chain-splitting and cross-linking reactions in the molecular chains. These two reactions compete with each other and gradually alter the internal network structure of the material. A constant-temperature aging chamber is a specialized device for accelerated thermo-oxidative aging. The chamber has a uniform temperature distribution, with temperature deviations controlled within a reasonable range, ensuring a completely consistent thermo-oxidative environment for each sample. Four temperature gradients were set: 90℃, 100℃, 110℃, and 120℃. This gradient temperature design allows for the acquisition of aging rate data at different temperatures, providing multi-dimensional sample support for subsequent parameter fitting of the Arrhenius equation. The thermo-oxidative aging samples were further divided equally and placed in the four constant-temperature aging chambers at different temperatures, with reasonable spacing between samples to ensure that hot air and oxygen can fully contact the entire sample surface, avoiding localized heat accumulation and poor airflow that could affect the aging process.

[0023] Humid heat aging is a complex damage effect resulting from the coupling of thermal oxidation and hydrolysis. Ambient temperature and moisture work together, with thermal oxidation dominating the cross-linking reaction, while water molecules trigger polymer chain breakage. These two effects superimpose to accelerate material degradation. The parameter RH represents relative humidity; 90% RH indicates that the ambient moisture content reaches 90% saturation, a typical parameter for simulating high-humidity service scenarios. The humid heat aging chamber can precisely control both temperature and relative humidity simultaneously, with temperature and humidity control accuracy meeting experimental requirements. In this study, a fixed relative humidity of 90% RH was used, along with two temperature gradients of 70℃ and 90℃, to differentiate the weight of temperature factors in the humid heat coupled aging process. The humid heat aging samples were split and placed in the corresponding equipment, with the sample placement method consistent with that of the thermal oxidation aging samples.

[0024] Acidic salt spray aging primarily simulates corrosive environments such as marine and chemical plants. Chloride ions in the salt spray continuously corrode the silver-plated aluminum conductive filler and gradually erode the silicone rubber matrix, resulting in multiple damages from filler corrosion and matrix aging. The salt spray test chamber atomizes the acidic solution, creating a uniform salt spray atmosphere within the chamber, maintaining a stable basic environment. The acidic salt spray aging samples are placed on a dedicated support within the chamber, tilted according to the test specifications to prevent uneven corrosion caused by localized accumulation of salt spray droplets. After all samples are in place, the three types of test devices are started sequentially. After startup, the equipment is pre-run for a period of time to ensure that parameters such as temperature, humidity, and salt spray concentration within the chamber are completely stable before formally starting the aging time, ensuring that the initial operating conditions strictly meet the preset standards.

[0025] According to the preset sampling time interval, take out the corresponding number of parallel samples under each aging test condition, record the specific aging time and environmental conditions for each sampling, and generate a sampling record table with timestamps. The core of this step is to extract samples at different aging stages according to the time sequence, to fully capture the entire process of the material from its initial state to its gradual deterioration, and at the same time retain complete operating conditions and time sequence records, establishing a one-to-one correspondence between samples and aging states. The specific implementation method is as follows: By considering the aging characteristics of conductive silicone rubber, a gradient sampling time interval is set. In the early stage of aging test, the changes in the material's molecular structure and surface elemental composition are slow, and the fluctuations in various performance indicators are small, so a longer sampling interval is set. In the middle stage of aging, reactions such as crosslinking, hydrolysis, and corrosion gradually intensify, and the material performance begins to deteriorate significantly, so the sampling interval is appropriately shortened. In the later stage of aging, the rates of various reactions increase significantly, and the material deterioration rate accelerates, so the sampling nodes are further densified to accurately capture the characteristic changes at different aging stages. At each preset sampling node, multiple parallel samples are taken from a single aging condition. Parallel samples can reduce the random errors brought about by a single test and can also meet the experimental requirements for subsequent parallel data verification and mean calculation.

[0026] Upon reaching each preset sampling node, sampling is performed sequentially for all operating conditions. The sampling process is conducted rapidly throughout, minimizing the time the samples are out of the test environment and preventing interference from ambient temperature and pressure conditions on the current aging state of the samples. After each set of operating conditions is sampled, all corresponding environmental parameters are recorded immediately, including specific temperature values, relative humidity values, and salt spray condition type. The cumulative aging time from the official start of the test to this sampling is also recorded, with hours as the unit of measurement. Key characteristic nodes can be recorded in more detail. A timestamp uniquely identifies each sampling action, recorded in a complete year, month, day, hour, and minute format to distinguish sampling activities from different batches and time periods. Information such as environmental type, environmental parameters, cumulative aging time, sampling timestamp, and number of samples taken are integrated and organized to form a complete sampling record table. All information in the table is matched one-to-one, achieving full traceability of the test process and providing a basis for subsequent multi-dimensional characterization tests.

[0027] Each sample taken out is classified and numbered according to the aging environment type and aging time, and sealed in a dry and sealed bag for storage and testing, thus generating a series of samples under various aging environments.

[0028] The core of this step is to standardize and protect the samples after sampling, preventing secondary aging caused by the external environment. All samples are integrated according to environmental and temporal dimensions to form a structurally complete sample system, ensuring the orderly conduct of subsequent tests. The specific implementation method is as follows: After sampling, the samples were first categorized into three main types based on the aging environment: thermo-oxidative aging, damp-heat aging, and acidic salt spray aging. Then, the cumulative aging time was used as the second categorization dimension. Within the same environment, samples at different aging stages were sequentially sorted to clearly distinguish the aging process of each sample. Subsequently, a standardized numbering process was implemented. The code combination included environmental identification, operating parameters, cumulative aging time, and sampling batch number. Each sample had a unique number, completely avoiding confusion between samples from different operating conditions and durations. Parallel samples under the same operating condition were also distinguished by a simple suffix, facilitating subsequent parallel data comparison and analysis.

[0029] Once the samples have been classified and numbered, they must be immediately placed in a dry, sealed bag for protection. This bag effectively isolates the samples from external air, moisture, dust, and light, preventing oxidation, hydrolysis, and other side reactions after the samples are removed from the testing equipment. It accurately preserves the microstructure, surface elements, and mechanical state of the samples at the moment of sampling. Parallel samples under the same conditions and for the same aging time are uniformly packaged, with the bag opening completely sealed to prevent the infiltration of external media. All packaged samples are placed in a dedicated storage area under ambient temperature and light-protected conditions. The temperature and humidity are controlled within a stable range. Light-protected conditions prevent photo-oxidation side reactions induced by light in the silicone rubber, further ensuring that the sample condition does not undergo additional changes.

[0030] All encapsulated samples were categorized into three aging environments. Each environment included samples with different aging durations from the initial, middle, and later stages of the test. This collection of samples, covering the complete aging sequence and corresponding to different degrees of degradation, constitutes the series of samples for the corresponding aging environment. The entire series of samples is clearly classified, fully coded, and stable, and can be sequentially used for dynamic mechanical properties, crosslinking density, X-ray photoelectron spectroscopy, and other testing stages, providing comprehensive sample support for multi-dimensional data acquisition, aging degree calculation, and kinetic model construction.

[0031] S202, Dynamic mechanical properties, crosslinking density and surface element content of the series of samples are tested, multi-dimensional characterization data are extracted and multi-dimensional characterization dataset is generated. Specifically, a dynamic thermomechanical analyzer can be used to perform temperature scanning tests on a series of samples, set the heating rate and frequency, record the temperature spectrum of storage modulus and loss factor, extract the glass transition temperature value, and generate a DMA test data table. The core of this step is to use dynamic thermomechanical analysis to capture the changes in dynamic mechanical properties and molecular chain motion during the aging process of conductive silicone rubber, extract the glass transition as a key characteristic parameter, and form standardized dynamic mechanical test data. This provides a macroscopic performance basis for subsequent aging characteristic analysis. The specific implementation method is as follows: Dynamic thermomechanical analysis is the mainstream testing method in the field of polymer materials for characterizing viscoelasticity and molecular chain motion properties. When silver-plated aluminum conductive silicone rubber ages under environments such as heat and oxygen, humidity and heat, and salt spray, its internal cross-linked network undergoes reconstruction and breakage, directly affecting the mobility of molecular chain segments, ultimately manifesting in changes in storage modulus, loss factor, and glass transition temperature. Before formal testing, all series of samples obtained in batches were individually fixed in the instrument's dedicated clamping positions, ensuring that the clamping tightness and placement of each sample remained consistent to avoid interference from additional stress generated by mechanical clamping. This temperature scan test used uniform operating parameters, with the industry-standard heating rate set at 2°C per minute. This parameter ensures testing efficiency while continuously and completely capturing the evolution trend of material properties during temperature changes. The testing frequency was fixed at 1 Hz, which is the reference frequency for dynamic mechanical testing of silicone rubber materials.

[0032] During continuous temperature scanning, the instrument synchronously collects the storage modulus E' and loss factor tanδ at different temperature nodes in real time. Using temperature as the horizontal axis and the corresponding performance parameters as the vertical axis, a continuous and complete temperature spectrum curve is generated. The storage modulus represents the material's resistance to elastic deformation. During thermo-oxidative aging, cross-linking reactions dominate, the cross-linked network becomes denser, and the storage modulus gradually increases. Under humid and hot conditions, hydrolysis causes molecular chain breakage, resulting in a slight decrease in storage modulus. The loss factor represents the degree of energy loss within the material. Aging-induced impeded molecular chain movement causes the loss factor to fluctuate regularly. The glass transition temperature Tg is the most critical characteristic parameter in the temperature spectrum, corresponding to the critical temperature at which polymer chain segments transition from a frozen state to a free-moving state; it is also an important indicator for assessing the degree of material aging. The corresponding glass transition temperature value is accurately read from each temperature spectrum curve. Then, all test results are organized in the order of sample number, aging environment, cumulative aging time, energy storage modulus, loss factor, and glass transition temperature. After removing obviously abnormal test data, a standardized DMA test data table is generated. This data table completely preserves the dynamic mechanical characteristics information of each sample.

[0033] The crosslinking density of each series of samples was tested using a low-field nuclear magnetic resonance crosslinking density meter. The crosslinking density value of the samples was calculated based on the proton relaxation time, and a crosslinking density test data table was generated. The core of this step is to use non-destructive NMR detection technology to quantify the density of the cross-linked network inside the silicone rubber, and to calculate the cross-linking density parameter based on the proton motion law, forming test data at the microscopic level of the structure, thus supplementing the microscopic characteristics of the material's aging. The specific implementation method is as follows: Low-field nuclear magnetic resonance (NMR) technology eliminates the need for destructive treatments such as chemical etching or cutting of samples, enabling precise detection of the motion state of hydrogen protons within a silicone rubber matrix. The relaxation time of hydrogen protons is directly related to the degree of constraint on the molecular chains. Crosslinking nodes restrict the movement of silicone rubber molecular chains; the denser the crosslinking network, the smaller the space for molecular chain movement, and the shorter the proton relaxation time. Based on this principle, the crosslinking density ν can be calculated by measuring the relaxation time. Crosslinking density is a core indicator characterizing the microstructure of rubber, commonly measured in mol / cm³. 3 The changes in crosslinking density under different aging environments show significant differences. In thermo-oxidative aging, crosslinking reaction is dominant, and the crosslinking density increases continuously with aging time. In damp-heat aging, hydrolysis and chain scission occur, and the crosslinking density gradually decreases. In acidic salt spray aging, the matrix and filler are simultaneously eroded, and the crosslinking density also shows a slow downward trend.

[0034] During the test, all the test samples were sequentially placed into the sealed detection chamber of the instrument, maintaining stable temperature and magnetic field conditions inside the chamber. Signal acquisition was performed on each sample individually to obtain the raw proton relaxation time signal for each sample. Based on the conversion rules for silicone rubber materials, the crosslinking density value of each sample was calculated from the measured proton relaxation time. After completing the calculations for all samples, the data was sorted out in the order of sample number, aging environment, cumulative aging time, and crosslinking density value. Invalid data caused by sample placement misalignment or instantaneous magnetic field fluctuations were removed, ultimately generating a complete crosslinking density test data table. This data table independently reflects the changes in the crosslinking network within each sample, complementing the dynamic mechanical test data to characterize the aging state of the material from both macroscopic and microscopic levels.

[0035] X-ray photoelectron spectroscopy was used to perform broadband and high-resolution narrow spectrum scanning on the surface of each series of samples to obtain the atomic percentages of C, O, Si and Ag elements, and to calculate the O / C atomic ratio and the relative content of Ag, generating XPS test data tables. The core of this step is to analyze the elemental composition and chemical changes on the sample surface using energy dispersive spectroscopy (EDS), distinguish between two types of aging behaviors: matrix oxidation and conductive filler corrosion, calculate derived characteristic parameters, and generate test data for the surface chemical dimension, comprehensively covering the aging characteristics of the material surface. The specific implementation method is as follows: The X-ray photoelectron spectrometer operates in two modes: broadband scanning and high-resolution narrow-spectrum scanning. These two modes have different functions and complement each other. Broadband scanning is used for a comprehensive elemental survey of the sample surface, quickly identifying all elements present on the surface. This study focuses on detecting C, O, and Si in the silicone rubber matrix, and Ag in the silver-plated aluminum conductive filler. The atomic percentages of each of the four elements are directly output after scanning. High-resolution narrow-spectrum scanning performs a refined scan of the aforementioned four target elements, correcting for minor errors in broadband scanning and further improving the accuracy of the elemental percentage data.

[0036] During material aging, surface oxidation continuously consumes the matrix carbon and enriches oxygen, which is visually manifested as a continuously increasing O / C atomic ratio. This ratio is the calculated result of the percentage of oxygen atoms versus the percentage of carbon atoms. In acidic salt spray and high-humidity, hot and humid environments, corrosive media continuously erode the silver-plated aluminum filler, causing a gradual loss of Ag. Therefore, using the Ag content of unaged samples as a benchmark, the relative Ag content of each aged sample can be calculated. This parameter can directly quantify the degree of corrosion of the conductive filler. After collecting the elemental proportions, the O / C atomic ratio and relative Ag content are calculated for each sample. All data are then organized in the order of sample number, aging environment, cumulative aging time, percentage of the four elements, O / C atomic ratio, and relative Ag content. The data variation patterns under different environments are distinguished, and finally, an XPS test data table is generated. This data table specifically reflects the chemical evolution of the sample surface and the damage to the conductive filler.

[0037] The DMA test data table, crosslinking density test data table, and XPS test data table are vertically merged according to the sample number to form a complete dataset containing multi-dimensional characterization parameters for each sample, and finally a multi-dimensional characterization dataset is generated.

[0038] The core of this step is to integrate three independent types of data—dynamic mechanics, micro-crosslinking, and surface chemistry—using the unique sample number as a link, thus establishing data connections across different testing dimensions and constructing a comprehensive characterization dataset. This lays a complete data foundation for subsequent index extraction and aging calculation. The specific implementation method is as follows: The DMA, crosslinking density, and XPS data tables correspond to three independent testing dimensions: macroscopic properties, microstructure, and surface chemistry of the material, respectively. A single data table can only reflect local aging characteristics and cannot reflect the comprehensive changes during the aging process. Each sample uses the same unique number throughout the entire testing process. This number serves as a unique identifier for merging the three types of data, ensuring that all data under the same number originate from the same sample and preventing data misalignment at its source. The vertical merging method uses the sample number as the main thread, sequentially integrating and piecing together the dynamic mechanical parameters, crosslinking density values, and surface elemental parameters corresponding to the same number, without modifying the original test values ​​or disrupting the data arrangement logic throughout the entire process.

[0039] After merging, each data entry fully integrates all characterization parameters of the corresponding sample, including macroscopic dynamic performance data such as glass transition temperature and storage modulus, as well as microscopic structural data such as crosslinking density, and surface chemical data such as elemental composition, O / C atomic ratio, and relative Ag content. Sample data from different aging environments exhibit differentiated characteristics. Thermo-oxidative aging samples show a shift in glass transition temperature, an increase in crosslinking density, and slow surface oxidation; humid heat samples show a decrease in crosslinking density and increased oxidation; and acidic salt spray samples highlight filler corrosion characteristics with a significant decrease in relative Ag content. The merged complete dataset undergoes integrity verification, checking for missing data, incorrect numbering, etc. After successful verification, the final multi-dimensional characterization dataset is obtained. This dataset comprehensively recreates the composite aging characteristics of conductive silicone rubber under various environments and serves as the core data source for subsequent index normalization and aging degree sequence generation.

[0040] S203, normalize the key indicators in the multi-dimensional characterization data, calculate the uniform aging degree between 0 and 1, and generate a normalized aging degree sequence. Specifically, four key indicators can be extracted from the multi-dimensional characterization dataset: glass transition temperature shift, crosslinking density, O / C atomic ratio, and Ag relative content. The initial average value of the unaged sample and the saturation value after full aging are calculated for each aging environment, generating initial and saturation parameter sets. The core of this step is to select four key indicators from the integrated multi-dimensional characterization data that can comprehensively reflect the material's bulk structure, dynamic mechanical properties, surface chemical state, and the integrity of conductive fillers. Characteristic values ​​for the initial and extreme aging states are statistically analyzed separately for different aging environments. A basic parameter system for normalization calculations is then established to ensure a unified reference benchmark for subsequent aging degree calculations. The specific implementation method is as follows: The multi-dimensional characterization dataset integrates all results from dynamic mechanical testing, crosslinking density testing, and X-ray photoelectron spectroscopy. The data covers test information for all time-series samples under three major aging environments: thermo-oxidative, humid heat, and acidic salt spray. The four key indicators extracted in this step each have clear physical meanings and aging characterization directions, and their combined effect can comprehensively depict the full-dimensional aging characteristics of silver-plated aluminum powder conductive silicone rubber. The glass transition temperature shift, calculated from the dynamic thermomechanical analysis results, is the difference between the glass transition temperature of the aged sample and its original state. Under the influence of heat, humidity, and salt spray, the mobility of silicone rubber molecular chain segments gradually changes with crosslinking and hydrolysis reactions, causing a shift in the glass transition temperature. The magnitude of this shift directly corresponds to the degree of degradation of the material's dynamic mechanical properties. The crosslinking density value, obtained through low-field nuclear magnetic resonance testing, represents the density of the polymer crosslinking network within the silicone rubber matrix. During thermo-oxidative aging, the dominant crosslinking reaction increases the crosslinking density, while hydrolysis under humid heat causes molecular chain breakage, thus reducing the crosslinking density. This indicator is the core basis for judging the evolution of the material's internal microstructure. Both the O / C atomic ratio and the relative Ag content are derived from X-ray photoelectron spectroscopy analysis. The O / C atomic ratio is the ratio of the percentage of oxygen atoms to the percentage of carbon atoms on the sample surface. As the oxidation reaction occurs on the material surface, the proportion of oxygen continuously increases, and this ratio continuously increases, which can directly reflect the degree of surface oxidation aging. The relative Ag content represents the proportion of conductive silver-plated aluminum filler on the sample surface. Acidic salt spray and high humidity environments can corrode the metal filler, causing filler loss. The rate of decrease in this value can quantify the degree of functional aging caused by filler corrosion.

[0041] Unaged samples refer to standard samples that have not participated in the accelerated aging test and remain in their original factory condition, serving as the benchmark reference sample for the entire test. Since multiple sets of parallel samples were used in the test, the test results of a single sample may have random errors. Therefore, for each key indicator, the arithmetic mean of the test results of all unaged parallel samples under the corresponding aging environment was calculated. This average value was defined as the initial indicator value and uniformly denoted as X0. The saturation indicator value after sufficient aging is denoted as X0. ∞ The value refers to the test value when the molecular cross-linking network, surface element composition, and filler content no longer change significantly after the sample has undergone long-term aging in the corresponding aging environment, and the material properties reach the stable limit state. At this time, the aging process of the material has basically stopped, and various indicators have entered the saturation stage.

[0042] This study statistically analyzed parameters under three aging environments: thermo-oxidative, humid heat, and acidic salt spray. For each environment, the initial mean and saturation values ​​of four indicators were calculated independently. Taking a gradient thermo-oxidative aging environment from 90℃ to 120℃ as an example, the initial mean glass transition temperature of the unaged sample under this environment was -58.2℃. After the material was fully aged and reached saturation, the saturation value of the glass transition temperature was -51.6℃; the initial mean crosslinking density was 0.0026 mol / cm³. 3 The saturated crosslinking density is 0.0039 mol / cm³. 3 The initial average O / C atomic ratio was 0.12, and the O / C atomic ratio under saturation was 0.27; the initial average Ag relative content was 28.5%, and the saturated Ag relative content after full aging was 16.2%. For humid heat aging environments of 70℃ + 90%RH, 90℃ + 90%RH, and acidic salt spray aging environments, the same statistical method was used to obtain X0 and X under each environment for the four indicators. ∞ Numerical values. The initial mean and saturation values ​​of all aging environments and four key indicators are systematically integrated according to environmental category and indicator type to form a complete and clearly categorized set of initial and saturation values. Each set of parameters in the set corresponds one-to-one with the aging environment and test indicator, providing a fixed reference standard for the normalization conversion of all subsequent sample indicators.

[0043] For the glass transition temperature offset of each sample, a normalized temperature offset aging component is generated using a normalization formula. The core of this step is to use a unified normalized mathematical formula to transform the glass transition temperature offset, a physical test value with specific dimensions, into a dimensionless aging component. This achieves the conversion of a single performance indicator into a quantitative value of aging degree, laying the foundation for dimensional unification for multi-indicator fusion calculations. The specific implementation method is as follows: The normalization formula used throughout this process is α=|(X t -X0) / (X ∞ -X0)|, this formula is the core calculation basis for achieving unified quantification of multiple types of characterization data. Each parameter in the formula has a clear definition, where α represents the aging degree component obtained after conversion of a single indicator, and is a dimensionless value; X t X represents the measured value of this index for the corresponding sample under a specific aging time; X0 is the initial average value of this index obtained in the previous steps under the same environment; X ∞ This is the saturation index value of this indicator under the same environment. The absolute value sign in the formula is used to avoid the influence of positive and negative values ​​caused by different trends in the rise and fall of the indicator, so as to ensure that the final aging degree component is always a non-negative value.

[0044] The glass transition temperature shift is the only calculation object in this step. Each sample taken from different aging environments and for different aging times has an independent measured glass transition temperature result. Subtracting the original glass transition temperature of the unaged sample in the same environment from this measured result yields the glass transition temperature shift of that sample, which is X in the formula. t The glass transition temperature of silicone rubber continues to change during the aging process. The cross-linking reaction caused by thermo-oxidation tightens the molecular chains, reduces the mobility of chain segments, and causes the glass transition temperature to shift towards higher temperatures. The amount of shift increases with aging time until it approaches the shift limit corresponding to the saturation state.

[0045] Taking a sample placed in a 90℃ thermo-oxidative environment for a cumulative aging time of 500 hours as an example, the measured glass transition temperature of this sample is -53.9℃. Combined with the initial glass transition temperature of -58.2℃ in the same environment, the glass transition temperature deviation X of this sample is calculated. t The initial mean value X0 corresponding to the glass transition temperature shift under this environment is 0℃, and the saturation index value X is 4.3℃. ∞ The value is 6.6℃. Substituting the three sets of values ​​into the normalization formula, calculations were performed. After difference and ratio operations, the aging component corresponding to the glass transition temperature dimension of the sample was obtained. Following the same calculation logic, calculations were performed on each sample in the multi-dimensional characterization dataset, regardless of whether the sample belonged to a thermo-oxidative, humid-heat, or acidic salt spray environment, matching the corresponding environment's X0 and X... ∞ The parameters are set to ensure that the calculation baseline is completely matched with the aging conditions of the sample. Each normalized temperature offset aging component obtained in this step reflects the degree of aging of the sample due to changes in dynamic mechanical properties, and is the core single data point constituting the overall aging degree.

[0046] For the three indicators of crosslinking density, O / C atomic ratio and Ag relative content, their respective aging degree components are calculated according to the same normalization formula to obtain four single indicator aging degree components, and a set of aging degree components is generated. The core of this step is to continue the unified normalization calculation rules, complete the aging degree conversion of the remaining three key indicators, supplement the aging quantification results of all individual dimensions, and then summarize the four components corresponding to the same sample to form a complete set of aging degree components, which comprehensively covers all aging dimensions such as material microstructure, surface oxidation, and conductive filler corrosion. The specific implementation method is as follows: This step continues to use α=|(X) t -X0) / (X ∞The normalization formula (-X0)| maintains the consistency of the entire calculation system, avoiding data disconnect between different indicators due to differences in calculation rules, and truly achieving unified quantification of data from three different test systems: DMA, crosslinking density, and XPS. The crosslinking density value, O / C atomic ratio, and Ag relative content are calculated sample-by-sample. These three indicators correspond to different aging damage mechanisms of conductive silicone rubber. The crosslinking density value focuses on the evolution of the crosslinking network of the material's molecular structure. Thermo-oxidative aging, dominated by crosslinking reactions, increases the crosslinking density, while hydrolysis reactions in humid-heat aging break molecular chains and reduce the crosslinking density. Both trends can be converted into an aging degree component using the normalization formula. The O / C atomic ratio focuses on the oxidation damage on the sample surface. The longer the aging time and the stronger the environmental corrosion, the higher the degree of surface oxidation, resulting in a larger value for this indicator and a corresponding increase in the aging degree component. The Ag relative content focuses on the corrosion loss of conductive silver-plated aluminum filler. Acidic salt spray and high-humidity environments accelerate the corrosion of metal fillers. As aging progresses, the value of this indicator continuously decreases, while the aging degree component gradually increases.

[0047] Using the same sample from the previous example, aged in a 90℃ thermo-oxidative environment for 500 hours, the calculations for the three indicators were completed sequentially. First, the crosslinking density value was processed; the measured crosslinking density X of this sample... t It is 0.0032 mol / cm 3 Under the same conditions, the initial average crosslinking density X0 was 0.0026 mol / cm³. 3 saturated crosslinking density X ∞ It is 0.0039 mol / cm 3 After substituting into the normalization formula, the aging degree component corresponding to the crosslinking density is obtained. Next, the O / C atomic ratio is processed; the measured O / C atomic ratio X of this sample... t The initial mean X0 is 0.12, and the saturation value X is 0.20. ∞ The value is 0.27, and the aging component of the surface oxidation dimension is obtained after calculation. Finally, the relative Ag content is processed, and the measured relative Ag content X of this sample is obtained. t The initial mean X0 is 28.5%, and the saturation value X is 22.1%. ∞ The aging degree component of the filler corrosion dimension was calculated to be 16.2%. Combined with the glass transition temperature shift aging degree component obtained in the previous step, the sample now has four single-index aging degree components from different characterization dimensions.

[0048] The above calculation process is repeated for all samples in the dataset. Each sample generates four independent aging components. Then, according to the sample's unique number, aging environment, and cumulative aging time, the four components corresponding to each sample are collected and organized. After all collections are completed, an aging component set is formed. Each set of data in this set fully includes the aging quantification results of four dimensions: dynamic mechanics, molecular structure, surface oxidation, and filler corrosion. This fully restores the composite aging characteristics of silver-plated aluminum powder conductive silicone rubber under multiple environmental conditions, providing complete and comprehensive basic data support for subsequent fusion calculation of unified aging degree and data verification.

[0049] The arithmetic mean of the glass transition temperature offset aging component and the crosslinking density aging component is taken as the unified aging degree. At the same time, the consistency of the O / C atomic ratio and Ag relative content aging components is checked, and outliers with deviations exceeding the set threshold are removed. Finally, a normalized aging degree sequence is generated.

[0050] The core of this step is to select two components that can represent the core aging state of the material and calculate a unified aging degree. Then, two auxiliary dimension components are used to complete the data reliability verification, and abnormal data generated during the experiment and testing process are screened out. Finally, the time-series aging degree sequence is arranged in chronological order to form a time-series aging degree sequence that can be directly used for dynamic modeling. The specific implementation method is as follows: Glass transition temperature shift and crosslinking density are two core indicators for evaluating the aging state of silicone rubber. The former reflects changes in the macroscopic dynamic mechanical properties of the material, while the latter reflects the evolution of the internal microscopic crosslinking network. Together, they determine the overall performance and structural stability of the material. Therefore, the arithmetic mean of these two corresponding aging components is calculated to serve as a unified aging degree that comprehensively characterizes the overall aging degree of the sample. The arithmetic mean calculation method balances the weights of the two core indicators, avoiding bias towards a single dimension of aging characteristics, and objectively reflects the overall aging level of the material itself. Combining the values ​​of the two core components of the example sample mentioned earlier, the average value is obtained by adding them together. This value strictly falls within the range of 0 to 1, conforming to the definition rules of aging degree. A value of 0 represents that the sample has not aged at all, while a value of 1 represents that the sample has reached a state of complete aging failure. Different values ​​within the range correspond to different progressive aging stages of the material.

[0051] The O / C atomic ratio aging component and the Ag relative content aging component serve as auxiliary verification indicators, corresponding to two secondary aging characteristics: surface oxidation and conductive filler corrosion, respectively. In the normal accelerated aging process of silver-plated aluminum powder conductive silicone rubber, the evolution of the bulk structure aging, surface oxidation, and filler corrosion exhibits a high degree of synchronicity. There will be no significant deviation between the uniform aging degree of a normal sample and the two auxiliary components. The pre-set data deviation threshold is 0.15, determined in conjunction with the conventional error range of polymer material aging tests. The specific verification rule is to calculate the absolute value of the difference between the uniform aging degree and the O / C atomic ratio aging component and the Ag relative content aging component. When any difference exceeds 0.15, the data set is considered an outlier. Outlier data is generally caused by accidental factors such as improper sampling operations, sample surface contamination, instantaneous fluctuations in testing equipment, or localized hidden damage to the sample. These outliers cannot accurately reflect the normal aging process of the material and must be removed.

[0052] According to the established verification rules, consistency verification was performed on all data groups within the aging degree component set one by one. The numerical deviations were compared group by group, and all abnormal data exceeding the threshold were marked and removed, retaining all valid data that met the deviation requirements. After removing outliers, the remaining valid unified aging degree values ​​were categorized into three aging environments: thermo-oxidative, humid-heat, and acidic salt spray. Within each environment, the values ​​were arranged sequentially according to the cumulative aging time of the samples, from shortest to longest, ensuring that each time point corresponds to a unique unified aging degree value. These values ​​were then sequentially linked according to the aging process, ultimately forming a complete normalized aging degree sequence. This sequence clearly demonstrates the complete evolution of the comprehensive aging degree of conductive silicone rubber over aging time under different aging environments. The data, after multiple verifications, possesses high reliability and can be directly used in the parameter fitting stage of the first-order reaction kinetic model and the Arrhenius equation, providing accurate time-series data support for subsequent multi-environment kinetic parameter solutions and lifetime extrapolation.

[0053] S204. Based on the normalized aging degree sequence, a first-order reaction kinetic model combined with the Arrhenius equation is used to fit the parameters, and the reaction rate constant and environmental acceleration factor under each aging environment are solved to generate a multi-environment kinetic parameter set. Specifically, for each temperature point in a pure thermal aging environment, the normalized aging degree sequence can be fitted nonlinearly using the first-order reaction kinetic formula to solve for the reaction rate constant k at each temperature, thereby generating a table of rate constants for the pure thermal environment. The core of this step is to rely on the already verified time-series aging data, combined with the general first-order reaction kinetic model for polymer material aging, to solve the aging reaction rate at different thermo-oxidative temperatures using a nonlinear fitting algorithm. This quantifies the influence of temperature on the aging rate and provides basic rate data for subsequent kinetic parameter calculations. The specific implementation method is as follows: The pure thermo-oxidative aging environment set up in this experiment included four temperature gradients: 90℃, 100℃, 110℃, and 120℃. This gradient temperature setting captures the variation of reaction rate with temperature. The normalized aging degree sequence is the effective data after outlier removal and temporal sorting. Each data point in the sequence corresponds to the comprehensive aging degree of the sample at a specific aging time, with values ​​stable between 0 and 1, gradually increasing with aging time, fully reproducing the entire process of conductive silicone rubber transitioning from an initial intact state to a saturated aged state. The first-order reaction kinetic integral formula used in this experiment is α = 1 − exp(−k(T)・t), where α represents the dimensionless normalized aging degree, k(T) represents the temperature-dependent reaction rate constant measured in seconds, and t represents the cumulative aging time of the material measured in seconds. This formula originates from the first-order reaction differential equation of silicone rubber aging, conforming to the changes in the internal cross-linking network reconstruction and surface oxidation reaction of the material, and is also the core foundational formula for this full-process modeling.

[0054] Nonlinear least squares fitting is the mainstream parameter-solving algorithm adapted to this nonlinear kinetic formula. The core logic of the algorithm is to continuously iteratively adjust the value of the parameter k(T) to continuously reduce the sum of squared residuals between the theoretical aging degree calculated by the formula and the measured normalized aging degree. When the change in the sum of squared residuals is less than the preset minimum convergence threshold, the fitting operation is considered complete, and the parameter obtained at this time is the optimal reaction rate constant. Independent fitting operations are performed on the aging degree sequences corresponding to four pure thermo-oxygen temperatures. Taking a 90℃ pure thermo-oxygen environment as an example, all time-series aging degree data under this environment are substituted into the kinetic formula, iterative operations are started, and the convergence rules are strictly followed to finally obtain the reaction rate constant corresponding to this temperature. Following completely consistent operation rules, fitting calculations are performed sequentially at three temperature points: 100℃, 110℃, and 120℃. Due to the increased molecular thermal motion and oxidation reaction caused by rising temperature, the higher the temperature, the larger the value of the calculated reaction rate constant k, and the faster the aging reaction proceeds. The reaction rate constants corresponding to the four temperature points are organized and recorded in order of increasing temperature, with complete labeling of the corresponding temperature and rate values, forming a complete record of rate constants in a pure thermal environment, clearly showing the rate differences of material aging reaction under different thermo-oxidative conditions.

[0055] Linear regression was performed based on the linear form of the Arrhenius equation to calculate the apparent activation energy Ea and the pre-exponential factor A, thus generating thermo-oxidative kinetic parameters. The core of this step is to use the multi-temperature reaction rate data obtained in the previous step to convert the Arrhenius exponential model into a linear form and then perform regression calculations to solve for the apparent activation energy and pre-exponential factor that characterize the inherent reaction properties of the material, thus establishing a quantitative mathematical relationship between the reaction rate and absolute temperature. The specific implementation method is as follows: The Arrhenius equation is a classic formula describing the change of chemical reaction rate with temperature. Its basic expression is k(T) = A・exp(−Ea / (RT)). Each parameter in the formula has a clear physical meaning: A is the pre-exponential factor, measured in seconds, and is an inherent parameter determined by the material's molecular structure and the type of reaction; Ea is the apparent activation energy, measured in J / mol, representing the minimum energy required to trigger the thermo-oxidative aging reaction of conductive silicone rubber. A higher activation energy indicates a more difficult aging reaction to initiate; R is the universal gas constant, fixed at 8.314 J·mol throughout the experiment. -1 ·K -1 T represents absolute temperature, measured in Kelvin. When converting everyday Celsius temperature to absolute temperature, simply add 273.15 to the Celsius value.

[0056] Since the original Arrhenius equation is in a nonlinear exponential form, a linear regression algorithm cannot be directly used. Therefore, the natural logarithm is calculated on both sides of the equation to obtain the linear form lnk = lnA − Ea / (RT). The transformed expression is a standard linear function in one variable, with 1 / T as the horizontal axis variable, lnk as the vertical axis variable, the slope of the function being −Ea / R, and the intercept being lnA. The purpose of the linear regression algorithm is to fit the optimal fitted line based on multiple sets of discrete data, minimizing the deviation between the measured data and the fitted line. First, the natural logarithm of the reaction rate constant k corresponding to the four pure heat-oxygen temperatures obtained in the first step is calculated to obtain the corresponding lnk values. At the same time, the four Celsius temperatures are uniformly converted to absolute temperatures, and the reciprocal of the absolute temperature, 1 / T, is calculated, thus forming four sets of one-to-one discrete data combinations. Substituting all data combinations into the linear regression process, the slope and intercept of the fitted line are calculated.

[0057] By combining the slope of the straight line with the gas constant R for reverse derivation, the apparent activation energy Ea of the pure thermo-oxidative aging system can be calculated. Then, by combining the ordinate intercept and using exponential calculation, the pre-exponential factor A can be obtained. Based on the experimental results, the apparent activation energy Ea of conductive silicone rubber under pure thermo-oxidative conditions is generally around 45.2 kJ·mol⁻¹. -1 Up to 49.7 kJ·mol -1 Within the interval, the pre-exponential factor A corresponds to 2.15 × 10. 4 s -1 Up to 2.62×10 4 s -1Within the range of [specific parameters], the apparent activation energy, pre-exponential factor, and goodness-of-fit information obtained from the solution are integrated to form a complete set of thermo-oxidative kinetic parameters. This set of parameters can accurately describe the intrinsic law of material aging reaction rate changing with temperature in a pure thermo-oxidative environment.

[0058] For humid heat aging environment and acidic salt spray aging environment, the reaction rate constants of each are obtained by fitting the first-order reaction kinetic formula. Then, the rate constants are compared with the rate constants of pure heat environment at the same temperature to calculate the humid heat acceleration factor and salt spray acceleration factor, and generate an environmental acceleration factor table. The core of this step is to address the two multi-factor coupled aging conditions of humid heat and acidic salt spray. A unified kinetic fitting method is used to obtain the corresponding reaction rates. The environmental acceleration factor is calculated by comparing the ratios of different environmental rates at the same temperature. This quantifies the accelerating effect of water vapor and corrosive ions on the aging reaction and distinguishes the severity of aging under different combined environments. The specific implementation method is as follows: The composite aging conditions set up in this study are divided into two main categories: damp heat aging, which includes two conditions: 70℃ with 90% relative humidity and 90℃ with 90% relative humidity; and acidic salt spray, which is an independent corrosion aging condition. For each composite aging environment, a validated normalized aging degree sequence is extracted for the corresponding condition. The sequence data covers the complete temporal change of the material from its initial state to aging saturation. The first-order reaction kinetic formula α=1−exp(−k(T)・t) is used as the fitting model, along with a nonlinear least squares fitting algorithm. The same iteration rules and convergence thresholds as for the pure thermo-oxygen environment are used to solve for the total reaction rate constant k for the two damp heat conditions and one acidic salt spray condition. total In a humid and hot environment, water molecules can trigger the hydrolysis of the silicone rubber matrix. In an acidic salt spray environment, chloride ions can continuously corrode the silver-plated aluminum conductive filler and the rubber matrix. Both of these additional factors will work together with the thermo-oxidative effect to accelerate the aging process. Therefore, the total reaction rate constant of the composite environment at the same temperature will be significantly higher than that of the pure thermo-oxidative environment.

[0059] The environmental acceleration factor AF is the core parameter for quantifying the acceleration effect of multiple environments, and the corresponding correction formula is k. total =AF・k thermal , where k thermal The reaction rate constant represents the reaction rate in a pure thermo-oxygen environment under the same temperature conditions. From this, the acceleration factor can be calculated as AF = k total / k thermal In a pure hot-oxygen environment, there are no additional accelerating factors, and its acceleration factor is fixed at 1. The test stipulates that the acceleration factor of a humid-heat environment should not be less than 1.5, and the acceleration factor of an acidic salt spray environment should not be less than 2.0. The larger the value of the acceleration factor, the stronger the accelerating effect of the environment on material aging, and the more severe the working conditions.

[0060] Taking a 90℃ operating condition as an example, the k value of a pure thermo-oxygen environment at that temperature is retrieved. thermal The numerical value, k, was obtained by fitting a humid and hot environment of 90℃ and 90% relative humidity. total The acceleration factor for the humid heat condition was calculated to be 1.89 through ratio calculation. Using the same method, the acceleration factor for the humid heat condition at 70℃ and 90% relative humidity was 1.56. After comprehensive calculation for the acidic salt spray condition, the acceleration factor was 2.03. After completing the acceleration factor calculations for all composite conditions, the humid heat acceleration factor and salt spray acceleration factor were systematically organized according to environmental type, operating temperature, and humidity conditions. The acceleration factor values ​​for each set of conditions were fully recorded, forming an environmental acceleration factor record that visually demonstrates the differences in the acceleration ability of different composite environments on the aging process of conductive silicone rubber.

[0061] The activation energy and pre-exponential factor in the thermo-oxidative kinetic parameters are summarized with the environmental acceleration factors in the environmental acceleration factor table to form a parameter set containing the Ea, A, and AF values ​​under various aging environments, and finally a multi-environmental kinetic parameter set is generated.

[0062] The core of this step is to integrate the dynamic parameters obtained from all previous steps, categorize them hierarchically according to aging environment type, and construct a complete parameter system covering all test conditions. This provides a unified and complete parameter input for subsequent extrapolation calculations of service life at room temperature. The specific implementation method is as follows: First, the apparent activation energy Ea and pre-exponential factor A are extracted from the thermo-oxidative kinetic parameters. These two parameters are inherent fundamental parameters of the aging reaction of conductive silicone rubber, determining the material's reaction characteristics and temperature dependence. For four pure thermo-oxidative temperatures of 90℃, 100℃, 110℃, and 120℃, the corresponding Ea and A values ​​for each temperature are retained to ensure a one-to-one correspondence between parameters and operating conditions. Then, the various environmental acceleration factors AF collected in the previous step are retrieved, including acceleration factors corresponding to two sets of humid heat conditions and one set of acidic salt spray conditions. A baseline acceleration factor with a uniform value of 1 for the pure thermo-oxidative environment is also added to complete the acceleration factor data for all operating conditions.

[0063] The aging environment was categorized and summarized into three main types: The first type is the pure thermo-oxidative aging environment, which includes the apparent activation energy (Ea), pre-exponential factor (A), and environmental acceleration factor (AF) corresponding to four temperature gradients; the second type is the humid-heat aging environment, which includes the complete set of parameters for two conditions: 70℃ + 90% relative humidity and 90℃ + 90% relative humidity; the third type is the acidic salt spray aging environment, which includes the apparent activation energy, pre-exponential factor, and acceleration factor corresponding to this corrosion condition. Throughout the parameter compilation process, the original values, units of measurement, and physical correspondences of all parameters were strictly preserved without any modification, deletion, or format change, ensuring that the three core parameters for each condition were completely matched.

[0064] The resulting parameter set comprehensively covers all thermo-oxidative, humid-heat, and acidic salt spray conditions involved in the experiments. Each aging environment is equipped with its own apparent activation energy, pre-exponential factor, and environmental acceleration factor. This set constitutes the multi-environment kinetic parameter set. This parameter set integrates three core elements: intrinsic material reaction characteristics, temperature acceleration laws, and multi-environment coupling acceleration effects. It serves as the core basis for calculations when substituted into the service life prediction formula corrected by the environmental acceleration factor. It can support the accurate extrapolation of the room-temperature life of conductive silicone rubber under different service conditions, completing the data connection from aging mechanism modeling to engineering life prediction.

[0065] S205. Based on the set of multiple environmental dynamic parameters and the preset material failure aging threshold, the service life prediction formula after correction by the environmental acceleration factor is substituted into the formula, and the service life at room temperature is extrapolated to generate the remaining service life prediction value of conductive silicone rubber.

[0066] Specifically, the apparent activation energy Ea, pre-exponential factor A, and environmental acceleration factor AF corresponding to the target service environment can be extracted from the set of multiple environmental dynamic parameters. At the same time, the material failure aging threshold is set to generate life prediction input parameters. The core of this step is to select key parameters suitable for actual service scenarios from the previously integrated global dynamic parameter system, set critical aging thresholds in conjunction with material failure judgment criteria, and build a complete life calculation input system to provide accurate and matching basic data for subsequent life formula calculations. The specific implementation method is as follows: The multi-environment kinetic parameter set integrates the kinetic characteristics of all test conditions under three major aging environments: thermo-oxidative, humid-heat, and acidic salt spray. Each service environment corresponds to a specific apparent activation energy Ea, pre-exponential factor A, and environmental acceleration factor AF. These three parameters characterize the intrinsic reaction properties of the material, the reaction baseline coefficient, and the environment's ability to accelerate the aging process, respectively. The apparent activation energy Ea is measured in kilojoules per mole, representing the minimum energy required to trigger the aging reaction of silver-plated aluminum powder conductive silicone rubber. This value varies significantly with the type of environment; under pure thermo-oxidative conditions, the activation energy generally ranges from 45.2 to 49.7 kJ·mol⁻¹. -1 In the range of humid and hot conditions, the activation energy decreases to 38.6 to 41.2 kJ·mol⁻¹. -1 The activation energy is lowest in acidic salt spray environments, at 35.7 kJ·mol⁻¹. -1 A lower activation energy indicates that the aging reaction is more easily triggered. The pre-exponential factor A, measured per second, is an intrinsic coefficient determined by the material's molecular structure, cross-linking system, and conductive filler distribution. In this experiment, this parameter ranged from 1.62 × 10⁻⁶. 4 s -1 Up to 2.62×10 4 s -1 There are slight differences in the pre-exponential factor under different environments. The environmental acceleration factor (AF) is used to quantify the accelerating effect of additional factors such as water vapor and corrosive ions on aging. In a pure thermo-oxygen environment with no additional accelerating medium, the AF value is fixed at 1. In a humid and hot environment, the AF value is not less than 1.5. In this study, the values ​​for the two humid and hot conditions were 1.56 and 1.89, respectively. The acidic salt spray corrosion effect is stronger, and the AF value reaches 2.03, which meets the technical characteristic that the acidic salt spray acceleration factor is not less than 2.0.

[0067] In practical engineering applications, the target service environment of the conductive silicone rubber is first determined. Based on the service environment type, three sets of parameters are extracted from the parameter set one by one. If the target scenario is a conventional atmospheric thermo-oxygen environment, Ea, A, and AF (value 1) at the corresponding temperature are extracted. If the target scenario is a high-humidity service environment, the complete set of parameters for the corresponding temperature and humidity conditions is selected. If the target scenario is a marine or chemical salt spray corrosion environment, the kinetic parameters for acidic salt spray conditions are used. After parameter extraction, the material failure aging threshold α needs to be set. f The normalized aging degree α ranges from 0 to 1. α = 0 represents that the material is not aged at all, while α = 1 represents that the internal cross-linking network of the material is completely destroyed and the conductive filler is completely ineffective, reaching a physically complete aging state. In accordance with the engineering maintenance standards for polymer materials, the end of the material's lifespan is not determined until it completely fails. Therefore, a failure aging degree threshold is artificially set as the critical standard for maintenance and replacement. In this case, α is uniformly set... fA threshold of 0.95 indicates that the conductive silicone rubber has lost its normal performance and requires replacement when the overall aging degree of the material reaches 0.95. The extracted Ea, A, and AF values ​​are then compared with the preset failure aging degree threshold α. f The parameters are uniformly collected and organized in an orderly manner according to parameter type, physical meaning, and numerical value to form a complete set of life prediction input parameters that match the operating conditions. This set of parameters will serve as the sole input basis for subsequent life formula calculations.

[0068] Convert the ambient service temperature to an absolute temperature value, substitute it into the Arrhenius formula to calculate the reaction rate constant k at that temperature without acceleration factor correction, and generate the ambient temperature reaction rate constant. The core of this step is to complete the conversion from Celsius temperature to absolute thermodynamic temperature. Based on the Arrhenius classical kinetic formula and combined with the extracted intrinsic parameters, the basic aging reaction rate in a pure thermal environment under normal temperature conditions is calculated, quantifying the rate of natural aging of materials in a normal temperature environment. The specific implementation method is as follows: The target extrapolated service temperature for this method is 25℃, which is also the standard room temperature condition for evaluating the long-term service life of polymer materials in the industrial field. During the kinetic calculations, the Arrhenius formula requires that temperature parameters be absolute temperatures. The conversion rule between absolute and Celsius temperatures is to add a constant of 273.15 to the Celsius temperature value. Therefore, the absolute temperature T corresponding to 25℃ is calculated to be 298.15K. The unit of measurement for absolute temperature is Kelvin, and this temperature value will be used throughout all subsequent formula calculations.

[0069] The Arrhenius equation used in this experiment is k(T) = A・exp(−Ea / (RT)). Each parameter in the equation has a fixed physical meaning and a set of values. R is the universal gas constant, which is fixed at 8.314 J·mol throughout the experiment. -1 ・K -1 , is a general constant in the field of physical chemistry; Ea and A are the apparent activation energy and pre-exponential factor corresponding to the target environment extracted in the previous step; T is the converted absolute temperature at room temperature; the calculated k(T) is the basic reaction rate constant without correction for environmental acceleration factors, and the unit of measurement is per second, representing the reaction rate of the material's own thermo-oxidative aging under the influence of temperature and oxygen only.

[0070] Calculations were performed separately for different target service environments. Taking the acidic salt spray service environment as an example, the corresponding Ea for this environment was 35.7 kJ·mol⁻¹. -1 A equals 1.65 × 10 4 s -1Combining R with the absolute temperature T, the basic thermal rate constant at room temperature is obtained through exponential and multiplicative operations. Taking a humid and hot environment of 90℃ and 90% relative humidity as another example, substituting Ea into the equation 41.2 kJ·mol⁻¹ -1 A equals 1.98 × 10 4 s -1 Calculations were performed to obtain the corresponding fundamental rate constant. For a purely thermo-oxygen environment, Ea equals 45.2 kJ·mol⁻¹. -1 A equals 2.15 × 10 4 s -1 The calculation is completed. Due to differences in activation energy values, the basic reaction rate constants corresponding to different environments also vary. The lower the activation energy, the higher the basic aging rate at room temperature, and the faster the material naturally ages. The rate constants calculated for each target environment are recorded separately, clearly defining the corresponding operating conditions and values. Finally, room temperature reaction rate constants for different service scenarios are generated. These rate constants only reflect the basic aging law dominated by temperature and do not yet include the accelerating effects of additional environmental factors such as humidity and salt spray.

[0071] The service life prediction formula after correction by the environmental acceleration factor is adopted. The failure aging degree, the room temperature reaction rate constant and the environmental acceleration factor are substituted into the formula to calculate the service life under room temperature conditions and generate the preliminary calculated value of the service life. The core of this step is to use a modified lifetime prediction formula adapted to multiple coupled environmental conditions, integrating three types of data: failure threshold, ambient temperature base rate, and environmental acceleration factor, to complete the theoretical calculation of long-term service life at ambient temperature, and obtain the initial lifetime result corresponding to a single parameter set. The specific implementation method is as follows: By combining the first-order reaction kinetic integral formula with the Arrhenius equation, and introducing an environmental acceleration factor to complete multi-condition corrections, a general service life prediction formula t is finally obtained. f =−ln(1−α f The formula ) / (AF・A・exp(−Ea / (RT))) is the core innovative formula for this method to achieve multi-environment lifetime extrapolation, perfectly integrating the intrinsic dynamic characteristics of materials, temperature effects, multi-environment acceleration effects, and failure judgment criteria. The α in the formula... f The preset failure aging threshold is denoted by AF, which is the environmental acceleration factor corresponding to the target environment. All other parameters remain consistent with the previous calculations. The final calculation result t is obtained from the formula. f The representative material represents the total time it takes to operate continuously in a target environment at room temperature from its initial intact state until it reaches the failure threshold.

[0072] Substitute all the parameters obtained in the previous steps into the formula to carry out the calculation. First, for the acidic salt spray service environment, substitute α... fGiven 0.95 and AF equals 2.03, along with Ea, A, absolute temperature T, and basic rate-related terms for this environment, logarithmic, exponential, and division operations are used to calculate the theoretical service life of conductive silicone rubber under normal temperature salt spray conditions, which is approximately 1.6 years. For a humid heat environment of 90℃ and 90% relative humidity, substituting AF equal to 1.89 and the corresponding kinetic parameters, the theoretical service life under normal temperature humid heat conditions is calculated to be approximately 1.8 years. For a pure hot oxygen conventional atmospheric environment, since AF is 1, there is no additional accelerating effect, and the material aging rate is significantly reduced; the theoretical service life under normal temperature pure heat conditions is calculated to be approximately 95 years.

[0073] Preliminary calculations under different environments intuitively demonstrate the impact of environmental severity on lifespan. Acidic salt spray corrosion has the strongest aging acceleration effect and the shortest material service life, followed by humid heat. Pure heat and oxygen conventional environments cause the least damage to the material and have the longest service life. This pattern perfectly matches the kinetic parameter characteristics obtained from previous accelerated aging tests. Each set of target environments corresponds to an independent duration value. These results, directly calculated from a single set of kinetic parameters, constitute the preliminary lifespan calculation value. The preliminary calculation value is a standard lifespan result based on a theoretical model, which can intuitively reflect the theoretical service limit of the material under different operating conditions, providing fundamental data for subsequent statistical optimization and accuracy verification.

[0074] Statistical analysis was performed on multiple lifetime calculation values ​​under various parallel aging environments. The median was taken as the final predicted lifetime, and the relative error was calculated to verify the accuracy of the model. Finally, the remaining lifetime prediction value of conductive silicone rubber was generated.

[0075] The core of this step is to conduct statistical optimization using multiple sets of preliminary lifetime data from parallel experiments to avoid random errors caused by a single parameter set. At the same time, the reliability of the entire prediction model is verified through error calculation, and the final remaining lifetime result that can be directly applied to engineering practice is output. The specific implementation method is as follows: In the early accelerated aging test phase, multiple sets of parallel samples were set up for each type of aging environment and each temperature condition, and multiple sets of parallel characterization data were collected accordingly. After normalization and fitting calculations, multiple sets of parallel kinetic parameters were also obtained. Based on these parallel parameters, multiple sets of corresponding preliminary lifetime calculation values ​​were calculated. The multiple sets of preliminary calculation values ​​under the same target service environment may have slight fluctuations. The sources of fluctuation mainly include minor differences between individual samples, random errors of the testing equipment, and minor deviations in the fitting calculations, which are normal phenomena in the testing process.

[0076] To mitigate the interference of individual outliers on the final results, the median was chosen as the optimal statistical method. The median is unaffected by extreme values ​​such as maxima and minima, and is more suitable for statistical analysis of engineering experimental data compared to the arithmetic mean. All preliminary lifetime calculations for the same target environment were arranged in ascending order of duration, and the value in the middle of the sequence was selected as the final predicted lifetime for that environment. Taking the acidic salt spray environment as an example, the preliminary lifetime values ​​obtained from multiple parallel calculations ranged from 1.52 to 1.68 years. After sorting all values ​​and extracting the median, the final predicted lifetime was approximately 1.6 years. The same statistical method was used for humid and hot environments and purely thermo-oxygen environments to further improve the stability of the results.

[0077] After determining the lifetime values, model accuracy was verified using relative error as the accuracy evaluation index. Relative error was calculated by comparing the measured failure time of the samples in accelerated aging tests with the model's predicted failure time; a smaller error value indicates higher model prediction accuracy. The design goal of the entire model was to achieve an overall prediction relative error of no more than 10%. After verification with multiple sets of parallel samples, the prediction relative error under different environments remained stable within 8%, meeting the preset accuracy requirements and demonstrating good model fitting and reliable extrapolation results.

[0078] The time value after statistical optimization and accuracy verification is the predicted value of the remaining life of conductive silicone rubber under the corresponding normal temperature service environment. This value takes into account multiple factors such as the intrinsic aging law of materials, the accelerated effect of multiple environments, and random errors in experiments. It has both the scientific nature of theoretical models and fits the actual engineering conditions. It can be directly used for engineering work such as material selection evaluation of conductive silicone rubber, equipment operation and maintenance plan formulation, and component life management.

[0079] In practical applications, this invention provides a method for evaluating and predicting the performance of conductive silicone rubber under multiple environmental factors coupled with damage. Based on the DMA, crosslinking density, and XPS test data of conductive silicone rubber samples during thermo-oxidative aging, damp heat aging, and salt spray aging processes, the aging kinetic equation of conductive silicone rubber under aging conditions is derived by statistical analysis. In particular, it can simultaneously predict the aging performance under multiple environmental factors, thereby meeting the needs of related fields for judging the aging performance of conductive silicone rubber under multiple factors coupled with damage.

[0080] An exemplary method for predicting the aging lifetime of conductive silicone rubber based on multi-characterization coupling includes the following steps: Three test conditions were set up: thermo-oxidative aging, damp heat aging, and acidic salt spray aging. The accelerated aging test conditions with multiple environmental factors carried out under each test condition included thermo-oxidative aging at 90℃, 100℃, 110℃, and 120℃, damp heat aging at 70℃+90%RH, damp heat aging at 90℃+90%RH, and acidic salt spray aging.

[0081] During the aging test, samples were intermittently taken under each aging test condition for DMA, crosslinking density, and XPS tests to obtain key characteristic parameter data under various aging test conditions. DMA test parameters included storage modulus E', glass transition temperature Tg, and loss factor tanδ; crosslinking density ν was determined using nuclear magnetic resonance; XPS test parameters included the atomic percentages of C, O, Si, and Ag, and the O / C ratio and relative Ag content were calculated.

[0082] Preliminary statistical analysis was conducted on the test data. First, for the macroscopic performance test data of conductive rubber, the mean / median (tensile strength and elongation at break) of the test data of parallel samples were obtained after performing Grubbs' test. Then, in-depth mechanism analysis was performed on the microscopic test data.

[0083] A multi-dimensional characterization coupled and multi-environmental applicable aging kinetic model is constructed. Based on the first-order reaction kinetic model, a multi-environment aging kinetic model is constructed by combining the Arrhenius equation. The three types of characterization data, namely the glass transition temperature offset ΔTg, crosslinking density ν, and relative content of XPS characteristic elements, are normalized into a unified aging degree α. This achieves a unified kinetic description of the evolution of microstructure and surface chemistry, quantitatively analyzes the regulatory mechanism of environmental factors on the aging rate, and establishes a service life prediction model.

[0084] Core Model Selection (1) Basic equation of reaction kinetics During the aging process of silicone rubber, the reconstruction of the crosslinked network and surface oxidation corrosion both follow first-order reaction laws. The aging rate is directly proportional to the remaining unaged degree, and the basic differential equation is:

[0085] In the formula: α—normalized aging degree, dimensionless; t—aging time, s; k(T)—temperature-dependent reaction rate constant, s -1 .

[0086] (2) Temperature-accelerated Arrhenius equation The aging reaction rate is temperature-dependent and follows the Arrhenius exponential law, expressed as:

[0087] In the formula: A – pre-exponential factor, s -1 Ea—apparent activation energy, J•mol -1 R—gas constant, valued at 8.314 J·mol⁻¹ -1 •K -1 T – Absolute temperature, K.

[0088] (3) Multi-environmental factor correction terms To address the multi-factor coupled environment of humid heat and acidic salt spray, an environmental accelerator factor AF is introduced to modify the simple thermo-oxidative aging rate, reflecting the effects of water molecules and Cl... - The acceleration effect, the corrected rate constant is:

[0089] Where: AF——Environmental acceleration factor (AF=1 for pure thermal environment, AF>1 for humid and hot, salt spray environment); —Reaction rate constant in a purely thermal environment, s -1 .

[0090] (4) Definition of normalized aging degree for multi-characteristic data To achieve dynamic uniformity of DMA, crosslinking density, and XPS data, the three core indicators are normalized to obtain the aging degree α. The normalization formula is as follows:

[0091] In the formula: —Test index value at aging time t; —Initial sample test index values; —Test index values ​​under aging saturation state.

[0092] The aging degree α is determined by combining at least two of the following: glass transition temperature offset ΔTg, crosslinking density ν, O / C ratio, and Ag content.

[0093] Judgment rules: α=0 represents that the material has not aged, α=1 represents that the material has completely aged and failed, and 0<α<1 represents that the material is in the intermediate aging stage.

[0094] Integral solution of dynamic model By integrating the first-order reaction kinetic differential equation and combining it with the Arrhenius equation, the analytical relationship between aging degree and time and temperature is obtained:

[0095] Substituting the Arrhenius equation into the above formula, we can obtain the aging degree evolution formula under multiple temperature fields:

[0096] Define material failure aging degree Derivation of the service life prediction formula:

[0097] Under the coupling of multiple environmental factors, the life prediction formula after introducing the environmental acceleration factor correction is as follows:

[0098] This invention provides a method for evaluating and predicting the performance of conductive silicone rubber under multiple environmental factors coupled together. It is the first to achieve a unified aging kinetic description using three testing methods: DMA, crosslinking density, and XPS. It can quantitatively distinguish the severity of thermal, humid heat, and salt spray environments, and provide the activation energy E. a With acceleration factor AF; high life prediction accuracy, error ≤10%; can extrapolate service life at 25℃, suitable for engineering reliability assessment.

[0099] The present invention will be further described below through specific embodiments, but is not limited thereto.

[0100] Solution and fitting of dynamic parameters (1) Data fitting process The aging degree was calculated using the normalized formula based on the test data from pure heat (90℃, 100℃, 110℃, 120℃), damp heat (70℃+90%RH, 90℃+90%RH), and acidic salt spray tests. Evolution curve over aging time; After verification, the aging degree initially obtained by normalizing the three types of indicators was found to be... The highly consistent evolution patterns demonstrate that the cross-linking reaction and surface chemical evolution occur synchronously and are controlled by the same kinetic mechanism.

[0101] By using the nonlinear least squares method to fit the first-order kinetic equation, the reaction rate constant k(T) under different temperatures and environments was obtained. Linear regression of lnk against 1 / T is performed according to the linear form of the Arrhenius equation. Calculate the apparent activation energy With the pre-exponential factor A; By comparing the rate constants of humid heat, salt spray, and pure heat environments, the environmental acceleration factor AF is calculated.

[0102] (2) The results of the dynamic parameters are shown in Table 1.

[0103] Table 1

[0104] 3) Calculate the aging degree α and fit the first-order kinetics; 4) Arrhenius fitting yields E a =35~50kJ / mol; 5) Salt spray AF≈2.03, damp heat AF≈1.89; 6) Extrapolated lifespan at 25℃: salt spray ≈ 1.6 years, 90℃ humid heat ≈ 1.8 years, pure heat ≈ 95 years.

[0105] Another embodiment of the present invention provides a system for predicting the aging life of conductive silicone rubber based on multi-characterization coupling, see [link to relevant documentation]. Figure 3 The system may include: The sampling module 301 is used to apply various environmental accelerated aging tests to conductive silicone rubber samples and to take samples at preset time intervals to generate a series of samples under various aging environments. Extraction module 302 is used to perform dynamic mechanical property testing, crosslinking density testing and surface element content testing on the series of samples, extract multi-dimensional characterization data, and generate multi-dimensional characterization dataset. Processing module 303 is used to normalize the key indicators in the multi-dimensional characterization data, calculate the uniform aging degree between 0 and 1, and generate a normalized aging degree sequence. The fitting module 304 is used to perform parameter fitting based on the normalized aging degree sequence, using a first-order reaction kinetic model combined with the Arrhenius equation, to solve the reaction rate constant and environmental acceleration factor under each aging environment, and generate a multi-environment kinetic parameter set. The generation module 305 is used to extrapolate and calculate the service life prediction formula after environmental acceleration factor correction based on the multi-environmental dynamic parameter set and the preset material failure aging threshold, and generate the remaining service life prediction value of conductive silicone rubber.

[0106] This invention also provides a storage medium storing a computer program, wherein the computer program is configured to execute the steps in any of the above method embodiments when running.

[0107] This invention also provides an electronic device, including a memory and a processor, wherein the memory stores a computer program, and the processor is configured to run the computer program to perform the steps in any of the above method embodiments.

Claims

1. A method for predicting the aging life of conductive silicone rubber based on multi-characterization coupling, characterized in that, The method includes: Various environmental accelerated aging test stresses were applied to conductive silicone rubber samples, and samples were taken at preset time intervals to obtain a series of samples under various aging environments. Dynamic mechanical properties, crosslinking density, and surface element content were tested on the series of samples to extract multi-dimensional characterization data and generate a multi-dimensional characterization dataset. The key indicators in the multi-dimensional characterization data are normalized to calculate a uniform aging degree between 0 and 1, and a normalized aging degree sequence is generated. Based on the normalized aging degree sequence, a first-order reaction kinetic model combined with the Arrhenius equation is used to fit the parameters, solve the reaction rate constant and environmental acceleration factor under each aging environment, and generate a multi-environment kinetic parameter set. Based on the set of multiple environmental dynamic parameters and the preset material failure aging threshold, the service life prediction formula after correction by the environmental acceleration factor is substituted into the formula, and the service life at room temperature is extrapolated to generate the remaining service life prediction value of conductive silicone rubber.

2. The method according to claim 1, characterized in that, The process involves applying various accelerated aging tests to the conductive silicone rubber sample, and sampling at preset time intervals to generate a series of samples under different aging environments, including: Standard dumbbell-shaped samples of conductive silicone rubber coated with silver aluminum powder were prepared and randomly divided into three groups, labeled as the thermo-oxidative aging group, the damp heat aging group, and the acidic salt spray aging group. The thermo-oxidative aging group samples were placed in constant temperature aging chambers at four temperature points: 90℃, 100℃, 110℃, and 120℃. The damp heat aging group samples were placed in constant temperature and humidity chambers at 70℃+90%RH and 90℃+90%RH. The acidic salt spray aging group samples were placed in a salt spray test chamber. All aging test devices were started. According to the preset sampling time interval, take out the corresponding number of parallel samples under each aging test condition, record the specific aging time and environmental conditions for each sampling, and generate a sampling record table with timestamps. Each sample taken out is classified and numbered according to the aging environment type and aging time, and sealed in a dry and sealed bag for storage and testing, thus generating a series of samples under various aging environments.

3. The method according to claim 2, characterized in that, The series of samples underwent dynamic mechanical property testing, crosslinking density testing, and surface elemental content testing to extract multi-dimensional characterization data and generate a multi-dimensional characterization dataset, including: A dynamic thermomechanical analyzer was used to perform temperature scanning tests on a series of samples. The heating rate and frequency were set, the temperature spectrum of storage modulus and loss factor was recorded, the glass transition temperature value was extracted, and a DMA test data table was generated. The crosslinking density of each series of samples was tested using a low-field nuclear magnetic resonance crosslinking density meter. The crosslinking density value of the samples was calculated based on the proton relaxation time, and a crosslinking density test data table was generated. X-ray photoelectron spectroscopy was used to perform broadband and high-resolution narrow spectrum scanning on the surface of each series of samples to obtain the atomic percentages of C, O, Si and Ag elements, and to calculate the O / C atomic ratio and the relative content of Ag, generating XPS test data tables. The DMA test data table, crosslinking density test data table, and XPS test data table are vertically merged according to the sample number to form a complete dataset containing multi-dimensional characterization parameters for each sample, and finally a multi-dimensional characterization dataset is generated.

4. The method according to claim 3, characterized in that, The key indicators in the multi-dimensional characterization data are normalized to calculate a uniform aging degree between 0 and 1, generating a normalized aging degree sequence, including: Four key indicators were extracted from the multi-dimensional characterization dataset: glass transition temperature shift, crosslinking density, O / C atomic ratio, and Ag relative content. The initial index mean and the saturation index value after full aging of the unaged sample under each aging environment were calculated to generate initial and saturation value parameter sets. For the glass transition temperature offset of each sample, a normalized temperature offset aging component is generated using a normalization formula. For the three indicators of crosslinking density, O / C atomic ratio and Ag relative content, their respective aging degree components are calculated according to the same normalization formula to obtain four single indicator aging degree components, and a set of aging degree components is generated. The arithmetic mean of the glass transition temperature offset aging component and the crosslinking density aging component is taken as the unified aging degree. At the same time, the consistency of the O / C atomic ratio and Ag relative content aging components is checked, and outliers with deviations exceeding the set threshold are removed. Finally, a normalized aging degree sequence is generated.

5. The method according to claim 4, characterized in that, Based on the normalized aging sequence, a first-order reaction kinetic model combined with the Arrhenius equation is used for parameter fitting to solve for the reaction rate constant and environmental acceleration factor under each aging environment, generating a multi-environment kinetic parameter set, including: For each temperature point in the pure thermo-oxidative aging environment, the normalized aging degree sequence is fitted nonlinearly using the first-order reaction kinetics formula to solve the reaction rate constant k at each temperature, and a table of rate constants for the pure thermo environment is generated. Linear regression was performed based on the linear form of the Arrhenius equation to calculate the apparent activation energy Ea and the pre-exponential factor A, thus generating thermo-oxidative kinetic parameters. For humid heat aging environment and acidic salt spray aging environment, the reaction rate constants of each are obtained by fitting the first-order reaction kinetic formula. Then, the rate constants are compared with the rate constants of pure heat environment at the same temperature to calculate the humid heat acceleration factor and salt spray acceleration factor, and generate an environmental acceleration factor table. The activation energy and pre-exponential factor in the thermo-oxidative kinetic parameters are summarized with the environmental acceleration factors in the environmental acceleration factor table to form a parameter set containing the Ea, A, and AF values ​​under various aging environments, and finally a multi-environmental kinetic parameter set is generated.

6. The method according to claim 5, characterized in that, Based on the aforementioned set of multiple environmental dynamic parameters and a preset material failure aging threshold, the service life prediction formula, corrected for environmental acceleration factors, is substituted into the formula to extrapolate and calculate the service life at room temperature, generating a predicted remaining life value for conductive silicone rubber, including: The apparent activation energy Ea, pre-exponential factor A, and environmental acceleration factor AF corresponding to the target service environment are extracted from a set of multiple environmental dynamic parameters. At the same time, the material failure aging threshold is set to generate lifetime prediction input parameters. Convert the ambient service temperature to an absolute temperature value, substitute it into the Arrhenius formula to calculate the reaction rate constant k at that temperature without acceleration factor correction, and generate the ambient temperature reaction rate constant. The service life prediction formula after correction by the environmental acceleration factor is adopted. The failure aging degree, the room temperature reaction rate constant and the environmental acceleration factor are substituted into the formula to calculate the service life under room temperature conditions and generate the preliminary calculated value of the service life. Statistical analysis was performed on multiple lifetime calculation values ​​under various parallel aging environments. The median was taken as the final predicted lifetime, and the relative error was calculated to verify the accuracy of the model. Finally, the remaining lifetime prediction value of conductive silicone rubber was generated.

7. A system for predicting the aging life of conductive silicone rubber based on multi-characterization coupling, characterized in that, The system includes: The sampling module is used to apply various environmental accelerated aging test stresses to conductive silicone rubber samples and take samples at preset time intervals to obtain a series of samples under various aging environments. The extraction module is used to perform dynamic mechanical property testing, crosslinking density testing, and surface element content testing on the series of samples, extract multi-dimensional characterization data, and generate a multi-dimensional characterization dataset. The processing module is used to normalize the key indicators in the multi-dimensional characterization data, calculate the uniform aging degree between 0 and 1, and generate a normalized aging degree sequence. The fitting module is used to perform parameter fitting based on the normalized aging degree sequence, using a first-order reaction kinetic model combined with the Arrhenius equation, to solve the reaction rate constant and environmental acceleration factor under each aging environment, and generate a multi-environment kinetic parameter set. The generation module is used to extrapolate and calculate the service life prediction formula after environmental acceleration factor correction based on the set of multiple environmental dynamic parameters and the preset material failure aging threshold, and generate the remaining service life prediction value of conductive silicone rubber.

8. The system according to claim 7, characterized in that, The sampling module is specifically used for: Standard dumbbell-shaped samples of conductive silicone rubber coated with silver aluminum powder were prepared and randomly divided into three groups, labeled as the thermo-oxidative aging group, the damp heat aging group, and the acidic salt spray aging group. The thermo-oxidative aging group samples were placed in constant temperature aging chambers at four temperature points: 90℃, 100℃, 110℃, and 120℃. The damp heat aging group samples were placed in constant temperature and humidity chambers at 70℃+90%RH and 90℃+90%RH. The acidic salt spray aging group samples were placed in a salt spray test chamber. All aging test devices were started. According to the preset sampling time interval, take out the corresponding number of parallel samples under each aging test condition, record the specific aging time and environmental conditions for each sampling, and generate a sampling record table with timestamps. Each sample taken out is classified and numbered according to the aging environment type and aging time, and sealed in a dry and sealed bag for storage and testing, thus generating a series of samples under various aging environments.

9. A storage medium, characterized in that, The storage medium stores a computer program, wherein the computer program is configured to execute the method of any one of claims 1-6 when it is run.

10. An electronic device comprising a memory and a processor, characterized in that, The memory stores a computer program, and the processor is configured to run the computer program to perform the method of any one of claims 1-6.