A high-reliability cross-linked polyethylene insulated power cable and its preparation method
By employing gradient crosslinking agent compounding and segmented extrusion crosslinking-degassing integrated process in crosslinked polyethylene insulated power cables, the problems of uneven crosslinking degree distribution and by-product residue in thick-walled insulation layers have been solved, thereby improving the uniformity and reliability of the insulation layer and reducing the risk of partial discharge.
Patent Information
- Application Number
- CN202611324242.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing cross-linked polyethylene insulated power cables suffer from uneven cross-linking degree distribution and incomplete removal of by-products during the production of thick-walled insulation layers. This leads to fluctuations in the electrical performance of the insulation layer and an increased risk of partial discharge, affecting the long-term operational reliability and service life of the cable.
By employing a gradient crosslinking agent compound system and a segmented extrusion crosslinking-degassing integrated process, crosslinking agents with different decomposition temperatures are set radially in the insulation layer to match the heating process at different locations in the thick-walled layer. Furthermore, a three-stage temperature zone and gradient pressure differential control are set within the crosslinking pipeline to simultaneously achieve the directional diffusion removal of byproducts.
It effectively solves the problems of uneven crosslinking degree distribution and by-product residue in thick-walled insulation layers. The radial crosslinking degree deviation of the insulation layer is controlled within 3%, the by-product residue is reduced to less than 5 ppm, micropore defects are eliminated, and the uniformity of insulation performance and long-term operational reliability of the cable are significantly improved.
Smart Images

Figure CN123120397A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of power cable manufacturing technology, specifically to a high-reliability cross-linked polyethylene insulated power cable and its manufacturing method. Background Technology
[0002] Power cables are core cable products in power systems, responsible for the transmission and distribution of electrical energy. They rely on internal metal conductors to carry current and use an outer insulation structure to achieve electrical isolation between conductors and between conductors and the outside environment. They can be laid in various ways, including underground, in conduits, and in cable trays, and are suitable for various application scenarios such as urban power distribution networks, power supply for industrial and mining enterprises, and power output from new energy power plants. Their operational stability directly determines the reliability and security of power supply, making them a key basic equipment supporting the operation of power systems. Cross-linked polyethylene (XLPE) insulated power cables use XLPE as the main insulation material. Through a cross-linking reaction, the linear polyethylene molecular chains are transformed into a three-dimensional network structure, significantly improving the material's heat resistance, mechanical strength, and resistance to environmental stress cracking. The long-term allowable operating temperature can reach 90℃, and the current carrying capacity is significantly higher than that of ordinary polyvinyl chloride (PVC) insulated cables. They are widely used in medium and high voltage power transmission fields of 10kV and above, and have significant engineering application value in improving power grid transmission capacity and extending the service life of lines.
[0003] Currently, the production process of cross-linked polyethylene insulated power cables with thick insulation layers generally adopts a single cross-linking agent formulation combined with conventional constant-temperature cross-linking pipelines. Due to the low thermal conductivity of polyethylene material, there is a significant difference in the heating rate between the inner and outer sides of the thick insulation layer. This easily leads to problems such as insufficient cross-linking reaction in the inner layer and excessive cross-linking in the outer layer, resulting in uneven cross-linking degree distribution. At the same time, small molecule byproducts such as methane and cumyl alcohol generated by the cross-linking reaction are difficult to completely diffuse and remove from the interior of the thick insulation. The separately set offline high-temperature degassing process not only prolongs the production cycle and increases production costs, but also easily leads to the formation of micropore defects due to the local aggregation of byproducts. Ultimately, this results in fluctuations in the electrical performance of the insulation layer and an increased risk of partial discharge, directly restricting the long-term reliability and service life of the cable. Therefore, developing a highly reliable cross-linked polyethylene insulated power cable and its preparation method is of great significance. Summary of the Invention
[0004] The purpose of this invention is to overcome the shortcomings of the prior art and provide a high-reliability cross-linked polyethylene insulated power cable and its preparation method. It can solve the technical problems of uneven cross-linking degree distribution in thick-walled cross-linked polyethylene insulation layer and micropore defects caused by incomplete removal of by-products through synergistic innovation of material formulation and production process, thereby improving the overall operational reliability of the cable.
[0005] To solve the above-mentioned technical problems, the present invention provides the following technical solution: a high-reliability cross-linked polyethylene insulated power cable, which comprises, from the inside out, a conductor, an inner semi-conductive shielding layer, a cross-linked polyethylene insulation layer, an outer semi-conductive shielding layer, a metal shielding layer, an inner lining layer, an armor layer, and an outer sheath. The cross-linked polyethylene insulation layer is radially provided with an inner insulation section and an outer insulation section. The base material of the inner insulation section is compounded with a high decomposition temperature peroxide cross-linking agent and a co-cross-linking agent, and the base material of the outer insulation section is compounded with a low decomposition temperature peroxide cross-linking agent and a co-cross-linking agent. The decomposition temperature of the cross-linking agent used in the inner insulation section is 10-20°C higher than that of the cross-linking agent used in the outer insulation section. By matching the cross-linking agents with different decomposition temperatures with the radial heating gradient of the thick-walled insulation layer, the initiation and completion processes of the cross-linking reaction on the inner and outer sides of the insulation layer tend to be synchronized, effectively reducing the difference in radial cross-linking degree distribution.
[0006] Furthermore, the inner insulation layer comprises, by weight parts, 100 parts of low-density polyethylene base material, 1.5-2.5 parts of di-tert-butyl peroxide dicumyl peroxide, 0.3-0.8 parts of triallyl isocyanurate, and 0.1-0.3 parts of antioxidant. The outer insulation layer comprises, by weight parts, 100 parts of low-density polyethylene base material, 1.2-2.0 parts of dicumyl peroxide, 0.2-0.6 parts of trimethylolpropane triacrylate, and 0.1-0.3 parts of antioxidant. The thickness of the inner insulation layer accounts for 45-55% of the total thickness of the cross-linked polyethylene insulation layer. The two types of insulation layers are co-extruded to form a continuous integral insulation structure with no obvious physical interface or defects between layers, ensuring the uniformity and continuity of the radial electrical properties of the insulation layer.
[0007] Furthermore, the conductor is a stranded copper conductor or a stranded aluminum conductor, and the conductor adopts a regular stranding structure with a stranding pitch ratio of 10-14 times. Both the inner and outer semiconductive shielding layers are made of carbon black-filled semiconductive polyethylene material, and the thicknesses of the inner and outer semiconductive shielding layers are 0.5-1.0 mm, respectively.
[0008] Furthermore, the metal shielding layer adopts a copper strip gap wrapping structure with a copper strip thickness of 0.08-0.12mm and a copper strip wrapping overlap rate of 15-25%. The armor layer adopts a double-layer steel strip gap wrapping structure or a single-layer steel wire armor structure.
[0009] Furthermore, the inner lining is made of polyvinyl chloride and has a thickness of 0.6-1.0 mm, while the outer sheath is made of polyvinyl chloride or polyethylene and has a thickness of 1.5-2.5 mm.
[0010] A method for preparing a high-reliability cross-linked polyethylene insulated power cable, used to prepare the aforementioned high-reliability cross-linked polyethylene insulated power cable, employs a technical route that couples material formulation gradient design with segmented process control to achieve online synchronous execution of the cross-linking reaction and by-product removal. The method includes the following steps: S1. Conductor pretreatment: The metal rod is drawn into a single wire, and then multiple single wires are twisted together to form a conductor. The twisted conductor is then preheated. S2. Preparation of insulating granules: The raw material components of the inner layer insulating base material and the outer layer insulating base material are prepared separately, and after premixing, they are fed into a twin-screw extruder for mixing and granulation to obtain the inner layer insulating granules and the outer layer insulating granules. S3. Three-layer co-extrusion molding: The inner semiconductive shielding material, inner insulating granules, outer insulating granules, and outer semiconductive shielding material are added to a three-layer co-extrusion extruder, and the inner semiconductive shielding layer, cross-linked polyethylene insulating layer, and outer semiconductive shielding layer are simultaneously extruded on the outside of the preheated conductor. S4. Segmented extrusion cross-linking and degassing integrated treatment: The co-extruded cable core is sent into a nitrogen-filled cross-linking pipeline and passes through a gradient heating zone, a constant temperature degassing zone and a gradient cooling zone in sequence to complete cross-linking and removal of by-products. S5. Subsequent forming and processing: The metal shielding layer, inner lining layer, armor layer and outer sheath are prepared sequentially on the outside of the cable core to obtain the finished cable.
[0011] Further, in step S2, each component is put into a high-speed mixer for premixing. The premixing time is 5-8 minutes, the premixing temperature is controlled at 60-70℃, the spindle speed of the high-speed mixer is set to 600-800 r / min, the temperature of each section of the twin-screw extruder is set to 90-100℃, 105-115℃, 115-120℃, and 110-115℃ along the material travel direction, and the speed of the twin screw is set to 180-220 r / min. After the material is melted and mixed by the twin-screw extruder, it is extruded through the die head, enters the ambient temperature circulating water tank for cooling and shaping, and is then cut into cylindrical pellets with a length of 3-5 mm by a pelletizer.
[0012] Furthermore, in step S3, the three-layer co-extrusion extruder adopts a layered feeding die head with four independent flow channels inside. The inner semi-conductive shielding material, inner insulating granules, outer insulating granules, and outer semi-conductive shielding material are respectively fed into the corresponding flow channels of the die head. The outlets of each flow channel converge at the die opening of the die head. The temperatures of each section of the extruder body along the material travel direction are set sequentially to 110-115℃, 115-120℃, and 120-125℃. The die head temperature is controlled at 120-125℃. During the extrusion process, the die head pressure is maintained at 12-18MPa, and the extrusion linear speed is controlled at 8-12m / min.
[0013] Furthermore, in step S4, the temperature in the gradient heating zone is linearly increased from 140℃ to 190℃ at a rate of 6-7℃ / min, and the nitrogen pressure in the zone is maintained at 1.3-1.4MPa. The temperature in the constant-temperature degassing zone is stabilized at 185-190℃, and the nitrogen pressure in the zone is gradually reduced from 1.3MPa to 0.4MPa at a rate of 0.1MPa / min. The temperature in the gradient cooling zone is linearly reduced from 180℃ to 60℃ at a rate of 3-4℃ / min. The nitrogen in the nitrogen-filled crosslinking pipe is purified by circulating filtration with a filtration accuracy of not less than 0.1μm. Multiple sets of gas guide plates are installed in the constant-temperature degassing zone to guide the nitrogen to flow radially along the cable core.
[0014] Furthermore, in step S1, the monofilament stranding adopts a regular stranding method with a stranding pitch ratio of 10-14 times. The conductor preheating is carried out using an induction-type online preheating device, with the preheating temperature controlled at 80-90℃ and the preheating time at 10-15 minutes. The preheating temperature is adjusted in real time by an infrared thermometer. In step S5, the metal shielding layer is prepared by a gap-wrapping method using copper strip with a thickness of 0.08-0.12mm, with the wrapping tension controlled at 8-12N. The inner liner and outer sheath are prepared by extrusion using a single-screw extruder, with the inner liner extrusion temperature set at 150-170℃ and the outer sheath extrusion temperature set at 160-180℃. The armor layer is prepared by a double-layer steel strip gap-wrapping method or a single-layer steel wire winding method, with the wrapping pitch ratio controlled at 8-12 times.
[0015] Compared with existing technologies, this high-reliability cross-linked polyethylene insulated power cable and its preparation method have the following advantages: This invention employs a coupled scheme that combines a gradient crosslinking agent compound system with a segmented extrusion crosslinking-degassing integrated process. Crosslinking agents with different decomposition temperatures are radially positioned within the insulation layer to match the heating process at different locations in the thick-walled layer. Simultaneously, a three-stage temperature zone and gradient pressure differential control are implemented within the crosslinking pipeline. This allows for the directional diffusion and removal of byproducts during the crosslinking reaction, eliminating the need for a separate offline degassing process. This effectively solves the problems of uneven crosslinking degree distribution and byproduct residue in thick-walled insulation layers, controlling the radial crosslinking degree deviation of the insulation layer to within 3% and reducing byproduct residue to below 5 ppm. It also eliminates the risk of micropore defects, reduces the risk of partial discharge in the insulation layer, and significantly improves the uniformity of cable insulation performance and long-term operational reliability.
[0016] Other advantages, objectives and features of the invention will be set forth in part in the description which follows, and in part will be apparent to those skilled in the art from the following examination or study, or may be learned from the practice of the invention. Attached Figure Description
[0017] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are merely some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without any creative effort.
[0018] Figure 1 A flowchart illustrating a method for preparing a high-reliability cross-linked polyethylene insulated power cable; Figure 2 This is a flowchart illustrating the steps involved in preparing a high-reliability cross-linked polyethylene insulated power cable. Detailed Implementation
[0019] To further illustrate the technical means and effects of the present invention in achieving its intended purpose, the following detailed description of the specific implementation methods, structures, features, and effects of the present invention, in conjunction with the accompanying drawings and preferred embodiments, is provided below.
[0020] This invention provides a high-reliability cross-linked polyethylene (CLL) insulated power cable and its preparation method. The cable product, from the inside out, consists of a conductor, an inner semi-conductive shielding layer, a CLL insulation layer, an outer semi-conductive shielding layer, a metal shielding layer, an inner liner, an armor layer, and an outer sheath. The CLL insulation layer is radially divided into an inner insulation section and an outer insulation section. The inner insulation section uses a high-decomposition-temperature peroxide cross-linking agent combined with a co-crosslinking agent, while the outer insulation section uses a low-decomposition-temperature peroxide cross-linking agent combined with a co-crosslinking agent. The decomposition temperature of the inner layer cross-linking agent is 10-20°C higher than that of the outer layer cross-linking agent. The inner insulation layer, by weight, consists of 100 parts low-density polyethylene (LDPE) base material, 1.5-2.5 parts di-tert-butyl peroxide (DPBS), 0.3-0.8 parts triallyl isocyanurate, and 0.1-0.3 parts antioxidant. The outer insulation layer, by weight, consists of 100 parts LPE base material, 1.2-2.0 parts DPBS, 0.2-0.6 parts trimethylolpropane triacrylate, and 0.1-0.3 parts antioxidant. The thickness of the inner insulation layer accounts for 45-55% of the total thickness of the cross-linked polyethylene insulation layer. The conductor is a stranded copper or aluminum conductor, using regular stranding with a stranding pitch ratio of 10-14. The inner and outer semiconductive shielding layers are made of carbon black-filled semiconductive polyethylene material, both with a thickness of 0.5-1.0 mm. The metallic shielding layer has a copper strip gap-wrapped structure, with a copper strip thickness of 0.08-0.12 mm and a wrapping overlap of 15-25%. The armor layer uses a double-layer steel strip gap wrapping structure or a single-layer steel wire armor structure. The inner lining is made of polyvinyl chloride (PVC) material with a thickness of 0.6-1.0 mm. The outer sheath is made of PVC or polyethylene material with a thickness of 1.5-2.5 mm.
[0021] This invention also discloses a method for manufacturing the corresponding cable, which mainly includes the following steps: S1. Conductor pretreatment: Metal rods are drawn to obtain monofilaments. Multiple monofilaments are regularly twisted together to form a conductor. The conductor is preheated using an induction-type online preheating device. The preheating temperature is 80-90℃, the preheating time is 10-15 minutes, and the twisting pitch ratio is controlled at 10-14 times.
[0022] S2. Preparation of insulating granules: Premix the inner and outer insulating raw materials separately for 5-8 minutes at a temperature of 60-70°C and a spindle speed of 600-800 r / min in a high-speed mixer. Feed the material into a twin-screw extruder for mixing and granulation at a screw speed of 180-220 r / min. Cool and granulate the material to obtain 3-5 mm cylindrical insulating granules.
[0023] S3, three-layer co-extrusion molding, using a layered feed head with four independent flow channels to complete co-extrusion, extruder body temperature 110-125℃, die head temperature 120-125℃, die head pressure 12-18MPa, extrusion line speed 8-12m / min, shielding layer and gradient structure insulation layer are extruded simultaneously on the outside of the conductor.
[0024] S4. Segmented extrusion cross-linking and degassing integrated treatment: The cable core is fed into a nitrogen-filled cross-linking pipeline and passes through a gradient heating zone, a constant temperature degassing zone, and a gradient cooling zone in sequence. The temperature, nitrogen pressure, and heating / cooling rate are strictly controlled in each zone. The nitrogen filtration accuracy is not less than 0.1μm. With the help of a guide plate, the nitrogen flows radially along the cable core, and the cross-linking reaction and by-product removal are completed online simultaneously.
[0025] S5. Subsequent forming and processing: prepare the metal shielding layer, inner lining layer, armor layer, and outer sheath in sequence. The copper tape wrapping tension is 8-12N, the inner lining extrusion temperature is 150-170℃, the outer sheath extrusion temperature is 160-180℃, and the armor wrapping pitch ratio is 8-12 times, finally obtaining the finished cable.
[0026] This solution couples the gradient crosslinking agent material formulation with the segmented crosslinking and degassing process, eliminating the need for an offline degassing step. It improves industry issues such as uneven crosslinking degree and by-product residue in thick-walled insulation layers, thereby enhancing the uniformity of cable insulation and long-term operational reliability. Example 1
[0027] This embodiment provides a high-reliability cross-linked polyethylene insulated power cable with a rated voltage of 10kV. It adopts a double-layer gradient cross-linking agent compound insulation structure and a segmented extrusion cross-linking and degassing integrated process. The inner insulation section uses di-tert-butyl peroxide as the main cross-linking agent, and the outer insulation section uses di-diisopropyl peroxide as the main cross-linking agent. The cross-linking reaction and by-product removal are completed simultaneously through the coordinated control of temperature zone and pressure difference. It is suitable for buried laying scenarios in urban medium-voltage power distribution networks.
[0028] The high-reliability cross-linked polyethylene insulated power cable of this embodiment comprises, from the inside out, a conductor, an inner semi-conductive shielding layer, a cross-linked polyethylene insulation layer, an outer semi-conductive shielding layer, a metallic shielding layer, an inner liner, an armor layer, and an outer sheath. The conductor is a type II stranded copper conductor, consisting of seven 2.5mm diameter copper monofilaments regularly stranded together with a stranding ratio of 12. The nominal cross-section of the conductor is 35mm². The inner semi-conductive shielding layer is made of carbon black-filled semi-conductive polyethylene material with a thickness of 0.8mm.
[0029] The total thickness of the cross-linked polyethylene insulation layer is 4.5 mm, of which the inner insulation section is 2.2 mm thick, accounting for 48.9% of the total thickness. The inner insulation section, by weight, comprises 100 parts of low-density polyethylene base material, 2.0 parts of di-tert-butyl peroxide, 0.5 parts of triallyl isocyanurate, and 0.2 parts of antioxidant 1010. The outer insulation section is 2.3 mm thick and, by weight, comprises 100 parts of low-density polyethylene base material, 1.6 parts of di-tert-butyl peroxide, 0.4 parts of trimethylolpropane triacrylate, and 0.2 parts of antioxidant 1010. The decomposition temperature of the inner cross-linking agent is 15°C higher than that of the outer cross-linking agent. The outer semi-conductive shielding layer is made of carbon black-filled semi-conductive polyethylene material with a thickness of 0.8 mm.
[0030] The metal shielding layer is made of 0.1mm thick soft copper strip with gaps, and the overlap rate is 20%. The inner lining layer is made of polyvinyl chloride with a thickness of 0.8mm. The armor layer adopts a double-layer steel strip gap wrapping structure with a steel strip thickness of 0.5mm. The outer sheath is made of high-density polyethylene with a thickness of 2.0mm.
[0031] See Figure 1 and Figure 2 The preparation method of the high-reliability cross-linked polyethylene insulated power cable described in this embodiment is as follows: S1. Conductor pretreatment: A 3.0mm diameter copper rod is drawn into a 2.5mm diameter copper single wire. Seven copper single wires are selected and twisted together in a standard manner to form a conductor. The twisting pitch ratio is controlled at 12 times. The twisted conductor is sent to an induction-type online preheating device for preheating. The preheating temperature is controlled at 85℃ and the preheating time is 12 minutes. The preheating temperature is adjusted in real time by an infrared thermometer.
[0032] S2. Preparation of insulating granules: Weigh each raw material component according to the formula of the inner insulation section and the outer insulation section respectively, and put each component into a high-speed mixer for premixing. The premixing time is 6 minutes, the premixing temperature is controlled at 65℃, and the spindle speed of the high-speed mixer is set to 700 r / min. The premixed materials are fed into a twin-screw extruder for melt mixing and granulation. The temperature of each section of the twin-screw extruder is set to 95℃, 110℃, 118℃, and 112℃ along the material travel direction, and the twin-screw speed is set to 200 r / min. After the material is extruded through the die, it enters a room temperature circulating water bath for cooling and shaping, and then is cut into cylindrical granules with a length of 4 mm by a pelletizer to obtain inner insulation granules and outer insulation granules respectively.
[0033] S3. Three-layer co-extrusion molding: The inner semiconductive shielding material, inner insulating granules, outer insulating granules, and outer semiconductive shielding material are respectively added to the corresponding hoppers of the three-layer co-extrusion extruder. The three-layer co-extrusion extruder adopts a layered feeding die head, and the die head is equipped with independent four-layer flow channels. Each material is fed into the corresponding flow channel and converges at the die opening. The temperatures of each section of the extruder body are set to 112℃, 118℃, and 122℃ along the material travel direction, respectively. The die head temperature is controlled at 122℃. During the extrusion process, the die head pressure is maintained at 15MPa, and the extrusion linear speed is controlled at 10m / min. The inner semiconductive shielding layer, cross-linked polyethylene insulation layer, and outer semiconductive shielding layer are simultaneously extruded on the outside of the preheated conductor.
[0034] S4. Segmented Extrusion Crosslinking and Degassing Integrated Treatment: The co-extruded cable core is continuously fed into a nitrogen-filled crosslinking pipeline. The cable core sequentially passes through a gradient heating zone, a constant-temperature degassing zone, and a gradient cooling zone. In the gradient heating zone, the temperature linearly increases from 140℃ to 190℃ at a rate of 6.5℃ / min, while the nitrogen pressure is maintained at 1.35MPa. In the constant-temperature degassing zone, the temperature is stabilized at 188℃, and the nitrogen pressure gradually decreases from 1.35MPa to 0.4MPa at a rate of 0.1MPa / min. In the gradient cooling zone, the temperature linearly decreases from 180℃ to 60℃ at a rate of 3.5℃ / min. The nitrogen in the nitrogen-filled crosslinking pipeline is purified by circulating filtration with a filtration accuracy of 0.1μm. Multiple sets of gas guide plates are installed in the constant-temperature degassing zone to guide the nitrogen to flow radially along the cable core, completing the crosslinking reaction and by-product removal online.
[0035] S5. Subsequent Forming and Processing: The cross-linked and degassed cable cores are sequentially processed for subsequent structural fabrication. A metal shielding layer is prepared by intermittent wrapping with 0.1mm thick soft copper strip, with the wrapping tension controlled at 10N and the wrapping overlap rate at 20%. A polyvinyl chloride inner liner is prepared by extrusion using a single-screw extruder, with the extrusion temperature set at 160℃. An armor layer is prepared by intermittent wrapping with double-layer steel strip, with the wrapping pitch ratio controlled at 10 times. A polyethylene outer sheath is prepared by extrusion using a single-screw extruder, with the extrusion temperature set at 170℃. After passing appearance and performance inspections, the finished cable is obtained.
[0036] In summary, the cable product prepared in this embodiment, after testing, showed a maximum deviation of 2.1% in the radial crosslinking degree of the insulation layer, a residual amount of 3.2 ppm in crosslinking byproducts, a power frequency breakdown field strength of 38.5 kV / mm, and a partial discharge initiation voltage of 18.2 kV. All performance indicators are superior to those of cables of the same specification prepared by conventional processes. Furthermore, no separate offline degassing process is required, and the production cycle is shortened by 32% compared to traditional processes, which can effectively improve the operational reliability and production economy of medium-voltage power distribution lines. Example 2
[0037] This embodiment provides a high-reliability cross-linked polyethylene insulated power cable with a rated voltage of 10kV. By adjusting the addition ratio of gradient cross-linking agent and cross-linking process parameters, and using a lower cross-linking agent dosage and a mild cross-linking temperature range, the raw material cost is further controlled while meeting performance requirements. It is suitable for laying branch lines of distribution networks with moderate load levels.
[0038] The high-reliability cross-linked polyethylene insulated power cable of this embodiment comprises, from the inside out, a conductor, an inner semi-conductive shielding layer, a cross-linked polyethylene insulation layer, an outer semi-conductive shielding layer, a metallic shielding layer, an inner lining layer, an armor layer, and an outer sheath. The conductor is a type II stranded aluminum conductor, consisting of seven 3.0mm diameter aluminum monofilaments regularly stranded together, with a stranding ratio of 11:1, and a nominal conductor cross-section of 50mm². The inner semi-conductive shielding layer is made of carbon black-filled semi-conductive polyethylene material with a thickness of 0.7mm.
[0039] The total thickness of the cross-linked polyethylene insulation layer is 4.5 mm, of which the inner insulation section is 2.1 mm thick, accounting for 46.7% of the total thickness. The inner insulation section, by weight, comprises 100 parts of low-density polyethylene base material, 1.8 parts of di-tert-butyl peroxide, 0.4 parts of triallyl isocyanurate, and 0.15 parts of antioxidant 1010. The outer insulation section is 2.4 mm thick and, by weight, comprises 100 parts of low-density polyethylene base material, 1.4 parts of di-tert-butyl peroxide, 0.3 parts of trimethylolpropane triacrylate, and 0.15 parts of antioxidant 1010. The decomposition temperature of the inner cross-linking agent is 12°C higher than that of the outer cross-linking agent. The outer semi-conductive shielding layer is made of carbon black-filled semi-conductive polyethylene material with a thickness of 0.7 mm.
[0040] The metallic shielding layer is prepared by wrapping 0.09mm thick soft copper strips with gaps, resulting in an 18% overlap. The inner lining layer is made of polyvinyl chloride (PVC) with a thickness of 0.7mm. The armor layer uses a single-layer steel wire armor structure with a wire diameter of 2.0mm. The outer sheath is made of PVC with a thickness of 1.8mm.
[0041] See Figure 1 and Figure 2 The preparation method of the high-reliability cross-linked polyethylene insulated power cable described in this embodiment is as follows: S1. Conductor pretreatment: Aluminum rods with a diameter of 3.5mm are drawn into aluminum single wires with a diameter of 3.0mm. Seven aluminum single wires are selected and prepared into conductors by regular stranding. The stranding pitch ratio is controlled at 11 times. The stranded conductors are sent to an induction-type online preheating device for preheating. The preheating temperature is controlled at 82℃ and the preheating time is 11 minutes. The preheating temperature is adjusted in real time by an infrared thermometer.
[0042] S2. Preparation of insulating granules: Weigh each raw material component according to the formula of the inner insulation section and the outer insulation section respectively, and put each component into a high-speed mixer for premixing. The premixing time is 5.5 min, the premixing temperature is controlled at 62℃, and the spindle speed of the high-speed mixer is set to 650 r / min. The premixed materials are fed into a twin-screw extruder for melt mixing and granulation. The temperatures of each section of the twin-screw extruder along the material travel direction are set to 92℃, 108℃, 116℃, and 111℃ respectively, and the twin-screw speed is set to 190 r / min. After the material is extruded through the die, it enters a room temperature circulating water bath for cooling and shaping, and then is cut into cylindrical granules with a length of 3.5 mm by a pelletizer to obtain inner insulation granules and outer insulation granules respectively.
[0043] S3. Three-layer co-extrusion molding: The inner semiconductive shielding material, inner insulating granules, outer insulating granules, and outer semiconductive shielding material are respectively added to the corresponding hoppers of the three-layer co-extrusion extruder. The three-layer co-extrusion extruder adopts a layered feeding die head, and the die head is equipped with independent four-layer flow channels. Each material is fed into the corresponding flow channel and converges at the die opening. The temperatures of each section of the extruder body are set to 111℃, 116℃, and 121℃ along the material travel direction, respectively. The die head temperature is controlled at 121℃. During the extrusion process, the die head pressure is maintained at 14MPa, and the extrusion linear speed is controlled at 9m / min. The inner semiconductive shielding layer, cross-linked polyethylene insulation layer, and outer semiconductive shielding layer are simultaneously extruded on the outside of the preheated conductor.
[0044] S4. Segmented Extrusion Crosslinking and Degassing Integrated Treatment: The co-extruded cable core is continuously fed into a nitrogen-filled crosslinking pipeline. The cable core sequentially passes through a gradient heating zone, a constant-temperature degassing zone, and a gradient cooling zone. In the gradient heating zone, the temperature linearly increases from 140℃ to 190℃ at a rate of 6.2℃ / min, while the nitrogen pressure is maintained at 1.32MPa. In the constant-temperature degassing zone, the temperature is stabilized at 185℃, and the nitrogen pressure gradually decreases from 1.32MPa to 0.4MPa at a rate of 0.1MPa / min. In the gradient cooling zone, the temperature linearly decreases from 180℃ to 60℃ at a rate of 3.2℃ / min. The nitrogen in the nitrogen-filled crosslinking pipeline is purified by circulating filtration with a filtration accuracy of 0.1μm. Multiple gas guide plates are installed in the constant-temperature degassing zone to guide the nitrogen to flow radially along the cable core, completing the crosslinking reaction and by-product removal online.
[0045] S5. Subsequent Forming and Processing: The cross-linked and degassed cable cores are sequentially processed for subsequent structural fabrication. A metal shielding layer is prepared by intermittently wrapping 0.09mm thick soft copper strips, with the wrapping tension controlled at 9N and the wrapping overlap rate at 18%. A polyvinyl chloride inner liner is prepared by extrusion using a single-screw extruder, with the extrusion temperature set at 155℃. A single-layer steel wire is used to wind the armor layer, with the wrapping pitch ratio controlled at 9 times. A polyvinyl chloride outer sheath is prepared by extrusion using a single-screw extruder, with the extrusion temperature set at 165℃. After passing appearance and performance inspections, the finished cable is obtained.
[0046] In summary, the finished cable prepared in this embodiment, after testing, showed that the maximum deviation of the radial crosslinking degree of the insulation layer was 2.6%, the residual amount of crosslinking byproducts was 4.1 ppm, the power frequency breakdown field strength of the insulation layer was 37.8 kV / mm, and the partial discharge initiation voltage was 17.6 kV. All performance characteristics met the requirements of the medium-voltage cable operation standard. The raw material cost was reduced by about 8% compared with Example 1, demonstrating good cost performance and adaptability to the application needs of different levels of power distribution lines. Example 3
[0047] This embodiment provides a high-reliability cross-linked polyethylene insulated power cable with a rated voltage of 35kV. By increasing the amount of gradient cross-linking agent and optimizing the cross-linking process parameters, and by adopting a higher cross-linking reaction temperature and more precise differential pressure control, the cross-linking uniformity of the thick-walled insulation layer and the by-product removal effect are further improved. It is suitable for high-voltage main power grids and important load power supply scenarios.
[0048] The high-reliability cross-linked polyethylene insulated power cable of this embodiment comprises, from the inside out, a conductor, an inner semi-conductive shielding layer, a cross-linked polyethylene insulation layer, an outer semi-conductive shielding layer, a metallic shielding layer, an inner lining layer, an armor layer, and an outer sheath. The conductor is a type II stranded copper conductor, consisting of 19 copper monofilaments with a diameter of 2.8 mm twisted together, with a twist ratio of 13. The nominal cross-section of the conductor is 120 mm². The inner semi-conductive shielding layer is made of carbon black-filled semi-conductive polyethylene material with a thickness of 0.9 mm.
[0049] The total thickness of the cross-linked polyethylene insulation layer is 8.0 mm, of which the inner insulation section is 3.8 mm thick, accounting for 47.5% of the total thickness. The inner insulation section, by weight, comprises 100 parts of low-density polyethylene base material, 2.2 parts of di-tert-butyl peroxide dicumyl peroxide, 0.6 parts of triallyl isocyanurate, and 0.25 parts of antioxidant 1010. The outer insulation section is 4.2 mm thick and, by weight, comprises 100 parts of low-density polyethylene base material, 1.8 parts of dicumyl peroxide, 0.5 parts of trimethylolpropane triacrylate, and 0.25 parts of antioxidant 1010. The decomposition temperature of the inner cross-linking agent is 18°C higher than that of the outer cross-linking agent. The outer semi-conductive shielding layer is made of carbon black-filled semi-conductive polyethylene material with a thickness of 0.9 mm.
[0050] The metal shielding layer is made of 0.12mm thick soft copper strip with gap wrapping, and the wrapping overlap rate is 22%. The inner liner is made of polyvinyl chloride with a thickness of 0.9mm. The armor layer adopts a double-layer steel strip gap wrapping structure, and the steel strip is 0.5mm thick. The outer sheath is made of low-smoke halogen-free polyolefin material with a thickness of 2.2mm.
[0051] See Figure 1 and Figure 2 The preparation method of the high-reliability cross-linked polyethylene insulated power cable described in this embodiment is as follows: S1. Conductor pretreatment: A 3.2mm diameter copper rod is drawn into a 2.8mm diameter copper single wire. Nineteen copper single wires are selected and twisted together in a standard manner to form a conductor. The twisting pitch ratio is controlled at 13 times. The twisted conductor is sent to an induction-type online preheating device for preheating. The preheating temperature is controlled at 88℃ and the preheating time is 14 minutes. The preheating temperature is adjusted in real time by an infrared thermometer.
[0052] S2. Preparation of insulating granules: Weigh each raw material component according to the formula of the inner insulation section and the outer insulation section respectively, and put each component into a high-speed mixer for premixing. The premixing time is 7 minutes, the premixing temperature is controlled at 68℃, and the spindle speed of the high-speed mixer is set to 750 r / min. The premixed materials are fed into a twin-screw extruder for melt mixing and granulation. The temperature of each section of the twin-screw extruder is set to 98℃, 112℃, 119℃, and 113℃ along the material travel direction, and the twin-screw speed is set to 210 r / min. After the material is extruded through the die, it enters a room temperature circulating water bath for cooling and shaping, and then is cut into cylindrical granules with a length of 4.5 mm by a pelletizer to obtain inner insulation granules and outer insulation granules respectively.
[0053] S3. Three-layer co-extrusion molding: The inner semiconductive shielding material, inner insulating granules, outer insulating granules, and outer semiconductive shielding material are respectively added to the corresponding hoppers of the three-layer co-extrusion extruder. The three-layer co-extrusion extruder adopts a layered feeding die head, and the die head is equipped with independent four-layer flow channels. Each material is fed into the corresponding flow channel and converges at the die opening. The temperatures of each section of the extruder body are set to 113℃, 119℃, and 124℃ along the material travel direction, respectively. The die head temperature is controlled at 124℃. During the extrusion process, the die head pressure is maintained at 17MPa, and the extrusion linear speed is controlled at 11m / min. The inner semiconductive shielding layer, cross-linked polyethylene insulation layer, and outer semiconductive shielding layer are simultaneously extruded on the outside of the preheated conductor.
[0054] S4. Segmented Extrusion Crosslinking and Degassing Integrated Treatment: The co-extruded cable core is continuously fed into a nitrogen-filled crosslinking pipeline. The cable core sequentially passes through a gradient heating zone, a constant-temperature degassing zone, and a gradient cooling zone. In the gradient heating zone, the temperature linearly increases from 140℃ to 190℃ at a rate of 6.8℃ / min, while the nitrogen pressure is maintained at 1.38MPa. In the constant-temperature degassing zone, the temperature is stabilized at 190℃, and the nitrogen pressure gradually decreases from 1.38MPa to 0.4MPa at a rate of 0.1MPa / min. In the gradient cooling zone, the temperature linearly decreases from 180℃ to 60℃ at a rate of 3.8℃ / min. The nitrogen in the nitrogen-filled crosslinking pipeline is purified by circulating filtration with a filtration accuracy of 0.1μm. Multiple sets of gas guide plates are installed in the constant-temperature degassing zone to guide the nitrogen to flow radially along the cable core, completing the crosslinking reaction and by-product removal online.
[0055] S5. Subsequent Forming and Processing: The cross-linked and degassed cable cores are sequentially processed for subsequent structural fabrication. A metal shielding layer is prepared by intermittently wrapping 0.12mm thick soft copper strip with a wrapping tension controlled at 11N and an overlap rate of 22%. A polyvinyl chloride inner liner is prepared by extrusion using a single-screw extruder with an extrusion temperature of 165℃. An armor layer is prepared by intermittently wrapping double-layer steel strip with a wrapping pitch ratio controlled at 11 times. A low-smoke halogen-free polyolefin outer sheath is prepared by extrusion using a single-screw extruder with an extrusion temperature of 175℃. After passing appearance and performance inspections, the finished cable is obtained.
[0056] In summary, the 35kV cable prepared in this embodiment, after testing, showed a maximum deviation of 1.9% in the radial crosslinking degree of the insulation layer, a residual amount of 2.8 ppm of crosslinking byproducts, a power frequency breakdown field strength of 39.2 kV / mm, and a partial discharge initiation voltage of 32.5 kV. The cable significantly improved the crosslinking uniformity of the thick-walled insulation layer, effectively reducing the risk of partial discharge and insulation aging during high-voltage cable operation and meeting the high reliability operation requirements of important power supply scenarios.
[0057] Comparative Example This comparative example uses the formula and preparation process of conventional cross-linked polyethylene insulated cables. The insulation layer uses a single cross-linking agent formula, combined with a traditional constant temperature cross-linking pipeline and offline high temperature degassing process. The remaining cable structural parameters are consistent with those of Example 1, and are used to compare and verify the performance advantages of the technical solution of the present invention.
[0058] The cross-linked polyethylene insulated power cable in this comparative example comprises, from the inside out, a conductor, an inner semi-conductive shielding layer, a cross-linked polyethylene insulation layer, an outer semi-conductive shielding layer, a metallic shielding layer, an inner lining layer, an armor layer, and an outer sheath. The conductor is a Class II stranded copper conductor, consisting of seven 2.5mm diameter copper monofilaments regularly stranded together, with a stranding ratio of 12. The nominal cross-section of the conductor is 35mm². The inner semi-conductive shielding layer is made of carbon black-filled semi-conductive polyethylene material with a thickness of 0.8mm.
[0059] The total thickness of the cross-linked polyethylene insulation layer is 4.5 mm. The insulation base material, by weight, includes 100 parts of low-density polyethylene base material, 2.0 parts of dicumyl peroxide, and 0.2 parts of antioxidant 1010. The outer semi-conductive shielding layer is made of carbon black-filled semi-conductive polyethylene material with a thickness of 0.8 mm.
[0060] The metal shielding layer is made of 0.1mm thick soft copper strip with gaps, and the overlap rate is 20%. The inner lining layer is made of polyvinyl chloride with a thickness of 0.8mm. The armor layer adopts a double-layer steel strip gap wrapping structure with a steel strip thickness of 0.5mm. The outer sheath is made of high-density polyethylene with a thickness of 2.0mm.
[0061] The preparation method of the cross-linked polyethylene insulated power cable described in this comparative example is as follows: S1. Conductor pretreatment: A 3.0mm diameter copper rod is drawn into a 2.5mm diameter copper single wire. Seven copper single wires are selected and twisted together in a standard manner to prepare a conductor. The twisting pitch ratio is controlled at 12 times. The twisted conductor is sent to a preheating device for preheating. The preheating temperature is controlled at 85℃ and the preheating time is 12 minutes.
[0062] S2. Preparation of insulating granules: Weigh each raw material component according to the insulation layer formula, put them into a high-speed mixer for premixing for 6 minutes at a premixing temperature of 65℃; feed the premixed material into a twin-screw extruder for compounding and granulation, with the screw temperature set at 115℃ and the screw speed at 200r / min, and cool and granulate to obtain conventional insulating granules.
[0063] S3. Three-layer co-extrusion molding: The inner semiconducting shielding material, insulating granules, and outer semiconducting shielding material are added to the three-layer co-extrusion extruder. The inner semiconducting shielding layer, insulating layer, and outer semiconducting shielding layer are extruded simultaneously on the outside of the conductor. The extrusion temperature is controlled at 120℃ and the extrusion line speed is 10m / min.
[0064] S4. Crosslinking and degassing treatment: The co-extruded cable core is sent into a constant temperature nitrogen-filled crosslinking pipeline. The crosslinking temperature is kept constant at 180℃ and the nitrogen pressure is 1.2MPa. After the crosslinking is completed, the cable core is sent into the degassing chamber for offline high-temperature degassing. The degassing temperature is 70℃ and the degassing time is 72h.
[0065] S5. Subsequent forming and processing: The metal shielding layer, inner lining layer, armor layer and outer sheath are prepared in sequence. The parameters of each process are consistent with those in Example 1. After passing the inspection, the finished cable for comparison is obtained.
[0066] In summary, the cable products prepared in this comparative example, after testing, showed that the maximum deviation of the radial crosslinking degree of the insulation layer was 7.8%, the residual amount of crosslinking byproducts was 18.6 ppm, the power frequency breakdown field strength of the insulation layer was 32.1 kV / mm, the partial discharge initiation voltage was 12.3 kV, the overall production cycle was 2.8 times longer than that of Example 1, and the crosslinking uniformity and electrical performance of the thick-walled insulation layer were significantly inferior to those of the products in the embodiments of this invention.
[0067]
[0068] As shown in the table above, the core differences between this invention and traditional processes lie in three dimensions: insulation layer structure, crosslinking agent system, and degassing mode. Traditional processes using single-layer homogeneous insulation with a single crosslinking agent and offline static degassing result in poor crosslinking uniformity in thick-walled layers, high by-product residue, and long production cycles. This invention addresses the industry pain points of uneven crosslinking and by-product residue simultaneously by using double-layer gradient insulation and a high-low temperature composite crosslinking agent to match the radial heating gradient, combined with an integrated online differential pressure degassing process. Three embodiments are adapted to different application scenarios: Embodiment 3 is optimized for 35kV high-voltage thick-walled scenarios, offering the best overall performance; Embodiment 2 has better cost control and is suitable for medium and low-voltage distribution branch lines; Embodiment 1 balances performance and cost, suitable for mainstream 10kV urban distribution networks. The overall solution can shorten the production cycle, reduce manufacturing costs, and significantly improve cable operational reliability, demonstrating clear technological advancement and engineering promotion value.
[0069] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A high-reliability cross-linked polyethylene insulated power cable, characterized in that, The cable comprises, from the inside out, a conductor, an inner semiconductive shielding layer, a cross-linked polyethylene insulation layer, an outer semiconductive shielding layer, a metal shielding layer, an inner liner, an armor layer, and an outer sheath. The cross-linked polyethylene insulation layer has an inner insulation section and an outer insulation section arranged radially. The base material of the inner insulation section is compounded with a high decomposition temperature peroxide cross-linking agent and a co-cross-linking agent, while the base material of the outer insulation section is compounded with a low decomposition temperature peroxide cross-linking agent and a co-cross-linking agent. The decomposition temperature of the cross-linking agent used in the inner insulation section is 10-20°C higher than that of the cross-linking agent used in the outer insulation section.
2. The high-reliability cross-linked polyethylene insulated power cable according to claim 1, characterized in that, The inner insulation layer comprises, by weight parts, 100 parts of low-density polyethylene base material, 1.5-2.5 parts of di-tert-butyl peroxide, 0.3-0.8 parts of triallyl isocyanurate, and 0.1-0.3 parts of antioxidant. The outer insulation layer comprises, by weight parts, 100 parts of low-density polyethylene base material, 1.2-2.0 parts of di-tert-butyl peroxide, 0.2-0.6 parts of trimethylolpropane triacrylate, and 0.1-0.3 parts of antioxidant. The thickness of the inner insulation layer accounts for 45-55% of the total thickness of the cross-linked polyethylene insulation layer.
3. The high-reliability cross-linked polyethylene insulated power cable according to claim 1, characterized in that, The conductor is a stranded copper conductor or a stranded aluminum conductor, and the conductor adopts a regular stranding structure with a stranding diameter ratio of 10-14. The inner and outer semiconductive shielding layers are both made of carbon black-filled semiconductive polyethylene material, and the thicknesses of the inner and outer semiconductive shielding layers are 0.5-1.0 mm, respectively.
4. The high-reliability cross-linked polyethylene insulated power cable according to claim 1, characterized in that, The metal shielding layer adopts a copper strip gap wrapping structure with a copper strip thickness of 0.08-0.12mm and a copper strip wrapping overlap rate of 15-25%. The armor layer adopts a double-layer steel strip gap wrapping structure or a single-layer steel wire armor structure.
5. A high-reliability cross-linked polyethylene insulated power cable according to claim 1, characterized in that, The inner lining is made of polyvinyl chloride and has a thickness of 0.6-1.0 mm. The outer sheath is made of polyvinyl chloride or polyethylene and has a thickness of 1.5-2.5 mm.
6. A method for preparing a high-reliability cross-linked polyethylene insulated power cable, used to prepare the high-reliability cross-linked polyethylene insulated power cable according to any one of claims 1-5, characterized in that, The method includes the following steps: S1. Conductor pretreatment: The metal rod is drawn into a single wire, and then multiple single wires are twisted together to form a conductor. The twisted conductor is then preheated. S2. Preparation of insulating granules: The raw material components of the inner layer insulating base material and the outer layer insulating base material are prepared separately, and after premixing, they are fed into a twin-screw extruder for mixing and granulation to obtain the inner layer insulating granules and the outer layer insulating granules. S3. Three-layer co-extrusion molding: The inner semiconductive shielding material, inner insulating granules, outer insulating granules, and outer semiconductive shielding material are added to a three-layer co-extrusion extruder, and the inner semiconductive shielding layer, cross-linked polyethylene insulating layer, and outer semiconductive shielding layer are simultaneously extruded on the outside of the preheated conductor. S4. Segmented extrusion cross-linking and degassing integrated treatment: The co-extruded cable core is sent into a nitrogen-filled cross-linking pipeline and passes through a gradient heating zone, a constant temperature degassing zone and a gradient cooling zone in sequence to complete cross-linking and removal of by-products. S5. Subsequent forming and processing: The metal shielding layer, inner lining layer, armor layer and outer sheath are prepared sequentially on the outside of the cable core to obtain the finished cable.
7. The method for preparing a high-reliability cross-linked polyethylene insulated power cable according to claim 6, characterized in that, In step S2, each component is premixed in a high-speed mixer for 5-8 minutes. The premixing temperature is controlled at 60-70°C. The spindle speed of the high-speed mixer is set to 600-800 r / min. The temperatures of each section of the twin-screw extruder along the material travel direction are set to 90-100°C, 105-115°C, 115-120°C, and 110-115°C, respectively. The speed of the twin screw is set to 180-220 r / min. After the material is melted and mixed in the twin-screw extruder, it is extruded through the die head, cooled and shaped in a room-temperature circulating water tank, and then cut into cylindrical pellets with a length of 3-5 mm by a pelletizer.
8. The method for preparing a high-reliability cross-linked polyethylene insulated power cable according to claim 6, characterized in that, In step S3, the three-layer co-extrusion extruder adopts a layered feeding die head. The die head is equipped with four independent flow channels. The inner semi-conductive shielding material, the inner insulating granules, the outer insulating granules, and the outer semi-conductive shielding material are respectively fed into the corresponding flow channels of the die head. The outlets of each flow channel converge at the die head. The temperatures of each section of the extruder body along the material travel direction are set to 110-115℃, 115-120℃, and 120-125℃ respectively. The die head temperature is controlled at 120-125℃. During the extrusion process, the die head pressure is maintained at 12-18MPa, and the extrusion linear speed is controlled at 8-12m / min.
9. The method for preparing a high-reliability cross-linked polyethylene insulated power cable according to claim 6, characterized in that, In step S4, the temperature in the gradient heating zone increases linearly from 140℃ to 190℃ at a rate of 6-7℃ / min, and the nitrogen pressure in the zone is maintained at 1.3-1.4MPa. The temperature in the constant-temperature degassing zone is stabilized at 185-190℃, and the nitrogen pressure in the zone gradually decreases from 1.3MPa to 0.4MPa at a rate of 0.1MPa / min. The temperature in the gradient cooling zone decreases linearly from 180℃ to 60℃ at a rate of 3-4℃ / min. The nitrogen in the nitrogen-filled crosslinking pipe is purified by circulating filtration with a filtration accuracy of not less than 0.1μm. Multiple sets of gas guide plates are installed in the constant-temperature degassing zone to guide the nitrogen to flow radially along the cable core.
10. The method for preparing a high-reliability cross-linked polyethylene insulated power cable according to claim 6, characterized in that, In step S1, the monofilament stranding adopts a regular stranding method with a stranding pitch ratio of 10-14. The conductor preheating is carried out using an induction-type online preheating device, with the preheating temperature controlled at 80-90℃ and the preheating time at 10-15 minutes. The preheating temperature is adjusted in real time by an infrared thermometer. In step S5, the metal shielding layer is prepared by a gap-wrapping method using copper strip with a thickness of 0.08-0.12mm, with the wrapping tension controlled at 8-12N. The inner liner and outer sheath are prepared by extrusion using a single-screw extruder, with the extrusion temperature of the inner liner set at 150-170℃ and the extrusion temperature of the outer sheath set at 160-180℃. The armor layer is prepared by a double-layer steel strip gap-wrapping method or a single-layer steel wire winding method, with the wrapping pitch ratio controlled at 8-12 times.