A ±800kV DC submarine cable

By optimizing the structural design of the ±800kV DC submarine cable, the problems of increased insulation thickness and insufficient mechanical protection caused by the increase in voltage level in the existing technology have been solved, realizing a high-reliability and long-life ultra-high voltage submarine cable that is suitable for deep-sea environments.

CN123120401APending Publication Date: 2026-11-17NINGBO ORIENT WIRES & CABLES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611619995.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing ±500kV DC submarine cable cannot meet the requirements of ±800kV ultra-high voltage power transmission, and there is no mature structure to refer to for the ±800kV level. There are problems such as a significant increase in insulation layer thickness, electric field distribution distortion, insufficient mechanical protection, and lack of design standards.

Method used

A ±800kV DC submarine cable was designed, comprising a multi-layer structure including conductors, insulation layers, and armor layers. By optimizing the thickness-to-diameter ratio, cross-sectional area ratio, and material combination, a balance of multiple physical fields of electricity, heat, and force is achieved. The cable employs double-layer steel wire reverse twisting and semi-conductive Tedoron tape wrapping to eliminate interlayer potential differences, balance torsional stress, and enhance mechanical reliability.

Benefits of technology

It has achieved a highly reliable and long-life ±800kV DC submarine cable, which has improved power transmission capacity, reduced engineering costs, ensured electrical safety and mechanical reliability, and is suitable for deep-sea laying environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120401A_ABST
    Figure CN123120401A_ABST
Patent Text Reader

Abstract

This application discloses a ±800kV DC submarine cable, which, from the inside out, comprises a conductor, a conductor-side water-blocking layer, a conductor shielding layer, an insulation layer, an insulation shielding layer, an insulation-side water-blocking layer, a metallic shielding layer, an inner sheath, an inner lining layer, an optical cable filling layer, an armor layer, and an outer sheath. The ratio of the insulation layer thickness to the conductor outer diameter is 0.45~0.55, and the sum of the cross-sectional areas of the conductor and the insulation layer accounts for 55%~65% of the total circular cross-sectional area of ​​the submarine cable. The armor layer includes, from the inside out, a first semi-conductive terylene tape wrapping layer, a first steel wire layer, a second semi-conductive terylene tape wrapping layer, and a second steel wire layer. The two steel wires are twisted in opposite directions, and their surfaces are coated with asphalt layers. Through the synergistic cooperation of each layer structure, this application can meet the electrical insulation, mechanical protection, and deep-sea laying requirements under the ±800kV transmission level.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of submarine cable technology, and in particular to a ±800kV DC submarine cable. Background Technology

[0002] With the continuous growth in demand for long-distance, high-capacity power transmission, especially the large-scale development of offshore wind power, cross-sea interconnection projects, and the rapid increase in power supply demand for islands, high-voltage direct current (HVDC) transmission technology has gradually become the mainstream technology for long-distance cross-sea power transmission due to its advantages such as large transmission capacity, low line loss, and narrow line corridor.

[0003] Currently, ±500kV DC submarine cables have been used in numerous projects. However, given the future trend of single-circuit line transmission power reaching several gigawatts, increasing the voltage level of DC submarine cables is an effective way to improve transmission efficiency and reduce unit capacity construction costs. Therefore, developing higher voltage levels (such as ±800kV) DC submarine cables has become an inevitable trend in the industry.

[0004] Compared to ±500kV submarine cables, ±800kV DC submarine cables face challenges of orders of magnitude increase in electrical performance, mechanical characteristics, and long-term operational reliability, mainly in the following aspects: In terms of electrical insulation, existing DC submarine cables mostly use cross-linked polyethylene (XLPE) as the main insulation material. When the voltage level is increased to ±800kV, the insulation layer needs to withstand extremely high DC electric field strength, resulting in significant increases in insulation thickness, distortion of electric field distribution, and problems with effective control of partial discharge. The space charge accumulation effect in XLPE insulation will further exacerbate the electric field concentration under high temperature gradients, accelerating the insulation aging process. Furthermore, existing insulation structure design experience and operational data based on the ±500kV level cannot be directly applied to the ±800kV level through simple extrapolation, and its long-term operational safety margin and lifespan assessment lack reliable verification basis.

[0005] In terms of mechanical protection and adaptability to deep-sea environments, ±800kV submarine cables have significantly increased conductor cross-section and insulation thickness, resulting in a much larger self-weight and outer diameter compared to ±500kV submarine cables. During deep-sea laying and operation, these cables must withstand immense water pressure, laying drag tension, seabed rock abrasion, and ocean current impacts, among other complex mechanical stresses. Currently, the industry lacks systematic armored structures and tensile-resistant waterproof layers for ±800kV cables, making it difficult to guarantee their structural integrity and long-term operational safety in harsh underwater environments.

[0006] Furthermore, since the ±800kV DC submarine cable is still in the research and development and engineering verification stage, there are no systematic design standards, test specifications and acceptance criteria for this voltage level at home and abroad. This results in a lack of clear reference basis in terms of structural design, material selection and manufacturing process control, which seriously restricts the product's research and development efficiency and engineering application process.

[0007] To address the aforementioned issues, this application proposes a ±800kV DC submarine cable structure based on multi-physics collaborative design. By accurately calculating the electrical, thermal, and mechanical parameters of each functional unit, including the conductor, insulation shield, insulation layer, sheath, and armor layer, a complete design process is formed. The aim is to achieve a highly reliable, long-life ±800kV DC submarine cable suitable for deep-sea laying, providing a technical foundation for the engineering application of ultra-high voltage DC submarine cables. Summary of the Invention

[0008] This application addresses the current situation where existing ±500kV DC submarine cables cannot meet the requirements of ±800kV ultra-high voltage power transmission, and there is no mature structure available for reference at the ±800kV level. It provides a ±800kV DC submarine cable, which, from the inside out, comprises a conductor, a conductor-side water-blocking layer, a conductor shielding layer, an insulation layer, an insulation shielding layer, an insulation-side water-blocking layer, a metallic shielding layer, an inner sheath, an inner lining layer, an optical cable filling layer, an armor layer, and an outer sheath. The insulation layer thickness is 0.45~0.55 mm from the conductor's outer diameter, and the sum of the conductor's and insulation layer's cross-sectional areas is... The armor layer, comprising 55% to 65% of the total circular cross-sectional area, employs a double-layer reverse-twisted steel wire structure. The steel wires are coated with asphalt, and a semi-conductive tertrol tape is wrapped between the two layers, forming a multi-level composite armor layer. Through systematic optimization of the thickness-to-diameter ratio and cross-sectional area proportion, a balance of electro-thermal-mechanical multi-fields is achieved. The semi-conductive tertrol tape balances the electric field of the armor layer and eliminates interlayer potential differences. Combined with the reverse-twisted double-layer steel wire balancing torsional stress and the multi-level mechanical gradient synergistic impact resistance, the electrical safety and mechanical reliability of the submarine cable in deep-sea environments are comprehensively ensured. The technical solution provided in this application is as follows: This application provides a ±800kV DC submarine cable, which comprises, from the inside out: a conductor, a conductor-side water-blocking layer, a conductor shielding layer, an insulation layer, an insulation shielding layer, an insulation-side water-blocking layer, a metal shielding layer, an inner sheath, an inner lining layer, an optical cable filling layer, an armor layer, and an outer sheath. Wherein, the ratio of the insulation layer thickness to the conductor outer diameter is 0.45~0.55; Based on the total circular cross-sectional area of ​​the submarine cable, the sum of the cross-sectional areas of the conductor and the insulation layer accounts for 55% to 65% of the total circular cross-sectional area of ​​the submarine cable; The armor layer includes a first semi-conductive terylene tape wrapping layer, a first steel wire layer, a second semi-conductive terylene tape wrapping layer, and a second steel wire layer arranged sequentially from the inside to the outside; the first steel wire layer and the second steel wire layer are twisted in opposite directions, and the steel wire surfaces of the two are respectively coated with an asphalt layer.

[0009] In some preferred embodiments, the diameter of a single steel wire in both the first steel wire layer and the second steel wire layer is 5.5mm to 6.5mm; The thickness of both the first and second semiconductive terylene tape wrapping layers is 0.3mm to 0.5mm, and the overlap rate is not less than 25%. The coating thickness of the asphalt layer is 0.1mm to 0.3mm, and the depth of the asphalt layer penetrating into the surface of the steel wire is 5% to 10% of the diameter of a single steel wire.

[0010] In some preferred embodiments, based on the total circular cross-sectional area of ​​the submarine cable, the cross-sectional area of ​​the armor layer accounts for 15% to 20%, the cross-sectional area of ​​the metal shielding layer accounts for 5% to 10%, and the cross-sectional area of ​​the optical cable filling layer accounts for 7% to 15%.

[0011] In some preferred embodiments, the thickness of the insulating layer is not less than 33.84 mm.

[0012] In some preferred embodiments, the optical cable filling layer includes a polyethylene filling strip, a glass fiber reinforcing rod, and an optical cable unit; The diameter of the polyethylene filler strip is 0.5~1.0 mm larger than the diameter of the optical cable unit.

[0013] In some preferred embodiments, the diameter of the optical cable unit is 5.0~7.0mm, and the diameters of the polyethylene filler strip and the glass fiber reinforcing rod are 6.0~8.0mm, respectively.

[0014] In some preferred embodiments, the metal shielding layer includes a lead alloy sheath and copper wires or strips loosely wound around the inner or outer wall of the lead alloy sheath; the thickness of the lead alloy sheath is 3.0 mm to 4.0 mm.

[0015] In some preferred embodiments, the inner sheath is made of semi-conductive polyethylene material with a thickness of 3.5 mm to 3.9 mm; The inner lining layer comprises two layers of polypropylene rope, the thickness of which is 0.45 to 0.55 compared to the thickness of the armor layer; The outer sheath includes an inner polypropylene rope and an outer polypropylene rope. The inner polypropylene rope is treated with asphalt impregnation, and the outer polypropylene rope has a black base with spiral blue stripes. The width of the blue stripes is not less than 100mm, and the total thickness of the inner and outer polypropylene ropes is 3.5mm to 4.5mm.

[0016] In some preferred embodiments, the conductor is an irregularly shaped copper conductor with a nominal cross-sectional area of ​​4000 mm², a compaction coefficient of not less than 0.95, and an outer diameter of 72 mm to 73 mm.

[0017] In some preferred embodiments, the ratio of the thickness of the conductor shielding layer to the thickness of the insulating shielding layer is 0.9 to 1.1.

[0018] By adopting the above technical solution, the ±800kV DC submarine cable provided in this application has the following beneficial effects: 1. This application provides a complete structural design scheme for a ±800kV DC submarine cable, with a single-circuit transmission capacity of up to 4500MW. Compared with existing ±500kV submarine cables (typical capacity of approximately 2000MW), this scheme has a significant advantage in transmission capacity. Under the same transmission capacity conditions, the number of required circuits is significantly reduced, which helps to save marine corridor resources and reduce overall project investment and subsequent marine use costs.

[0019] 2. In this application, the ratio of insulation thickness to conductor outer diameter is 0.45~0.55, meaning the radial dimension of the insulation layer is essentially equivalent to that of the conductor. This ratio is a typical structural feature that distinguishes ±800kV UHVDC submarine cables from ±500kV and lower-level submarine cables. Based on the overall circular cross-sectional area of ​​the submarine cable, the sum of the conductor and insulation cross-sectional areas accounts for 55%~65% of the overall circular cross-sectional area, making the insulation layer the functional layer with the largest volume in the entire submarine cable cross-section. At this voltage level, the insulation layer transforms from an auxiliary layer in the traditional structure into the dominant layer in the cross-section, reflecting the fundamental change in cross-sectional structure brought about by the voltage level transition. This insulation-dominated cross-sectional structure is a hallmark distinguishing UHVDC submarine cables from medium and low-voltage submarine cables. Based on measured breakdown field strength data at different temperatures, combined with a long-term aging life model with a design life of 40 years, an insulation thickness of no less than 33.84mm is determined. This effectively avoids electric field concentration and thermal aging problems, ensuring long-term safe and stable operation of the cable at a maximum operating temperature of 70℃.

[0020] 3. This application employs a double-layer steel wire armor, with a semi-conductive terylene tape wrapping layer between the two layers of steel wire. The steel wire surface is coated with asphalt, forming a multi-stage composite armor structure of asphalt-semi-conductive terylene tape-steel wire. The volume resistivity of the semi-conductive terylene tape is controlled at 10 Ω·cm. 4 ~10 6The Ω·cm coating creates a resistive connection between the double-layer armored steel wires, bringing the potentials of the two layers of wires closer together and forming an equipotential surface. This eliminates interlayer potential differences and the risk of tip discharge, improving the uniformity of the electric field distribution on the armor surface under ±800kV high voltage levels. Simultaneously, the tertrol tape wrapping acts as a flexible insulating layer sandwiched between the double-layer rigid steel wires, allowing for slight relative slippage between the two layers when the cable bends. Combined with the reverse twisting structure of the double-layer steel wires, this effectively balances torsional stress, suppresses torsional effects during deep-sea laying, and prevents the cable from forming loops. Furthermore, the asphalt coating, the semi-conductive tertrol tape wrapping, and the steel wires form a mechanical transition. External impact energy is initially absorbed and damped by the viscoelastic deformation of the asphalt coating, further buffered and dispersed by the elastic deformation of the semi-conductive tertrol tape wrapping, and finally resisted by the rigid structure of the double-layer steel wires. This synergistic effect of the three materials gives the armor layer multiple protective capabilities of damping, buffering, and load-bearing, which is beneficial for improving its impact toughness and long-term fatigue resistance under complex deep-water conditions.

[0021] 4. This application employs a composite metal shielding structure consisting of a lead alloy sheath and loosely wound copper wires or strips on the inner / outer walls. Compared to a scheme using only a lead alloy sheath as the shielding layer, this structure enables the short-circuit current (50kA / 1s) carrying capacity to be more than three times that of a pure lead sheath structure. Simultaneously, the loosely wound copper wires or strips serve as redundant parts of the electric field shielding. Even when the resistivity of the lead alloy sheath increases or thermal damage occurs due to a large fault current, the cable can still maintain its normal electric field shielding function, preventing damage to the cable body due to the failure of a single shielding layer. This improves the operational reliability of the cable under system short-circuit fault conditions.

[0022] 5. This application simultaneously arranges polyethylene filler strips, fiberglass reinforcing rods, and optical cable units within the optical cable filling layer. The diameter of the polyethylene filler strip is slightly larger than that of the optical cable unit, suspending the optical cable unit in the cable core gap, thus providing physical isolation and mechanical buffering between it and surrounding components. The fiberglass reinforcing rod provides additional tensile strength. The polyethylene filler strip, fiberglass reinforcing rod, and optical cable together fill the cable core gap, maintaining a round cable cross-section and ensuring uniform stress during subsequent armor layer wrapping. This effectively reduces the risk of optical cable unit damage due to increased cable diameter and higher laying tension at ±800kV levels, while also improving the overall lateral pressure resistance of the cable. Attached Figure Description

[0023] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0024] Figure 1A schematic diagram of the structure of a ±800kV DC submarine cable provided in the embodiments of this application.

[0025] The following is supplementary explanation of the attached figures: 1-Conductor; 2-Conductor-side water-blocking layer; 3-Conductor shielding layer; 4-Insulation layer; 5-Insulation shielding layer; 6-Insulation-side water-blocking layer; 7-Metallic shielding layer; 8-Inner sheath; 9-Inner lining layer; 10-Optical cable filling layer; 11-Armor layer; 12-Outer sheath. Detailed Implementation

[0026] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this application without creative effort are within the scope of protection of this application.

[0027] The term "an embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of this application. In the description of this application, it should be understood that the terms "upper," "lower," "top," "bottom," etc., indicating orientation or positional relationships based on the orientation or positional relationships shown in the accompanying drawings, are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application. Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. Moreover, the terms "first," "second," etc., are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments of this application described herein can be implemented in orders other than those illustrated or described herein.

[0028] When a numerical range is disclosed herein, the range is considered continuous and includes the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to an integer, it includes every integer between the minimum and maximum values ​​of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are included. For example, a specified range from “1 to 10” should be considered to include any and all subranges between the minimum value 1 and the maximum value 10. Exemplary subranges of the range 1 to 10 include, but are not limited to, 1 to 6.1, 3.5 to 7.8, 5.5 to 10, etc.

[0029] like Figure 1 As shown in the figure, this application provides a ±800kV DC submarine cable, which includes, from the inside out: conductor 1, conductor-side water-blocking layer 2, conductor shielding layer 3, insulation layer 4, insulation shielding layer 5, insulation-side water-blocking layer 6, metal shielding layer 7, inner sheath 8, inner lining layer 9, optical cable filling layer 10, armor layer 11, and outer sheath 12.

[0030] The ratio of the thickness of the insulation layer 4 to the outer diameter of the conductor 1 is 0.45 to 0.55, for example, 0.45, 0.48, 0.50, 0.52, or 0.55. This means the radial dimension of the insulation layer 4 is essentially equivalent to that of the conductor 1. This ratio is a significant structural feature that distinguishes ±800kV UHVDC submarine cables from ±500kV and lower voltage submarine cables. The insulation layer 4 changes from an auxiliary layer to a dominant layer, reflecting the change in cross-sectional structure brought about by the voltage level transition. Limiting this ratio within the above range ensures sufficient insulation margin while avoiding excessive increases in the cable's outer diameter and weight, thus balancing laying flexibility and economy. Furthermore, based on the total cross-sectional area of ​​the submarine cable, the sum of the cross-sectional areas of conductor 1 and insulation layer 4 accounts for 55% to 65% of the total cross-sectional area of ​​the submarine cable, for example, 56%, 58%, 60%, 62%, and 65%. Insulation layer 4 is the functional layer with the largest volume in the entire cross-section of the submarine cable. Limiting this proportion to the above range can ensure current carrying capacity and insulation reliability while reserving sufficient cross-sectional space for the metal shielding layer 7, optical cable filling layer 10, and armor layer 11, thus ensuring mechanical protection and optical cable integration functions.

[0031] The conductor-side water-blocking layer 2 and the insulation-side water-blocking layer 6 are wrapped around the outside of the conductor 1 and the insulation shielding layer 5, respectively, both using semi-conductive water-resistant tape. The conductor-side water-blocking layer 2 can be made of two layers of semi-conductive water-resistant tape, each layer approximately 0.2mm thick; the insulation-side water-blocking layer 6 can be made of two layers of semi-conductive water-resistant tape, each layer approximately 2.0mm thick. During wrapping, the semi-conductive water-resistant tape should be tight, flat, and wrinkle-free. The overlap width can be adjusted according to the actual specifications, for example, but not limited to, 12mm~16mm. The expandable side of the conductor-side water-blocking layer 2 faces away from the conductor, while the expandable side of the insulation-side water-blocking layer 6 faces the metal shielding layer 7. This ensures that when the water-blocking tape expands upon contact with water, it expands in a direction away from the conductor (i.e., towards the outside of the cable core or the metal shielding layer), effectively preventing seawater from seeping in along the cable axis.

[0032] The armor layer 11 comprises, from the inside out, a first semi-conductive terylene tape wrapping layer, a first steel wire layer, a second semi-conductive terylene tape wrapping layer, and a second steel wire layer; the first and second steel wire layers are twisted in opposite directions, and the surfaces of the steel wires in both layers are coated with an asphalt layer. The first and second steel wire layers are preferably made of galvanized steel wire. By forming a multi-level composite armor structure of asphalt (viscoelastic) - semi-conductive terylene tape (elastic) - steel wire (rigid) between the semi-conductive terylene tape wrapping layer and the double-layer steel wire, systematic synergistic optimization of electrical and mechanical performance is achieved.

[0033] Regarding electric field homogenization, the volume resistivity of the semiconducting Terdroleon strip is 10. 4 ~10 6 The resistance of the double-layered armored steel wires (Ω·cm) creates a resistive connection, neither fully conductive nor fully insulated, thus aligning the potentials of the two layers and forming an equipotential surface. This effectively eliminates interlayer potential differences and the risk of tip discharge, resulting in a uniform electric field distribution on the surface of the armor layer 11 and significantly improving its electric field stability under ±800kV high voltage levels. Simultaneously, the semi-conductive Tedoron tape acts as a flexible spacer, completely isolating the double-layered steel wires and preventing direct contact between them that could cause wear and localized stress concentration.

[0034] In terms of mechanical properties, the flexible buffering characteristics of the semi-conductive tertrol tape and the rigid load-bearing characteristics of the steel wire constitute an alternating structure of a flexible isolation layer and a rigid load-bearing layer. This structure can absorb and disperse the torsional stress generated when the two layers of steel wires are twisted in opposite directions, allowing the two layers of steel wires to produce slight relative slippage when the submarine cable is bent. Combined with the reverse twisting of the two layers of steel wires, it effectively balances the torsional stress, suppresses the torsional effect during deep-sea laying, and prevents the formation of loops in the submarine cable. At the same time, the external impact energy is initially absorbed and damped by the viscoelastic deformation of the asphalt, further buffered and uniformly dispersed by the elastic deformation of the semi-conductive tertrol tape, and finally supported and resisted by the rigid structure of the two layers of steel wires. The synergistic effect of the three materials significantly improves the impact toughness and fatigue resistance of the armor layer 11, thereby comprehensively ensuring the electrical safety and mechanical reliability of the ±800kV DC submarine cable in the deep-sea environment.

[0035] In some preferred embodiments, the diameter of a single steel wire in both the first and second steel wire layers is 5.5 mm to 6.5 mm, more preferably 6.0 mm. The thickness of both the first and second semi-conductive terylene tape wrapping layers is 0.3 mm to 0.5 mm, and the overlap rate is not less than 25%. The coating thickness of the asphalt layer is 0.1 mm to 0.3 mm, and the depth to which the asphalt layer penetrates the surface of the steel wire is 5% to 10% of the diameter of a single steel wire.

[0036] By synergistically limiting the above parameter ranges, the overall electro-mechanical performance of the armor layer 11 can be further optimized: a single steel wire diameter of 5.5mm~6.5mm (preferably 6.0mm) ensures sufficient mechanical load-bearing strength while taking into account the flexibility and bending performance of the submarine cable, avoiding difficulties in laying due to excessively thick steel wires or insufficient tensile and compressive strength due to excessively thin steel wires; a semi-conductive tertrol tape wrapping layer thickness of 0.3mm~0.5mm and an overlap rate of ≥25% ensures a resistive connection between the two steel wires, achieving electric field homogenization, and also provides sufficient flexible buffer layer thickness to absorb torsional stress and impact energy; an asphalt coating thickness of 0.1mm~0.3mm and a filling effect of 5%~10% of the steel wire diameter in the stranding gap ensures that the asphalt forms a continuous and uniform viscoelastic coating on the steel wire surface, providing effective damping dissipation and corrosion protection, while preventing excessive coating thickness from causing excessive increase in the outer diameter of the armor layer 11 or asphalt flow and accumulation, which would affect the laying performance and structural compactness of the submarine cable. The parameters of the above three layers are matched with each other and work together to achieve the integrated functions of potential balancing, torsional stress balancing and shock resistance protection of the armor layer 11, thereby improving the long-term operational reliability and service life of the ±800kV DC submarine cable in the complex environment of the deep sea.

[0037] In some preferred embodiments, based on the total circular cross-sectional area of ​​the submarine cable, the cross-sectional area ratio of the armor layer is 15%~20%, for example, 15%, 18%, or 20%; the cross-sectional area ratio of the metal shielding layer is 5%~10%, for example, 5%, 6%, 8%, or 10%; and the cross-sectional area ratio of the optical fiber filling layer is 7%~15%, for example, 7%, 10%, 12%, or 15%. Through the synergistic limitation of the cross-sectional area ratios of the above functional layers, combined with the optimization of the thickness-to-diameter ratio of the insulation layer 4 to the conductor 1 (the ratio of the thickness of the insulation layer 4 to the outer diameter of the conductor 1 is 0.45~0.55), the sum of the cross-sectional areas of the conductor 1 and the insulation layer 4 accounts for 55%~65% of the total circular cross-sectional area of ​​the submarine cable, thereby achieving a comprehensive balance of the electric field, thermal field, and force field of the submarine cable under ±800kV UHV operating conditions. Specifically: the armor layer 11 accounts for 15%~20% of the total area, providing sufficient mechanical strength and impact resistance to withstand complex loads such as dragging, compression, and rock abrasion during deep-sea laying and operation. Its large cross-sectional area ensures sufficient radial stiffness to resist radial compression deformation under high water pressure in the deep sea. The metal shielding layer 7 accounts for 5%~10%, ensuring the conductivity of short-circuit fault current and acting as a radial waterproof barrier to prevent moisture penetration into the insulation system. The optical cable filling layer 10 accounts for 7%~15%, providing ample integration space. The combination of polyethylene filler strips and fiberglass reinforcing rods can share some radial pressure and improve the overall roundness of the submarine cable. This synergistic optimization of the cross-sectional area proportions of the aforementioned functional layers, while ensuring long-term operational reliability, also considers the electrical performance, mechanical strength, communication integration capabilities, and deep-sea environmental adaptability of the submarine cable, providing a structural parameter design basis for the engineering application of ±800kV DC submarine cables.

[0038] In some preferred embodiments, the thickness of the insulation layer 4 is not less than 33.84 mm, preferably 36 mm. The thickness is determined based on the electrical strength test and long-term operational reliability calculation of the system.

[0039] Insulation layer 4 can be made of cross-linked polyethylene (XLPE), such as Borealis LS4258DCE type insulation material. To determine the electrical strength limit of this material at operating temperature, lightning impulse breakdown field strength tests were conducted on 1 mm thick samples at 20°C and 70°C, four times each. The results showed that at 20°C, the breakdown field strengths measured in the four tests were 120 kV / mm, 95 kV / mm, 90 kV / mm, and 90 kV / mm, with an average value of 98.75 kV / mm; at 70°C, the results were 100 kV / mm, 105 kV / mm, 105 kV / mm, and 105 kV / mm, with an average value of 103.75 kV / mm. Based on the above test data, to ensure sufficient electrical margin of the insulation at the highest design temperature, this design uses the maximum allowable DC design field strength E at 70°C. dc(70) 80kV / mm is used as the benchmark value for calculating insulation thickness.

[0040] Based on this, the insulation thickness is calculated according to the long-term operation requirements of a submarine cable's design life of 40 years. DC withstand voltage U′ dc Determine using the following formula:

[0041] Wherein, U0 is the rated voltage (±800kV). This is the voltage coefficient (usually taken as 1). The aging factor is given by the formula. =(t1 / t2) 1 / n The calculation is performed, where t1 is the design life (40 years), t2 is the test pressurization time (30 min), and n is the DC aging life index of XLPE insulation (taken as 13). The results are as follows: ≈2.82, A safety factor (usually taken as 1.2) is used. Substituting these parameters, the DC withstand voltage is calculated. It is 2707.2kV.

[0042] Thickness design based on long-term operational requirements: d= / E dc(70) =2707.2 / 80=33.84mm.

[0043] Therefore, under the condition of the highest design temperature of 70°C, the theoretical minimum insulation thickness of ±800kV DC submarine cable should not be less than 33.84mm.

[0044] To further ensure long-term operational reliability and provide a margin of safety, the thickness of insulation layer 4 is preferably designed to be 36mm. This thickness design ensures that insulation layer 4 has sufficient electrical safety margin under the action of ultra-high voltage DC electric field, and effectively reduces the average electric field strength of insulation layer 4. This significantly slows down the local electric field distortion and electrical aging process caused by space charge accumulation, providing a reliable guarantee for the long-term stable operation of ±800kV DC submarine cable.

[0045] In some preferred embodiments, the optical cable filling layer 10 includes a polyethylene (PE) filler strip, a fiberglass reinforced rod (FRP), and an optical cable unit; wherein the diameter of the PE filler strip is 0.5~1.0 mm larger than the diameter of the optical cable unit. For example, the optical cable unit is a 2×24 core optical cable with a diameter of 6.0 mm. This optical cable unit is inserted into the core filling structure formed by the PE filler strip and multiple fiberglass reinforced rods, which can effectively reduce damage to the optical cable unit during submarine cable laying and also protect the internal structure of the submarine cable. During the stranding process of the ±800kV submarine cable, the optical cable unit is in direct contact with rigid structures such as the armor layer 11. Under the enormous stranding tension and bending stress, the optical cable unit is easily crushed or worn. By making the diameter of the PE filler strip slightly larger than that of the optical cable unit (e.g., a 6.0mm optical cable unit matched with a 6.5mm PE filler strip and a 6.5mm glass fiber reinforcing rod), the optical cable unit is suspended in the gap of the cable core by the PE filler strip, avoiding rigid contact with the surrounding rigid structure. The PE material itself has a certain degree of elasticity and cushioning properties, which can absorb and disperse external compressive forces, ensuring that the optical cable unit does not bear direct external forces during production, transportation and laying.

[0046] Preferably, the PE filler strip adopts a twisting method in the opposite direction to the armor layer 11, with a twisting pitch ratio of 10 to 15 times the cable diameter. The reverse twisting offsets the torsional moment of the submarine cable under tension, effectively suppressing torsional deformation during the laying process.

[0047] Preferably, the diameter of the optical cable unit is 5.0~7.0mm, and the diameters of the PE filler strip and the glass fiber reinforcing rod are each independently selected from 6.0mm~8.0mm.

[0048] In some preferred embodiments, the metal shielding layer 7 includes a lead alloy sheath and copper wires or strips loosely wound around the inner or outer wall of the lead alloy sheath. The lead alloy sheath effectively provides radial waterproofing and mechanical protection under submarine cable laying, normal operation, and fault conditions. Given that the single-phase ground fault current of the ±800kV submarine cable can be designed at 50kA for a duration of 1s, and considering the high resistivity of lead (22×10⁻⁶), this is suitable for applications where lead has a high resistivity (22×10⁻⁶). -8The lead alloy sheath has a short-circuit current resistance of approximately 13 times that of copper (Ω·m, about 13 times that of copper). Therefore, this application employs a composite structure of a lead alloy sheath and a copper wire or copper strip shielding layer. Specifically, a layer of copper wire or copper strip (nominal cross-section 120mm²) is placed on the inner or outer wall of the lead alloy sheath. 2 This allows it to form a parallel circuit with the lead alloy sheath, sharing the short-circuit current.

[0049] The lead alloy sheath thickness is 3.0mm~4.0mm, preferably 5mm. According to EN60811-506 standard, the bending test requirement for the lead alloy sheath is that the ratio of the bending diameter D to the cable diameter d, D / d, must be ≥15. It has been verified that a 3.0mm~4.0mm thick lead alloy sheath can meet the minimum bending radius requirement (20 times the cable diameter) for submarine cables.

[0050] In terms of manufacturing process, a continuous lead extrusion machine can be used to uniformly extrude molten lead alloy (temperature approximately 420℃) onto the outside of the insulating side water-blocking layer 6, followed by water cooling for shaping. After lead extrusion, the surface of the lead alloy sheath should be smooth and free of pores, and it must be inspected by eddy current testing.

[0051] Furthermore, a layer of loosely wound copper wire or strip is added to the inner or outer wall of the lead alloy sheath, with a wrapping pitch of 10-12 mm. When this copper wire or strip is connected in parallel with the lead alloy sheath, the short-circuit current carrying capacity can be increased by more than three times. Simultaneously, the copper wire or strip can also serve as redundancy for electric field shielding. To prevent electrochemical corrosion between copper and lead, the surface of the copper wire or strip is preferably tin-plated.

[0052] In some preferred embodiments, the inner sheath 8 is made of semi-conductive polyethylene material with a thickness of 3.5 mm to 3.9 mm, preferably with a nominal thickness of 3.7 mm. It covers the metal shielding layer 7 and is used to protect the metal shielding layer 7 and eliminate the induced voltage difference between it and the armored steel wire.

[0053] The inner lining layer 9 comprises two layers of polypropylene (PP) rope, wrapped around the inner sheath 8. The thickness ratio of the inner lining layer 9 to the armor layer 11 is 0.45~0.55, which ensures mechanical strength while avoiding excessive structural bulk. The two layers of PP rope have good abrasion resistance, effectively protecting the inner sheath 8 and internal structure from mechanical damage.

[0054] The outer sheath 12 includes an inner polypropylene rope and an outer polypropylene rope. The inner polypropylene rope is treated with asphalt impregnation to enhance its waterproof and corrosion-resistant properties; the outer polypropylene rope has a black base and is decorated with spiral blue stripes, the width of which is not less than 100mm, to facilitate visual identification and maintenance inspection after the submarine cable is laid.

[0055] The total thickness of the inner and outer polypropylene ropes is 3.5mm to 4.5mm, preferably 4.0mm. This thickness provides sufficient abrasion and impact resistance while preventing the outer sheath 12 from becoming excessively bulky, thus helping to control the overall outer diameter and weight of the submarine cable.

[0056] In this application, both the inner liner 9 and the outer sheath 12 are made of PP rope material, forming a synergistic protective effect. On the one hand, the inner liner 9, as a buffer layer inside the armor layer 11, can absorb the impact energy generated by armor twisting and external compression, preventing stress concentration from being transmitted to the inner sheath 8 and the metal shielding layer 7. On the other hand, the outer sheath 12, as the outermost layer of the submarine cable, is in direct contact with the seabed, laying equipment, and other external environments, and must withstand potential mechanical damage such as rock abrasion and anchor damage during the laying process. PP rope material has excellent insulation, anti-aging and anti-oxidation properties, dimensional stability, non-absorbency, light weight, and high tensile strength, while also possessing high abrasion resistance and impact resistance, effectively absorbing and dispersing external impact energy to protect the internal structure. The inner and outer PP rope structures complement each other, with the inner layer focusing on buffering and isolation, and the outer layer focusing on abrasion protection, together forming a mechanical protection system for the internal structure of the submarine cable, improving the operational reliability and service life of the submarine cable in complex deep-sea environments.

[0057] In some preferred embodiments, conductor 1 is a non-circular copper conductor 1 with a nominal cross-sectional area of ​​4000 mm². 2 The compression coefficient is not less than 0.95, and the outer diameter (including the water-blocking adhesive filled in the stranding gaps) is 72mm~73mm. The copper conductor 1 has low resistivity (approximately 0.01724Ω·mm). 2 Although heavier, copper conductor 1 has good conductivity, effectively reducing line loss and temperature rise; therefore, it is the preferred choice. Based on a transmission power of 4500MW, voltage ±800kV, and a rated current of approximately 2812.5A, a design current of 2950A is taken after considering a safety factor of 1.05. Calculations based on the allowable current carrying capacity of copper conductor 1 under seabed laying conditions (burial depth 3m, ambient temperature 70℃, soil thermal resistance 0.7℃·m / W) indicate a required cross-section of approximately 4000mm². 2 The corresponding DC resistance (20℃) is not greater than 0.0058Ω / km, and the allowable short-circuit current is 150kA per second.

[0058] In addition, the strand gaps of the irregularly shaped copper conductor 1 are filled with water-blocking adhesive to achieve the longitudinal water-blocking function of conductor 1 and prevent moisture from penetrating along the axial direction of conductor 1. At the same time, a compaction coefficient of not less than 0.95 can effectively reduce the gaps between the strands of conductor 1, making the surface of conductor 1 smooth and round, thereby suppressing electric field distortion and partial discharge, and improving the long-term operational reliability of the insulation system.

[0059] In some preferred embodiments, the thickness ratio of the conductor shielding layer 3 to the insulation shielding layer 5 is 0.9 to 1.1 to ensure a good interface transition between the two and the insulation layer 4, thereby effectively suppressing partial discharge and interface discharge.

[0060] Preferably, the conductor shielding layer 3 can be made of semi-conductive cross-linked XLPE base material with a volume resistivity ≤1Ω·m, and co-extruded with the insulation layer 4. According to GB / T31489 standard, for submarine cables with a rated voltage of 320kV and above, the minimum thickness of the extruded conductor shielding layer 3 should not be less than 1.2mm. In this application, the thickness of the conductor shielding layer 3 is preferably set to 2.2mm to ensure that it can fully cover the surface unevenness generated by the stranding of the conductor 1 and eliminate the electric field concentration effect on the surface of the conductor 1. Similarly, the insulation shielding layer 5 can also be made of semi-conductive cross-linked XLPE base material and co-extruded with the insulation layer 4. According to GB / T31489 standard, for submarine cables with a voltage of 320kV and above, the minimum thickness of the insulation shielding layer 5 should not be less than 1.0mm. In this application, the thickness of the insulation shielding layer 5 is preferably set to 2.0mm to ensure that it forms a reliable equipotential surface with the metal shielding layer 7 and effectively prevents the occurrence of interface discharge.

[0061] The following detailed description of examples of this application is exemplary and is only used to explain this application, and should not be construed as limiting this application. Specifically, the insulating layer uses BOREAL ISLS4258DCE insulating material supplied by Borealis, and both the conductor shielding layer and the insulating shielding layer use semi-conductive shielding material LE0650DC.

[0062] Example 1 A ±800kV DC submarine cable, its structure from the inside out includes: an outer diameter of 72.1mm, a nominal cross-sectional area of ​​4000mm², etc. 2The cable consists of an irregularly shaped copper conductor (compression factor 0.95), with gaps filled with water-blocking adhesive. Two layers of 0.2mm thick semi-conductive water-blocking tape and a 2.2mm thick conductor shielding layer are wrapped around the conductor. A 36mm thick cross-linked polyethylene insulation layer is extruded, followed by a 2.0mm thick insulating shielding layer and two more 2.0mm thick semi-conductive water-blocking tapes. A 5mm thick lead alloy + copper wire metal shielding layer is placed outside the water-blocking layer. A 0.3mm thick semi-conductive polyethylene inner sheath is extruded outside the metal shielding layer, followed by two 6.0mm thick polypropylene rope (PP rope) inner lining layers. A 6.5mm thick optical cable filling layer is then provided, consisting of a 6.5mm diameter PE filling strip, a 6.5mm diameter glass fiber reinforcing rod, and a 6.0mm diameter 2×24 core optical cable unit. An armor layer is placed outside the optical cable filling layer, consisting of a thick... The armor layer consists of a first semi-conductive terylene tape wrapping layer with a thickness of 0.3 mm (overlap rate not less than 25%), a first galvanized steel wire layer with a single diameter of 6.3 mm (the steel wire surface is coated with an asphalt layer with a coating thickness of 0.2 mm and the asphalt penetrates the steel wire surface to a depth of 0.5 mm), a second semi-conductive terylene tape wrapping layer with a thickness of 0.3 mm (overlap rate not less than 25%), and a second galvanized steel wire layer with a single diameter of 6.3 mm (the steel wire surface is coated with an asphalt layer with a coating thickness of 0.2 mm and the asphalt penetrates the steel wire surface to a depth of 0.5 mm), and the first galvanized steel wire layer and the second galvanized steel wire layer are twisted in opposite directions; the armor layer is wrapped with an outer sheath with a total thickness of 4.0 mm, the outer sheath comprising an inner polypropylene rope impregnated with asphalt and an outer polypropylene rope with a black base and spiral blue stripes (stripes width 100 mm). Tests showed that, under a 50kA / 1s short-circuit fault, the composite shielding layer of the ±800kV DC submarine cable in this embodiment experienced a temperature rise of approximately 145°C, which is lower than the short-time withstand temperature of lead alloys. The insulation layer was estimated to have a service life of over 40 years at 70°C. The measured pressure on the optical cable unit side was 0.8kN / m, and no fiber breakage occurred after bending fatigue. The armor layer exhibited sufficient tensile breaking strength, good corrosion resistance, and excellent stranding lubrication. The overall design life of the submarine cable reached 40 years.

[0063] Example 2 Referring to the ±800kV DC submarine cable of Example 1, the difference is that the metallic shielding layer only uses a lead alloy sheath, without any loosely wound copper wires or strips. Calculations show that under a 50kA / 1s short-circuit fault, the temperature rise of the pure lead sheath alone, bearing the current, is approximately three times that of the composite shielding structure in Example 1 (the temperature rise of the composite shielding in Example 1 is approximately 145℃, while the temperature rise of the pure lead sheath in this example reaches approximately 468℃), far exceeding the allowable short-term withstand temperature of the lead alloy (approximately 200℃). This could lead to sheath melting or deformation, drastically increasing the risk of shielding failure. Simultaneously, the lack of copper wires also reduces the electric field shielding redundancy, making it impossible to maintain normal shielding function when the lead sheath is damaged due to a fault.

[0064] Example 3 Referring to the ±800kV DC submarine cable of Example 1, the difference is that the diameter of each single wire in the first and second galvanized steel wire layers of the armor is 5.0mm. Reducing the wire diameter from 6.3mm to 5.0mm results in a reduction of approximately 37% in the cross-sectional area per wire (5.0 / 6.3). 2 (≈0.63), the total cross-sectional area of ​​the double-layer steel wires is reduced accordingly, resulting in a decrease of about 36% in the overall tensile breaking strength of the armor layer (estimated based on the principle that the breaking strength of the steel wire is proportional to the cross-sectional area). Although the flexibility of the submarine cable is slightly improved, its ability to resist dragging and rock abrasion during deep-sea laying is insufficient, and the long-term operational safety margin is reduced.

[0065] Example 4 Referring to the ±800kV DC submarine cable of Example 1, the difference lies in the diameter of the PE filler strip and glass fiber reinforcing rod in the optical cable filling layer, both being 4.5mm in diameter. The PE filler strip diameter (4.5mm) is smaller than the optical cable unit diameter (6.0mm), making it impossible to suspend the optical cable unit above the cable core gap, resulting in direct contact between the optical cable and rigid structures such as the armor layer and metal shielding layer. In the cabling and bending tests, the lateral pressure borne by the optical cable unit increased by approximately 2.3 times compared to Example 1 (the measured lateral pressure increased from 0.8kN / m to 2.6kN / m), and the risk of fiber breakage after bending fatigue increased significantly. Simultaneously, the insufficient diameter of the glass fiber reinforcing rod reduced its additional tensile strength contribution, decreasing the overall lateral pressure resistance of the submarine cable by approximately 15%.

[0066] Comparative Example 1 Referring to the ±800kV DC submarine cable of Example 1, the difference is that the insulation layer thickness is 30mm. Reducing the insulation layer thickness from 36mm to 30mm is lower than the theoretical minimum calculated value of 33.84mm. Based on the accelerated thermal aging model with a 40-year design life, the actual lifespan of the insulation layer in this comparative example at 70℃ is only about 26 years, far below the design target, indicating insufficient long-term operational reliability and a risk of early breakdown.

[0067] Comparative Example 2 Referring to the ±800kV DC submarine cable of Example 1, the difference is that the armor layer only has a single layer of galvanized steel wire, without the first semi-conductive terylene tape wrapping layer, the second semi-conductive terylene tape wrapping layer, and the second galvanized steel wire layer. The single-layer armor structure halves the total cross-sectional area of ​​the steel wires, reducing the tensile breaking strength by approximately 52%.

[0068] Comparative Example 3 Referring to the ±800kV DC submarine cable of Example 1, the difference is that the steel wires in the armor layer are not coated with an asphalt layer. This significantly reduces corrosion resistance, accelerating the corrosion rate of the steel wires in the deep-sea environment, and shortening the armor layer's lifespan to an estimated 15 years. Furthermore, the absence of an asphalt layer weakens the lubrication effect during wire stranding, making it difficult to release stranding stress and leading to increased residual stress in the armor layer.

[0069] Based on the above embodiments and comparative examples, it can be seen that this application addresses the technical problems of ±800kV UHVDC submarine cables in terms of electrical insulation margin, short-circuit current carrying capacity, and deep-sea machinery protection. It ensures insulation reliability by setting the insulation layer thickness to conductor outer diameter ratio to 0.45~0.55, employs a lead alloy and copper wire composite metal shielding structure to achieve a short-circuit carrying capacity more than three times that of a pure lead sheath, and uses a double-layer reverse-stranded galvanized steel wire armor combined with a semi-conductive terylene tape wrapping layer and asphalt coating to balance torsional stress and ensure wear resistance and corrosion resistance. Furthermore, it uses PE filler strips with a diameter larger than the optical cable unit and glass fiber reinforcing rods to suspend the optical cable above the cable core gaps, enabling the submarine cable to achieve a single-circuit transmission capacity of 4500MW, meeting the long-term operation requirements of the ±800kV level.

[0070] The above description is only an optional embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A ±800kV DC submarine cable, characterized in that, The submarine cable comprises, from the inside out: a conductor, a conductor-side water-blocking layer, a conductor shielding layer, an insulation layer, an insulation shielding layer, an insulation-side water-blocking layer, a metal shielding layer, an inner sheath, an inner lining layer, an optical cable filling layer, an armor layer, and an outer sheath. Wherein, the ratio of the insulation layer thickness to the conductor outer diameter is 0.45~0.55; Based on the total circular cross-sectional area of ​​the submarine cable, the sum of the cross-sectional areas of the conductor and the insulation layer accounts for 55% to 65% of the total circular cross-sectional area of ​​the submarine cable; The armor layer includes a first semi-conductive terylene tape wrapping layer, a first steel wire layer, a second semi-conductive terylene tape wrapping layer, and a second steel wire layer arranged sequentially from the inside to the outside; the first steel wire layer and the second steel wire layer are twisted in opposite directions, and the steel wire surfaces of the two are respectively coated with an asphalt layer.

2. The ±800kV DC submarine cable according to claim 1, characterized in that, The diameter of a single steel wire in both the first and second steel wire layers is 5.5mm to 6.5mm. The thickness of both the first and second semiconductive terylene tape wrapping layers is 0.3mm to 0.5mm, and the overlap rate is not less than 25%. The coating thickness of the asphalt layer is 0.1mm to 0.3mm, and the depth of the asphalt layer penetrating into the surface of the steel wire is 5% to 10% of the diameter of a single steel wire.

3. The ±800kV DC submarine cable according to claim 1, characterized in that, Based on the total circular cross-sectional area of ​​the submarine cable, the cross-sectional area of ​​the armor layer accounts for 15% to 20%, the cross-sectional area of ​​the metal shielding layer accounts for 5% to 10%, and the cross-sectional area of ​​the optical cable filling layer accounts for 7% to 15%.

4. The ±800kV DC submarine cable according to claim 1, characterized in that, The thickness of the insulating layer is not less than 33.84 mm.

5. The ±800kV DC submarine cable according to claim 1, characterized in that, The optical cable filling layer includes polyethylene filling strips, glass fiber reinforcing rods, and optical cable units; The diameter of the polyethylene filler strip is 0.5~1.0 mm larger than the diameter of the optical cable unit.

6. The ±800kV DC submarine cable according to claim 5, characterized in that, The diameter of the optical cable unit is 5.0~7.0mm, and the diameters of the polyethylene filler strip and the glass fiber reinforcing rod are 6.0~8.0mm respectively.

7. The ±800kV DC submarine cable according to claim 1, characterized in that, The metal shielding layer includes a lead alloy sheath and copper wires or strips loosely wound around the inner or outer wall of the lead alloy sheath; the thickness of the lead alloy sheath is 3.0 mm to 4.0 mm.

8. The ±800kV DC submarine cable according to claim 1, characterized in that, The inner sheath is made of semi-conductive polyethylene material with a thickness of 3.5mm to 3.9mm; The inner lining layer comprises two layers of polypropylene rope, the thickness of which is 0.45 to 0.55 compared to the thickness of the armor layer; The outer sheath includes an inner polypropylene rope and an outer polypropylene rope. The inner polypropylene rope is treated with asphalt impregnation, and the outer polypropylene rope has a black base with spiral blue stripes. The width of the blue stripes is not less than 100mm, and the total thickness of the inner and outer polypropylene ropes is 3.5mm to 4.5mm.

9. The ±800kV DC submarine cable according to claim 1, characterized in that, The conductor is an irregularly shaped copper conductor with a nominal cross-sectional area of ​​4000 mm². 2 The compression coefficient is not less than 0.95, and the outer diameter is 72mm~73mm.

10. The ±800kV DC submarine cable according to claim 1, characterized in that, The ratio of the thickness of the conductor shielding layer to the thickness of the insulating shielding layer is 0.9 to 1.1.