A method for preparing a composite electromagnetic shielding slurry and the composite electromagnetic shielding slurry

By preparing a composite treatment of nickel nanowires and acidified carbon nanotubes, combined with sand milling dispersion technology, the shielding performance of electromagnetic shielding slurry was improved, solving the problem of insufficient electromagnetic shielding performance in existing technologies and achieving a more efficient electromagnetic shielding effect.

CN123120426APending Publication Date: 2026-11-17SHENZHEN SUNWAY COMM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611466995.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing methods for preparing electromagnetic shielding pastes result in poor electromagnetic shielding performance.

Method used

Nickel nanowires were prepared by hydrothermal reaction using nickel chloride hexahydrate, solvent, reducing agent, and reaction vessel. Combined with acidification treatment of carbon nanotubes and mixing with adhesive, the composite electromagnetic shielding slurry was dispersed by sand mill.

Benefits of technology

The shielding performance of the electromagnetic shielding paste is improved. Through the synergistic effect of nickel nanowires and carbon nanotubes, the connectivity and dielectric loss of the conductive network are enhanced, resulting in a better electromagnetic shielding effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120426A_ABST
    Figure CN123120426A_ABST
Patent Text Reader

Abstract

This invention discloses a composite electromagnetic shielding slurry, comprising adding nickel chloride hexahydrate and a second solvent to a first solvent to obtain a first mixed solution, adding a reducing agent to the first mixed solution and transferring it to a reaction vessel, performing a hydrothermal reaction at a first preset temperature for a first preset time to obtain an initial solution, centrifuging and drying to obtain nickel nanowires, adding carbon nanotubes to a third solvent, refluxing at a second preset temperature for a second preset time, washing and drying to obtain acidified carbon nanotubes, providing an adhesive, adding the nickel nanowires and acidified carbon nanotubes to the adhesive, stirring to obtain an initial composite slurry, dispersing the initial composite slurry through a sand mill to obtain a composite electromagnetic shielding slurry. By introducing nickel nanowires into the preparation of the electromagnetic shielding slurry, carbon nanotubes contribute dielectric loss and conduction loss, while nickel nanowires contribute magnetic loss and enhance the connectivity of the conductive network, resulting in a composite electromagnetic shielding slurry with better shielding performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of composite electromagnetic shielding technology, and in particular to a method for preparing a composite electromagnetic shielding slurry and the composite electromagnetic shielding slurry itself. Background Technology

[0002] In electromagnetic shielding technology, electromagnetic shielding slurry can reflect and absorb electromagnetic waves, confining electromagnetic interference to a specific area, thereby achieving effective protection for electronic devices. Electromagnetic shielding slurry has advantages such as excellent conductivity and high shielding effectiveness, and is widely used in electromagnetic protection treatment for scenarios such as 5G communication base stations, mobile terminals, and Internet of Things devices.

[0003] The current method for preparing electromagnetic shielding slurry includes: providing carbon nanotubes and a solvent, adding carbon nanotubes to the solvent, stirring and treating at a preset temperature for a preset time, washing and drying to obtain acidified carbon nanotubes, providing an adhesive, adding acidified carbon nanotubes to the adhesive, stirring to obtain an initial composite slurry, providing a sand mill, and dispersing the initial composite slurry through the sand mill to obtain an electromagnetic shielding slurry. However, the electromagnetic shielding performance of the electromagnetic shielding slurry prepared in this way is poor. Summary of the Invention

[0004] In view of the above problems, this invention provides a method for preparing a composite electromagnetic shielding slurry and the composite electromagnetic shielding slurry, which overcomes the above problems.

[0005] This invention provides a method for preparing a composite electromagnetic shielding slurry, comprising providing nickel chloride hexahydrate, a first solvent, and a second solvent; adding the nickel chloride hexahydrate and the second solvent to the first solvent to obtain a first mixed solution; providing a reducing agent and a reaction vessel; adding the reducing agent to the first mixed solution and transferring it to the reaction vessel; performing a hydrothermal reaction at a first preset temperature for a first preset time to obtain an initial solution; centrifuging and drying the initial solution to obtain nickel nanowires; providing carbon nanotubes and a third solvent; adding the carbon nanotubes to the third solvent; refluxing at a second preset temperature for a second preset time, followed by washing and drying to obtain acidified carbon nanotubes; providing an adhesive; adding the nickel nanowires and acidified carbon nanotubes to the adhesive; stirring to obtain an initial composite slurry; and providing a sand mill to disperse the initial composite slurry through the sand mill to obtain a composite electromagnetic shielding slurry.

[0006] In one optional embodiment, the step of adding nickel chloride hexahydrate and the second solvent to the first solvent to obtain a first mixed solution further includes: adding nickel chloride hexahydrate and the second solvent to the first solvent, and then magnetically stirring to obtain the first mixed solution.

[0007] In one optional embodiment, the step of adding the reducing agent to the first mixed solution and transferring it to the reaction vessel, performing a hydrothermal reaction at a first preset temperature for a first preset time to obtain an initial solution further includes: adding the reducing agent to the first mixed solution and stirring for a third preset time; transferring the stirred first mixed solution to the reaction vessel and performing a hydrothermal reaction at a first preset temperature for a first preset time to obtain an initial solution.

[0008] In one optional embodiment, the step of centrifuging and drying the initial solution to obtain nickel nanowires further includes: centrifuging the initial mixed solution to obtain initial nickel solid; providing a first detergent and a second detergent; adding the first detergent to the initial nickel solid for washing, and then adding the second detergent for washing; and vacuum drying the washed initial nickel solid at a third preset temperature for a fourth preset time to obtain nickel nanowires.

[0009] In one alternative embodiment, the first detergent is a polar solvent and the second detergent is an organic solvent.

[0010] In one optional embodiment, the step of adding the carbon nanotubes to the third solvent, stirring and mixing at a second preset temperature for a second preset time, and then washing and drying to obtain acidified carbon nanotubes further includes: adding the carbon nanotubes to the third solvent, stirring and mixing at a second preset temperature for a second preset time to obtain initial carbon nanotubes; centrifuging and washing the initial carbon nanotubes, and vacuum drying at a fourth preset temperature for a fifth preset time to obtain acidified carbon nanotubes.

[0011] In one optional embodiment, the step of adding the nickel nanowires and acidified carbon nanotubes to the adhesive and stirring to obtain an initial composite slurry further includes: providing a fourth solvent, a dispersant, a defoamer, a thickener, and a mixer; adding the adhesive, nickel nanowires, acidified carbon nanotubes, the fourth solvent, the dispersant, the defoamer, and the thickener to the mixer, and stirring at a first preset speed for a sixth preset time to obtain the initial composite slurry.

[0012] In one alternative embodiment, the fourth solvent is a polar solvent.

[0013] In one alternative embodiment, the first solvent is a polyol solvent, the second solvent is an alkaline precipitant, the third solvent is an acidifier, and the adhesive is an aqueous film-forming resin.

[0014] According to another aspect of the present invention, a composite electromagnetic shielding paste is provided, which is prepared by the preparation method described above.

[0015] This invention provides a method for preparing a composite electromagnetic shielding paste, comprising providing nickel chloride hexahydrate, a first solvent, and a second solvent; adding the nickel chloride hexahydrate and the second solvent to the first solvent to obtain a first mixed solution; providing a reducing agent and a reaction vessel; adding the reducing agent to the first mixed solution and transferring it to the reaction vessel; performing a hydrothermal reaction at a first preset temperature for a first preset time to obtain an initial solution; centrifuging and drying the initial solution to obtain nickel nanowires; providing carbon nanotubes and a third solvent; and adding... The carbon nanotubes are refluxed at a second preset temperature for a second preset time, then washed and dried to obtain acidified carbon nanotubes. An adhesive is provided, and the nickel nanowires and acidified carbon nanotubes are added to the adhesive. The mixture is stirred to obtain an initial composite slurry. A sand mill is provided, and the initial composite slurry is dispersed through the sand mill to obtain a composite electromagnetic shielding slurry. By introducing nickel nanowires into the preparation of the electromagnetic shielding slurry in the above manner, the carbon nanotubes contribute dielectric loss and conduction loss, while the nickel nanowires contribute magnetic loss and enhance the connectivity of the conductive network. The resulting composite electromagnetic shielding slurry has better shielding performance. Attached Figure Description

[0016] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the embodiments of this application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on the drawings without creative effort.

[0017] Figure 1 This is a flowchart of the preparation method of the composite electromagnetic shielding slurry according to an embodiment of the present invention; Figure 2 This is a flowchart of the preparation of the initial solution in the preparation method of the composite electromagnetic shielding slurry according to an embodiment of the present invention; Figure 3 This is a flowchart of the preparation of primary nickel nanowires in the preparation method of composite electromagnetic shielding paste according to an embodiment of the present invention; Figure 4 This is a flowchart of the preparation of acidified carbon nanotubes in the preparation method of composite electromagnetic shielding slurry according to an embodiment of the present invention; Figure 5 This is a flowchart of another embodiment of the preparation method of the composite electromagnetic shielding slurry of the present invention. Detailed Implementation

[0018] To facilitate understanding of the present invention, a more detailed description is provided below with reference to the accompanying drawings and specific embodiments. It should be noted that when an element is described as being "fixed to" another element, it can be directly on the other element, or one or more intermediate elements may exist between them. When an element is described as being "connected to" another element, it can be directly connected to the other element, or one or more intermediate elements may exist between them. The terms "vertical," "horizontal," "left," "right," and similar expressions used in this specification are for illustrative purposes only.

[0019] Unless otherwise defined, all technical and scientific terms used in this specification have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used in this specification is for the purpose of describing particular embodiments only and is not intended to limit the invention. The term "and / or" as used in this specification includes any and all combinations of one or more of the associated listed items.

[0020] Please see Figure 1 The preparation methods of composite electromagnetic shielding paste include: Step S1: Provide nickel chloride hexahydrate, a first solvent, and a second solvent; The nickel chloride hexahydrate is used to provide nickel ions. The first solvent is a polyol solvent, which is used to dissolve the nickel chloride hexahydrate. The polyol has a certain complexing effect on the nickel ions, which helps to control the reaction rate and particle growth. The second solvent is an alkaline precipitant, which is used to adjust the pH value. In some embodiments, the first solvent is ethylene glycol and the second solvent is sodium hydroxide.

[0021] S2 adds the nickel chloride hexahydrate and the second solvent to the first solvent to obtain a first mixed solution; In a polyol solvent, nickel ions are precipitated in situ to form a nickel hydroxide precursor through the action of an alkaline precipitant.

[0022] Step S3: Provide the reducing agent and the reaction vessel; In some embodiments, the reducing agent is hydrazine hydrate, which is used to reduce nickel ions to metallic nickel, and the reaction vessel is used to provide a high-temperature and high-pressure closed environment for subsequent reactions.

[0023] Step S4: Add the reducing agent to the first mixed solution and transfer it to the reaction vessel. Perform a hydrothermal reaction at a first preset temperature for a first preset time to obtain an initial solution. Under closed, high-temperature and high-pressure conditions, the reducing agent reduces nickel ions to metallic nickel, while the hydrothermal environment promotes the crystallization and growth of the product, resulting in a uniformly dispersed initial solution with controllable phase.

[0024] Step S5: After centrifuging and drying the initial solution, nickel nanowires are obtained; The nickel nanowires generated by the hydrothermal reaction were extracted from the liquid phase by centrifugation, and then dried to remove residual solvent and moisture from the surface, finally obtaining a pure and dry nickel nanowire product.

[0025] Step S6: Provide carbon nanotubes and a third solvent; The third solvent is an acidifier, which is used to introduce oxygen-containing functional groups such as carboxyl and hydroxyl groups onto the surface of carbon nanotubes. In some embodiments, the acidifier is nitric acid.

[0026] Step S7: Add the carbon nanotubes to the third solvent, reflux at a second preset temperature for a second preset time, then wash and dry to obtain acidified carbon nanotubes; By oxidizing carbon nanotubes under reflux conditions with an acidifying agent, oxygen-containing functional groups such as carboxyl and hydroxyl groups are introduced onto their surface, while impurities and amorphous carbon are removed, resulting in acidified carbon nanotubes with better dispersibility and higher surface activity.

[0027] Step S8: Provide adhesive; The adhesive is an aqueous film-forming resin, which is used to provide a film-forming matrix for subsequent composite slurry. The aqueous film-forming resin is used to bind functional fillers together and form a continuous coating after coating and drying, while determining the adhesion and flexibility of the coating.

[0028] Step S9: Add the nickel nanowires and acidified carbon nanotubes to the adhesive and stir to obtain an initial composite slurry; This allows the nickel nanowires and acidified carbon nanotubes to be initially and uniformly mixed in the adhesive, avoiding local agglomeration and preparing for subsequent sand milling and dispersion.

[0029] Step S10: Provide a sand mill to disperse the initial composite slurry to obtain a composite electromagnetic shielding slurry.

[0030] By using a sand mill to break up filler agglomerates through high-speed shearing and collision, nickel nanowires and acidified carbon nanotubes can achieve a finer and more uniform dispersion in the adhesive, resulting in a composite electromagnetic shielding slurry with uniform dispersion and good stability.

[0031] In some embodiments, the step of adding the nickel chloride hexahydrate and the second solvent to the first solvent to obtain a first mixed solution further includes: The nickel chloride hexahydrate and the second solvent are added to the first solvent, and after magnetic stirring, a first mixed solution is obtained.

[0032] Magnetic stirring can ensure that nickel chloride hexahydrate, the second solvent, and the first solvent are thoroughly and evenly mixed, which accelerates the dissolution and dispersion of nickel ions, promotes uniform contact between the alkaline precipitant and nickel ions, and avoids uneven precipitation or particle agglomeration caused by excessively high local concentrations.

[0033] Please see Figure 2 In some embodiments, the step of adding the reducing agent to the first mixed solution and transferring it to the reaction vessel, performing a hydrothermal reaction at a first preset temperature for a first preset time to obtain an initial solution further includes: Step S41: The reducing agent is added to the first mixed solution, and the mixture is stirred for a third preset time; Stirring ensures a uniform concentration distribution of the reducing agent in the system, preventing localized excessively high or low concentrations, which is beneficial for subsequent hydrothermal reduction reactions.

[0034] Step S42: Transfer the stirred first mixed solution to a reaction vessel and carry out a hydrothermal reaction at a first preset temperature for a first preset time to obtain an initial solution.

[0035] In the high-temperature, high-pressure, and sealed environment provided by the reactor, the reducing agent reduces nickel ions to metallic nickel, and promotes the crystallization and growth of the product with the help of hydrothermal conditions, finally obtaining the initial solution containing nickel nanowires.

[0036] Please see Figure 3 In some embodiments, the step of centrifuging and drying the initial solution to obtain nickel nanowires further includes: Step S51: Centrifuge the initial mixed solution to obtain initial nickel solid; The nickel nanowires in the initial mixed solution were separated from the liquid phase by centrifugation.

[0037] Step S52: Provide the first detergent and the second detergent; The first detergent is a polar solvent, and the second detergent is an organic solvent. In some embodiments, the first detergent is deionized water, and the second solvent is anhydrous ethanol. The first detergent is used to remove residual polyol solvent, unreacted reducing agent, and some alkaline residues, while the second detergent is mainly used to remove other inorganic salt residues and adjust the surface condition.

[0038] Step S53: After washing the initial nickel solid with the first detergent, wash it with the second detergent. Two-step washing process more thoroughly removes impurities and residues from the surface of nickel nanowires.

[0039] Step S54: The washed initial nickel solid is vacuum dried at a third preset temperature for a fourth preset time to obtain nickel nanowires.

[0040] Washing the initial nickel solid and then vacuum drying can reduce the drying temperature, prevent the nickel nanowires from oxidizing at high temperatures, and prevent particle agglomeration, ultimately yielding a pure, dry, and well-dispersed nickel nanowire product.

[0041] Please see Figure 4 In some embodiments, the step of adding the carbon nanotubes to the third solvent, stirring and mixing at a second preset temperature for a second preset time, and then washing and drying to obtain acidified carbon nanotubes further includes: Step S71: The carbon nanotubes are added to the third solvent and stirred and mixed at a second preset temperature for a second preset time to obtain the initial carbon nanotubes; Under heating and stirring conditions, an acidifying agent oxidizes and etches the surface of carbon nanotubes, introducing oxygen-containing functional groups such as carboxyl and hydroxyl groups, while removing amorphous carbon and impurities, thus obtaining surface-functionalized initial carbon nanotubes.

[0042] Step S72: The initial carbon nanotubes are centrifuged and washed, and then vacuum dried at a fourth preset temperature for a fifth preset time to obtain acidified carbon nanotubes.

[0043] By centrifugation, washing, and vacuum drying, pure, dry acidified carbon nanotubes with oxygen-containing functional groups on their surface are obtained. Vacuum drying can avoid high-temperature oxidation, maintain the integrity of the carbon nanotube structure, and prevent agglomeration.

[0044] Please see Figure 5 In some embodiments, the step of adding the nickel nanowires and acidified carbon nanotubes to the adhesive and stirring to obtain an initial composite slurry further includes: Step S91: Provide a fourth solvent, dispersant, defoamer, thickener, and mixer; The fourth solvent is a polar solvent, serving as a dispersion medium to ensure uniform mixing of the components in the liquid phase. The dispersant is used to adsorb onto the surfaces of nickel nanowires and acidified carbon nanotubes, reducing interfacial tension between filler particles and preventing re-agglomeration. The defoamer is used to suppress and eliminate bubbles generated during stirring, and the thickener is used to adjust the slurry viscosity. In some embodiments, the fourth solvent is deionized water, the dispersant is a sodium polycarboxylate anionic dispersant, the defoamer is an aqueous silicone defoamer, and the thickener is a polyurethane thickener.

[0045] Step S92: Add the adhesive, nickel nanowires, acidified carbon nanotubes, fourth solvent, dispersant, defoamer and thickener to the mixer, and stir at the first preset speed for a sixth preset time to obtain the initial composite slurry.

[0046] By stirring, nickel nanowires and acidified carbon nanotubes are initially and uniformly dispersed in the adhesive and the fourth solvent, resulting in an initial composite slurry with uniform composition and stable dispersion.

[0047] To further compare the existing methods for preparing composite electromagnetic shielding slurries with this method, the applicant conducted experiments and comparative experiments.

[0048] Experiment 1: Provide 0.5 g nickel chloride hexahydrate, 0.3 g sodium hydroxide, and 40 mL ethylene glycol. The nickel chloride hexahydrate and the sodium hydroxide are added to the ethylene glycol to obtain a first mixed solution; Provide 0.5 mL of hydrazine hydrate and a reaction vessel; The hydrazine hydrate was added to the first mixed solution and transferred to the reaction vessel. A hydrothermal reaction was carried out at 180°C for 12 hours to obtain the initial solution. The initial solution was centrifuged and dried to obtain nickel nanowires; The initial mixed solution was centrifuged to obtain the initial nickel solid; Deionized water and anhydrous ethanol are available. After washing the initial nickel solid with deionized water three times, the initial nickel solid was washed with anhydrous ethanol three times. The washed initial nickel solid was then vacuum dried at 60°C for 6 h to obtain nickel nanowires. Provide 0.2 g of multi-walled carbon nanotubes and 50 mL of concentrated nitric acid; The carbon nanotubes were added to the concentrated nitric acid, and after reflux treatment at 80°C for 4 hours, they were washed and dried to obtain acidified carbon nanotubes. Provides waterborne polyurethane emulsions; We provide a fourth solvent, dispersant, defoamer, thickener, and mixer; The adhesive, nickel nanowires, acidified carbon nanotubes, fourth solvent, polyester-based aqueous dispersant, defoamer and thickener are added to the mixer and stirred at 800 rpm for 30 min to obtain the initial composite slurry. A sand mill is provided to disperse the initial composite slurry for 2 hours to obtain a composite electromagnetic shielding slurry. The composite electromagnetic shielding slurry was coated onto a polyethylene terephthalate (PET) base film and dried at 100°C for 20 minutes to cure it.

[0049] Experiment 2: Provide 0.5 g nickel chloride hexahydrate, 0.3 g sodium hydroxide, and 40 mL ethylene glycol. The nickel chloride hexahydrate and the sodium hydroxide are added to the ethylene glycol to obtain a first mixed solution; Provide 0.5 mL of hydrazine hydrate and a reaction vessel; The hydrazine hydrate was added to the first mixed solution and transferred to the reaction vessel. A hydrothermal reaction was carried out at 180°C for 12 hours to obtain the initial solution. The initial solution was centrifuged and dried to obtain nickel nanowires; The initial mixed solution was centrifuged to obtain the initial nickel solid; Deionized water and anhydrous ethanol are available. After washing the initial nickel solid with deionized water three times, the initial nickel solid was washed with anhydrous ethanol three times. The washed initial nickel solid was then vacuum dried at 60°C for 6 h to obtain nickel nanowires. Provide 0.2 g of multi-walled carbon nanotubes and 50 mL of concentrated nitric acid; The carbon nanotubes were added to the concentrated nitric acid, and after reflux treatment at 80°C for 6 hours, they were washed and dried to obtain acidified carbon nanotubes. Provides waterborne polyurethane emulsions; We provide a fourth solvent, dispersant, defoamer, thickener, and mixer; The adhesive, nickel nanowires, acidified carbon nanotubes, fourth solvent, polyester-based aqueous dispersant, defoamer and thickener are added to the mixer and stirred at 1000 rpm for 40 min to obtain the initial composite slurry. A sand mill is provided to disperse the initial composite slurry for 2.5 hours to obtain a composite electromagnetic shielding slurry; The composite electromagnetic shielding slurry was coated onto a polyethylene terephthalate (PET) base film and dried at 100°C for 20 minutes to cure it.

[0050] Comparative Experiment 1: Provide 0.2 g of multi-walled carbon nanotubes and 50 mL of concentrated nitric acid; The carbon nanotubes were added to the concentrated nitric acid, and after reflux treatment at 80°C for 4 hours, they were washed and dried to obtain acidified carbon nanotubes. Provides waterborne polyurethane emulsions; We provide a fourth solvent, dispersant, defoamer, thickener, and mixer; The adhesive, nickel nanowires, acidified carbon nanotubes, fourth solvent, polyester-based aqueous dispersant, defoamer and thickener are added to the mixer and stirred at 800 rpm for 30 min to obtain the initial slurry; A sand mill is provided to disperse the initial composite slurry for 2 hours to obtain a composite electromagnetic shielding slurry. The composite electromagnetic shielding slurry was coated onto a polyethylene terephthalate (PET) film and then dried at 80°C for 30 minutes to cure it.

[0051] To compare the performance of the composite electromagnetic shielding slurry prepared in Experiment 1, Experiment 2, and Comparative Experiment 1, the applicant conducted corresponding performance tests. The parameters tested included X-band shielding effectiveness, sheet resistance, adhesion, and VOC (Volatile Organic Compounds) content. X-band shielding effectiveness measures the material's ability to attenuate electromagnetic waves in the 8.2–12.4 GHz frequency band, reflecting the strength of its electromagnetic shielding performance. Sheet resistance measures the conductivity of the film or coating; a lower value indicates better conductivity. Adhesion measures the bonding strength between the coating and the substrate, reflecting the mechanical reliability of the coating in actual use. VOC content measures the content of volatile organic compounds in the material, reflecting its environmental friendliness and construction safety.

[0052] The test results show that the composite electromagnetic shielding slurry prepared in Experiment 1 has a shielding effectiveness of 55.3 dB in the X-band, a sheet resistance of 2.1 Ω / sq, an adhesion of 4B, and a VOC content of <50 g / L; the composite electromagnetic shielding slurry prepared in Experiment 2 has a shielding effectiveness of 52.6 dB in the X-band, a sheet resistance of 2.8 Ω / sq, an adhesion of 4B, and a VOC content of <50 g / L; in comparison, the composite electromagnetic shielding slurry prepared in Experiment 1 has a shielding effectiveness of 28.4 dB and a sheet resistance of 8.5 dB in the X-band. Ω / sq, adhesion reaches 3B; compared with the composite electromagnetic shielding paste prepared in Experiment 1, which does not contain nickel nanowires and relies solely on the single dielectric loss mechanism of carbon nanotubes, it lacks magnetic loss contribution. The introduction of nickel nanowires provides magnetic loss, forming a conductive-magnetic synergistic loss mechanism with the dielectric loss of carbon nanotubes. At the same time, the nickel nanowires interspersed in the carbon nanotube network further enhance the connectivity of the conductive pathway, enabling the composite electromagnetic paste to achieve higher shielding effectiveness with a lower total filler content.

[0053] This invention provides a method for preparing a composite electromagnetic shielding paste, comprising providing nickel chloride hexahydrate, a first solvent, and a second solvent; adding the nickel chloride hexahydrate and the second solvent to the first solvent to obtain a first mixed solution; providing a reducing agent and a reaction vessel; adding the reducing agent to the first mixed solution and transferring it to the reaction vessel; performing a hydrothermal reaction at a first preset temperature for a first preset time to obtain an initial solution; centrifuging and drying the initial solution to obtain nickel nanowires; providing carbon nanotubes and a third solvent; and adding... The carbon nanotubes are refluxed at a second preset temperature for a second preset time, then washed and dried to obtain acidified carbon nanotubes. An adhesive is provided, and the nickel nanowires and acidified carbon nanotubes are added to the adhesive. The mixture is stirred to obtain an initial composite slurry. A sand mill is provided, and the initial composite slurry is dispersed through the sand mill to obtain a composite electromagnetic shielding slurry. By introducing nickel nanowires into the preparation of the electromagnetic shielding slurry in the above manner, the carbon nanotubes contribute dielectric loss and conduction loss, while the nickel nanowires contribute magnetic loss and enhance the connectivity of the conductive network. The resulting composite electromagnetic shielding slurry has better shielding performance.

[0054] This invention also provides a composite electromagnetic shielding slurry, which is prepared by the above-described preparation method. For the specific structure and function of the above-described preparation method, please refer to the above embodiments, which will not be repeated here.

[0055] It should be noted that while the preferred embodiments of the present invention are given in the specification and accompanying drawings, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. These embodiments are not intended to impose additional limitations on the content of the present invention; their purpose is to provide a more thorough and comprehensive understanding of the disclosure of the present invention. Furthermore, the above-described technical features can be combined with each other to form various embodiments not listed above, all of which are considered to be within the scope of the present invention specification. Moreover, those skilled in the art can make improvements or modifications based on the above description, and all such improvements and modifications should fall within the protection scope of the appended claims.

Claims

1. A method for preparing a composite electromagnetic shielding paste, characterized in that, include: Provide nickel chloride hexahydrate, a first solvent, and a second solvent; The nickel chloride hexahydrate and the second solvent are added to the first solvent to obtain a first mixed solution; Provide reducing agent and reaction vessel; The reducing agent is added to the first mixed solution and transferred to the reaction vessel. A hydrothermal reaction is carried out at a first preset temperature for a first preset time to obtain an initial solution. The initial solution was centrifuged and dried to obtain nickel nanowires; Provide carbon nanotubes and a third solvent; The carbon nanotubes are added to the third solvent, refluxed at a second preset temperature for a second preset time, and then washed and dried to obtain acidified carbon nanotubes. Provide adhesives; The nickel nanowires and acidified carbon nanotubes are added to the adhesive and stirred to obtain an initial composite slurry; A sand mill is provided to disperse the initial composite slurry to obtain a composite electromagnetic shielding slurry.

2. The preparation method according to claim 1, characterized in that, The step of adding nickel chloride hexahydrate and the second solvent to the first solvent to obtain a first mixed solution further includes: The nickel chloride hexahydrate and the second solvent are added to the first solvent, and after magnetic stirring, a first mixed solution is obtained.

3. The preparation method according to claim 1, wherein the step of adding the reducing agent to the first mixed solution and transferring it to the reaction vessel, performing a hydrothermal reaction at a first preset temperature for a first preset time to obtain an initial solution, further comprises: The reducing agent is added to the first mixed solution, and the mixture is stirred for a third preset time. The first mixed solution after stirring is transferred to a reaction vessel and subjected to a hydrothermal reaction at a first preset temperature for a first preset time to obtain the initial solution.

4. The preparation method according to claim 1, characterized in that, The step of centrifuging and drying the initial solution to obtain nickel nanowires further includes: The initial mixed solution was centrifuged to obtain the initial nickel solid; Provide first and second detergents; After washing the initial nickel solid with the first detergent, the second detergent is then added for further washing. The washed initial nickel solid was vacuum dried at a third preset temperature for a fourth preset time to obtain nickel nanowires.

5. The preparation method according to claim 4, characterized in that, The first detergent is a polar solvent, and the second detergent is an organic solvent.

6. The preparation method according to claim 1, characterized in that, The step of adding the carbon nanotubes to the third solvent, stirring and mixing at a second preset temperature for a second preset time, and then washing and drying to obtain acidified carbon nanotubes further includes: The carbon nanotubes are added to the third solvent and stirred at a second preset temperature for a second preset time to obtain initial carbon nanotubes. The initial carbon nanotubes are centrifuged and washed, and then vacuum dried at a fourth preset temperature for a fifth preset time to obtain acidified carbon nanotubes.

7. The preparation method according to claim 1, characterized in that, The step of adding the nickel nanowires and acidified carbon nanotubes to the adhesive and stirring to obtain an initial composite slurry further includes: We provide a fourth solvent, dispersant, defoamer, thickener, and mixer; The adhesive, nickel nanowires, acidified carbon nanotubes, fourth solvent, dispersant, defoamer and thickener are added to the mixer and stirred at a first preset speed for a sixth preset time to obtain an initial composite slurry.

8. The preparation method according to claim 7, characterized in that, The fourth solvent is a polar solvent.

9. The preparation method according to claim 1, characterized in that, The first solvent is a polyol solvent, the second solvent is an alkaline precipitant, the third solvent is an acidifier, and the adhesive is an aqueous film-forming resin.

10. A composite electromagnetic shielding paste, characterized in that, It is prepared by the preparation method described in any one of claims 1-9 above.