A method for preparing medical rare-earth strong magnetic materials and magnets by grain boundary diffusion
By preparing a Tb/TiN/Ti three-layer composite film on the surface of NdFeB magnets and performing a high-temperature heat treatment, the biocompatibility and corrosion resistance problems of grain boundary diffused NdFeB magnets were solved, the magnetic properties and protective layer were constructed simultaneously, the coercivity and temperature stability were improved, and the process was simplified.
Patent Information
- Application Number
- CN202611618492.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing grain boundary diffused NdFeB magnets have poor biocompatibility and insufficient corrosion resistance. The separation process between grain boundary diffusion and protective coating is lengthy, and the heavy rare earth diffusion source and the outer metal protective layer undergo severe interdiffusion during high-temperature heat treatment, resulting in the consumption and loss of the protective layer.
A Tb/TiN/Ti three-layer composite film was prepared on the surface of a NdFeB magnet by magnetron sputtering. Grain boundary diffusion and medical protective surface layer were constructed simultaneously through a single high-temperature heat treatment. The TiN isolation layer was used to prevent interdiffusion of elements, forming a Tb-Fe-B shell and a Ti protective layer.
This process achieves improved coercivity, enhanced temperature stability, high utilization of heavy rare earth elements, and yields medical-grade neodymium iron boron magnets that are both corrosion-resistant and biocompatible. The process is shortened, and the preparation of additional protective coatings is avoided.
Smart Images

Figure CN123120500A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of rare earth permanent magnet materials technology, and in particular to a method for preparing medical rare earth strong magnetic materials and magnets by grain boundary diffusion. Background Technology
[0002] Sintered neodymium iron boron (Nd-Fe-B) permanent magnets, renowned as the "King of Magnets" due to their extremely high energy product and coercivity, are widely used in new energy vehicles, wind power generation, and industrial robots. With the rapid development of minimally invasive surgery, interventional therapy, and surgical robots, the demand for Nd-Fe-B magnets in the medical device field is growing rapidly. Applications such as precision drives for surgical robots, vascular magnetic anastomosis devices, and implantable blood pump micromotors place stringent requirements on the magnetic properties, temperature stability, and biosafety of magnets.
[0003] Grain boundary diffusion technology is a mainstream technique for improving the coercivity of sintered NdFeB magnets and reducing the consumption of heavy rare earth elements. Grain boundary diffusion involves forming a heavy rare earth film on the magnet surface, followed by heat treatment, where the heavy rare earth elements diffuse along the grain boundaries into the magnet's interior, forming a core-shell structure of heavy rare earth-iron-boron in the epitaxial layer of the main phase grains. This enhances the grain anisotropy field and improves coercivity. Existing published literature extensively utilizes magnetron sputtering for grain boundary diffusion. For example, patent CN112802677B uses a spherical Nd-Tb-Cu diffusion source combined with a rotating furnace for rotary diffusion; patent CN108305772B uses R1-R2-M alloy hydride powder coating, followed by dehydrogenation before grain boundary diffusion; and patent CN113394017B uses electroplating and electrophoresis combined deposition to deposit a heavy rare earth composite film on the magnet surface. However, the research focus of these patents is primarily on improving the magnetic properties of the magnets, without addressing biocompatibility and corrosion resistance issues for medical applications.
[0004] Furthermore, existing technologies also disclose schemes for preparing multilayer thin films by magnetron sputtering for grain boundary diffusion. For example, CN114678202A discloses a three-layer sputtering structure of heavy rare earth, non-rare earth, and high-temperature resistant inorganic film. The outermost inorganic film of this scheme is made of oxides and carbides such as silicon oxide, aluminum oxide, and silicon carbide. Its function is to prevent the magnets from sticking together during the heat treatment process and to increase the amount of material in the cassette. This inorganic film is a finished film formed by sputtering and is not used to construct a medical biocompatible protective layer.
[0005] The NdFeB-rich grain boundary phase of sintered NdFeB magnets is highly chemically reactive and easily corrodes in humid environments and human bodily fluids. Corrosion products cause magnet pulverization and magnetic performance degradation. For use in medical devices that come into contact with the human body, the magnets must also meet ISO 10993 biocompatibility testing, which includes evaluation indicators such as cytotoxicity, sensitization, intradermal reaction, and acute systemic toxicity. Currently, medical-grade NdFeB magnets typically have a pyrelin protective coating deposited after grain boundary diffusion; the grain boundary diffusion process and the protective coating preparation are independent of each other, resulting in a lengthy process flow. Summary of the Invention
[0006] The purpose of this invention is to provide a method and magnet for preparing medical rare earth strong magnetic materials by grain boundary diffusion, which solves the technical problems of poor biocompatibility, insufficient corrosion resistance, and lengthy separation process between grain boundary diffusion and protective coating in existing grain boundary diffused NdFeB magnets.
[0007] Another technical problem that this invention aims to solve is that when the heavy rare earth diffusion source comes into direct contact with the outer metal protective layer, severe interdiffusion of elements occurs during high-temperature heat treatment, resulting in the loss of a large amount of outer protective metal and making it difficult to form a complete and effective protective surface layer. This invention, through a specific film structure, improves coercivity, temperature stability, and heavy rare earth utilization while simultaneously completing grain boundary diffusion and medical protective surface layer construction in a single heat treatment, thereby obtaining a medical neodymium iron boron magnet that combines magnetic properties, corrosion resistance, and biocompatibility.
[0008] To achieve the above objectives, the solution of the present invention is as follows: In a first aspect, the present invention provides a method for preparing medical rare-earth strong magnetic materials by grain boundary diffusion, comprising the following steps: S1: Pretreatment of NdFeB magnets: The sintered NdFeB blanks are processed, cleaned, and dried for later use. S2: Magnetron sputtering deposition of a three-layer composite thin film: Under vacuum conditions, a magnet coated with a three-layer composite film was obtained by sequential physical vapor deposition of a bottom Tb film, a TiN isolation layer film, and an outer Ti film on the surface of a sintered NdFeB magnet. S3, Grain boundary diffusion heat treatment: The magnet coated with a three-layer composite film is placed in a vacuum heat treatment device for high-temperature diffusion heat treatment, followed by tempering treatment, to obtain a medical rare earth strong magnet.
[0009] In a preferred embodiment, in step S1, the sintered NdFeB blank is processed to a size of 8mm×5mm×3.5mm, and then subjected to degreasing, pickling with 3~6% dilute nitric acid, water washing, and ultrasonic cleaning in sequence. The pickling removes a thickness of 3~5 mils, and the drying temperature is 55~75℃.
[0010] In a preferred embodiment, in step S2, the thickness of the bottom Tb film is 15 μm; the thickness of the TiN isolation layer film is 10 μm; and the thickness of the outer Ti film is 10 μm.
[0011] In a preferred embodiment, the vacuum degree in the high-temperature diffusion heat treatment of step S3 is 1×10⁻⁶. -2~ 1×10 -3 Pa, heat treatment temperature is 850~950℃, holding time is 5h; tempering treatment temperature is 480~550℃, holding time is 2h.
[0012] In a preferred embodiment, the entire magnetron sputtering deposition process in step S2 is carried out in a vacuum environment, and the thin film is deposited on the surface of the magnet parallel to the easy magnetization axis.
[0013] In a second aspect, the present invention provides a medical sintered neodymium iron boron permanent magnet, which is prepared by a method for preparing medical rare earth strong magnetic materials by grain boundary diffusion as described in any of the above claims; The magnet has a Tb-Fe-B shell core-shell structure formed around the main phase grains inside; a Ti protective layer is formed on the outer surface of the magnet.
[0014] After adopting the above solution, the beneficial effects of the present invention are as follows: 1. This invention uses magnetron sputtering to prepare a three-layer composite thin film of Tb / TiN / Ti from the inside out. After a single grain boundary diffusion heat treatment, the heavy rare earth grain boundary diffusion and the construction of the medical protective surface layer are completed simultaneously, eliminating the need for subsequent additional pyrelin coating and shortening the process flow. The heavy rare earth Tb diffuses into the magnet grain boundary, forming a Tb-Fe-B shell around the main phase grains, which greatly improves the coercivity, enhances the temperature stability of the magnet, and has a high utilization rate of heavy rare earth.
[0015] 2. This invention features a specially designed TiN isolation layer that inhibits interdiffusion of elements between the bottom Tb layer and the outer Ti layer during high-temperature heat treatment, preventing the loss of the outer Ti layer and thus protecting the integrity of the protective layer. This ensures that the outer Ti layer forms a dense Ti protective layer after heat treatment, and the surface Ti protective layer imparts excellent corrosion resistance and biocompatibility to the magnet, making it suitable for use in medical devices that come into contact with the human body. Attached Figure Description
[0016] Figure 1 These are SEM-EDS images of the pre-diffusion sintered NdFeB magnets in Embodiment 2 of the present invention; Figure 2 These are SEM-EDS images of the sintered NdFeB magnet after heat treatment of the grain boundary diffused Tb-TiN-Ti three-layer composite thin film in Embodiment 2 of the present invention. Figure 3 This is a photograph of the magnet's appearance after diffusion treatment in Embodiment 2 of the present invention; Figure 4 This is a cross-sectional metallographic photograph of the sample after heat treatment and annealing in Embodiment 2 of the present invention at the first observation position (the scale in the figure represents the actual length of the three measurement positions, showing the thickness of the outer Ti film). Figure 5 This is a cross-sectional metallographic photograph of the sample after heat treatment and annealing in Embodiment 2 of the present invention at the second observation position (the scale in the figure represents the actual length of the three measurement positions, showing the thickness of the outer Ti film). Figure 6 This is a comparison graph of the demagnetization curves of the embodiments of the present invention and the comparative sample. Detailed Implementation
[0017] The present invention will now be further described in conjunction with the accompanying drawings and specific embodiments.
[0018] General preparation method This invention provides a method for preparing medical rare-earth strong magnetic materials by grain boundary diffusion, comprising the following steps: S1: Pretreatment of NdFeB magnets: The sintered NdFeB blanks are processed, cleaned, and dried for later use. S2: Magnetron sputtering deposition of a three-layer composite thin film: Under vacuum conditions, a magnet coated with a three-layer composite film was obtained by sequential physical vapor deposition of a bottom Tb film, a TiN isolation layer film, and an outer Ti film on the surface of a sintered NdFeB magnet. S3, Grain boundary diffusion heat treatment: The magnet coated with a three-layer composite film is placed in a vacuum heat treatment device for high-temperature diffusion heat treatment, followed by tempering treatment, to obtain a medical rare earth strong magnet.
[0019] Example 1 Select a large blank of 54H sintered NdFeB, polish it on all six sides until it is smooth, and process it into a size of 8mm×5mm×3.5mm by multi-wire cutting; put it into a degreasing agent solution and ultrasonically clean it for 30~60s to remove oil; use 3~6% dilute nitric acid to pickle it, removing 3~5 mils of the substrate thickness; wash it with water, ultrasonically clean it, and dry it at 55~75℃ for later use.
[0020] The pretreated magnet is placed in a magnetron sputtering apparatus. Under vacuum, a Tb target is first used to deposit a Tb bottom film with a thickness of 15 μm on both sides parallel to the easy magnetization axis. Then, a TiN isolation layer film with a thickness of 10 μm is deposited. Finally, an outer Ti film with a thickness of 10 μm is deposited to obtain a three-layer composite film-coated magnet.
[0021] The coated magnet is placed in a vacuum heat treatment furnace, and the vacuum is evacuated to 1×10⁻⁶. - ³Pa; heat to 900℃ and hold for 5 hours for grain boundary diffusion; cool to 500℃ and temper for 2 hours; after processing, remove the magnet, clean and dry with ultrasonic degreasing.
[0022] Example 2 Select a large N58 sintered NdFeB blank, polish all six sides to a shine, and process it to a size of 8mm×5mm×3.5mm using multi-wire cutting; immerse it in a degreasing agent solution for ultrasonic cleaning for 30~60s to remove oil; use 3~6% dilute nitric acid for pickling to remove 3~5 mils of substrate thickness; wash with water, perform ultrasonic cleaning, and dry at 55~75℃ for later use.
[0023] The pretreated magnet is placed in a magnetron sputtering apparatus. Under vacuum, a Tb target is first used to deposit a Tb bottom film with a thickness of 15 μm on both sides parallel to the easy magnetization axis. Then, a TiN isolation layer film with a thickness of 10 μm is deposited. Finally, an outer Ti film with a thickness of 10 μm is deposited to obtain a three-layer composite film-coated magnet.
[0024] The coated magnet is placed in a vacuum heat treatment furnace, and the vacuum is evacuated to 1×10⁻⁶. - ³Pa; heat to 900℃ and hold for 5 hours for grain boundary diffusion; cool to 500℃ and temper for 2 hours; after processing, remove the magnet, clean and dry with ultrasonic degreasing.
[0025] Comparative Example 1 Select a large N58 sintered NdFeB blank, polish all six sides to a shine, and process it to a size of 8mm×5mm×3.5mm using multi-wire cutting; immerse it in a degreasing agent solution for ultrasonic cleaning for 30~60s to remove oil; use 3~6% dilute nitric acid for pickling to remove 3~5 mils of substrate thickness; wash with water, perform ultrasonic cleaning, and dry at 55~75℃ for later use.
[0026] The pretreated magnet is placed in a magnetron sputtering apparatus. Under vacuum, a Tb target is first used to deposit a Tb bottom film with a thickness of 15 μm on both sides parallel to the easy magnetization axis. Then, a TiN isolation layer film with a thickness of 5 μm is deposited. Finally, an outer Ti film with a thickness of 10 μm is deposited to obtain a three-layer composite film-coated magnet.
[0027] The coated magnet is placed in a vacuum heat treatment furnace, and the vacuum is evacuated to 1×10⁻⁶. - ³Pa; heat to 900℃ and hold for 5 hours for grain boundary diffusion; cool to 500℃ and temper for 2 hours; after processing, remove the magnet, clean and dry with ultrasonic degreasing.
[0028] Comparative Example 2 (Blank Comparative Example) Select a large N58 sintered NdFeB blank, polish all six sides to a shine, and process it to a size of 8mm×5mm×3.5mm using multi-wire cutting; immerse it in a degreasing agent solution for ultrasonic cleaning for 30~60s to remove oil; use 3~6% dilute nitric acid for pickling to remove 3~5 mils of substrate thickness; wash with water, perform ultrasonic cleaning, and dry at 55~75℃ for later use.
[0029] Only a 15 μm Tb underlayer film was deposited on the magnet surface by magnetron sputtering, without depositing a TiN isolation layer or an outer Ti film; then it was placed in a vacuum heat treatment furnace and evacuated to 1×10⁻⁶ vacuum. - ³Pa; heat to 900℃ and hold for 5 hours for grain boundary diffusion; cool to 500℃ and temper for 2 hours; after processing, remove the magnet, clean and dry with ultrasonic degreasing.
[0030] The magnetic properties, corrosion resistance, and biocompatibility of the magnets obtained in the above four embodiments were tested, and the test results are shown in Table 1.
[0031] It should be noted that the TiN isolation layer thickness in Examples 1 and 2 was 10 μm; the TiN isolation layer thickness in Comparative Example 1 was 5 μm; Comparative Example 2 was a blank comparative example that only underwent Tb grain boundary diffusion and did not deposit a TiN / Ti coating; the neutral salt spray test conditions were: temperature 35℃±2℃, NaCl brine concentration 50g / L±5g / L, pH value: 6.5~7.2; the samples of each example were subjected to biocompatibility testing according to the ISO10993 series standards, and the test results showed no cytotoxicity, no skin sensitization, no skin / mucous membrane irritation, and no acute systemic toxicity.
[0032] Table 1 Performance test results of each embodiment
[0033] As shown in Table 1, Examples 1 and 2 differ only in the content of the blank, but the increase in coercivity is slightly different, achieving the goal of synergistic improvement in magnetic properties, medical biocompatibility, and corrosion resistance. Example 2 and Comparative Example 1 use the same blank, process parameters, and operating steps, differing only in the thickness of the TiN diffusion barrier layer. While coercivity is improved, medical biocompatibility and corrosion resistance are not significantly improved. This is because the high-temperature tempering heat treatment, with its slightly thinner barrier layer, does not effectively prevent inter-element diffusion, leading to the loss of the outermost Ti film coating during high-temperature heat treatment. Comparative Example 2 does not have a TiN / Ti coating, only Tb grain boundary diffusion, resulting in improved magnetic properties, but poor corrosion resistance and biocompatibility, making it unsuitable for direct use in human contact medical devices. Therefore, the thickness and material of the diffusion composite film barrier layer after a single tempering heat treatment significantly affect its final diffusion performance.
[0034] Figure 6 This is a comparison of demagnetization curves for embodiments and comparative samples of the present invention. The black curve represents the original NdFeB magnet without grain boundary diffusion treatment; the red curve represents the magnet with only a Tb layer diffused; the blue curve represents the Tb-TiN bilayer grain boundary diffused magnet; and the green curve represents the Tb-TiN-Ti three-layer composite thin film grain boundary diffused magnet of the present invention. As can be seen from the demagnetization curves: the original magnet without diffusion treatment has the lowest coercivity; Tb grain boundary diffusion alone can improve coercivity; adding a TiN barrier layer on top of the Tb layer further improves coercivity; the magnet prepared using the Tb-TiN-Ti three-layer composite thin film single-stage heat treatment grain boundary diffusion scheme of this application achieves higher coercivity while maintaining high remanence, and the magnet exhibits the best demagnetization resistance.
[0035] In Example 2, SEM-EDS analysis was performed on the neodymium iron boron before and after diffusion. The electron microscope images show that... Figure 1 Before diffusion, the NdFeB magnets had a grain size of 3-5 μm and a thin, continuous grain boundary phase, compared to... Figure 2 Electron microscopy images of a grain boundary-diffused Tb-TiN-Ti three-layer composite film and a NdFeB magnet after a single heat treatment reveal a low-contrast, highly anisotropic TbFeB "shell" encapsulating the outer periphery of the NdFeB main phase grains. This shell acts as a pinning agent during demagnetization, making magnetization reversal difficult. This is the fundamental reason for the improved intrinsic coercivity.
[0036] Figure 3 The images show the appearance of the NdFeB magnet after a single heat treatment of the grain boundary diffused Tb-TiN-Ti three-layer composite film of Example 2. As can be seen from the appearance, a dense Ti oxide layer is formed on the surface after high-temperature grain boundary diffusion, which protects the internal NdFeB substrate from corrosion. This prevents allergies or other reactions when biological organisms come into contact with the magnet surface, thus solving the biocompatibility problem and providing a new method for improving magnetic performance and biocompatibility advantages in medical applications.
[0037] Figure 4 and Figure 5 This is a metallographic photograph of the same sample cross-section at two different observation positions after grain boundary diffusion at 900℃ and heat treatment annealing at 500℃, as described in Example 2 of this invention. The two images were collected from different regions of the sample to observe the actual thickness of the outer Ti film at different locations. The metallographic morphology shows that the outer Ti film does not melt within the heat treatment temperature range of 850~950℃ in this application. After heat treatment, the sample forms a structure of NdFeB substrate and an outer Ti oxide layer. While the thickness of the outer Ti film varies slightly at different locations, the Ti film remains continuous and intact, with clear film interfaces, and no melting or mixing damage caused by elemental interdiffusion is observed. Combined with... Figure 2 It can be seen that after heat treatment, Tb diffuses into the NdFeB main phase grains through grain boundaries, forming an outer Tb-Fe-B core-shell structure. The TiN layer acts as a barrier, inhibiting the interdiffusion between the Tb layer and the Ti layer. Tb rarely migrates outward into the outer Ti film region, ultimately resulting in a NdFeB substrate coated with a Ti oxide film.
[0038] The above description is only a preferred embodiment of the present invention and is not intended to limit the design of this case. All equivalent changes made based on the key design features of this case shall fall within the protection scope of this case.
Claims
1. A method for preparing medical rare-earth strong magnetic materials by grain boundary diffusion, characterized in that: Includes the following steps: S1: Pretreatment of NdFeB magnets: The sintered NdFeB blanks are processed, cleaned, and dried for later use. S2: Magnetron sputtering deposition of a three-layer composite thin film: Under vacuum conditions, a magnet coated with a three-layer composite film was obtained by sequential physical vapor deposition of a bottom Tb film, a TiN isolation layer film, and an outer Ti film on the surface of a sintered NdFeB magnet. S3, Grain boundary diffusion heat treatment: The magnet coated with a three-layer composite film is placed in a vacuum heat treatment device for high-temperature diffusion heat treatment, followed by tempering treatment, to obtain a medical rare earth strong magnet.
2. The method for preparing medical rare-earth strong magnetic materials by grain boundary diffusion as described in claim 1, characterized in that: In step S1, the sintered NdFeB blank is processed to a size of 8mm×5mm×3.5mm, and then subjected to degreasing, pickling with 3~6% dilute nitric acid, water washing, and ultrasonic cleaning in sequence. The pickling removes 3~5 mils of thickness, and the drying temperature is 55~75℃.
3. The method for preparing medical rare-earth strong magnetic materials by grain boundary diffusion as described in claim 1, characterized in that: In step S2, the thickness of the bottom Tb film is 15 μm; the thickness of the TiN isolation layer film is 10 μm; and the thickness of the outer Ti film is 10 μm.
4. The method for preparing medical rare-earth strong magnetic materials by grain boundary diffusion as described in claim 1, characterized in that: In the high-temperature diffusion heat treatment of step S3, the vacuum degree is 1×10⁻⁶. -2 ~1×10 -3 Pa, heat treatment temperature is 850~950℃, holding time is 5h; tempering treatment temperature is 480~550℃, holding time is 2h.
5. The method for preparing medical rare-earth strong magnetic materials by grain boundary diffusion as described in claim 1, characterized in that: The entire magnetron sputtering deposition process in step S2 is carried out in a vacuum environment, and the thin film is deposited on the surface of the magnet parallel to the easy magnetization axis.
6. A medical sintered NdFeB permanent magnet, characterized in that: The magnet is prepared by a method for preparing medical rare earth strong magnetic materials by grain boundary diffusion as described in any one of claims 1 to 5; The magnet has a Tb-Fe-B shell core-shell structure formed around the main phase grains inside; a Ti protective layer is formed on the outer surface of the magnet.
Citation Information
Patent Citations
A method for grain boundary diffusion in sintered NdFeB magnets
CN108305772B
A method for simultaneously improving the coercivity and mechanical properties of small-sized sintered NdFeB magnets
CN112802677B
A method for electroplating and electrophoresis co-deposition diffusion sintering of NdFeB
CN113394017B
NdFeB magnet grain boundary diffusion method
CN114678202A