Anode structure for seawater-based zinc-ion batteries, its preparation method and application
By forming a zinc-based alloy layer and a metal fluoride layer on the zinc current collector, the corrosion and hydrogen evolution problems of zinc-ion batteries in seawater electrolytes are solved, improving the cycle performance and lifespan of the battery, making it suitable for the field of fast-charging batteries.
Patent Information
- Application Number
- CN202611410702.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-11
- Publication Date
- 2026-11-17
AI Technical Summary
When zinc-ion batteries use seawater as the electrolyte solvent, zinc metal easily reacts with the electrolyte to generate corrosion byproducts, leading to negative electrode corrosion, zinc dendrite growth, and hydrogen evolution side reactions, which affect battery performance. In particular, ions in seawater have an adverse effect on battery performance, causing electrode interface instability and rapid degradation.
A zinc-based alloy layer and a metal fluoride layer are formed on a zinc current collector. The alloy layer has a three-dimensional porous structure, while the metal fluoride layer has a dense structure. The process is carried out by electroplating and vacuum evaporation. The alloy layer has a high hydrogen evolution overpotential and good conductivity, while the metal fluoride layer has hydrophobicity and uniform nucleation sites, which inhibits corrosion and hydrogen evolution reaction.
It improves the cycle performance and long cycle life of zinc-ion batteries, especially significantly improving performance under high-rate conditions, reducing battery impedance and nucleation overpotential, inhibiting zinc dendrite growth and electrode corrosion, and extending battery life.
Smart Images

Figure CN123120600A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of aqueous zinc-ion battery technology, specifically relating to a negative electrode structure for seawater-based aqueous zinc-ion batteries, its preparation method and application. Background Technology
[0002] Zinc-ion batteries have advantages such as high theoretical specific capacity, suitable redox potential, high conductivity, high safety, low toxicity, and low cost, making them a promising candidate for large-scale energy storage.
[0003] Aqueous zinc-ion batteries typically use deionized water as the electrolyte, which is usually prepared by desalinating freshwater. In contrast, natural seawater, which accounts for approximately 96.5% of the Earth's total water volume, possesses high conductivity and is a highly promising material rich in electrolytes. Directly using seawater as the electrolyte solvent could further reduce costs and enable large-scale energy storage. However, zinc is chemically reactive and readily reacts with the electrolyte during battery charging and discharging, generating corrosion byproducts that can lead to negative electrode corrosion, zinc dendrite growth, and hydrogen evolution side reactions. Especially when using seawater as the electrolyte solvent for zinc-ion batteries, the sodium content in the seawater... + K + Ca 2+ Mg 2+ SO4 2- Cl - Plasma can adversely affect battery performance in terms of ion migration, adsorption, diffusion and electrode corrosion. Higher concentrations of chloride ions exacerbate electrode corrosion and hydrogen evolution, ultimately leading to electrode interface instability and rapid degradation of battery performance. Summary of the Invention
[0004] To solve all or part of the above-mentioned technical problems, the present invention provides the following technical solutions: A first aspect of the present invention provides a negative electrode structure for a seawater-based zinc-ion battery, comprising a current collector, the current collector being made of zinc; and further comprising an alloy layer and a metal fluoride layer sequentially formed on the current collector in the thickness direction; The alloy layer comprises zinc and a first metal, the first metal comprising one or more of indium, tin, copper, manganese, and nickel; the metal fluoride layer comprises one or more of NaF, CaF2, and ZnF2; the alloy layer has a three-dimensional porous structure, and the porosity of the metal fluoride layer is less than that of the alloy layer.
[0005] This invention first forms a zinc-based alloy layer on the surface of a zinc current collector. The first metal alloyed with zinc has a high hydrogen evolution overpotential and good conductivity, which can reduce battery impedance and nucleation overpotential, promote the adsorption, migration, and deposition of zinc ions, inhibit pitting corrosion of Cl elements in seawater and hydrogen evolution reactions during battery cycling, and the alloying can enhance the mechanical strength of the negative electrode. Then, a dense metal fluoride layer is formed on the alloy layer. On the one hand, this metal fluoride layer is hydrophobic, which can inhibit the decomposition and corrosion of water molecules on the negative electrode surface, isolate seawater-based electrolyte erosion, and reduce interfacial side reactions and corrosion byproducts. On the other hand, it can also provide uniform nucleation sites for zinc ion deposition and inhibit zinc dendrite growth. The inner alloy layer is designed as a three-dimensional porous structure, while the outer metal fluoride layer is designed as a denser structure with a lower porosity than the alloy layer. This allows it to both physically repel Cl ions to inhibit pitting corrosion and retain the advantage of the three-dimensional structure in homogenizing the electric field.
[0006] In some embodiments, the porosity of the alloy layer is 5% to 45%.
[0007] In some embodiments, the porosity of the metal fluoride layer is less than 5%, for example, greater than or equal to 1% and less than 5%.
[0008] In some embodiments, the thickness of the alloy layer is 5µm-20µm.
[0009] In some embodiments, the thickness of the metal fluoride layer is 100 nm to 2 µm.
[0010] In some embodiments, the atomic percentage of zinc in the alloy layer is 50-90 at.%, and the atomic percentage of the first metal is 10-50 at.%.
[0011] In some embodiments, the surface of the negative electrode structure has a three-dimensional structure with a surface roughness Ra of 0.35-0.55. The three-dimensional structure is preserved after a metal fluoride layer is formed on the three-dimensional porous alloy layer.
[0012] In some embodiments, the alloy layer is formed by electroplating. Electroplating can form an alloy layer with a three-dimensional porous structure.
[0013] In some embodiments, the metal fluoride layer is formed by vacuum evaporation. Vacuum evaporation can form a dense metal fluoride layer without damaging the three-dimensional structure.
[0014] In a preferred embodiment, the surface of the negative electrode structure for the seawater-based zinc-ion battery has a three-dimensional structure, and its surface roughness R aThe porosity is 0.35~0.55, and the metal fluoride layer is a dense outer layer formed by vacuum evaporation on an alloy layer with a three-dimensional porous structure; the porosity of the alloy layer is 5%~45%, and the porosity of the metal fluoride layer is greater than or equal to 1% and less than 5%.
[0015] In a more preferred embodiment, the first metal is indium and / or tin, and the metal fluoride layer is a ZnF2 layer; the porosity of the alloy layer is 5%~45%, the porosity of the ZnF2 layer is greater than or equal to 1% and less than 5%, and the negative electrode surface retains a three-dimensional structure after the ZnF2 layer is formed, with a surface roughness R a The ZnF2 layer is 0.35~0.55. The ZnF2 layer is formed by controlled vacuum evaporation to obtain a relatively dense outer layer without destroying the three-dimensional structure of the inner alloy.
[0016] A second aspect of the present invention provides a method for preparing a negative electrode structure for a seawater-based aqueous zinc-ion battery, comprising: A current collector is provided, wherein the material of the current collector includes zinc; An alloy layer is formed on the current collector by electroplating to obtain an intermediate material; wherein the alloy layer comprises zinc and a first metal, the first metal comprising one or more combinations of indium, tin, copper, manganese, and nickel; A metal fluoride layer is formed on the alloy layer by vacuum evaporation. The metal fluoride layer includes one or more combinations of NaF, CaF2, and ZnF2 to obtain a negative electrode structure for seawater-based zinc-ion batteries.
[0017] The alloy layer formed by electroplating has good three-dimensional porous characteristics, while the metal fluoride layer formed by vacuum evaporation is relatively dense. Moreover, since the thickness of vacuum evaporation is controllable, the evaporated metal fluoride layer will not destroy the three-dimensional structure, so that the final negative electrode surface still retains a certain three-dimensional structure.
[0018] In some embodiments, the electroplating method specifically includes: using the current collector as the working electrode, placing it and the counter electrode in an electroplating solution, and performing electroplating under constant current or constant pressure conditions.
[0019] In some embodiments, the zinc ion concentration in the electroplating solution is 0.1 mol / L. -1 ~1 mol L -1 The concentration of the first metal ion is 0.1 mol L. -1 ~1 mol L -1 .
[0020] In some embodiments, the source of the first metal ion includes a salt containing the first metal, including one or more of indium salts, tin salts, copper salts, manganese salts, and nickel salts. The indium salt includes, but is not limited to, indium sulfate, indium chloride, and indium nitrate; the tin salt includes, but is not limited to, stannous chloride, stannous sulfate, and sodium stannate; the copper salt includes, but is not limited to, copper sulfate, copper chloride, and copper nitrate; the manganese salt includes, but is not limited to, manganese acetate, manganese sulfate, manganese chloride, and manganese nitrate; and the nickel salt includes, but is not limited to, nickel sulfate, nickel chloride, nickel acetate, and nickel nitrate.
[0021] In some embodiments, the electroplating method is performed under constant current conditions, with a current of 0.01 A cm⁻¹. -2 ~1 A cm -2 The deposition time is 5 min to 30 min.
[0022] In some embodiments, ultrasonic waves and / or stirring are used as auxiliary methods during the electroplating process.
[0023] In some embodiments, the frequency of the ultrasonic wave is 20~100 kHz.
[0024] In some embodiments, the stirring speed is 50~150 r / min. -1 .
[0025] In some embodiments, the temperature of the electrolyte is controlled to be between room temperature and 40°C during the electroplating process.
[0026] In some embodiments, the electroplating solution further includes additives, which include one or more combinations of polyethylene glycol, sodium citrate, sodium dodecyl sulfate, disodium ethylenediaminetetraacetate, boric acid, ascorbic acid, oxalic acid, citric acid, hydroquinone, and thiourea, wherein the volume molar ratio of the additive to zinc ions is 1:1 to 2:1.
[0027] In some embodiments, the solvent of the electroplating solution includes one or more combinations of water, ethylene glycol, acetone, and propylene glycol.
[0028] In some embodiments, the vacuum evaporation includes: evaporating the evaporation chamber to a vacuum level of 1×10⁻⁶. -6 Below Pa, a protective atmosphere is then introduced, and the evaporation voltage is controlled at 0.85~1.2 V, and the temperature at 35~60 ℃; the first stage evaporation and the second stage evaporation are performed sequentially, with the first stage at a evaporation rate of 1~2 Å s. -1 The evaporation rate is used to deposit the fluoride layer to 10%–30% of its total thickness, followed by a second stage at 3–6 Å s⁻¹. -1 The evaporation rate continues to deposit to the target thickness; after the evaporation is complete, heating is stopped, and the evaporation chamber is evacuated to 5×10⁻⁶. -4Below Pa, vacuum heat treatment is carried out at 35~60 ℃ for 10~30 min.
[0029] In a preferred embodiment, the vacuum evaporation method employs the following combination of process conditions: The intermediate structure is placed in the substrate tray of the vapor deposition chamber, with the distance between the substrate stage and the evaporation source being 25-40 mm, and the substrate stage is rotated at 20-40 rpm. During the vapor deposition process, the substrate temperature is controlled to maintain the substrate temperature at 35-60℃ to reduce local deposition differences caused by temperature fluctuations during the vapor deposition process. The metal fluoride was placed in a tungsten boat, facing the substrate stage, and the evaporation chamber was evacuated to 1×10⁻⁶. -6 Below Pa, Ar gas is then introduced; the evaporation voltage is slowly increased until the tungsten boat glows slightly red for preheating; Metal fluorides are deposited using a staged evaporation rate: the first stage uses 1–2 Å / s. -1 The first stage uses a low evaporation rate to form a continuous nucleation layer with a target film thickness of 10%–30%; the second stage adjusts the evaporation rate to 3–6 Å / s. -1 The deposition continues until the target thickness is reached. Through a "low-speed nucleation-medium-speed growth" method, a continuous coating of metal fluoride is first established along the three-dimensional porous alloy surface, followed by the completion of subsequent film growth. The total thickness of the formed metal fluoride layer is controlled to be 100 nm to 2 µm, and its porosity is greater than or equal to 1% and less than 5%. After the metal fluoride layer is formed under the above combined conditions, the negative electrode surface still retains a three-dimensional structure and the surface roughness Ra is 0.35 to 0.55. After the vapor deposition is completed, stop heating the evaporation source and evaporate the vapor deposition chamber again to a vacuum level not exceeding 5 × 10⁻⁶. -4 The sample is then subjected to vacuum insulation at 35–60 °C for 10–30 min after evaporation. Subsequently, it is cooled to no higher than 30 °C under vacuum or Ar protection before being removed. Vacuum insulation after evaporation is used to alleviate internal stress in the film layer, improve the stability of the interface between the film layer and the alloy layer, and reduce the risk of microcracks or local warping caused by rapid cooling without introducing air and moisture.
[0030] In the preferred embodiment described above, vacuum evaporation is not only used to form the outer layer, but also, through a combination of controlled vacuum level, distance between the substrate stage and the evaporation source, substrate stage rotation, evaporation source preheating, evaporation voltage, evaporation rate, and evaporation thickness, to maintain a low porosity in the metal fluoride layer and avoid damaging the three-dimensional porous alloy layer formed by electroplating, thereby obtaining an ordered hierarchical interface of "inner three-dimensional porous alloy layer / outer relatively dense metal fluoride layer". Specifically, the controlled substrate temperature and low-speed nucleation stage are beneficial to improving the conformal coverage and initial adhesion of metal fluorides on the three-dimensional porous alloy surface; the subsequent higher evaporation rate is used to complete the continuous film growth and reduce the long-term heating of the substrate; and the vacuum insulation after evaporation is beneficial to alleviate film stress and improve interface stability. Thus, a more continuous and denser metal fluoride outer layer can be obtained while preserving the inner three-dimensional structure as much as possible, which is different from the ordinary coating layer obtained by simply using conventional constant-rate evaporation in terms of process formation mechanism.
[0031] Vacuum evaporation can precisely control the formation of a uniform, dense, and thickness-controllable metal fluoride layer on the surface of zinc metal without disrupting the three-dimensional structure created by electroplating. It allows for precise control of the thickness and composition of the metal fluoride layer at the microscale, avoiding problems such as uneven thickness and poor interlayer adhesion inherent in existing coating technologies, or inconsistencies in morphology and bulk phase that may occur with smelting and rolling methods. Therefore, vacuum evaporation ensures the uniformity and stability of the metal fluoride layer, further enhancing its performance during long-term cycling, and requires only a thin artificial interface to achieve corrosion resistance, dendrite suppression, and hydrogen evolution inhibition.
[0032] The preparation method described in the second aspect of this invention can be used to prepare the negative electrode structure for seawater-based aqueous zinc-ion batteries described in the first aspect of this invention.
[0033] A third aspect of the present invention provides a negative electrode structure for a seawater-based aqueous zinc-ion battery, which is prepared by the preparation method described in any of the technical solutions.
[0034] A fourth aspect of the present invention provides a seawater-based aqueous zinc-ion battery, comprising a positive electrode, a negative electrode, an electrolyte, and a separator, wherein the negative electrode is a negative electrode structure for a seawater-based aqueous zinc-ion battery as described in any of the technical solutions; and the dissolving medium for dissolving zinc salts in the electrolyte includes seawater.
[0035] Seawater-based zinc-ion batteries based on this negative electrode structure exhibit excellent cycle performance and long cycle life, especially with significant improvements in cycle performance under high-rate conditions, making them suitable for the fast-charging battery field.
[0036] In some embodiments, the seawater is clarified seawater obtained by filtering natural seawater to remove solid impurities. The seawater-based electrolyte used only requires simple filtration of the seawater, reducing the overall cost of the battery and conserving freshwater resources.
[0037] In some embodiments, the zinc salt includes one or more combinations of zinc sulfate, zinc chloride, zinc perchlorate, zinc acetate, zinc phosphate, zinc trifluoromethanesulfonate, and zinc borate.
[0038] The positive electrode and separator of the seawater-based zinc-ion battery can be made of suitable materials known in the art, such as vanadium-based positive electrode materials (e.g., NH4V4O). 10 The membrane is made of one or more of the following: V2O5, manganese-based cathode (e.g., MnO2) or Prussian blue, and the membrane is made of glass fiber membrane GF / D.
[0039] Compared with existing technologies, the present invention has some or all of the following beneficial effects: First, a zinc-based alloy layer is formed on the surface of the zinc current collector. The first metal alloyed with zinc has a high hydrogen evolution overpotential and good conductivity, which can reduce battery impedance and nucleation overpotential, promote the adsorption, migration, and deposition of zinc ions, inhibit pitting corrosion of Cl elements in seawater, suppress hydrogen evolution reactions during battery cycling, and the alloying can enhance the mechanical strength of the negative electrode. Then, a metal fluoride layer is formed on the alloy layer. On the one hand, this metal fluoride layer is hydrophobic, which can inhibit the decomposition and corrosion of water molecules on the negative electrode surface, isolate seawater-based electrolyte erosion, and reduce interfacial side reactions and corrosion byproducts. On the other hand, it can also provide uniform nucleation sites for zinc ion deposition and inhibit zinc dendrite growth. The alloy layer formed by electroplating has a three-dimensional porous structure, while the metal fluoride layer formed by vacuum evaporation has a denser structure with a lower porosity than the alloy layer. The resulting negative electrode structure can both physically repel Cl ions to inhibit pitting corrosion and retain the advantages of a three-dimensional structure that homogenizes the electric field. Attached Figure Description
[0040] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0041] Figure 1 This is a scanning electron microscope image of the InZn-ZnF2@Zn anode structure prepared in Example 1; Figure 2 This is a scanning electron microscope image of the SnZn-ZnF2@Zn anode structure prepared in Example 6; Figure 3 The image shows the XRD pattern of the negative electrode structure of Example 1 after immersion in seawater for 10 days. Figure 4The image shows the XRD pattern of the negative electrode structure of Comparative Example 1 after immersion in seawater for 10 days. Figure 5 For a symmetrical battery based on the negative electrode structure of Example 1 and Comparative Example 1, at a current density of 1 mA cm⁻¹ 2 Area capacity is 1 mAh cm 2 Figure showing the results of constant current charge-discharge test under the specified conditions; Figure 6 For the full cell based on the negative electrode structure of Example 1 and Comparative Example 1, at 5 A g -1 Cyclic performance curves under charge-discharge tests at current density; Figure 7 The rate performance curves of the full cell based on the negative electrode structure of Example 1 and Comparative Example 1 are shown. Figure 8 For the symmetrical battery based on the negative electrode of Example 6 and Comparative Example 1, at a current density of 1 mA cm⁻¹ 2 The surface area capacity is 1mAh cm 2 The results of constant current charge-discharge test under the specified conditions are shown in the figure. Detailed Implementation
[0042] The invention will be more fully understood through the following detailed description. The detailed embodiments disclosed herein are merely illustrative, and the invention may be embodied in various forms. Therefore, the specific functional details disclosed herein should not be construed as limiting, but rather as the basis for the claims and as a representative basis for teaching those skilled in the art.
[0043] In addition, unless otherwise specified, all raw materials used in the following embodiments can be purchased from the market or other sources, and all production and testing equipment used are known in the art, as are the testing methods used.
[0044] Example 1 This embodiment provides a negative electrode structure for seawater-based aqueous zinc-ion batteries and its preparation method, including the following steps: (1) Preparation of electroplating solution: The solvent of the electroplating solution is deionized water and ethylene glycol in a volume ratio of 1:1. Add 1 mol L to it. -1 Zinc sulfate heptahydrate (ZnSO4·7H2O), 0.01 mol L -1 Anhydrous indium sulfate (InSO4), 0.6 mol L -1 Sodium ethylenediaminetetraacetate (C 10 H 14 N2Na2O8), 0.4 mol L-1 Sodium citrate dihydrate (C6H5Na3O7) Add 2H2O and stir at room temperature until the electroplating solution becomes clear.
[0045] (2) A clean zinc current collector was used as the working electrode and placed in the electroplating solution together with the Pt counter electrode. A DC power supply was applied to the working electrode and the counter electrode, and constant current electrodeposition was performed with the aid of ultrasonic treatment. The current was set to 0.01 Acm. -2 The ultrasonic frequency was 20 kHz and the deposition time was 10 min to form an InZn binary alloy layer with a thickness of 5 μm on the zinc current collector. After deposition, the obtained intermediate structure was taken out of the electrolytic cell, soaked in deionized water and rinsed repeatedly, and then dried at room temperature.
[0046] (3) Place the intermediate structure obtained in step (2) into the substrate tray of the evaporation chamber. The distance from the substrate stage to the evaporation source is 25 mm, the substrate stage rotation speed is 20 rpm, and the vacuum is evacuated to 1×10⁻⁶ rpm. -6 Pa, then Ar gas was added to create a positive pressure. ZnF2 was selected as the evaporation material, and dual-source evaporation was performed in a crucible. Dual-source evaporation ensures uniformity and avoids uneven evaporation thickness due to the distance between the evaporation sources. At a voltage of 0.85 V, the initial evaporation was performed at 1 Å s. -1 The average evaporation rate was adjusted to achieve an evaporation thickness of 20 nm, and then the evaporation rate was adjusted to 3 Å / s. - 1. Continue deposition until the total thickness reaches 100 nm; after evaporation, re-evacuate to a vacuum level not exceeding 5 × 10⁻⁶. - 4 Pa was steamed at 50 °C for 20 min and then vacuum-insulated, followed by cooling under Ar protection to a temperature not exceeding 30 °C to obtain a negative electrode structure for seawater-based aqueous zinc-ion batteries (denoted as InZn-ZnF2@Zn).
[0047] (4) Take the negative electrode structure obtained by vapor deposition out of the vapor deposition chamber and cut it into 1cm×1cm negative electrode sheets at room temperature.
[0048] Examples 2-5 Examples 2-5 are basically the same as Example 1, except that the first metal ion source is varied according to Table 1 to form different binary alloy layers, and / or the vapor deposition material is varied according to Table 1. The rest are the same as in Example 1, and will not be described again here.
[0049] Table 1. Composition of binary alloy layer and metal fluoride layer in Examples 1-5 Example 6 This embodiment provides a negative electrode structure for seawater-based aqueous zinc-ion batteries and its preparation method, including the following steps: (1) Preparation of electroplating solution: The solvent of the electroplating solution is deionized water and ethylene glycol in a volume ratio of 1:1. Add 0.1 mol L to it. -1 Zinc sulfate heptahydrate (ZnSO4·7H2O), 0.1 mol L -1 Stannous sulfate (SnSO4), 0.06 mol L -1 Sodium ethylenediaminetetraacetate (C 10 H 14 N2Na2O8), 0.04 mol L -1 Sodium citrate dihydrate (C6H5Na3O7) Add 2H2O and stir at room temperature until the electroplating solution becomes clear.
[0050] (2) A clean zinc current collector is used as the working electrode and placed in the electroplating solution together with the counter electrode. A DC power supply is applied to the working electrode and the counter electrode, and constant current electrodeposition is used with auxiliary ultrasonic treatment. The current is set to 1 A cm⁻¹. -2 The ultrasonic frequency was 50 kHz and the deposition time was 20 min to form a SnZn binary alloy layer with a thickness of 15 μm on the zinc current collector. After deposition, the obtained intermediate structure was taken out of the electrolytic cell, soaked in deionized water and rinsed repeatedly, and then dried at room temperature.
[0051] (3) Place the intermediate structure obtained in step (2) into the substrate tray of the evaporation chamber. The distance from the substrate stage to the evaporation source is 35 mm, the substrate stage rotation speed is 30 rpm, and the vacuum is evacuated to 1×10⁻⁶ rpm. -6 Pa, then Ar gas was added to create a positive pressure. ZnF2 was selected as the evaporation material, and dual-source evaporation was performed in a crucible. At a voltage of 1.2 V, the evaporation was first carried out at 1.5 Å s. -1 The average evaporation rate was adjusted to reach an evaporation thickness of 30 nm, and then the evaporation rate was adjusted to 6 Å s. - 1. Continue deposition until the total thickness reaches 150 nm; after evaporation, re-evacuate to a vacuum level not exceeding 5 × 10⁻⁶. -4 Pa was subjected to evaporation at 50 °C for 20 min followed by vacuum holding, and then cooled to no higher than 30 °C under Ar protection. A ZnF2 layer with a thickness of 150 nm was formed on the SnZn binary alloy layer to obtain a negative electrode structure for seawater-based zinc-ion batteries (denoted as SnZn-ZnF2@Zn).
[0052] (4) Take the negative electrode structure obtained by vapor deposition out of the vapor deposition chamber and cut it into 1cm×1cm negative electrode sheets at room temperature.
[0053] Example 7 This embodiment provides a negative electrode structure for seawater-based aqueous zinc-ion batteries and its preparation method, including the following steps: (1) Preparation of electroplating solution: The electroplating solution solvent is deionized water and ethylene glycol in a volume ratio of 1:1. Add 0.2 mol L to it. -1 Zinc sulfate heptahydrate (ZnSO4·7H2O), 0.05 mol L -1 Copper sulfate pentahydrate (CuSO4·5H2O), 0.1 mol / L -1 Sodium ethylenediaminetetraacetate (C 10 H 14 N2Na2O8), 0.02 mol L -1 Polyethylene glycol, 0.04 mol L -1 Hydroquinone, heat the electroplating solution to 30 ℃, and stir until the electroplating solution is clear.
[0054] (2) A clean zinc current collector is used as the working electrode and placed in the electroplating solution together with the counter electrode. A DC power supply is applied to the working electrode and the counter electrode, and deposition is carried out under constant current conditions with the assistance of magnetic stirring. The current is set to 1 A cm⁻¹. -2 The deposition time was 5 min to form a 20 μm thick CuZn binary alloy layer on the zinc current collector. After deposition, the obtained intermediate structure was removed from the electrolytic cell, soaked in deionized water and rinsed repeatedly, and then air-dried at room temperature.
[0055] (3) Place the intermediate structure obtained in step (2) into the substrate tray of the evaporation chamber. The distance from the substrate stage to the evaporation source is 40 mm, the substrate stage rotation speed is 40 rpm, and the vacuum is evacuated to 1×10⁻⁶ rpm. -6 Pa, then Ar gas was added to create a positive pressure. NaF was selected as the evaporation material, and dual-source evaporation was performed in crucibles. At a voltage of 1.0 V, the evaporation was first carried out at 1.2 Å s. -1 Evaporation was carried out at an average rate until the evaporation thickness reached 100 nm, and then the evaporation rate was adjusted to 5 Å s. - 1. Continue deposition until the total thickness is 2 μm; after evaporation, re-evacuate to a vacuum level not exceeding 5 × 10⁻⁶. -4 Pa was subjected to evaporation at 50 °C for 20 min followed by vacuum holding, and then cooled to no higher than 30 °C under Ar protection. A NaF layer with a thickness of 2 μm was formed on the CuZn binary alloy layer to obtain a negative electrode structure for seawater-based zinc-ion batteries (denoted as CuZn-NaF@Zn).
[0056] (4) Take the negative electrode structure obtained by vapor deposition out of the vapor deposition chamber and cut it into 1cm×1cm negative electrode sheets at room temperature.
[0057] Example 8 This embodiment provides a negative electrode structure for seawater-based aqueous zinc-ion batteries and its preparation method, including the following steps: (1) Preparation of electroplating solution: The electroplating solution solvent is deionized water and ethylene glycol in a volume ratio of 1:1. Add 0.5 mol L to it. -1 Zinc sulfate heptahydrate (ZnSO4·7H2O), 0.05 mol L -1 Nickel sulfate hexahydrate (NiSO4) 6H2O), 0.25 mol L -1 Sodium ethylenediaminetetraacetate (C 10 H 14 N2Na2O8), 0.02 mol L -1 Boric acid (H3BO3), 0.25 mol L -1 Sodium citrate dihydrate (C6H5Na3O7) 2H2O) is used to heat the electroplating solution to 40 ℃.
[0058] (2) A clean zinc current collector was used as the working electrode and placed in the electroplating solution together with the counter electrode. A DC power supply was then applied to the working electrode and the counter electrode, and electrodeposition was performed under constant current conditions with the assistance of magnetic stirring. The current was set to 1.2 A cm⁻¹. -2 The stirring speed is 50 r / min. -1 The deposition time was 40 min to form a 10 μm thick NiZn layer on the zinc current collector. After deposition, the obtained intermediate structure was removed from the electrolytic cell, soaked in deionized water and rinsed repeatedly, and then air-dried at room temperature.
[0059] (3) Place the intermediate structure obtained in step (2) into the substrate tray of the evaporation chamber. The distance from the substrate stage to the evaporation source is 30 mm, the substrate stage rotation speed is 10 rpm, and the vacuum is evacuated to 1×10⁻⁶ rpm. -6 Pa, then Ar gas was added to create a positive pressure. NaF was selected as the evaporation material, and dual-source evaporation was performed in crucibles. At a voltage of 1.2 V, the evaporation was first carried out at 2 Å s. -1 The average evaporation rate was adjusted to a thickness of 20 nm, and then the evaporation rate was further adjusted to 6 Å s. - 1. Continue deposition until the total thickness reaches 150 nm; after evaporation, re-evacuate to a vacuum level not exceeding 5 × 10⁻⁶. -4 Pa was subjected to evaporation at 50 °C for 20 min followed by vacuum holding, and then cooled to no higher than 30 °C under Ar protection. A NaF layer with a thickness of 150 nm was formed on the NiZn layer to obtain a negative electrode structure for seawater-based zinc-ion batteries (denoted as NiZn-NaF@Zn).
[0060] (4) Take the negative electrode structure obtained by vapor deposition out of the vapor deposition chamber and cut it into 1cm×1cm negative electrode sheets at room temperature.
[0061] Example 9 This embodiment provides a negative electrode structure for seawater-based aqueous zinc-ion batteries and its preparation method, including the following steps: (1) Preparation of electroplating solution: The electroplating solution solvent is deionized water and ethylene glycol in a volume ratio of 1:1. Add 0.2 mol L to it. -1 Zinc sulfate heptahydrate (ZnSO4·7H2O), 0.03 mol L -1 Bismuth nitrate (BiNO3), 0.06 mol L -1 Sodium ethylenediaminetetraacetate (C 10 H 14 N2Na2O8), 0.02 mol L -1 Boric acid (H3BO3), 0.2 mol L -1 Sodium citrate dihydrate (C6H5Na3O7) Heat the electroplating solution to 40 °C using 2H2O and stir until the solution becomes clear.
[0062] (2) A clean zinc current collector is used as the working electrode and placed in the electroplating solution together with the counter electrode. A DC power supply is applied to the working electrode and the counter electrode, and electrodeposition is performed under constant current conditions with the assistance of magnetic stirring. The current is set to 1.6 A cm⁻¹. -2 The deposition time was 40 min to form a 15 μm thick BiZn layer on the zinc current collector. After deposition, the obtained intermediate material was removed from the electrolytic cell, soaked in deionized water and rinsed repeatedly, and then air-dried at room temperature.
[0063] (3) Place the intermediate material obtained in step (2) into the substrate tray of the evaporation chamber. The distance from the substrate stage to the evaporation source is 30 mm, the substrate stage rotation speed is 30 rpm, and the vacuum is evacuated to 1×10⁻⁶ rpm. -6 Pa, then Ar gas was added to create a positive pressure. CaF2 was selected as the evaporation material, and dual-source evaporation was performed in a crucible. At a voltage of 1.0 V, the evaporation was first carried out at 1.5 Å s. -1 The average evaporation rate was adjusted to a thickness of 50 nm, and then the evaporation rate was further adjusted to 4 Å s. -1 Continue deposition until a total thickness of 500 nm is achieved; after evaporation, vacuum is applied again to a depth not exceeding 5 × 10⁻⁶ nm. -4 The electrode was subjected to evaporation at 50 °C for 20 min followed by vacuum holding, and then cooled to no higher than 30 °C under Ar protection. The resulting evaporation layer was 500 nm thick, yielding a negative electrode structure for seawater-based zinc-ion batteries (denoted as BiZn-CaF2@Zn).
[0064] (4) Take the negative electrode structure obtained by vapor deposition out of the vapor deposition chamber and cut it into 1cm×1cm negative electrode sheets at room temperature.
[0065] Comparative Example 1 Comparative Example 1 uses pure zinc foil directly as the negative electrode of a seawater-based zinc-ion battery.
[0066] Comparative Example 2 The only difference between Comparative Example 2 and Example 1 is that Comparative Example 2 does not perform step (2), that is, the negative electrode of Comparative Example 2 is a structure in which a ZnF2 layer is directly deposited on a zinc current collector. The rest is the same as in Example 1, and will not be described again here.
[0067] Comparative Example 3 The only difference between Comparative Example 3 and Example 1 is that Comparative Example 3 does not perform step (3), that is, the negative electrode of Comparative Example 3 has only an InZn binary alloy layer formed by electroplating on the zinc current collector. The rest is the same as that of Example 1, and will not be described again here.
[0068] Comparative Example 4 Comparative Example 4 uses a vacuum evaporation method to simultaneously deposit a first metal and a metal fluoride layer on a zinc current collector, obtaining a modified layer with a uniform composite of the first metal and metal fluoride layers. The specific steps include: The cleaned Zn wafer was placed in the substrate tray of the evaporation chamber. The distance between the substrate stage and the evaporation source was 35 mm, and the substrate stage rotated at 40 rpm. The vacuum was then evacuated to 1×10⁻⁶. -6 Pa, then Ar gas was introduced to create a positive pressure. In metal particles and ZnF2 were selected as evaporation materials and placed in separate crucibles for dual-source evaporation, under a voltage of 1.0 V and a evaporation time of 1.5 Å s. -1 The average rate of evaporation is used to form a 2 μm thick In metal and ZnF2 mixed modification layer on the Zn surface, thereby obtaining a negative electrode structure for seawater-based zinc-ion batteries (denoted as In-ZnF2@Zn).
[0069] Comparative Example 5 Comparative Example 5 uses a magnetron sputtering method to simultaneously deposit a mixed layer of a first metal and a metal fluoride on a zinc current collector, obtaining a modified layer in which the first metal and metal fluoride layers are uniformly mixed. The specific steps include: High-purity zinc foil (50 μm thick, purity ≥99.99%) is first cut to the required size, then ultrasonically cleaned with anhydrous ethanol and deionized water for 10 min each, and then dried in a vacuum drying oven at 60 ℃ for 12 h for later use.
[0070] The treated zinc foil was fixed on a magnetron sputtering sample stage. Using a high-purity In target (99.99%) and a ZnF2 target (99.99%) as sputtering sources, an In-ZnF2 composite interface layer was constructed on the zinc foil surface via dual-target RF magnetron co-sputtering. Before sputtering, the cavity was evacuated to a base vacuum of 6.0 × 10⁻⁶. -4 The working pressure was adjusted to 0.45 Pa by introducing high-purity Ar gas (99.999%). During sputtering, the target-substrate distance was maintained at 10 cm, the substrate temperature was controlled at 25-30 °C, and the stage rotation speed was set to 16 rpm. The In and ZnF2 targets were driven by RF power supplies, with the In target power at 60 W and the ZnF2 target power at 20 W. The total deposition time was 3 min. After deposition, the substrate was allowed to cool naturally to room temperature, resulting in a zinc anode with a uniform In-ZnF2 mixed layer on its surface. The thickness of the resulting interface layer was approximately 80-150 nm, denoted as In+ZnF2@Zn.
[0071] Using the negative electrode sheets from the above embodiments and comparative examples, zinc-ion symmetric batteries, asymmetric batteries, and full batteries are assembled. Taking the negative electrode sheet of Example 1 as an example, the battery assembly steps are as follows: Assembly of symmetrical cells: The prepared negative electrode InZn-ZnF2@Zn was used as both the positive and negative electrodes of a coin cell. A glass fiber GF / D separator was used, and seawater was selected as the solvent to prepare a solution containing 2 mol L... -1 The electrolyte of ZnSO4 is placed in the battery case under normal conditions (no need for anhydrous and oxygen-free environment) to assemble a symmetrical battery, which is marked as InZn-ZnF2@Zn / / InZn-ZnF2@Zn symmetrical battery.
[0072] Assembly of asymmetric cells: The prepared zinc negative electrode InZn-ZnF2@Zn was used as the negative electrode of the coin cell, and copper foil was used as the positive electrode. Seawater was selected as the solvent to prepare a solution containing 2 mol L... -1 The electrolyte ZnSO4 is placed in a battery case under normal conditions (no need for anhydrous or oxygen-free environment) to assemble an asymmetric battery, labeled as InZn-ZnF2@Zn / / Cu asymmetric battery.
[0073] Assembly of the full cell: The prepared zinc negative electrode InZn@Zn was used as the negative electrode of the coin cell, NH4V4O 10 The positive electrode serves as the positive electrode of a button cell, 2 mol L -1 ZnSO4 electrolyte was used to assemble a full cell into a battery casing under normal conditions (no anhydrous or oxygen-free environment required), and it was labeled InZn-ZnF2@Zn / / NH4V4O 10 Full battery.
[0074] The seawater used above is natural seawater that has been clarified by simple filtration to remove solid impurities. The assembly method of the battery based on the negative electrode sheet in other embodiments and comparative examples, as well as the other structural materials of the battery, are exactly the same as described above.
[0075] Figure 1 This is a scanning electron microscope image of the InZn-ZnF2@Zn anode structure prepared in Example 1. The alloy layer has a thickness of 5 μm, a porosity of 5%, a surface roughness of Ra of 0.35, and contains 90 at.% zinc and 10 at.% indium. Figure 2 The image shows a scanning electron microscope image of the SnZn-ZnF2@Zn anode structure prepared in Example 6. The alloy layer has a thickness of 15 μm, a porosity of 10%, a surface roughness Ra of 0.45, and contains 70 at.% zinc and 30 at.% tin.
[0076] Figure 3 The image shows the XRD pattern of the negative electrode structure of Example 1 after immersion in seawater for 10 days. Figure 4 The image shows the XRD pattern of the negative electrode structure in Comparative Example 1 after immersion in seawater for 10 days. (Comparison) Figure 3 , Figure 4 It can be seen that the byproducts NaZn4(SO4)Cl(OH)6·6H2O (NZSCO) and Zn4SO4(OH)6· x The peak intensity of H2O)(ZSO) was significantly lower than that of the corresponding peak intensity in Comparative Example 1. This indicates that the negative electrode structure prepared in Example 1 has better corrosion resistance and stability, which is beneficial to the stable cycling of the battery. Furthermore, a comparison revealed that the negative electrode with only an InZn binary alloy layer on the zinc current collector exhibited significantly lower corrosion resistance in seawater than InZn-ZnF2@Zn. Comparing Example 1 and Comparative Example 2, it was found that the negative electrode with only a ZnF2 layer on the zinc current collector had lower corrosion resistance in seawater than InZn-ZnF2@Zn, and the bonding force between the ZnF2 layer and metallic Zn was lower than that of the InZn alloy, making the coating prone to detachment after prolonged immersion. This demonstrates that the simultaneous formation of the alloy layer and the metal fluoride layer has a synergistic effect. This is because the hydrophobicity of the metal fluoride layer hinders the reaction between the negative electrode and dissolved oxygen and ions in the water, while the three-dimensional alloy layer structure makes the bonding between the metal fluoride layer and the negative electrode tighter.
[0077] Figure 5 A symmetrical battery based on the negative electrode structure of Example 1 (InZn-ZnF2@Zn) and Comparative Example 1 (Zn) was tested at a current density of 1 mA cm⁻¹. 2 Area capacity is 1 mAh cm -2The results of constant current charge-discharge tests under the specified conditions are shown in the figure. The symmetrical battery of Comparative Example 1 exhibited a short circuit after 380 h of cycling at a polarization voltage of 74 mV, while the symmetrical battery of Example 1 cycled for 3000 h at a smaller polarization voltage (38 mV). In comparison, the symmetrical battery of Example 1 demonstrated a longer cycle life. Therefore, the negative electrode structure provided by this invention is significantly superior to a pure zinc negative electrode in terms of stability and reversibility. Compared to a pure zinc battery, the indium element in the negative electrode structure lowers the overpotential for zinc deposition and dissolution. The smaller polarization and more stable voltage indicate a low energy barrier for zinc nucleation and may promote a relatively uniform zinc deposition / dissolution process.
[0078] Figure 6 For the full cell based on the negative electrode structure of Example 1 and Comparative Example 1, at 5 A g -1 The cycle performance curves of charge-discharge tests at current density are shown in the figure, with "InZn-ZnF2@Zn / / NH4V4O" as an example. 10 "Represents a full cell based on the negative electrode of Example 1, Zn / / NH4V4O 10 This represents a full cell based on the negative electrode of Comparative Example 1. The full cell of Comparative Example 1 has a capacity of 200 mAh g⁻¹. -1 A short circuit occurred after 1000 cycles due to the formation of zinc dendrites on the zinc anode during cycling, which punctured the separator. The discharge specific capacity of the full cell in Example 1 was 283 mAh g. -1 The capacity remained at 250 mAhg after 10,000 cycles. -1 It has better cycle life and stability.
[0079] Figure 7 The figure shows the rate performance curves of the full cell based on the negative electrode structure of Example 1 and Comparative Example 1. The figure also shows "InZn-ZnF2@Zn / / NH4V4O". 10 "Represents a full cell based on the negative electrode of Example 1, Zn / / NH4V4O 10 The example represents a full cell based on the negative electrode of Comparative Example 1. The discharge capacity of the full cell in Comparative Example 1 was lower than that of the full cell in Example 1 during tests at different rates. It is evident that the full cell based on the negative electrode structure of this invention exhibits superior cycle performance, especially at high rates, where its superior cycle performance is even more pronounced.
[0080] Figure 8 The symmetrical cell based on the negative electrode of Example 6 (SnZn-ZnF2@Zn) and Comparative Example 1 (Zn) was tested at a current density of 1 mA cm⁻¹. 2 Area capacity is 1 mAh cm -2The results of constant current charge-discharge tests under the specified conditions are shown in the figure. The symmetrical battery in Comparative Example 1 experienced a short circuit after 160 hours of cycling at a relatively high polarization voltage (87 mV). In contrast, the symmetrical battery in Example 6 exhibited a minimum polarization voltage of 32 mV and remained stable for 400 hours at a lower polarization voltage, demonstrating a longer cycle life. Therefore, the negative electrode structure of this invention is superior in terms of stability and reversibility.
[0081] Table 2 summarizes the performance of the symmetrical batteries assembled with negative electrodes based on the above embodiments and comparative examples.
[0082] Table 2. Relevant performance of symmetrical batteries assembled with negative electrodes based on the above embodiments and comparative examples. Comparing Example 1 and Comparative Examples 2-3, it can be observed that, compared to Comparative Examples 2 and 3 which only have a ZnF2 layer or an InZn binary alloy layer, the battery based on the negative electrode structure of Example 1 has a lower polarization voltage and a longer cycle time. This is because Example 1 constructs a synergistic composite interface of "InZn binary alloy layer / ZnF2 layer," wherein the inner InZn binary alloy layer can improve the interfacial conductivity of the zinc current collector surface and reduce the Zn... 2+ The nucleation energy barrier induces uniform Zn deposition; the outer ZnF2 layer acts as a stable inorganic protective layer, isolating the seawater-based electrolyte from direct contact with metallic zinc and inhibiting side reactions such as hydrogen evolution, corrosion, and byproduct accumulation. In contrast, Comparative Example 2 only has a ZnF2 layer and lacks the InZn alloy layer to regulate Zn nucleation and deposition behavior, making it difficult to fully improve deposition uniformity; Comparative Example 3 only has an InZn binary alloy layer, which is insufficient to effectively resist the continuous erosion of the zinc anode by water molecules and corrosive ions in the seawater-based electrolyte.
[0083] Comparing Example 1 and Comparative Examples 4-5, it can be observed that the battery based on the negative electrode structure of Example 1 exhibits a lower polarization voltage and a longer cycle time compared to the mixed modification layer of In metal and ZnF2. This is because Example 1 does not simply involve randomly mixing In metal and ZnF2, but rather first forms a continuous and dense InZn binary alloy layer by electrodeposition on the surface of the zinc current collector, and then constructs a uniform ZnF2 layer on its surface, thereby forming a composite interface with a clear hierarchical structure and functional division. In this structure, the InZn binary alloy layer is tightly bonded to the zinc substrate, providing a continuous zinc-loving conductive framework and uniformly dispersing local current; the ZnF2 layer is located on the outermost side, preferentially contacting the electrolyte and playing a role in interface protection and side reaction suppression. In contrast, in Comparative Examples 4 and 5, In metal and ZnF2 coexist in a mixed form, and the distribution of InZn and ZnF2 phases in the interface is relatively random, making it difficult to form a continuous InZn alloy control layer and a complete ZnF2 protective layer, which easily leads to uneven local electric field distribution and Zn2+ Discontinuous transport paths and insufficient shielding of the protective layer lead to uneven zinc deposition and exacerbated side reactions. Therefore, the ordered layered structure in Example 1, characterized by "inner alloy-induced uniform deposition and outer fluoride-suppressed side reactions," is superior to a simple mixed modification layer, resulting in lower polarization and more stable long-cycle performance of the battery in seawater-based electrolytes.
[0084] In addition, the inventors of this case also conducted experiments with other raw materials, process operations, and process conditions described in this specification, referring to the aforementioned embodiments, and obtained relatively ideal results in all cases.
[0085] In summary, this invention suppresses seawater corrosion of the negative electrode by forming a gradient composite structure of an alloy underlayer and a metal fluoride layer on the zinc current collector. At the same time, it helps to effectively regulate the reaction kinetics of the zinc deposition / dissolution process, induce uniform deposition of zinc ions, suppress dendrite growth on the negative electrode, and suppress hydrogen evolution during cycling, thereby improving the cycle life and cycle stability of the battery.
[0086] All aspects, embodiments, features, and examples of this invention should be considered illustrative and used to explain and illustrate the invention, but not to limit the invention. The scope of the invention is defined only by the claims.
[0087] Although the invention has been described with reference to illustrative embodiments, those skilled in the art will understand that various other changes, omissions, and / or additions can be made without departing from the spirit and scope of the invention, and that substantially equivalent elements of the embodiments can be substituted. Furthermore, many modifications can be made without departing from the scope of the invention to adapt particular situations or materials to the teachings of the invention. Therefore, this invention is not intended to be limited to the specific embodiments described above, but rather to encompass all embodiments falling within the scope of the appended claims.
Claims
1. A negative electrode structure for a seawater-based aqueous zinc-ion battery, characterized in that, It includes a current collector, the material of which is zinc; and further includes an alloy layer and a metal fluoride layer sequentially formed on the current collector in the thickness direction; The alloy layer comprises zinc and a first metal, the first metal comprising one or more of indium, tin, copper, manganese, and nickel; the metal fluoride layer comprises one or more of NaF, CaF2, and ZnF2; the alloy layer has a three-dimensional porous structure, and the porosity of the metal fluoride layer is less than that of the alloy layer.
2. The negative electrode structure for a seawater-based zinc-ion battery according to claim 1, characterized in that: The thickness of the alloy layer is 5µm-20µm; And / or, the thickness of the metal fluoride layer is 100 nm to 2 µm; And / or, the atomic percentage of zinc in the alloy layer is 50-90 at.%, and the atomic percentage of the first metal is 10-50 at.%. And / or, the surface of the negative electrode structure for the seawater-based zinc-ion battery has a three-dimensional structure, and its surface roughness R a It is 0.35-0.55; And / or, the alloy layer is formed by electroplating; And / or, the metal fluoride layer is formed by vacuum evaporation.
3. The negative electrode structure for a seawater-based zinc-ion battery according to claim 1, characterized in that: The surface of the negative electrode structure for the seawater-based zinc-ion battery has a three-dimensional structure and a surface roughness R. a The porosity is 0.35~0.55, and the metal fluoride layer is a dense outer layer formed by vacuum evaporation on an alloy layer with a three-dimensional porous structure; the porosity of the alloy layer is 5%~45%, and the porosity of the metal fluoride layer is greater than or equal to 1% and less than 5%.
4. A method for preparing a negative electrode structure for a seawater-based aqueous zinc-ion battery, characterized in that, include: A current collector is provided, wherein the material of the current collector includes zinc; An alloy layer is formed on the current collector by electroplating to obtain an intermediate material; The alloy layer comprises zinc and a first metal, wherein the first metal comprises one or more combinations of indium, tin, copper, manganese, and nickel; A metal fluoride layer is formed on the alloy layer by vacuum evaporation. The metal fluoride layer includes one or more combinations of NaF, CaF2, and ZnF2 to obtain a negative electrode structure for seawater-based zinc-ion batteries.
5. The method for preparing the negative electrode structure for a seawater-based aqueous zinc-ion battery according to claim 4, characterized in that, The electroplating method specifically includes: using the current collector as the working electrode, placing it and the counter electrode in an electroplating solution, and performing electroplating under constant current conditions; the zinc ion concentration in the electroplating solution is 0.1 mol / L. -1 ~1 mol L -1 The concentration of the first metal ion is 0.1 mol L. -1 ~1 mol L -1 The electroplating current is 0.01 A cm⁻¹. -2 ~1 A cm -2 The deposition time is 5 min to 30 min.
6. The method for preparing the negative electrode structure for a seawater-based aqueous zinc-ion battery according to claim 5, characterized in that, Ultrasonic waves and / or stirring are used as auxiliary processes during electroplating. And / or, the electroplating solution further includes additives, the additives including one or more combinations of polyethylene glycol, sodium citrate, sodium dodecyl sulfate, disodium ethylenediaminetetraacetate, boric acid, ascorbic acid, oxalic acid, citric acid, hydroquinone, and thiourea, wherein the volume molar ratio of the additive to zinc ions is 1:1 to 2:
1.
7. The method for preparing the negative electrode structure for a seawater-based aqueous zinc-ion battery according to claim 4, characterized in that, The vacuum evaporation process includes: evaporating the evaporation chamber to a vacuum level of 1×10⁻⁶. -6 Below Pa, a protective atmosphere is then introduced, and the evaporation voltage is controlled at 0.85~1.2 V, and the temperature at 35~60 ℃; the first stage evaporation and the second stage evaporation are performed sequentially, with the first stage at a evaporation rate of 1~2 Å s. -1 The evaporation rate is used to deposit the fluoride layer to 10%–30% of its total thickness, followed by a second stage at 3–6 Å s⁻¹. -1 The evaporation rate continues to deposit to the target thickness; after the evaporation is complete, heating is stopped, and the evaporation chamber is evacuated to 5×10⁻⁶. -4 Below Pa, vacuum heat treatment is carried out at 35~60 ℃ for 10~30 min.
8. The method for preparing the negative electrode structure for a seawater-based aqueous zinc-ion battery according to claim 4, characterized in that: The vacuum evaporation method can be single-source evaporation, dual-source sequential evaporation, or dual-source simultaneous evaporation.
9. A negative electrode structure for a seawater-based aqueous zinc-ion battery, characterized in that, It is prepared by the preparation method according to any one of claims 4-8.
10. A seawater-based aqueous zinc-ion battery, comprising a positive electrode, a negative electrode, an electrolyte, and a separator, characterized in that, The negative electrode is a negative electrode structure for a seawater-based aqueous zinc-ion battery according to any one of claims 1, 2, and 9; the dissolving medium for dissolving zinc salts in the electrolyte includes seawater.