A method for preparing tin alloy modified copper current collector for anode-free batteries

By constructing a three-dimensional porous Cu-Sn alloy framework in an anode-free lithium metal battery, the problems of uneven lithium deposition and volume expansion were solved, achieving uniform lithium distribution and improved battery stability, significantly extending battery life and increasing coulombic efficiency.

CN123120610APending Publication Date: 2026-11-17HARBIN UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611579903.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In anode-free lithium metal batteries, uneven lithium deposition and dendrite growth lead to poor battery stability, and the volume expansion of lithium-loving alloy materials during alloying/dealloying processes results in structural pulverization and electrolyte consumption.

Method used

A dynamic hydrogen bubble template-assisted electrochemical deposition technique was used to construct a uniform and firmly bonded three-dimensional porous Cu-Sn alloy framework on the surface of a copper foil current collector. The deposition behavior was regulated by introducing benzotriazole to form a porous framework to buffer volume changes and provide abundant lithiophilic sites.

Benefits of technology

It effectively suppresses the formation of lithium dendrites and dead lithium, improves lithium deposition/stripping stability, extends battery life and enhances coulombic efficiency, exhibiting excellent cycle performance and high capacity retention.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120610A_ABST
    Figure CN123120610A_ABST
Patent Text Reader

Abstract

A method for preparing a tin alloy modified copper current collector for anode-free batteries is disclosed. The invention aims to simultaneously address the problems of insufficient lithiophilicity of the current collector surface during lithium deposition and severe volume expansion caused by alloying / dealloying reactions after introducing lithiophilic elements. This invention employs dynamic hydrogen bubble template-assisted electrochemical deposition technology and introduces benzotriazole as an electrodeposition regulator. By controlling the deposition behavior and crystal growth process, a uniform and firmly bonded three-dimensional porous Cu-Sn alloy framework is constructed in situ on the surface of the copper foil current collector. The Cu-Sn alloy phase provides abundant lithiophilic sites, effectively preventing lithium metal deposition. Simultaneously, the three-dimensional porous framework reduces local current density, thereby effectively suppressing the formation of lithium dendrites and "dead lithium," improving the cycle stability and coulombic efficiency of anode-free lithium metal batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for preparing a modified copper current collector. Background Technology

[0002] With human development's over-reliance on fossil fuels, the depletion of non-renewable resources and the accompanying environmental pollution problems are becoming increasingly serious. Therefore, renewable energy sources such as solar and wind power have been vigorously developed, but their intermittency and instability place higher demands on energy storage systems. Lithium metal, due to its extremely high theoretical specific capacity (3860 mAh g⁻¹),... -1 It has the lowest redox potential (-3.04 V vs. SHE) and the lowest density (0.534 g cm⁻¹). -3 Lithium metal (LiMe) is considered an ideal anode material for next-generation high-energy-density energy storage devices. However, the use of excess lithium in the anode of traditional lithium metal batteries (N / P >> 1) severely limits the improvement of the overall energy density of the battery. To address this, anode-free lithium metal batteries (AFLMBs) have emerged, which completely remove lithium metal from the anode side, retaining only the current collector, reducing the N / P ratio to 0, thus showing significant potential in terms of energy density, safety, and cost. However, the development of this system still faces severe challenges: the fundamental lack of an initial lithium source means that the battery cycle life depends entirely on the limited lithium inventory of the cathode; the inherent low lithium affinity of the copper foil current collector leads to a high initial nucleation overpotential and kinetic lag in lithium deposition, which in turn causes uneven lithium deposition and dendrite growth, accompanied by the formation of a structurally fragile and unstable SEI layer; these unstable interfacial behaviors continuously consume active lithium and electrolyte, accelerating capacity decay and ultimately leading to battery failure.

[0003] To address the aforementioned issues with AFLMBs, researchers have proposed various strategies, including controlling lithium nucleation, constructing artificial SEI layers, and optimizing testing conditions. These strategies have made some progress in suppressing dendrite formation and reducing nucleation overpotential, but still cannot meet the requirements for practical applications of AFLMBs. Notably, the strategy of designing porous three-dimensional current collector structures and introducing lithiophilic alloys is considered an effective method to simultaneously reduce local current density and suppress dendrite growth, showing great potential in overcoming long-standing challenges associated with anode-less lithium metals (such as dendrite growth and capacity loss). Common porous three-dimensional frameworks possess advantages such as good and uniform electronic conductivity, chemical, physical, and electrochemical stability, satisfactory mechanical properties, low processing costs, and ease of large-scale fabrication. Combining them with lithiophilic alloy materials (Sn-Ni, Sn-Cu, Au-Zn, Ag-Zn) to form a porous three-dimensional host is an effective method to suppress lithium dendrite growth. The introduction of lithiophilic elements can effectively improve the lithium dendrite growth rate. + The diffusion coefficient reduces the lithium nucleation overpotential, promotes uniform lithium nucleation, thereby suppressing the formation of local dendrites, improving battery cycle performance, and extending battery life.

[0004] The significant volume expansion and contraction of pure alloys as anode materials during alloying / dealloying processes can lead to pulverization of the active material structure and destruction of electrode integrity, resulting in rapid failure. Secondly, the drastic volume changes cause repeated rupture and regeneration of the solid electrolyte interface (SEI), continuously consuming electrolyte and active lithium, leading to low coulombic efficiency and accelerated capacity decay. Furthermore, in traditional two-dimensional planar current collectors, the limited specific surface area severely restricts the number and uniformity of alloy active sites. During charging, lithium ions cannot be completely contained by the alloy phase, easily depositing unevenly on the surface, forming dendrites or "dead lithium," further causing irreversible lithium loss. Summary of the Invention

[0005] The purpose of this invention is to simultaneously solve the problems of insufficient lithiophilicity of the current collector surface during lithium deposition and severe volume expansion caused by alloying / dealloying reactions after the introduction of lithiophilic elements, and to provide a method for preparing tin alloy modified copper current collectors for anode-free batteries.

[0006] A method for preparing a tin alloy modified copper current collector for anode-free batteries is specifically carried out according to the following steps:

[0007] 1. Dissolve copper sulfate pentahydrate and stannous sulfate in deionized water, stir, then add ammonium sulfate, continue stirring, then add sulfuric acid and benzotriazole, continue stirring to obtain the electrodeposition solution;

[0008] Second, first immerse the copper foil in a sulfuric acid solution with a concentration of 0.1 mol / L to 0.2 mol / L, then take out the copper foil and immerse it in acetone, and finally dry the copper foil to obtain the pretreated copper foil;

[0009] III. Electrodeposition:

[0010] Using pretreated copper foil as the working electrode and a platinum sheet as the counter electrode, the working electrode and counter electrode were immersed in an electrodeposition solution at a current density of 3 A cm⁻¹. -2 Electrodeposition was performed under specific conditions. During the electrodeposition process, the precipitated hydrogen bubbles served as a dynamic template, guiding the formation of a three-dimensional porous structure. After the electrodeposition was completed, the working electrode was removed, cleaned, and dried to obtain a tin alloy modified copper current collector for anode-free batteries.

[0011] The principles and advantages of this invention:

[0012] I. This invention employs dynamic hydrogen bubble template-assisted electrochemical deposition technology and introduces benzotriazole (C6H5N3) as an electrodeposition regulator. By controlling the deposition behavior and crystal growth process, a uniform and firmly bonded three-dimensional porous Cu-Sn alloy framework is constructed in situ on the surface of a copper foil current collector. Compared with the absence of C6H5N3, the resulting three-dimensional framework exhibits higher structural continuity and mechanical stability, and forms a deposition structure more conducive to lithium storage. The Cu-Sn alloy phase provides abundant lithiophilic sites, allowing lithium ions to preferentially undergo alloying reactions within a set capacity range and be stored in the alloy phase, effectively avoiding metallic lithium deposition. Simultaneously, the three-dimensional porous framework can reduce local current density, promote uniform lithium distribution within the main body, and buffer volume changes during alloying / dealloying processes, thereby effectively suppressing the formation of lithium dendrites and "dead lithium," and improving the cycle stability and coulombic efficiency of anode-free lithium metal batteries.

[0013] II. The electrochemical performance of the obtained copper-tin alloy (BTA-CS) anode material was tested and compared with that of the copper-tin alloy (CS) anode without C6H5N3. The results showed that at 1 mA cm⁻¹, the copper-tin alloy (BTA-CS) anode material exhibited better performance. -2 Current density and 1 mAh cm -2 At the given areal capacity, the half-cell assembled using BTA-CS exhibited an average coulombic efficiency of 94.11% over 70 cycles, while the control group showed a rapid decline in coulombic efficiency after 40 cycles, indicating that the BTA-CS material provided by this invention possesses excellent lithium deposition / stripping stability. When assembled with a lithium iron phosphate (LiFePO4) cathode, the BTA-CS electrode achieved an initial capacity of 124 mAh g⁻¹ under 0.2C charge-0.5C discharge conditions. -1 After 30 cycles, it showed 52 mAh g. -1 The high discharge specific capacity and 41.94% capacity retention rate of the tin alloy modified copper current collector for anode-free batteries, compared to only 30.83% of the capacity retention rate of the CS full cell after 30 cycles, demonstrate that the tin alloy modified copper current collector provided by this invention has a high cycle life. Attached Figure Description

[0014] Figure 1 These are scanning electron microscope (SEM) images. In the figure, a is a low-magnification SEM image of BTA-CS, b is a high-magnification SEM image of BTA-CS, c is a low-magnification SEM image of CS, and d is a high-magnification SEM image of CS.

[0015] Figure 2 The image shows XRD patterns, where a represents BTA-CS and b represents CS.

[0016] Figure 3 The cycling performance of half-cells Li||BTA-CS and Li||CS assembled using BTA-CS and CS, respectively;

[0017] Figure 4 The charge / discharge voltage-specific capacity curves of half-cells Li||BTA-CS and Li||CS assembled using BTA-CS and CS, respectively.

[0018] Figure 5 The cycle performance of full cells assembled using BTA-CS and CS, respectively. Detailed Implementation

[0019] Specific Implementation Method 1: This implementation method is a method for preparing a tin alloy modified copper current collector for anode-free batteries, characterized in that the preparation method is specifically completed according to the following steps:

[0020] 1. Dissolve copper sulfate pentahydrate and stannous sulfate in deionized water, stir, then add ammonium sulfate, continue stirring, then add sulfuric acid and benzotriazole, continue stirring to obtain the electrodeposition solution;

[0021] Second, first immerse the copper foil in a sulfuric acid solution with a concentration of 0.1 mol / L to 0.2 mol / L, then take out the copper foil and immerse it in acetone, and finally dry the copper foil to obtain the pretreated copper foil;

[0022] III. Electrodeposition:

[0023] Using pretreated copper foil as the working electrode and a platinum sheet as the counter electrode, the working electrode and counter electrode were immersed in an electrodeposition solution at a current density of 3 A cm⁻¹. -2 Electrodeposition was performed under specific conditions. During the electrodeposition process, the precipitated hydrogen bubbles served as a dynamic template, guiding the formation of a three-dimensional porous structure. After the electrodeposition was completed, the working electrode was removed, cleaned, and dried to obtain a tin alloy modified copper current collector for anode-free batteries.

[0024] Specific Implementation Method Two: This implementation method differs from Specific Implementation Method One in that the concentration of copper sulfate pentahydrate in the electrodeposition solution described in step one is 0.2 mol / L to 0.3 mol / L. The other steps are the same as in Specific Implementation Method One.

[0025] Specific Implementation Method Three: This implementation method differs from Specific Implementation Method One or Two in that the concentration of stannous sulfate in the electrodeposition solution described in step one is 0.1 mol / L to 0.3 mol / L. The other steps are the same as in Specific Implementation Method One or Two.

[0026] Specific Implementation Method Four: This implementation method differs from Specific Implementation Methods One to Three in that the concentration of ammonium sulfate in the electrodeposition solution described in step one is 1 mol / L to 1.5 mol / L. The other steps are the same as in Specific Implementation Methods One to Three.

[0027] Specific Implementation Method Five: This implementation method differs from Specific Implementation Methods One to Four in that the concentration of sulfuric acid in the electrodeposition solution described in step one is 1.4 mol / L to 1.6 mol / L. The other steps are the same as in Specific Implementation Methods One to Four.

[0028] Specific Implementation Method Six: This implementation method differs from Specific Implementation Methods One to Five in that the concentration of benzotriazole in the electrodeposition solution described in step one is 0.3 mol / L to 0.5 mol / L. The other steps are the same as in Specific Implementation Methods One to Five.

[0029] Specific Implementation Method Seven: This implementation method differs from Specific Implementation Methods One to Six in that: the stirring time in step one is 10-30 minutes; the drying temperature in step two is 50-60°C, and the drying time is 10-20 minutes. Other steps are the same as in Specific Implementation Methods One to Six.

[0030] Specific Implementation Method Eight: The difference between this implementation method and Specific Implementation Methods One to Seven is that in step two, the copper foil is immersed in a sulfuric acid solution with a concentration of 0.1 mol / L to 0.2 mol / L for 10 to 15 seconds, and then immersed in acetone for 10 to 15 seconds. The other steps are the same as in Specific Implementation Methods One to Seven.

[0031] Specific Implementation Method Nine: This implementation method differs from Specific Implementation Methods One to Eight in that the electrodeposition time in step three is 10s to 20s. The other steps are the same as in Specific Implementation Methods One to Eight.

[0032] Specific Implementation Method Ten: This implementation method differs from Specific Implementation Methods One to Nine in that: the cleaning in step three involves washing with deionized water 3 to 5 times; the drying temperature is 50℃ to 60℃, and the drying time is 5 hours to 7 hours. Other steps are the same as in Specific Implementation Methods One to Nine.

[0033] The beneficial effects of the present invention are verified using the following embodiments:

[0034] Example 1: A method for preparing a tin alloy modified copper current collector for anode-free batteries, specifically comprising the following steps:

[0035] 1. Dissolve copper sulfate pentahydrate and stannous sulfate in deionized water and stir for 10 min. Then add ammonium sulfate and continue stirring. Then add sulfuric acid and benzotriazole (C6H5N3) and continue stirring for 10 min to obtain the electrodeposition solution.

[0036] In step one, the electrodeposition solution contains copper sulfate pentahydrate at a concentration of 0.24 mol / L, stannous sulfate at a concentration of 0.2 mol / L, ammonium sulfate at a concentration of 1.2 mol / L, sulfuric acid at a concentration of 1.5 mol / L, and benzotriazole at a concentration of 0.4 mol / L.

[0037] 2. Immerse the copper foil in a 0.1 mol / L sulfuric acid solution for 10 seconds, then immerse it in acetone for 10 seconds. Finally, place the copper foil in a 55°C forced-air oven and dry it for 15 minutes to obtain the pretreated copper foil.

[0038] III. Electrodeposition:

[0039] Using pretreated copper foil as the working electrode and a platinum sheet as the counter electrode, the working electrode and counter electrode were immersed in an electrodeposition solution at a current density of 3 A cm⁻¹. -2 Electrodeposition was performed for 15 seconds under the specified conditions. During the electrodeposition process, the precipitated hydrogen bubbles served as a dynamic template to guide the formation of a three-dimensional porous structure. After the electrodeposition was completed, the working electrode was removed, washed three times with deionized water, and then dried at 55°C for 6 hours to obtain a tin alloy modified copper current collector (BTA-CS) for anodeless batteries.

[0040] Comparing with Example 1: The preparation method of copper-tin alloy (CS) is specifically carried out according to the following steps:

[0041] 1. Dissolve copper sulfate pentahydrate and stannous sulfate in deionized water and stir for 10 min. Then add ammonium sulfate and continue stirring for 10 min. Finally, add sulfuric acid and continue stirring for 30 min to obtain the electrodeposition solution.

[0042] In step one, the concentration of copper sulfate pentahydrate in the electrodeposition solution is 0.24 mol / L, the concentration of stannous sulfate is 0.2 mol / L, the concentration of ammonium sulfate is 1.2 mol / L, and the concentration of sulfuric acid is 1.5 mol / L.

[0043] 2. Immerse the copper foil in a 0.1 mol / L sulfuric acid solution for 10 seconds, then immerse it in acetone for 10 seconds. Finally, place the copper foil in a 55°C forced-air oven and dry it for 15 minutes to obtain the pretreated copper foil.

[0044] III. Electrodeposition:

[0045] Using pretreated copper foil as the working electrode and a platinum sheet as the counter electrode, the working electrode and counter electrode were immersed in an electrodeposition solution at a current density of 3 A cm⁻¹. -2Electrodeposition was performed for 15 seconds under the specified conditions. During the electrodeposition process, the precipitated hydrogen bubbles served as a dynamic template to guide the formation of a three-dimensional porous structure. After the electrodeposition was completed, the working electrode was removed, washed three times with deionized water, and then dried at 55°C for 6 hours to obtain a copper-tin alloy (CS).

[0046] Figure 1 These are scanning electron microscope (SEM) images. In the figure, a is a low-magnification SEM image of BTA-CS, b is a high-magnification SEM image of BTA-CS, c is a low-magnification SEM image of CS, and d is a high-magnification SEM image of CS.

[0047] from Figure 1 As shown in a, the BTA-CS material exhibits a three-dimensional interconnected porous network structure with uniform pore size distribution and an average pore size of approximately 21 µm, which is beneficial for electrolyte wetting and ion transport. Figure 1 b is a magnified view of the pore connection area, showing that the skeleton at the connection is dense and the structure is continuous, exhibiting good mechanical integrity, which helps to buffer volume changes during cycling and maintain the stability of the electrode structure. Figure 1 As shown in c, the CS material exhibits a loose three-dimensional porous structure with uneven pore size distribution. Figure 1 Image d is a magnified view of the connection point, revealing that its framework is mainly composed of interlocking sheet-like structures, with a relatively loose connection area and poor structural continuity. In contrast, the BTA-CS material exhibits a denser and more stable three-dimensional network framework, indicating that the addition of C6H5N3 is beneficial for optimizing the material's microstructure and improving the mechanical stability and overall structural integrity of the framework.

[0048] Figure 2 The image shows XRD patterns, where a represents BTA-CS and b represents CS.

[0049] like Figure 2 As shown in Figure a, characteristic diffraction peaks of Cu (PDF#04-0836), Cu6Sn5 (PDF#45-1488), and metallic Sn (PDF#04-0673) are clearly visible in the BTA-CS sample. Figure 2 As shown in b, only characteristic diffraction peaks of Cu and Cu6Sn5 were detected in the CS sample, while no obvious Sn diffraction peaks were observed. This may be due to the low content of residual Sn, which is below the detection limit of XRD, thus failing to detect its diffraction signal. However, the Cu6Sn5 alloy phase is still the main crystalline phase in the sample. This result indicates that the introduction of C6H5N3 did not change the formation of the Cu6Sn5 alloy phase. At the same time, some Sn was retained in the BTA-CS sample, ultimately forming a multiphase composite structure composed of Cu, Cu6Sn5, and Sn. Among them, Cu serves as both a conductive framework and can form a stable Cu6Sn5 alloy phase with Sn.

[0050] A coin cell half-cell was assembled using a BTA-CS or CS electrode as the working electrode and a lithium metal sheet as the counter electrode. During assembly, the working electrode, separator, and lithium metal sheet were sequentially placed in the coin cell casing, and 50 μL of electrolyte was dropped onto the surface of both the working electrode and the lithium sheet. Subsequently, the corresponding gaskets and spring sheets were placed in sequence, and the encapsulation was completed. The electrolyte was 1.0M LiPF6 in EC:DMC:DEC=1:1:1 vol% with 5% FEC.

[0051] At 1 mA cm -2 Constant current deposition was performed at a current density with a cutoff capacity of 1 mAh cm⁻¹. -2 This was used to evaluate the lithium deposition / stripping behavior and coulombic efficiency of the material.

[0052] To verify the application potential of the BTA-CS current collector obtained by introducing C6H5N3 to regulate the electrodeposition structure in anode-free lithium metal batteries, its coulombic efficiency was tested in half-cells of Li||BTA-CS and Li||CS, such as... Figure 3 As shown;

[0053] Figure 3 The cycling performance of half-cells Li||BTA-CS and Li||CS assembled using BTA-CS and CS, respectively;

[0054] from Figure 3 It can be seen that at 1 mA cm -2 1 mAh cm -2 Under the given conditions, the average coulombic efficiency of BTA-CS after 70 cycles was 94.11%, while CS decreased rapidly after 40 cycles. This indicates that the introduction of C6H5N3 can effectively regulate the Cu-Sn deposition structure, construct a more stable three-dimensional porous framework, provide more uniform nucleation sites for lithium deposition, thereby promoting uniform lithium deposition, reducing irreversible lithium loss, improving the reversibility of the lithium deposition / stripping process, and ultimately significantly improving the cycle stability of the battery.

[0055] Figure 4 The charge / discharge voltage-specific capacity curves of half-cells Li||BTA-CS and Li||CS assembled using BTA-CS and CS, respectively.

[0056] from Figure 4 It can be seen that during the discharge process, the Cu-Sn phase in BTA-CS and CS materials first undergoes an alloying reaction with lithium to form a Li-Sn alloy. For example... Figure 4 As shown in a, when the discharge capacity reaches 1 mAh cm⁻¹ -2During this period, the voltage of the BTA-CS half-cell remained higher than the lithium deposition potential, indicating that lithium ions mainly participated in the Cu-Sn phase alloying reaction at this stage, without significant metallic lithium deposition on the electrode surface. The presence of only a dealloying plateau during charging further demonstrates that the electrode undergoes a reversible alloying / dealloying process, which is beneficial for suppressing lithium dendrite growth and the formation of "dead lithium." Figure 4 As shown in b, the voltage of the CS half-cell is lower than the lithium deposition potential in the later stage of discharge, indicating that lithium metal deposition begins after the alloying reaction is completed, corresponding to the lithium stripping process during charging. This deposited lithium is more prone to forming dendrites and irreversible "dead lithium," leading to a decrease in the reversibility of lithium deposition / stripping and thus causing a rapid decline in coulombic efficiency.

[0057] To verify the application performance of the BTA-CS current collector obtained by introducing C6H5N3 to regulate the electrodeposition structure in anode-free lithium metal full cells, full cells were assembled with high-load LiFePO4 as the positive electrode and BTA-CS or CS as the negative electrode current collector. During assembly, the positive electrode, separator, and negative electrode were sequentially placed in a coin cell casing. 50 μL of electrolyte was dropped onto the surfaces of both the positive and negative electrodes. Subsequently, the corresponding gaskets and spring sheets were placed sequentially, and the cell was encapsulated. The electrolyte was 1.0 M LiPF6 in EC:DMC:DEC = 1:1:1 vol% with 5% FEC.

[0058] Figure 5 The cycle performance of full cells assembled using BTA-CS and CS, respectively;

[0059] from Figure 5 It can be seen that under the conditions of 0.2C charging and 0.5C discharging, N / P=0 (no active lithium on the negative electrode side initially, and the negative electrode capacity is zero) and carbonate electrolyte, the average coulombic efficiency of the BTA-CS full cell reaches 97.12%, and the capacity retention rate is still 41.93% after 30 cycles. In contrast, the capacity retention rate of the CS full cell after 30 cycles is only 30.83%, and the average coulombic efficiency is 95.83%.

Claims

1. A method for preparing a tin alloy modified copper current collector for anode-free batteries, characterized in that... The preparation method is specifically carried out according to the following steps:

1. Dissolve copper sulfate pentahydrate and stannous sulfate in deionized water, stir, then add ammonium sulfate, continue stirring, then add sulfuric acid and benzotriazole, continue stirring to obtain the electrodeposition solution; Second, first immerse the copper foil in a sulfuric acid solution with a concentration of 0.1 mol / L to 0.2 mol / L, then take out the copper foil and immerse it in acetone, and finally dry the copper foil to obtain the pretreated copper foil; III. Electrodeposition: Using pretreated copper foil as the working electrode and a platinum sheet as the counter electrode, the working electrode and counter electrode were immersed in an electrodeposition solution at a current density of 3 A cm⁻¹. -2 Electrodeposition was performed under specific conditions. During the electrodeposition process, the precipitated hydrogen bubbles served as a dynamic template, guiding the formation of a three-dimensional porous structure. After the electrodeposition was completed, the working electrode was removed, cleaned, and dried to obtain a tin alloy modified copper current collector for anode-free batteries.

2. The method for preparing a tin alloy modified copper current collector for an anode-free battery according to claim 1, characterized in that... The concentration of copper sulfate pentahydrate in the electrodeposition solution described in step one is 0.2 mol / L to 0.3 mol / L.

3. The method for preparing a tin alloy modified copper current collector for an anode-free battery according to claim 1, characterized in that... The concentration of stannous sulfate in the electrodeposition solution described in step one is 0.1 mol / L to 0.3 mol / L.

4. The method for preparing a tin alloy modified copper current collector for an anode-free battery according to claim 1, characterized in that... The concentration of ammonium sulfate in the electrodeposition solution described in step one is 1 mol / L to 1.5 mol / L.

5. The method for preparing a tin alloy modified copper current collector for an anode-free battery according to claim 1, characterized in that... The concentration of sulfuric acid in the electrodeposition solution described in step one is 1.4 mol / L to 1.6 mol / L.

6. The method for preparing a tin alloy modified copper current collector for an anodeless battery according to claim 1, characterized in that... The concentration of benzotriazole in the electrodeposition solution described in step one is 0.3 mol / L to 0.5 mol / L.

7. The method for preparing a tin alloy modified copper current collector for an anode-free battery according to claim 1, characterized in that... The stirring time in step one is 10 min to 30 min; the drying temperature in step two is 50℃ to 60℃, and the drying time is 10 min to 20 min.

8. The method for preparing a tin alloy modified copper current collector for an anode-free battery according to claim 1, characterized in that... In step two, the copper foil is immersed in a sulfuric acid solution with a concentration of 0.1 mol / L to 0.2 mol / L for 10 to 15 seconds, and then immersed in acetone for 10 to 15 seconds.

9. The method for preparing a tin alloy modified copper current collector for an anode-free battery according to claim 1, characterized in that... The electrodeposition time described in step three is 10s to 20s.

10. The method for preparing a tin alloy modified copper current collector for an anode-free battery according to claim 1, characterized in that... The cleaning described in step three involves rinsing with deionized water 3 to 5 times; the drying temperature is 50℃ to 60℃, and the drying time is 5h to 7h.