Positive electrode for lithium-ion secondary batteries
By introducing closed pores into the positive electrode active material of lithium-ion secondary batteries, the problem of increased resistance caused by internal cracks in polycrystalline particles was solved, thereby reducing battery resistance and improving cycle stability.
Patent Information
- Application Number
- CN202610502400.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-16
- Filing Date
- 2026-04-16
- Publication Date
- 2026-11-17
AI Technical Summary
During the charge-discharge cycle of lithium-ion secondary batteries, the formation of cracks within polycrystalline particles leads to an increase in resistance, a problem that is difficult to effectively solve with existing technologies.
In the positive electrode active material of lithium-ion secondary batteries, by introducing closed pores within primary particles and at grain boundaries, the number density and average diameter of these pores are controlled to alleviate stress concentration and reduce the generation and growth of cracks.
By introducing closed pores within primary particles and at grain boundaries, the rate of increase in resistivity is reduced, thereby improving the cycle stability and electrical performance of lithium-ion secondary batteries.
Smart Images

Figure CN123120615A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the positive electrode for lithium-ion secondary batteries. Background Technology
[0002] Chinese Patent Application Publication No. 116565133 discloses positive electrode active material particles with a polycrystalline structure (hereinafter sometimes referred to as "polycrystalline particles"). Summary of the Invention
[0003] During charge-discharge cycles, cracks may form within the polycrystalline particles, potentially leading to an increase in the rate of increase in resistivity.
[0004] The purpose of this invention is to reduce the rate of increase in resistance after cycling.
[0005] The technical structure and effects of the present invention will be described below. However, the mechanism of action includes speculation. The mechanism of action does not limit the technical scope of the present invention.
[0006] 1. A positive electrode for a lithium-ion secondary battery according to one embodiment of the present invention comprises a positive electrode active material. The positive electrode active material comprises secondary particles. The secondary particles comprise a plurality of primary particles. Closed pores are formed within the primary particles and at the grain boundaries between the primary particles. The number density of closed pores is greater than the number density of primary particles.
[0007] During the synthesis of polycrystalline particles, primary particles (single crystal particles) merge and grow, thus achieving dense packing. During charge-discharge cycles, these primary particles expand and contract. Due to the volume change of the primary particles, stress concentrates at the grain boundaries between them, potentially leading to large cracks. The formation of large cracks may result in a greater rate of increase in resistivity after cycling.
[0008] To reduce crack formation, it's possible to introduce closed or open pores at the grain boundaries between primary particles from the outset. The presence of pores from the beginning can alleviate stress concentration. However, pores formed at grain boundaries tend to propagate along those boundaries, potentially leading to the growth of large cracks. Furthermore, since open pores are connected to the outside, their expansion can also cause secondary particle fracture.
[0009] In this invention, in addition to closed pores at grain boundaries, closed pores are also introduced within primary particles. By making the number density of closed pores greater than the number density of primary particles, it is expected that stress concentration caused by volume changes in primary particles will be reduced. Furthermore, since closed pores also exist within primary particles, it is expected that the volume changes in primary particles will be smaller, and therefore, it is also expected that closed pores at grain boundaries will be less likely to grow. By reducing crack initiation and growth, a decrease in the rate of increase in resistivity after cycling is expected.
[0010] 2. The positive electrode for lithium-ion secondary batteries described in item "1" above may, for example, include the following configuration: A closed-pore density of 20 pores / μm. 2 above.
[0011] By setting the number density of closed pores to 20 per μm 2 Therefore, we can expect a decrease in the rate of increase in resistance after cycling.
[0012] 3. The positive electrode for lithium-ion secondary batteries described in item "1" or "2" above may, for example, include the following configuration: The average diameter of the closed pores is 20 nm or more.
[0013] By making the average diameter of the closed pores greater than 20 nm, a reduction in the rate of increase in resistance after cycling can be expected.
[0014] 4. The positive electrode for a lithium-ion secondary battery according to any one of items "1" to "3" above may, for example, include the following configuration: Primary particle number density of 1 particle / μm. 2 ~10 particles / μm 2 .
[0015] By making the number density of primary particles 1 / μm 2 ~10 particles / μm 2 We can expect a decrease in the rate of increase in resistance after cycling.
[0016] 5. A positive electrode for a lithium-ion secondary battery according to one embodiment of the present invention comprises a positive electrode active material. The positive electrode active material comprises secondary particles. The secondary particles comprise a plurality of primary particles. Closed pores are formed within the primary particles and at the grain boundaries between the primary particles. The average diameter of the closed pores located within the primary particles is smaller than the average diameter of the closed pores located at the grain boundaries. The average diameter of all closed pores is 20 nm to 100 nm. The number density of primary particles is 1 particle / μm. 2 ~10 particles / μm 2 The number density of closed pores is 50 / μm. 2 ~150 cells / μm 2 .
[0017] For example, by making the closed pores within primary particles smaller than the closed pores at grain boundaries, a decrease in the rate of increase in resistivity after cycling can be expected.
[0018] Hereinafter, one embodiment of the present invention (hereinafter sometimes simply referred to as "this embodiment") and one example of the present invention (hereinafter sometimes simply referred to as "this embodiment") will be described. However, this embodiment and this embodiment do not limit the technical scope of the present invention. This embodiment and this embodiment are illustrative in all respects. This embodiment and this embodiment are non-limiting. The technical scope of the present invention includes the meaning equivalent to the description in the claims and all modifications within the scope thereof. For example, it is foreseeable from the outset that any configuration can be extracted from this embodiment and combined arbitrarily. Attached Figure Description
[0019] The features, advantages, and technical and industrial significance of exemplary embodiments of the present invention will now be described with reference to the accompanying drawings, wherein like reference numerals denote like elements.
[0020] Figure 1 This is a conceptual diagram illustrating an example of a lithium-ion secondary battery in this embodiment.
[0021] Figure 2 This is a conceptual diagram illustrating an example of the positive electrode active material in this embodiment.
[0022] Figure 3 This is a schematic flowchart illustrating the first synthesis method in this embodiment.
[0023] Figure 4 This is a schematic flowchart illustrating the second synthesis method in this embodiment.
[0024] Figure 5 This is a table showing an example of the experimental results of this embodiment. Detailed Implementation
[0025] Terms and statements
[0026] The terms "possessing," "including," and "having," and their variations, are open-ended expressions. Regarding a composition expressed in an open-ended manner, additional elements may be included beyond the necessary elements, or no additional elements may be included. A statement such as "consisting of..." is a closed-ended expression. However, even a closed-ended composition may include impurities or additional elements unrelated to the target technology. A statement such as "substantially constituted of..." is a semi-closed-ended expression. In a semi-closed-ended composition, elements that do not substantially affect the fundamental and novel characteristics of the target technology are permitted to be added.
[0027] Geometric terms should not be interpreted in a strict sense. As geometric terms, they can, for example, represent "parallel," "perpendicular," and "orthogonal." For instance, directions, angles, and distances can be relatively offset within a range that achieves substantially the same or similar function. Geometric terms can also encompass tolerances and errors in design, operation, and manufacturing. Dimensional relationships in drawings sometimes differ from actual dimensional relationships. To aid understanding, dimensional relationships in drawings may be altered. For example, lengths, widths, and thicknesses may be changed. Sometimes, certain components are omitted.
[0028] Unless otherwise specified, the singular form is not limited to a single element. The singular form can also include two or more elements.
[0029] The shape and size of particles and pores are determined using microscopy. For example, various image analyses can be performed on cross-sectional SEM (Scanning Electron Microscope) images of the positive electrode active material layer, powder, secondary particles, etc. The magnification can be appropriately varied according to, for example, the size of primary particles and pores. The magnification can be, for example, 5000 to 50000 times. The various image analyses and size measurements in this embodiment can be performed with software assistance, or by software itself, or by using AI with machine learning models. As an example of software, "ImageJ" can be considered.
[0030] Unless otherwise specified, the numerical range "m~n%" includes both an upper and lower limit. That is, "m~n%" represents a numerical range of "m% and above and n% and below". Furthermore, "m% and above and n% and below" includes "greater than m% and less than n%". "Above" and "below" are indicated by inequality signs "≤" and "≥" with an equal sign. "Greater than" and "less than" are indicated by inequality signs "<" and ">" without an equal sign. Any value selected from the numerical range can be used as a new upper or lower limit. For example, a new numerical range can be set by arbitrarily combining values within the numerical range with values described in other parts of this specification, tables, figures, etc. Regarding numerical ranges (intervals), for example, "the range formed by any one or two endpoints selected from the group a, b, c, d" includes "a≤x", "x≤a", "b≤x", "x≤b", "c≤x", "x≤c", "d≤x", "x≤d", "a≤x≤b", "a≤x≤c", "a≤x≤d", "b≤x≤c", "b≤x≤d", and "c≤x≤d". All ranges may or may not include endpoints. That is, the above ranges, for example, include not only "a≤x" but also "a<x". The above ranges, for example, include not only "a≤x≤b" but also "a<x≤b", "a≤x<b", and "a<x<b".
[0031] "Open pore" refers to a void that appears to be connected to the outside in a cross-sectional SEM image. "Closed pore" refers to a void that appears to be not connected to the outside in a cross-sectional SEM image.
[0032] The particle's "particle size" is the arithmetic mean of the long and short sides of the minimum bounding rectangle (MBR) of the particle's two-dimensional image. The "average particle size" is the arithmetic mean of the particle sizes of 10 randomly selected particles.
[0033] The number density of closed pores can be determined by the following steps: In a cross-sectional SEM image, 30 secondary particles are randomly selected. Within each secondary particle, closed pores (voids) are distinguished from solid particles (primary particles) using binarization. The number of closed pores is counted. The number of closed pores is calculated by dividing the number of closed pores by the cross-sectional area of each secondary particle. The arithmetic mean of the number densities of closed pores is then calculated for each of the 30 secondary particles.
[0034] The average diameter of closed pores can be determined through the following steps. In the binarized cross-sectional SEM image described above, the diameter of each closed pore is measured. "Diameter" represents the arithmetic mean of the long and short sides of the MBR of the two-dimensional image of the closed pores. The arithmetic mean of the diameters of closed pores measured within 30 secondary particles is the "average diameter". Alternatively, closed pores within primary particles and closed pores at grain boundaries can be counted separately. Thus, the number density and average diameter of closed pores within primary particles, as well as the number density and average diameter of closed pores at grain boundaries, can be determined.
[0035] Lithium-ion secondary batteries
[0036] The lithium-ion secondary battery (hereinafter sometimes simply referred to as "battery") in this embodiment includes at least one selected from the group consisting of liquid electrolytes, gel electrolytes, and solid electrolytes. The battery can be a liquid battery, polymer battery, solid-state battery, or all-solid-state battery. "Solid-state battery" refers to a battery containing a solid electrolyte. In addition to containing a solid electrolyte, a solid-state battery may further contain other electrolytes.
[0037] Figure 1 This is a conceptual diagram illustrating an example of a lithium-ion secondary battery according to this embodiment. The battery 1000 may include, for example, a power generation element 500 and a casing 600. The casing 600 houses the power generation element 500. The casing 600 may be, for example, a metal container, an aluminum-plastic film soft case, etc. The power generation element 500 may include, for example, a positive electrode 100, a negative electrode 200, a separator 300, and an electrolyte (not shown). The power generation element 500 may be, for example, a wound type or a stacked type. The power generation element 500 may have a unipolar structure or a bipolar structure. The separator 300 electrically separates the negative electrode 200 from the positive electrode 100. The separator 300 may, for example, be a porous membrane made of resin. The electrolyte is a Li-ion conductor. The electrolyte may, for example, contain Li salt and an organic solvent. The electrolyte may, for example, be impregnated in the separator 300. The separator 300 may contain a solid electrolyte. The electrolyte may, for example, contain a polymer electrolyte, a gel electrolyte, a solid electrolyte, etc. Solid electrolytes may include, for example, sulfide solid electrolytes, oxide solid electrolytes, halide solid electrolytes, etc. The negative electrode 200 contains a negative electrode active material. The negative electrode active material may be, for example, at least one selected from the group consisting of natural graphite, artificial graphite, silicon, silicon oxide, silicon-based alloys, and Si-C. "Si-C" indicates a composite particle containing at least one of silicon and silicon oxide, and carbon. For example, Si may be loaded onto a carbon material.
[0038] positive electrode
[0039] The positive electrode 100 includes a positive electrode active material. The positive electrode 100 may, for example, include a positive electrode current collector and a positive electrode active material layer. The positive electrode active material layer may be supported by the positive electrode current collector. The positive electrode active material layer may contain positive electrode active material. In addition to containing the positive electrode active material, the positive electrode active material layer may further contain conductive materials and binders, etc. For example, the positive electrode active material layer may contain 0-10% conductive material, 1-10% binder, and the balance positive electrode active material by mass fraction.
[0040] Figure 2This is a conceptual diagram illustrating an example of the positive electrode active material in this embodiment. The positive electrode active material comprises secondary particles 20. The secondary particles 20 comprise a plurality of primary particles 10. The number of primary particles 10 constituting the secondary particles 20 can, for example, be a range formed by any one or two endpoints selected from the group consisting of 50, 100, 500, 1000, 3000, 5000, and 10000. The number of primary particles 10 constituting the secondary particles 20 can, for example, be "more than 50", "less than 10000", or "50 to 10000". The number of primary particles 10 represents the number counted in the SEM image (particle surface or particle cross-section).
[0041] The average particle size of the secondary particles 20 can be, for example, a range formed by any one or two endpoints selected from the group consisting of 3 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, and 30 μm. The average particle size of the secondary particles 20 can be, for example, "above 3 μm", "below 30 μm", or "3 μm to 30 μm".
[0042] The secondary particle 20 can have any shape. For example, the secondary particle 20 can be spherical, ellipsoidal, etc. The range of the roundness of the secondary particle 20 can be, for example, a range formed by any one or two endpoints selected from the group consisting of 0.50, 0.60, 0.70, 0.80, 0.90, 0.95, and 1.00. The range of the roundness of the secondary particle 20 can be, for example, "above 0.50", "below 1.00", or "0.50 to 1.00".
[0043] "Circularity" can be determined from the SEM image of the particles. Circularity is calculated using the following formula, taking the arithmetic mean of the circularity of 10 particles.
[0044] ψ=4πS / L 2
[0045] ψ: Circularity
[0046] π: Pi
[0047] S: Cross-sectional area of the particle (the area of the region enclosed by the particle's outline)
[0048] L: The perimeter of the particle (the length of the particle's outline)
[0049] The primary particle 10 can have any shape. For example, the primary particle 10 can be spherical, ellipsoidal, rod-shaped, columnar, plate-shaped, etc. The average particle size of the primary particle 10 can, for example, be a range formed by any one or two endpoints selected from the group consisting of 0.1 μm, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, and 3 μm. The average particle size range of the primary particle 10 can, for example, be "above 0.1 μm", "below 3 μm", or "0.1 μm to 3 μm".
[0050] The number density of primary particles 10 can, for example, be selected from 1 particle / μm. 2 2 per μm 2 3 per μm 2 4 per μm 2 5 per μm 2 6 per μm 2 7 per μm 2 8 per μm 2 9 per μm 2 10 cells / μm 2 15 cells / μm 2 20 cells / μm 2 The range formed by any one or two endpoints of the group. The number density of primary particles 10 can be, for example, "1 particle / μm". 2 "Above", "10 / μm" 2 "below" or "1 / μm" 2 ~10 particles / μm 2 ".
[0051] A first closed pore 2 is formed within a primary particle 10. A second closed pore 4 is formed at the grain boundaries between the primary particles 10. The number density of closed pores (the sum of the number densities of the first closed pore 2 and the second closed pore 4) is greater than the number density of the primary particles 10. The number density of closed pores can, for example, be selected from 20 pores / μm. 2 25 cells / μm 2 50 cells / μm 2 75 cells / μm 2 100 cells / μm 2 125 cells / μm 2 150 cells / μm 2 175 cells / μm 2 200 / μm 2 250 cells / μm 2 The range formed by any one or two endpoints of the group. The range of closed pore density can be, for example, "20 pores / μm". 2 "Above", "250 / μm" 2"Below", "20 / μm" 2 ~250 cells / μm 2 "or 50 cells / μm" 2 ~150 cells / μm 2 ".
[0052] The number density "n1" of the first closed pore 2 can be greater than the number density "n2" of the second closed pore 4. The range of the ratio "n1 / n2" of the number density "n1" of the first closed pore 2 relative to the number density "n2" of the second closed pore 4 can be, for example, a range formed by any one or two endpoints selected from the group consisting of 1.2, 1.5, 2, 3, 4, 5, 6, 7, 8, 9, 10, 12, 15, and 20. The range of the ratio "n1 / n2" can be, for example, "more than 1.2", "less than 20", or "1.2 to 20".
[0053] The number density "n1" of the first closed pore 2 can, for example, be selected from 25 pores / μm. 2 50 cells / μm 2 75 cells / μm 2 100 cells / μm 2 125 cells / μm 2 150 cells / μm 2 175 cells / μm 2 200 / μm 2 250 cells / μm 2 The range formed by any one or two endpoints of the group. The range of the number density "n1" can be, for example, "25 particles / μm". 2 "Above", "250 / μm" 2 "below" or "25 cells / μm" 2 ~250 cells / μm 2 ".
[0054] The range of the average diameter of the closed vent (the overall average diameter of the first closed vent 2 and the second closed vent) can, for example, be a range formed by any one or two endpoints selected from the group consisting of 10 nm, 20 nm, 25 nm, 50 nm, 75 nm, 100 nm, 125 nm, 150 nm, 175 nm, 200 nm, 250 nm, and 300 nm. The range of the average diameter of the closed vent can, for example, be "above 10 nm", "below 300 nm", or "10 nm to 300 nm".
[0055] For example, the average diameter "r1" of the first occluded hole 2 can be smaller than the average diameter "r2" of the second occluded hole 4. The range of the ratio "r1 / r2" of the average diameter "r1" of the first occluded hole 2 relative to the average diameter "r2" of the second occluded hole 4 can, for example, be a range formed by any one or two endpoints selected from the group consisting of 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, and 0.9. The range of the ratio "r1 / r2" can, for example, be "greater than 0.05", "less than 0.9", or "0.05 to 0.9".
[0056] The range of the average diameter "r1" of the first closed vent 2 can, for example, be a range formed by any one or two endpoints selected from the group consisting of 10nm, 20nm, 25nm, 50nm, 75nm, 100nm, 125nm, 150nm, 175nm, 200nm, 250nm, and 300nm. The range of the average diameter "r1" of the first closed vent 2 can, for example, be "above 10nm", "below 300nm", or "10nm to 300nm".
[0057] Secondary particles 20 can also have open pores (not shown). The number density of open pores can be smaller than that of closed pores. The number density of open pores can, for example, range from 0 pores / μm. 2 5 per μm 2 10 cells / μm 2 15 cells / μm 2 20 cells / μm 2 25 cells / μm 2 The range formed by any one or two endpoints of the group. The number density of pores can be, for example, "0 pores / μm". 2 "Above", "25 cells / μm" 2 "Below", "0 per μm" 2 ~25 cells / μm 2 "or 0 cells / μm" 2 ~5 per μm 2 ".
[0058] The first closed pore 2 and the second closed pore 4 may each have a smaller average particle size than the open pore. The range of the average diameter "r3" of the open pore may, for example, be a range formed by any one or two endpoints selected from the group consisting of 150 nm, 200 nm, 250 nm, 300 nm, 400 nm, 500 nm, and 600 nm. The range of the average diameter "r3" of the open pore may, for example, be "above 150 nm", "below 600 nm", or "150 nm to 600 nm".
[0059] The positive electrode active material can have any composition. For example, the positive electrode active material can contain at least one selected from the group consisting of a first particle (secondary particle 20) and a second particle (secondary particle 20). The first particle has a first composition. The second particle has a second composition. For example, it can satisfy a mass ratio such as "first particle:second particle = 6:4 to 9:1" or "first particle:second particle = 7:3 to 8:2".
[0060] The first component, for example, can be composed of the first formula "LiNi". x Co y Mn z O2 represents the value. In the first formula, the range of "x" can be, for example, a range formed by any one or two endpoints selected from the group of 0.70, 0.75, 0.80, 0.85, 0.90, 0.95, and 1.00. For example, it can satisfy the relationship "0.700≤x<1.00". In the first formula, the ranges of "y" and "z" can be, for example, a range formed by any one or two endpoints selected from the group of 0.05, 0.10, 0.15, and 0.20. For example, it can satisfy the relationship "0≤y≤0.20" and "0≤z≤0.20". The first component can, for example, include LiNi. 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.9 Co 0.05 Mn 0.05 O2, etc.
[0061] The second component can be, for example, from the second formula "LiNi". u Co v Mn w O2 represents the value. In the second formula, the range of "u" can be, for example, formed by any one or two endpoints selected from the group of 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, and 0.65. For example, it can satisfy the relationship "0.30≤u≤0.65". In the second formula, the ranges of "v" and "w" can be, for example, formed by any one or two endpoints selected from the group of 0.05, 0.10, 0.15, 0.20, 0.25, 0.30, and 0.35. For example, it can satisfy the relationship "0≤v≤0.35" and "0≤z≤0.35". The second component can, for example, include LiNi. 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 0.4 Co 0.3 Mn 0.3 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, LiNi0.5 Co 0.3 Mn 0.2 O2, LiNi 0.5 Co 0.4 Mn 0.1 O2, LiNi 0.5 Co 0.1 Mn 0.4 O2, LiNi 0.6 Co 0.3 Mn 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.6 Co 0.1 Mn 0.3 O2, etc.
[0062] For example, the first and second equations can satisfy relationships such as "0.8≤x<1.0", "0<2y≤v", "0<3z≤w", "0.5≤u≤0.6", "0.1≤v≤0.2" and "0.2≤w≤0.3". In the first and second equations, some or all of Co and Mn can be substituted, for example, Al.
[0063] The first and second particles can each independently contain large and small particles. A "large particle" refers to a primary particle with a peak having a relatively large modal diameter in the particle size distribution. A "small particle" refers to a primary particle with a peak having a relatively small modal diameter in the particle size distribution. The "modal diameter" refers to the particle size at the peak apex. The particle size distribution can be a number distribution or a volume distribution. The number distribution can be determined by microscopy. The volume distribution can be determined, for example, by laser diffraction. The range of the ratio of the modal diameter of the large particle peak to the modal diameter of the small particle peak can, for example, be a range formed by any one or two endpoints of a group selected from 2, 3, 4, 5, 6, 7, 8, 9, 10. The range of the ratio of the modal diameter of the large particle peak to the modal diameter of the small particle peak can, for example, be "greater than 2", "less than 10", or "2 to 10". For example, it can satisfy relationships such as "large particle:small particle = 9:1 to 6:4" or "large particle:small particle = 9:1 to 7:3" in terms of mass ratio.
[0064] The conductive material may include, for example, at least one selected from the group consisting of carbon black (acetylene black, Ketjen black "registered trademarks"), flake graphite, vapor-grown carbon fibers, carbon nanotubes, and graphene sheets. The flake graphite may, for example, have an average particle size larger than that of the secondary particles 20. The range of the ratio of the average particle size of the flake graphite to the average particle size of the secondary particles 20 may, for example, be a range formed by any one or two endpoints selected from the group consisting of 1.2, 1.5, 2, 3, 4, and 5. The range of the ratio of the average particle size of the flake graphite to the average particle size of the secondary particles 20 may, for example, be "more than 1.2", "less than 5", or "1.2 to 5".
[0065] The adhesive may, for example, comprise at least one selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyacrylic acid (PAA), carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR).
[0066] Manufacturing method
[0067] The positive electrode active material in this embodiment can be manufactured, for example, by the following method. A precursor (transition metal hydroxide) is formed through a crystallization reaction. Then, the precursor is mixed with a Li compound (LiOH, Li₂CO₃, etc.). The mixture is then subjected to a first firing in a firing furnace (e.g., a muffle furnace). The first firing is carried out under reduced pressure and at the melting temperature of Li (approximately 500°C). This allows Li to penetrate well to the grain boundaries. The reduced pressure atmosphere can be, for example, an atmosphere below 1 kPa. Then, a second firing is carried out under an oxygen atmosphere at a high temperature (700°C to 1100°C). During the second firing, components other than Li (H₂O, etc.) evaporate, thereby forming pores. It can be considered that primary particles fuse together to form a single primary particle, thus forming a first closed pore within the primary particle. It can be considered that in the portions where primary particles are not completely fused together, grain boundaries remain, forming a second closed pore. After the second firing, the fired material can be broken up using a pulverizer (e.g., a jet mill).
[0068] Example
[0069] No.1
[0070] Figure 3 This is a schematic flowchart illustrating the first synthesis method in this embodiment. The first synthesis method is used to produce the No. 1 positive electrode active material.
[0071] (a1) Crystallization
[0072] NiSO4, CoSO4, and MnSO4 are dissolved in ion-exchange water in a molar ratio of 8:1:1 to form a raw material aqueous solution. The concentration of the raw material aqueous solution is 30% by mass fraction.
[0073] Add a specified amount of NH3 aqueous solution to the reaction vessel. While stirring the NH3 aqueous solution with a stirrer, purge the reaction vessel with nitrogen gas. Add a specified amount of NaOH to the reaction vessel to adjust the pH to alkaline. Add the raw material aqueous solution and NH3 aqueous solution dropwise to the reaction vessel. Adjust the dropping rate of each aqueous solution to maintain a certain pH range in the reaction solution within the reaction vessel. Allow the precursor (transition metal hydroxide) to precipitate for 3 hours. Recover the precursor by filtration. Wash the precursor with water. That is, disperse the precursor in ion-exchanged water using a spoon or similar object. Recover the precursor again by filtration. Dry the precursor at 120°C for 16 hours.
[0074] (b1) Mixing
[0075] The precursor and LiOH are mixed in a mortar to obtain a mixture.
[0076] (c1) Firing
[0077] In a firing furnace, the mixture is fired at 700°C to 1100°C for 10 hours under an oxygen atmosphere to obtain the fired product.
[0078] (d1) Broken
[0079] The sintered material is broken up by jet milling, thereby adjusting the particle size of the secondary particles.
[0080] No.2
[0081] Figure 4 This is a schematic flowchart illustrating the second synthesis method in this embodiment. The positive electrode active material No. 2 is produced using the second synthesis method.
[0082] (a2) Crystallization
[0083] Prepare the precursor in the same way as for “(a1) crystallization”.
[0084] (b2) Mixing
[0085] The precursor and LiOH are mixed in a mortar to obtain a mixture.
[0086] (c2) First firing
[0087] In a firing furnace, the mixture is fired at 500°C for 1 hour under reduced pressure to obtain the first fired product.
[0088] (d2) Second firing
[0089] In a firing furnace, the mixture is fired at 700°C to 1100°C for 6 hours under an oxygen atmosphere to obtain a second fired product.
[0090] (e2) broken
[0091] The second sintered material is broken up by jet milling, thereby adjusting the particle size of the secondary particles.
[0092] evaluate
[0093] Manufacturing cylindrical lithium-ion secondary batteries (evaluation batteries). The composition of the evaluation battery is as follows.
[0094] Power generation element: wound type
[0095] Positive electrode: Positive electrode active material / AB / PVDF = 88 / 10 / 2 (mass ratio)
[0096] Negative electrode: Negative electrode active material (natural graphite), CMC, SBR
[0097] Electrolytes: LiPF6 (1 mol / L), EC / DMC / EMC = 3 / 4 / 3 (volume ratio)
[0098] The positive and negative electrodes are manufactured by coating a slurry onto the surface of a substrate (metal foil). A thin-film coater (with film thickness adjustment function) manufactured by Allgood Corporation is used as the coating apparatus. After coating, the film is dried at 80°C for 5 minutes.
[0099] Measure the initial resistance of the evaluation battery. After measuring the initial resistance, perform 100 charge-discharge cycles. Measure the resistance of the evaluation battery after the cycles. Divide the resistance after the cycles by the initial resistance to determine the rate of increase in resistance.
[0100] result
[0101] Figure 5 This is a table showing an example of the experimental results of this embodiment. Compared to No. 1, the rate of increase in resistivity is lower in No. 2. In No. 2, the number density of closed pores is greater than the number density of primary particles.
Claims
1. A positive electrode for a lithium-ion secondary battery, comprising a positive electrode active material, The positive electrode active material contains secondary particles. The secondary particle contains multiple primary particles. Closed pores are formed within the primary particles and at the grain boundaries between the primary particles. Furthermore, the number density of the closed pores is greater than the number density of the primary particles.
2. The positive electrode for a lithium-ion secondary battery according to claim 1, wherein, The density of the closed pores is 20 per μm. 2 above.
3. The positive electrode for a lithium-ion secondary battery according to claim 1 or 2, wherein, The average diameter of the closed pore is above 20 nm.
4. The positive electrode for a lithium-ion secondary battery according to claim 1 or 2, wherein, The number density of the primary particles is 1 particle / μm. 2 ~10 particles / μm 2 .
5. A positive electrode for a lithium-ion secondary battery, comprising a positive electrode active material. The positive electrode active material contains secondary particles. The secondary particle contains multiple primary particles. Closed pores are formed within the primary particles and at the grain boundaries between the primary particles. The average diameter of the closed pores located within the primary particles is smaller than the average diameter of the closed pores located at the grain boundaries. The average diameter of all the described closed pores is 20 nm to 100 nm. The number density of the primary particles is 1 particle / μm. 2 ~10 particles / μm 2 ,and, The density of the closed pores is 50 per μm. 2 ~150 cells / μm 2 .