A negative electrode sheet and its preparation method, a secondary battery and an electrochemical device

By combining low binder content and large-particle active materials with vacuum heat treatment, the electrode structure is optimized, solving the problem of uneven distribution of active materials in lithium-ion batteries and achieving high energy density and long lifespan battery performance.

CN123120628APending Publication Date: 2026-11-17ZHEJIANG LIWINON ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611305970.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-26
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium-ion batteries, after increasing the silicon content and particle size of the silicon-carbon anode, have defects in electrode structure and electrochemical performance, resulting in uneven distribution of active materials and uneven pore structure, which affects battery cycle life and safety.

Method used

By employing a negative electrode structure with low binder content, combined with large-particle active materials and specific vacuum heat treatment, the binder distribution and interface contact mode are optimized to form a dual stable structure of mechanical interlocking and chemical bonding, thereby improving adhesion and porosity consistency.

Benefits of technology

It enhances the adhesion and cohesion of the electrode sheets, reduces lithium plating in the later stages of cycling, and improves the energy density and cycle stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention discloses a negative electrode sheet, its preparation method, a secondary battery, and an electrochemical device. The negative electrode sheet includes a negative electrode current collector and a negative electrode coating disposed on the surface of the current collector. The negative electrode coating includes a negative electrode active material, a negative electrode conductive agent, a thickener, and a negative electrode binder. The negative electrode coating satisfies: K=(K1+K2+K3) / 3, 0.34<K<0.7; where K1 is the binder content factor, K1=(5-A) / 3, and A% is the mass percentage of the negative electrode binder in the negative electrode coating; K2 is the silicon-carbon secondary particle size factor, K2=(B-8) / 17, and B μm is the particle size of the negative electrode active material; K3 is the silicon doping factor, K3=(C-10) / 40, and C% is the mass percentage of silicon in the negative electrode active material. This negative electrode sheet has higher adhesion, cohesion, and porosity consistency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of new energy technology, specifically relating to a negative electrode sheet and its preparation method, a secondary battery, and an electrochemical device. Background Technology

[0002] With the rapid development of the new energy industry, lithium-ion batteries, thanks to their excellent energy storage characteristics, are widely used in power batteries, energy storage devices, and digital products. Market demands for their energy density, range, and energy storage efficiency continue to rise. In the research and development of lithium-ion battery cells, increasing the silicon content of the silicon-carbon anode, increasing the particle size of secondary silicon-carbon particles, and reducing the amount of electrode binder are currently the mainstream technical approaches in the industry to improve cell energy density and optimize battery energy storage performance. Increasing the silicon content leverages the high theoretical capacity of silicon materials to enhance the electrode's lithium storage capacity. Increasing the size of secondary silicon-carbon particles reduces the specific surface area of ​​the particles and lowers interfacial side reactions. Reducing the amount of binder increases the proportion of active material within the electrode, thereby comprehensively raising the upper limit of the cell's energy density.

[0003] However, this optimization approach has significant technical drawbacks, easily leading to defects in electrode structure and electrochemical performance. Reducing the binder content prevents the formation of a complete and uniform bonding network on the surface of the active material particles. Combined with the application of large-sized silicon-carbon secondary particles, this results in uneven distribution of active material within the electrode, forming numerous pores of varying sizes and disordered distribution. This defect not only significantly weakens the cohesive force between active material particles and the adhesion force between the active material and the current collector, causing a decrease in the overall structural stability of the electrode, but also disrupts the uniformity and connectivity of the electrode pores. During long-term charge-discharge cycles, uneven electrolyte wetting can occur, preventing some pores from fully contacting the electrolyte. This leads to differences in lithium-ion insertion / extraction kinetics, ultimately resulting in localized lithium-ion enrichment in the electrode, inducing severe lithium plating problems. This not only significantly reduces battery cycle life but also affects battery charge-discharge safety and stability, hindering the large-scale application of high-energy-density silicon-carbon anode lithium-ion batteries. Summary of the Invention

[0004] The present invention aims to at least solve one of the technical problems existing in the prior art. To this end, the present invention proposes a negative electrode sheet that has higher adhesion, cohesion and porosity consistency, and can reduce lithium deposition caused by local liquid interruption in the electrode sheet during the later stages of battery cycling.

[0005] The present invention also proposes a method for preparing the above-mentioned negative electrode sheet.

[0006] The present invention also proposes a secondary battery comprising the above-mentioned negative electrode sheet.

[0007] The present invention also proposes an electrochemical device comprising the above-mentioned negative electrode secondary battery.

[0008] According to one aspect of the present invention, a negative electrode sheet is provided, the negative electrode sheet comprising a negative electrode current collector and a negative electrode coating disposed on at least one side surface of the negative electrode current collector; the negative electrode coating comprising a negative electrode active material, a negative electrode conductive agent, a thickener and a negative electrode binder; The negative electrode coating satisfies: K=(K1+K2+K3) / 3, 0.34<K<0.7; Wherein, K1 is the binder content factor, K1=(5-A) / 3, and A% is the mass percentage of the negative electrode binder in the negative electrode coating; K2 is the particle size factor of silicon-carbon secondary particles, K2=(B-8) / 17, and B μm is the Dv50 particle size of the negative electrode active material. K3 is the silicon doping factor, K3=(C-10) / 40, and C% is the mass percentage of silicon in the negative electrode active material.

[0009] The main differences between the negative electrode sheet provided by this invention and conventional negative electrode sheet structures include: 1) Low binder content (high active material content, high energy density) and different distribution patterns: Conventional negative electrodes, due to their silicon-carbon structure, require 3%-5% binder, which affects the proportion of active material. The negative electrode sheet provided by this invention uses a lower binder content, thereby increasing the energy density of the battery cell.

[0010] 2) Large-particle negative electrode active materials can be added to the negative electrode: Conventional processes use 8-18 μm secondary particles, which have a large specific surface area and require more binder coverage. This invention increases the particle size to 12-25 μm and achieves high adhesion and high energy density with low binder content through interface characteristic optimization and contact mode upgrade. ① The increased particle size significantly reduces the specific surface area of ​​the particles, improving the adhesive coating efficiency per unit area. At the same time, the contact mode between particles is upgraded from "point contact" to "surface contact", greatly increasing the contact area. Combined with the interface anchoring of the adhesive, a dual stable structure of "mechanical interlocking + chemical bonding" is formed, significantly enhancing the adhesion.

[0011] ② The large-diameter secondary particles have abundant internal pores, which can buffer the volume expansion of silicon carbon, reduce the risk of particle breakage, reduce the generation of new interfaces, avoid secondary consumption of binder, and further improve long-term bonding stability.

[0012] 3) Further increase the silicon doping content: Excessive silicon doping can lead to insufficient adhesion of the electrode sheet during the later stages of cycling, resulting in electrode breakage and demolding. The negative electrode sheet provided by this invention can improve adhesion to prevent breakage problems caused by insufficient adhesion in the later stages.

[0013] In some embodiments of the present invention, the particle size of the negative electrode active material is 8-25 μm.

[0014] In some embodiments of the present invention, the particle size of the negative electrode active material is 15-25 μm.

[0015] In some embodiments of the present invention, the mass percentage of the negative electrode binder in the negative electrode coating is 1%-5%.

[0016] In some embodiments of the present invention, the silicon element in the negative electrode active material is 10%-50% by mass.

[0017] In some embodiments of the present invention, the silicon element in the negative electrode active material is 25%-50% by mass.

[0018] In some embodiments of the present invention, the mass ratio of the negative electrode active material, negative electrode binder, thickener and negative electrode conductive agent is (93-97):(1-5):(1-3):(1-3).

[0019] In some embodiments of the present invention, the mass ratio of the negative electrode active material, negative electrode binder, thickener and negative electrode conductive agent is (93-97):(1-5):(1-2):(1-2).

[0020] In some embodiments of the present invention, the negative electrode active material includes carbon-based active materials and silicon-based active materials.

[0021] In some embodiments of the present invention, the negative electrode active material includes at least one of natural graphite particles, synthetic graphite particles, hard carbon, soft carbon, mesophase carbon microspheres, Sn, SnO2, SnO, LTO, Si materials, silicon-carbon composite materials, silicon-nitrogen composite materials, and silicon-oxygen composite materials. The negative electrode active material of the present invention is not limited to the above-mentioned materials, but also includes other materials that can be used as negative electrode active materials for batteries.

[0022] In some embodiments of the present invention, the negative electrode current collector is a metal foil or a composite current collector.

[0023] In some embodiments of the present invention, the metal foil includes copper foil.

[0024] In some embodiments of the present invention, the composite current collector includes an insulating support layer, a first metal layer, and a second metal layer, wherein the insulating support layer is a polymer, and the first metal layer and the second metal layer are respectively disposed on the upper and lower surfaces of the insulating metal layer; both the first metal layer and the second metal layer are copper metal layers, and the polymer is selected from one or more of terephthalate, polyamide, polyimide, polyethylene, polypropylene, polystyrene, polyvinyl chloride, and polyethylene terephthalate.

[0025] In some embodiments of the present invention, the negative electrode conductive agent includes at least one of carbon, carbon black, graphite, expanded graphite, graphene, graphene nanosheets, carbon fiber, carbon nanofiber, graphitized carbon sheet, carbon tube, carbon nanotube, activated carbon, and mesoporous carbon.

[0026] In some embodiments of the present invention, the negative electrode binder includes at least one of the following: polyacrylic acid, polymethacrylic acid, polyacrylate, polymethacrylate, polyacrylamide, styrene-butadiene rubber, acrylic styrene-butadiene rubber, acrylic acid-acrylonitrile-acrylamide copolymer, acrylic acid-acrylonitrile-acrylate copolymer, acrylonitrile-butadiene rubber, nitrile rubber, acrylonitrile-styrene-butadiene copolymer, acryloyl rubber, butyl rubber, fluororubber, polytetrafluoroethylene, polyvinyl alcohol, polyvinyl acetate, polyepoxychloropropane, polyphosphonic acid, polyacrylonitrile, polystyrene, latex, acrylic resin, phenolic resin, epoxy resin, carboxymethyl cellulose, hydroxypropyl cellulose, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl cellulose, carboxymethyl chitosan, polyester, polyamide, polyether, polyimide, polycarboxylic acid ester, polycarboxylic acid, polyurethane, alginate, fluorinated polymer, chlorinated polymer, and polyvinylidene fluoride. The negative electrode binder of the present invention is not limited to the above materials, but also includes other materials that can be used as battery negative electrode binders.

[0027] In some embodiments of the present invention, the thickener includes sodium carboxymethyl cellulose.

[0028] According to a second aspect of the present invention, a method for preparing the negative electrode sheet described in the first aspect of the present invention is provided, the method comprising the following steps: The negative electrode active material, negative electrode conductive agent, thickener and negative electrode binder are mixed to obtain a negative electrode slurry. The negative electrode slurry is coated on the surface of the negative electrode current collector, dried, rolled and then heat-treated to obtain a negative electrode sheet. The heat treatment conditions include heating at 200℃-350℃ for 3-7 h under vacuum conditions.

[0029] Conventional silicon-carbon anodes rely on a high binder content of 3%-5% to compensate for poor interparticle contact and uneven surface distribution. This invention utilizes specific heat treatment conditions to position and distribute the binder at specific interfaces, achieving a binding mechanism that reduces binder usage while ensuring stable adhesion and electrochemical performance. 1) After being baked at high temperature, the binder softens and redistributes itself, preferentially distributing itself at the interface of silicon-carbon particles and in the pores and gaps, rather than being enriched on the surface. A small amount of binder can form a three-dimensional anchoring network, which not only enhances the cohesion between particles, but also prevents the surface of active materials from being covered by an insulating layer, reduces interfacial impedance, and ensures smooth ion and electron transport.

[0030] 2) The increased porosity resulting from low binder content provides a buffer space for the volume expansion of silicon-carbon, reduces the risk of electrode cracking and pulverization during cycling, maintains the integrity of the electrode structure, and ensures long-term cycling performance.

[0031] According to a third aspect of the present invention, a secondary battery is provided, the secondary battery comprising the negative electrode sheet described in the first aspect of the present invention or the negative electrode sheet prepared by the preparation method described in the second aspect of the present invention.

[0032] In some embodiments of the present invention, the secondary battery further includes a positive electrode, a separator, and an electrolyte.

[0033] In some embodiments of the present invention, the diaphragm is located between the positive and negative electrodes.

[0034] According to a fourth aspect of the present invention, an electrochemical device is provided, the electrochemical device comprising the secondary battery described in the third aspect of the present invention.

[0035] The present invention has at least the following beneficial effects: The negative electrode sheet provided by this invention has a lower binder content and more uniform distribution compared to conventional negative electrode sheets. Under the premise of using large-particle active materials, specific vacuum heat treatment enables the binder to effectively fill the pores between the active materials, improve the overall adhesion, cohesion and pore consistency of the material, and reduce lithium deposition caused by local liquid interruption in the later stages of cycling. Attached Figure Description

[0036] The present invention will be further described below with reference to the accompanying drawings and embodiments, wherein: Figure 1 The images shown are SEM images of the negative electrode sheet in Embodiment 1 of the present invention before and after vacuum heating; the scale bar is 300 nm. Figure 2 This is a schematic diagram of the experimental setup for porosity testing in the experimental examples of this invention. Detailed Implementation

[0037] The following will describe the concept and technical effects of the present invention clearly and completely with reference to embodiments, so as to fully understand the purpose, features and effects of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are all within the scope of protection of the present invention.

[0038] Example 1 This embodiment provides a negative electrode sheet, which is composed of a negative electrode current collector copper foil and a negative electrode coating disposed on both sides of the negative electrode current collector; the negative electrode coating is composed of a negative electrode active material, a negative electrode conductive agent, a thickener and a negative electrode binder.

[0039] The negative electrode active material is silicon-carbon secondary particles, purchased from Shanshan Technology, item number SG90; the particle size of the silicon-carbon secondary particles is 15 μm, and the silicon doping content of the silicon-carbon secondary particles is 25%, which refers to the mass percentage of silicon in the silicon-carbon secondary particles.

[0040] The negative electrode conductive agent in the negative electrode coating is conductive carbon black Super P.

[0041] The thickener in the negative electrode coating is sodium carboxymethyl cellulose (CMC).

[0042] The negative electrode binder in the negative electrode coating is styrene-butadiene rubber (SBR).

[0043] In the negative electrode coating, the mass ratio of silicon-carbon secondary particles, SBR, CMC and conductive carbon black Super P is 96.5:1.2:1.2:1.1.

[0044] The preparation method of the negative electrode sheet is as follows: The components of the negative electrode coating are added to water and mixed evenly to form a negative electrode slurry. The negative electrode slurry is then evenly coated onto the surface of the negative electrode current collector copper foil, baked and dried, and then rolled (compacted density 1.7 g / cm³). 3 The negative electrode sheet is obtained by rolling it into a roll and vacuum heating it at 110℃ for 5 hours.

[0045] The surface morphology of the aforementioned negative electrode sheet before and after vacuum heating is as follows: Figure 1 As shown, Figure 1 The SEM results showed that the active materials in the untreated sample had a large number of pores in some parts, and the overall pore distribution was not very consistent. However, the active materials that were treated by vacuum heating softened at high temperature, and the adhesive filled the gaps, which improved the pore consistency and increased the adhesion and cohesion.

[0046] Example 2 This embodiment provides a negative electrode sheet, the only difference between which is the preparation method and that of Embodiment 1: the vacuum heating temperature is adjusted to 200°C, and the remaining steps are consistent with those of Embodiment 1.

[0047] Example 3 This embodiment provides a negative electrode sheet, the only difference between which is the preparation method and that of Embodiment 1: the vacuum heating temperature is adjusted to 250°C, and the remaining steps are consistent with those of Embodiment 1.

[0048] Example 4 This embodiment provides a negative electrode sheet, the only difference between which is the preparation method and that of Embodiment 1: the vacuum heating temperature is adjusted to 300°C, and the remaining steps are consistent with those of Embodiment 1.

[0049] Example 5 This embodiment provides a negative electrode sheet, the only difference between which is the preparation method and that of Embodiment 1: the vacuum heating temperature is adjusted to 350°C, and the remaining steps are consistent with those of Embodiment 1.

[0050] Example 6 This embodiment provides a negative electrode sheet, which consists of a negative electrode current collector copper foil and a negative electrode coating disposed on both sides of the negative electrode current collector; the negative electrode coating consists of a negative electrode active material, a conductive agent, a thickener and a binder.

[0051] The negative electrode active material is silicon-carbon secondary particles with a particle size of 15 μm and a silicon doping content of 25%.

[0052] The conductive agent in the negative electrode coating is conductive carbon black Super P.

[0053] The thickener in the negative electrode coating is sodium carboxymethyl cellulose (CMC).

[0054] The binder in the negative electrode coating is styrene-butadiene rubber (SBR).

[0055] In the negative electrode coating, the mass ratio of silicon-carbon secondary particles, SBR, CMC and conductive carbon black Super P is 96.7:1.0:1.2:1.1.

[0056] The method for preparing the negative electrode sheet is as follows: the components of the negative electrode coating are added to water and mixed evenly to form a negative electrode slurry. The negative electrode slurry is evenly coated on the surface of the negative electrode current collector copper foil, baked and dried, and rolled into a roll. The roll is then heated under vacuum at 300°C for 5 hours to obtain the negative electrode sheet.

[0057] Among them, the binder content A% is 3%, and the binder content factor K1=(5-A) / 3; the particle size B of the silicon-carbon secondary particles is 15μm, and the particle size factor K2=(B-8) / 17; the silicon doping content C% of the silicon-carbon secondary particles is 25%, and the silicon doping factor K3=(C-10) / 40; the energy density factor K=(K1+K2+K3) / 3, and the larger the K value, the higher the energy density of the secondary battery cell made from the negative electrode sheet.

[0058] Example 7 This embodiment provides a negative electrode sheet, the only difference between which is the preparation method and that of Example 6: the particle size of the silicon-carbon secondary particles is adjusted to 25 μm, and the remaining steps are consistent with those of Example 6.

[0059] Example 8 This embodiment provides a negative electrode sheet, the only difference between which is the preparation method and that of Example 6: the silicon doping content of the silicon-carbon secondary particles is adjusted to 10%, and the remaining steps are consistent with those of Example 6.

[0060] Example 9 This embodiment provides a negative electrode sheet, the only difference between which is the preparation method and that of Example 6: the silicon content of the secondary silicon-carbon particles is adjusted to 50%, and the remaining steps are consistent with those of Example 6.

[0061] Example 10 This embodiment provides a negative electrode sheet, the only difference between which is the preparation method and that of Example 6: the particle size of the silicon-carbon secondary particles is adjusted to 8 μm and the binder content is adjusted to 1%, while the remaining steps are the same as those of Example 6.

[0062] Example 11 This embodiment provides a negative electrode sheet, the only difference between which is the preparation method and that of Example 6: the particle size of the silicon-carbon secondary particles is adjusted to 8 μm, and the remaining steps are consistent with those of Example 6.

[0063] Example 12 This embodiment provides a negative electrode sheet, the only difference between which is the preparation method and that of Example 6: the binder content is adjusted to 4%, the particle size of the silicon-carbon secondary particles is adjusted to 20 μm, and the silicon doping content of the silicon-carbon secondary particles is adjusted to 5%. All other steps are the same as those in Example 6.

[0064] Example 13 This embodiment provides a negative electrode sheet, the only difference between which is the preparation method and that of Example 6: the binder content is adjusted to 5%, and the remaining steps are consistent with those of Example 6.

[0065] Comparative Example 1 This comparative example provides a negative electrode sheet whose preparation method differs from that of Example 1 only in that the vacuum heating step is omitted, and the electrode is simply placed in a vacuum chamber and left to stand for 5 hours. All other steps are consistent with those of Example 1.

[0066] Comparative Example 2 This comparative example provides a negative electrode sheet, the preparation method of which differs from that of Example 1 only in that the vacuum heating temperature is adjusted to 360°C, and the remaining steps are consistent with those of Example 1.

[0067] Comparative Example 3 This comparative example provides a negative electrode sheet, the preparation method of which differs from that of Example 6 only in that the binder content is adjusted to 10%, and the remaining steps are consistent with those of Example 6.

[0068] Comparative Example 4 This comparative example provides a negative electrode sheet, the preparation method of which differs from that of Example 6 only in that the particle size of the silicon-carbon secondary particles is adjusted to 50 μm, and the remaining steps are consistent with those of Example 6.

[0069] Comparative Example 5 This comparative example provides a negative electrode sheet whose preparation method differs from that of Example 6 only in that the silicon doping content of the silicon-carbon secondary particles is adjusted to 1%, while the remaining steps are consistent with those of Example 6.

[0070] Test case This experiment tested the porosity consistency, adhesion, and cohesion of the negative electrode sheets provided in Examples 1-5 and Comparative Examples 1-2. It also measured the cell energy density of the secondary batteries prepared from the negative electrode sheets provided in Examples 6-12 and Comparative Examples 3-5. The specific experimental methods and results are as follows: 1. Determination of porosity consistency, adhesion, and cohesion. 1) The porosity of the negative electrode sheets provided in Examples 1-5 and Comparative Examples 1-2 was tested in accordance with the national standard "GB / T 10799-2008 Determination of open and closed cell volume percentage of rigid foamed plastics".

[0071] Experimental principle: A schematic diagram of the experimental setup is shown below. Figure 2 As shown. Helium is used as the gas medium to displace the air in the voids and pores of the material, creating a sealed environment in the sample chamber. Valve 1 is opened, allowing gas to enter the sample chamber. After reaching a certain pressure, the valve closes. Once the sample and gas reach equilibrium, the pressure sensor reads pressure P1. Then, valve 2 is opened, allowing gas to diffuse from the sample chamber into the expansion chamber. After the gas and sample in both chambers reach equilibrium, the pressure sensor reads pressure P2. Finally, based on the ideal gas law PV=nRT, the true volume V of the material is calculated. 真 .

[0072] Porosity calculation formula: Among them, V 表 V is the apparent volume of the negative electrode. 表 =Area × Thickness × Number of negative electrode plates; V 真 V0 represents the actual volume of the negative electrode sheet, i.e., the volume obtained by the true density meter. V0 represents the current collector volume of the negative electrode sheet, V0 = area × current collector thickness × number of negative electrode sheets.

[0073] Porosity consistency calculation: The negative electrode sheet to be tested was divided into 9 regions of 100μm×100μm under SEM. The porosity of each of the 9 regions was calculated. Finally, the standard deviation of the 9 sets of data was calculated to obtain the porosity consistency. The results are shown in Table 1.

[0074] 2) Adhesion test: The adhesion of the negative electrode sheet was tested on a high-tensile testing machine. The negative electrode sheet was attached to the material surface with high-viscosity yellow adhesive, then one side was fixed and the other side was pulled with a clamp. The reading was taken when the equipment was stable. Comparative Example 1 was used as a control group to calculate the improvement rate of adhesion. The results are shown in Table 1.

[0075] 3) Cohesion test: Take three sections of double-sided tape with a length ≥15 cm and attach them to the material area of ​​the short film surface of the negative electrode sheet along the coating direction; cut off the area with double-sided tape and cut it into three long strips; peel off the sticker of the double-sided tape and attach the adhesive side to one end of the glass plate; peel off the anode current collector, leaving a layer of double-sided tape and a single layer of negative electrode coating on the glass plate; take three sections of transparent adhesive with a length ≥20 cm and attach them to the single layer of negative electrode coating along the length direction, making sure the transparent adhesive completely covers the coating. Subsequently, the cohesion was tested using the adhesion test method. Comparative Example 1 was used as a control group to calculate the cohesion improvement rate. The results are shown in Table 1.

[0076] Table 1. Vacuum heating conditions and porosity consistency, adhesion, and cohesion test results for Examples 1-5 and Comparative Examples 1-2.

[0077] As shown in Table 1, when the vacuum heating temperature t1 satisfies 100℃<t1≤350℃, the adhesive is in a softened state. At this time, it will flow and redistribute into the pores, improving the pore uniformity. The adhesion and cohesion also increase with the increase of the vacuum heating temperature. The sudden and significant decrease above 350℃ is due to the continuous softening of the adhesive during the 100℃ < t1 ≤ 350℃ range. Before reaching 200℃, the adhesion and cohesion increase rapidly because most adhesives (PAA / SBR) have a glass transition temperature of 100℃ to 200℃. At this temperature, the adhesive softens rapidly, redistributes, and fills the pores between the active materials, significantly improving porosity consistency and increasing adhesion and cohesion. In the 200℃ to 350℃ range, the distribution of the already glass-transformed adhesive is basically fixed, and it will no longer rapidly increase porosity, causing adhesion and cohesion to stabilize. Above 350℃, the adhesive decomposition temperature is reached, and some adhesive begins to decompose, reducing the amount of adhesive. Therefore, the porosity difference increases, and adhesion and cohesion drop sharply, even worse than before vacuum heating treatment.

[0078] 2. Cell energy density measurement This experiment prepared secondary batteries based on the negative electrode sheets provided in Examples 6-12 and Comparative Examples 3-5 and tested their cell energy density. The results are shown in Table 2.

[0079] Table 2. Negative electrode coating composition parameters of negative electrode sheets in Examples 6-12 and Comparative Examples 3-5, and cell energy density test results of the secondary batteries prepared therefrom.

[0080] As shown in Table 2, the energy density of the secondary battery made from the negative electrode sheet provided by this invention is closely related to the binder content, large secondary silicon-carbon particles, and high silicon doping in the negative electrode sheet. Using low binder content, large secondary silicon-carbon particles, and high silicon doping significantly improves the cell's energy density. Compared to Example 6, Comparative Example 3, by increasing the binder content to 10%, resulted in a significantly lower final energy density. Compared to Example 6, Comparative Examples 4 and 5, by increasing the particle size of the secondary silicon-carbon particles and decreasing the silicon doping, respectively, led to a decrease in cell energy density.

[0081] The embodiments of the present invention have been described in detail above with reference to the accompanying drawings. However, the present invention is not limited to the above embodiments, and various changes can be made within the scope of knowledge possessed by those skilled in the art without departing from the spirit of the present invention. Furthermore, the embodiments of the present invention and the features thereof can be combined with each other unless otherwise specified.

Claims

1. A negative electrode sheet, characterized in that, The negative electrode sheet includes a negative electrode current collector and a negative electrode coating disposed on at least one side surface of the negative electrode current collector; the negative electrode coating includes a negative electrode active material, a negative electrode conductive agent, a thickener, and a negative electrode binder; The negative electrode coating satisfies: K=(K1+K2+K3) / 3, 0.34<K<0.7; Wherein, K1 is the binder content factor, K1=(5-A) / 3, and A% is the mass percentage of the negative electrode binder in the negative electrode coating; K2 is the particle size factor of silicon-carbon secondary particles, K2=(B-8) / 17, and B μm is the Dv50 particle size of the negative electrode active material. K3 is the silicon doping factor, K3=(C-10) / 40, and C% is the mass percentage of silicon in the negative electrode active material.

2. The negative electrode sheet according to claim 1, characterized in that, The particle size of the negative electrode active material is 8-25 μm.

3. The negative electrode sheet according to claim 1, characterized in that, The negative electrode binder in the negative electrode coating has a mass percentage of 1%-5%.

4. The negative electrode sheet according to claim 1, characterized in that, The silicon element in the negative electrode active material has a mass percentage of 10%-50%.

5. The negative electrode sheet according to claim 3, characterized in that, The mass ratio of the negative electrode active material, negative electrode binder, thickener and negative electrode conductive agent is (93-97):(1-5):(1-3):(1-3).

6. The negative electrode sheet according to claim 1, characterized in that, The negative electrode active material includes carbon-based active materials and silicon-based active materials.

7. The method for preparing the negative electrode sheet according to any one of claims 1-6, characterized in that, The preparation method includes the following steps: The negative electrode active material, negative electrode conductive agent, thickener and negative electrode binder are mixed to obtain a negative electrode slurry. The negative electrode slurry is coated on the surface of the negative electrode current collector, dried, rolled and heat-treated to obtain a negative electrode sheet. The heat treatment conditions include heating at 200℃-350℃ for 3-7 hours under vacuum conditions.

8. A secondary battery, characterized in that, The secondary battery includes the negative electrode sheet according to any one of claims 1-6 or the negative electrode sheet prepared by the preparation method according to claim 7.

9. The secondary battery according to claim 8, characterized in that, The secondary battery also includes a positive electrode, a separator, and an electrolyte.

10. An electrochemical device, characterized in that, The electrochemical device includes the secondary battery as described in claim 8 or 9.