Carbon black dispersion liquid for lithium ion battery positive electrode slurry and preparation method and application thereof

By combining hydrogenated nitrile rubber and styrene-butadiene-styrene block copolymer in a specific weight ratio, a dense coating network was constructed, which solved the problem of uneven carbon black dispersion in lithium-ion battery cathode slurry, and achieved a carbon black dispersion with high stability and low viscosity, thereby improving battery performance.

CN123120732APending Publication Date: 2026-11-17XIAMEN HEWU RUISHENG NEW MATERIALS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611175924.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-04
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Uneven carbon black dispersion in existing lithium-ion battery cathode slurries leads to increased cell internal resistance and reduced cycle life. Furthermore, existing dispersants exhibit abnormally high viscosity and poor storage stability.

Method used

Hydrogenated nitrile rubber and styrene-butadiene-styrene block copolymer in a specific weight ratio were used as dispersants. A dense coating network was constructed by chemically anchoring the polar cyano groups of hydrogenated nitrile rubber to the carbon black surface and by the π-π stacking effect of styrene-butadiene-styrene block copolymer, thereby improving the dispersion stability of carbon black.

Benefits of technology

It significantly reduced the initial viscosity and scraper fineness of the dispersion, inhibited secondary sedimentation and flocculation of carbon black particles, and endowed the carbon black dispersion with excellent long-term stability and processing adaptability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The application discloses a carbon black dispersion liquid for a lithium ion battery positive electrode slurry and a preparation method and application thereof, and relates to the technical field of batteries.The carbon black dispersion liquid comprises the following raw materials by weight: 8-40 parts of carbon black, 1-10 parts of hydrogenated butyronitrile rubber, 0.04-0.48 parts of styrene-butadiene-styrene block copolymer and 170-960 parts of a dispersion medium;the content of acrylonitrile in the hydrogenated butyronitrile rubber is 20-40 wt%, and the Mooney viscosity ML(1+4) 100 DEG C is 30-80.The application has the effect of improving dispersion stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of battery technology, and in particular to a carbon black dispersion for lithium-ion battery cathode slurry, its preparation method, and its application. Background Technology

[0002] Lithium-ion rechargeable batteries, with their high energy density, are widely used in consumer electronics, new energy vehicles, and energy storage, and market demand continues to grow. The positive electrode system of a lithium-ion battery mainly consists of positive electrode active material, conductive carbon black, binder, and metal current collector. To improve the energy density of the cell, the industry generally tends to reduce the amount of non-active components such as conductive agents and additives. Highly conductive carbon blacks such as Super P possess high structure and large specific surface area, resulting in excellent conductivity; however, they have a strong tendency to agglomerate, making uniform dispersion difficult in organic solvent systems. Poor carbon black dispersion easily leads to uneven distribution of the conductive network inside the electrode, thereby causing increased internal resistance and reduced cycle life.

[0003] Current industrial processes generally employ a method of first pre-dispersing carbon black with a polymeric dispersant to prepare a conductive slurry, and then compounding it with positive electrode active powder and a binder to prepare a positive electrode coating slurry. The pre-dispersed carbon black slurry must meet two requirements: first, it must effectively deagglomerate in the initial dispersion stage, resulting in uniform particle distribution; second, the slurry must possess long-term storage stability, with no abnormal increase in viscosity or sedimentation / stratification during standing. If secondary agglomeration of carbon black occurs during storage, the slurry viscosity will significantly increase, directly deteriorating the coating smoothness and ultimately leading to dispersion of the internal resistance of the finished electrode and poor battery consistency.

[0004] Currently, commonly used dispersants for lithium-ion battery carbon black mainly include cellulose-based dispersants, polyacrylic acid resins, and polyvinylpyrrolidone (PVP). Cellulose-based dispersants are particularly prone to generating numerous microbubbles during slurry preparation, leading to pinholes and pits on the coated electrode, increasing the cell's internal resistance. Polyacrylic acid and PVP dispersants have insufficient interfacial bonding strength with the carbon black surface, causing the carbon black to agglomerate and separate during long-term storage. Existing optimization methods, such as adding organic acids or alkalis, can improve dispersion in the short term, but residual acidic or alkaline substances can harm the battery's electrochemical performance. Forcibly dispersing the carbon black by extending the milling or high-speed dispersion time results in high equipment energy consumption, long production cycles, and significantly increased manufacturing costs.

[0005] Chinese patent CN108028091A discloses a technical solution using hydrogenated nitrile butadiene rubber (NBR) as a carbon black dispersant. By controlling the proportions of structural units that can interact with carbon black and those that can interact with the dispersion medium, carbon black is uniformly dispersed in the medium. However, hydrogenated NBR has limited depolymerization and dispersion capabilities in high-viscosity carbon black dispersions. High-structure carbon black particles are prone to re-agglomeration during storage, resulting in relatively poor slurry storage stability. Summary of the Invention

[0006] To improve dispersion stability, this application provides a carbon black dispersion for lithium-ion battery cathode slurry, its preparation method, and its application.

[0007] In a first aspect, this application provides a carbon black dispersion for lithium-ion battery cathode slurry, employing the following technical solution: A carbon black dispersion for lithium-ion battery cathode slurry comprises the following raw materials in parts by weight: 8-40 parts carbon black, 1-10 parts hydrogenated nitrile rubber, 0.04-0.48 parts styrene-butadiene-styrene block copolymer, and 170-960 parts dispersion medium; wherein the hydrogenated nitrile rubber has an acrylonitrile content of 20-40 wt% and a Mooney viscosity ML(1+4) of 30-80 at 100°C.

[0008] By adopting the above technical solution, the strongly polar cyano groups on the hydrogenated nitrile rubber molecular chain can form a strong chemical anchoring effect with the active oxygen-containing functional groups on the carbon black surface, while the styrene blocks in the styrene-butadiene-styrene block copolymer molecular chain form a strong interfacial bond with the graphite microcrystals on the carbon black surface through the π-π stacking effect. This dual effect of "polar adsorption + π-π stacking" not only effectively fills the physical gaps generated when a single hydrogenated nitrile rubber molecular chain coats carbon black, but also significantly reduces the surface energy between carbon black particles, thereby greatly enhancing the depolymerization and wetting ability of high-structure carbon black.

[0009] Optionally, the weight ratio of the hydrogenated nitrile rubber and the styrene-butadiene-styrene block copolymer is 1:(0.04-0.1).

[0010] By adopting the above technical solution, this application uses a specific weight ratio of hydrogenated nitrile butadiene rubber and styrene-butadiene-styrene block copolymer to optimize the dispersibility of the two types of polymeric materials on the carbon black surface. The main dispersant, hydrogenated nitrile butadiene rubber, with its high content of polar cyano groups, forms a strong chemical anchor with the active sites of carbon black, constructing a stable main coating layer with steric hindrance effect. The styrene-butadiene-styrene block copolymer utilizes the π-π stacking effect between its styrene blocks and the carbon black graphite microcrystals to efficiently fill and locally densify the microscopic gaps created by the hydrogenated nitrile butadiene rubber molecular chain coating. At this preferred weight ratio, the polar anchoring of the hydrogenated nitrile butadiene rubber and the π-π stacking of the styrene-butadiene-styrene block copolymer form a dense coating network of "main-auxiliary synergy and orientation complementarity," which not only effectively breaks the strong agglomeration tendency of high-structure carbon black and significantly reduces the initial viscosity and scraper fineness of the dispersion, but also significantly inhibits secondary sedimentation and flocculation during storage, giving the carbon black dispersion excellent long-term stability and processing adaptability.

[0011] Optionally, the weight-average molecular weight of the styrene-butadiene-styrene block copolymer is 100,000-200,000 g / mol.

[0012] By adopting the above technical solution, this application uses a styrene-butadiene-styrene block copolymer with a weight-average molecular weight of 100,000-200,000 g / mol, which enables the auxiliary dispersant to possess both sufficient chain length extension and excellent surface adsorption conformation in the dispersion medium. Within this specific high molecular weight range, the styrene segments of the styrene-butadiene-styrene block copolymer can form a stable and deep anchorage on the surface of carbon black graphite microcrystals due to strong π-π stacking. At the same time, its sufficiently long flexible butadiene segments can construct an elastic barrier layer with significant steric hindrance effect, effectively preventing the depolymerized carbon black particles from re-aggregating and re-aggregating due to van der Waals forces under thermal motion.

[0013] Optionally, the carbon black is at least one of Super P, Ketjen black, and acetylene black.

[0014] By adopting the above technical solution, this application uses conductive carbon blacks with high structural density and high specific surface area, such as Super P, Ketjen black, and acetylene black. Utilizing the abundant oxygen-containing active functional groups on their surface and the microcrystalline lamellar structure with high graphitization characteristics, they form a strong chemical anchoring effect with the high content of polar cyano groups on the hydrogenated nitrile rubber molecular chain. At the same time, the styrene segments in the styrene-butadiene-styrene block copolymer can also be strongly inserted into the aromatic ring clusters on the carbon black surface through the π-π stacking effect, thereby maintaining the initial slurry with low viscosity and high fluidity.

[0015] Optionally, the particle size of the carbon black is 20-100 nm.

[0016] By adopting the above technical solution, this application uses 20-100nm carbon black, which helps to construct a dense and efficient conductive network.

[0017] Optionally, the hydrogenated nitrile butadiene rubber is one of a first hydrogenated nitrile butadiene rubber, a second hydrogenated nitrile butadiene rubber, and a third hydrogenated nitrile butadiene rubber; the acrylonitrile content of the first hydrogenated nitrile butadiene rubber is 20-25 wt%, and the dispersion medium is xylene; the acrylonitrile content of the second hydrogenated nitrile butadiene rubber is >25-33 wt%, and the dispersion medium is cyclohexanone; the acrylonitrile content of the third hydrogenated nitrile butadiene rubber is >33-40 wt%, and the dispersion medium is N-methylpyrrolidone.

[0018] By adopting the above technical solution, this application selects dispersion media with corresponding compatibility polarity levels based on the acrylonitrile content of the hydrogenated nitrile butadiene rubber (NBR): xylene is matched with NBR containing 20-25 wt% acrylonitrile; cyclohexanone is matched with NBR containing >25-33 wt% acrylonitrile; and N-methylpyrrolidone is matched with NBR containing >33-40 wt% acrylonitrile. Through precise matching of the dispersion media with the polarity and compatibility of the NBR, the complete dissolution of the NBR and efficient wetting and dispersion of the carbon black are achieved, which is beneficial for obtaining a carbon black slurry with uniform dispersion and excellent storage stability.

[0019] Secondly, this application provides a method for preparing a carbon black dispersion for lithium-ion battery cathode slurry, employing the following technical solution: A method for preparing a carbon black dispersion for lithium-ion battery cathode slurry includes the following steps: S1. Divide the dispersion medium into two parts; add hydrogenated nitrile rubber and styrene-butadiene-styrene block copolymer to one part of the dispersion medium in sequence, heat and stir to obtain a premix; S2. Add carbon black to the premixed liquid, then add the remaining dispersion medium, stir evenly to obtain a carbon black dispersion for lithium-ion battery cathode slurry.

[0020] Optionally, in step S1, the solid content in the premixed liquid is 4-10 wt%.

[0021] By adopting the above technical solution, this application precisely limits the solid content of the dispersant and dispersant premix in step S1 to 4-10 wt%, which is beneficial to promote the full dissociation and unfolding of the polymer chains of hydrogenated nitrile rubber and styrene-butadiene-styrene block copolymer from the physical entanglement state at room temperature, exposing a large number of effective polar cyano anchoring sites and styrene π-π adsorption sites; when carbon black is added for mixing in the subsequent process, the fully unfolded polymer chains can quickly penetrate into the high surface energy agglomeration pores of carbon black nanoparticles, thereby achieving all-round and deep wetting and coating.

[0022] In summary, this application includes at least one of the following beneficial technical effects: 1. This application uses a specific weight ratio of hydrogenated nitrile butadiene rubber and styrene-butadiene-styrene block copolymer as a dispersant composition. The main dispersant, hydrogenated nitrile butadiene rubber, with its high content of polar cyano groups, forms a strong chemical anchor with the active sites of carbon black, constructing a stable main coating layer with steric hindrance effect. The styrene-butadiene-styrene block copolymer utilizes the π-π stacking effect between its styrene blocks and the carbon black graphite microcrystals to efficiently fill and locally densify the microscopic gaps created by the hydrogenated nitrile butadiene rubber molecular chain coating. At this preferred weight ratio, the polar anchoring of the hydrogenated nitrile butadiene rubber and the π-π stacking of the styrene-butadiene-styrene block copolymer form a dense coating network of "main-auxiliary synergy and orientation complementarity," which not only effectively breaks the strong agglomeration tendency of high-structure carbon black and significantly reduces the initial viscosity and scraper fineness of the dispersion, but also significantly inhibits secondary sedimentation and flocculation during storage, giving the carbon black dispersion excellent long-term stability and processing adaptability. 2. This application selects dispersion media with corresponding compatibility polarity levels based on the mass content of hydrogenated nitrile butadiene rubber (NBR) and acrylonitrile: xylene is matched with NBR containing 20-25 wt% acrylonitrile; cyclohexanone is matched with NBR containing >25-33 wt% acrylonitrile; and N-methylpyrrolidone is matched with NBR containing >33-40 wt% acrylonitrile. Through precise matching of the dispersion media with the polarity and compatibility of the NBR, the complete dissolution of the NBR and efficient wetting and dispersion of carbon black are simultaneously achieved. Detailed Implementation

[0023] The technical solutions in the embodiments of this application will be clearly and completely described below with reference to the embodiments of this application. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.

[0024] This application discloses a carbon black dispersion for lithium-ion battery cathode slurry, comprising the following raw materials in parts by weight: 8-40 parts carbon black, 1-10 parts hydrogenated nitrile rubber, 0.04-0.48 parts styrene-butadiene-styrene block copolymer, and 170-960 parts dispersion medium; wherein the hydrogenated nitrile rubber has an acrylonitrile content of 20-40 wt% and a Mooney viscosity ML(1+4) of 30-80 at 100°C.

[0025] This application discloses a method for preparing a carbon black dispersion for lithium-ion battery cathode slurry, comprising the following steps: S1. Divide the dispersion medium into two parts; add hydrogenated nitrile rubber and styrene-butadiene-styrene block copolymer to one part of the dispersion medium in sequence, heat and stir at 40-60℃ for 2-3 hours to obtain a premix with a solid content of 4-10wt%. S2. Add carbon black to the premixed liquid, then add the remaining dispersion medium, stir at 100-300 rpm for 10-20 min, then stir at 1000-3000 rpm for 40-60 min to obtain a carbon black dispersion for lithium-ion battery cathode slurry.

[0026] This application discloses a lithium-ion battery positive electrode slurry, including a carbon black dispersion for use in lithium-ion battery positive electrode slurries. The specific preparation method is as follows: 0.994g of polyvinylidene fluoride (PVDF) and 13.206g of N-methylpyrrolidone (N-Methylpyrrolidone) are mixed to obtain a PVDF solution; 37.5g of the carbon black dispersion for lithium-ion battery positive electrode slurry, 14.2g of the PVDF solution, 47.5g of lithium iron phosphate, and 0.8g of N-methylpyrrolidone are mixed and stirred at 1000rpm for 2 hours to obtain the lithium-ion battery positive electrode slurry.

[0027] All raw materials used in the embodiments of this application are commercially available, wherein: Styrene-butadiene-styrene block copolymer, item number B768465, weight average molecular weight 140000 g / mol, Shanghai Maclean Biochemical Technology Co., Ltd. Polyvinylpyrrolidone K30, Shanghai Maclean Biochemical Technology Co., Ltd.; Super P, 30-45nm, Dongguan Kelude New Energy Technology Co., Ltd. Ketjen Black, 20-100nm, Dongguan Kelude New Energy Technology Co., Ltd. Acetylene black, 20-100nm, Dongguan Kelude New Energy Technology Co., Ltd. Lithium iron phosphate, Hunan Yuneng New Energy Battery Materials Co., Ltd.; Amino chelate ion exchange resin, Xi'an Lanxiao Technology New Materials Co., Ltd.; Nitrile rubber, acrylonitrile content of 33wt%, Nandi Chemical Industry Co., Ltd. Nitrile rubber, acrylonitrile content of 17wt%, Nandi Chemical Industry Co., Ltd. Nitrile rubber, acrylonitrile content of 41 wt%, Nan Di Chemical Industry Co., Ltd. Polyvinylidene fluoride, weight-average molecular weight 650,000 g / mol, Dongguan Kelude New Energy Technology Co., Ltd. N-Methylpyrrolidone, Shanghai Aladdin Biochemical Technology Co., Ltd.; Cyclohexanone, Shanghai Aladdin Biochemical Technology Co., Ltd.; Xylene, Shanghai Aladdin Biochemical Technology Co., Ltd.

[0028] Preparation Example 1 Preparation of hydrogenated nitrile butadiene rubber (acrylonitrile content 33wt%, Mooney viscosity ML(1+4) 100℃ 60): 10g of nitrile butadiene rubber (acrylonitrile content 33wt%) and 100g of chlorobenzene were mixed to prepare a 10wt% rubber solution, which was then placed in an autoclave. Nitrogen gas was continuously bubbled for 30min to completely replace the oxygen in the autoclave. Under nitrogen protection, 0.002g of tris(triphenylphosphine) ruthenium dichloride was added, and the mixture was stirred at 118℃ and 300rpm for 60min. Pure hydrogen gas was then introduced to maintain a hydrogen pressure of 5MPa in the autoclave, and the mixture was stirred at 118℃ and 300rpm for 8h. The mixture was then cooled to 60℃, and an amino chelating ion exchange resin was added and stirred for 2h. After filtration, chlorobenzene was removed by steam stripping, and the mixture was vacuum dried at 50℃ for 8h to obtain hydrogenated nitrile butadiene rubber with an acrylonitrile content of 33wt% and a Mooney viscosity ML(1+4) 100℃ of 60.

[0029] Preparation Example 2 Preparation of hydrogenated nitrile rubber (acrylonitrile content of 17wt%, Mooney viscosity ML(1+4) 100℃ is 60): The difference between this preparation example and preparation example 1 is that the nitrile rubber (acrylonitrile content of 33wt%) in preparation example 1 is replaced by nitrile rubber with an acrylonitrile content of 17wt%.

[0030] Preparation Example 3 The difference between this preparation example and preparation example 1 is that the nitrile rubber (acrylonitrile content of 33 wt%) in preparation example 1 is replaced by nitrile rubber with an acrylonitrile content of 41 wt%.

[0031] Preparation Example 4 Preparation of hydrogenated nitrile butadiene rubber (acrylonitrile content of 33wt%, Mooney viscosity ML(1+4) 100℃ of 25): The difference between this preparation example and preparation example 1 is that the amount of tris(triphenylphosphine) ruthenium chloride used in preparation example 1 is doubled in this preparation example. Specifically, the amount of tris(triphenylphosphine) ruthenium chloride used is 0.004g.

[0032] Preparation Example 5 Preparation of hydrogenated nitrile butadiene rubber (acrylonitrile content 33wt%, Mooney viscosity ML(1+4) 85 at 100℃): The difference between this preparation example and Preparation Example 1 is that the reaction time in Preparation Example 1 is replaced with 14h. Specific preparation steps: 10g of nitrile butadiene rubber (acrylonitrile content 33wt%) and 100g of chlorobenzene are mixed to prepare a 10wt% rubber solution, which is then placed in a high-pressure reactor. Nitrogen gas is continuously bubbled for 30min to completely replace the oxygen in the reactor. Under nitrogen protection, 0.002g of tris(triphenylphosphine)ruthenium dichloride is added, and the mixture is stirred at 118℃ and 300rpm for 60min. Pure hydrogen gas is then introduced to maintain a hydrogen pressure of 5MPa in the reactor, and the mixture is stirred at 118℃ and 300rpm for 14h. Then, the temperature was lowered to 60°C, amino chelating ion exchange resin was added and stirred for 2 hours, filtered, and chlorobenzene was removed by steam stripping. The mixture was then vacuum dried at 50°C for 8 hours to obtain hydrogenated nitrile rubber with an acrylonitrile content of 33 wt% and a Mooney viscosity of ML(1+4)100°C of 85.

[0033] Preparation Example 6 Preparation of hydrogenated nitrile rubber (acrylonitrile content of 22wt%, Mooney viscosity ML(1+4) 100℃ is 60): The difference between this preparation example and preparation example 1 is that the nitrile rubber (acrylonitrile content of 33wt%) in preparation example 1 is replaced by nitrile rubber with an acrylonitrile content of 22wt%.

[0034] Example 1 1g of hydrogenated nitrile rubber obtained in Preparation Example 1 and 0.04g of styrene-butadiene-styrene block copolymer were added sequentially to 24.96g of cyclohexanone. The mixture was heated and stirred at 50°C for 2.5h. Then, 8g of Ketjen black and 146.8g of cyclohexanone were added sequentially. The mixture was stirred at 200rpm for 15min and then at 2000rpm for 50min to obtain a carbon black dispersion for lithium-ion battery cathode slurry.

[0035] Example 2 5g of hydrogenated nitrile rubber obtained in Preparation Example 1 and 0.2g of styrene-butadiene-styrene block copolymer were added sequentially to 59.8g of N-methylpyrrolidone. The mixture was heated and stirred at 40°C for 3 hours. Then, 20g of Super P and 419g of N-methylpyrrolidone were added sequentially. The mixture was stirred at 300rpm for 10 minutes and then at 1000rpm for 60 minutes to obtain a carbon black dispersion for lithium-ion battery cathode slurry.

[0036] Example 3 10g of hydrogenated nitrile rubber obtained in Preparation Example 6 and 0.4g of styrene-butadiene-styrene block copolymer were added sequentially to 93.6g of xylene. The mixture was heated and stirred at 60°C for 2 hours. Then, 40g of acetylene carbon black and 864g of xylene were added sequentially. The mixture was stirred at 100rpm for 20 minutes and then at 3000rpm for 40 minutes to obtain a carbon black dispersion for lithium-ion battery cathode slurry.

[0037] Comparative Example 1 The difference between this comparative example and Example 2 is that the hydrogenated nitrile rubber in Example 2 is replaced by polyvinylpyrrolidone K30.

[0038] Comparative Example 2 The difference between this comparative example and Example 2 is that the styrene-butadiene-styrene block copolymer in Example 2 is replaced by hydrogenated nitrile rubber in this comparative example.

[0039] Comparative Example 3 The difference between this comparative example and Example 2 is that the hydrogenated nitrile rubber in Example 2 is replaced by styrene-butadiene-styrene block copolymer.

[0040] Comparative Example 4 The difference between this comparative example and Example 2 is that the hydrogenated nitrile rubber in Example 2 is replaced by the hydrogenated nitrile rubber obtained in Preparation Example 2.

[0041] Comparative Example 5 The difference between this comparative example and Example 2 is that the hydrogenated nitrile rubber in Example 2 is replaced by the hydrogenated nitrile rubber obtained in Preparation Example 3.

[0042] Comparative Example 6 The difference between this comparative example and Example 2 is that the hydrogenated nitrile rubber in Example 2 is replaced by the hydrogenated nitrile rubber obtained in Preparation Example 4.

[0043] Comparative Example 7 The difference between this comparative example and Example 2 is that the hydrogenated nitrile rubber in Example 2 is replaced by the hydrogenated nitrile rubber obtained in Preparation Example 5.

[0044] Performance Test 1 The carbon black dispersions prepared in Examples 1-3 and Comparative Examples 1-7 for use in lithium-ion battery cathode slurries were tested for viscosity change rate and fineness. The results are shown in Table 1.

[0045] Viscosity change rate: The initial viscosity and viscosity after one week were measured using a rotational viscometer, and the viscosity change rate was calculated. Viscosity change rate = (Viscosity after one week - Initial viscosity) / Initial viscosity × 100%.

[0046] Fineness: The fineness is tested using a scraper fineness tester.

[0047] Table 1 Performance of carbon black dispersion used in lithium-ion battery cathode slurry

[0048] As shown in Examples 1-3, Comparative Example 1, and Table 1, the carbon black dispersions for lithium-ion battery cathode slurries in Examples 1-3 of this application exhibit a viscosity change rate below 28.40% and a fineness below 30 μm, significantly superior to Comparative Example 1. This indicates that compared to using polyvinylpyrrolidone K30 as a dispersant, this application, using hydrogenated nitrile rubber compounded with styrene-butadiene-styrene block copolymer, can construct a dense and tough coating barrier through the dual effects of "polar adsorption + π-π stacking," greatly inhibiting secondary agglomeration and sedimentation stratification of carbon black particles during long-term storage, thereby improving dispersion stability.

[0049] As shown in Example 2, Comparative Examples 2-3, and Table 1, the viscosity change rate of the carbon black dispersion for lithium-ion battery cathode slurry in Example 2 of this application is 19.06%, which is significantly better than that of Comparative Examples 2-3. This indicates that the application uses a compound of hydrogenated nitrile rubber and styrene-butadiene-styrene block copolymer, which can exert a synergistic dispersion mechanism of "polar adsorption + π-π stacking": on the one hand, the highly polar cyano groups on the molecular chain of hydrogenated nitrile rubber form a strong chemical anchor with the surface active functional groups of carbon black, effectively wetting and depolymerizing carbon black particles and reducing the initial viscosity; on the other hand, the styrene blocks in the styrene-butadiene-styrene block copolymer tightly fill the microscopic gaps of the hydrogenated nitrile rubber coating layer through the π-π stacking effect, and construct a steric barrier with flexible butadiene segments, thereby significantly inhibiting the secondary agglomeration and sedimentation of carbon black during storage. Although the initial viscosity is low when using hydrogenated nitrile rubber alone, the non-dense coating leads to a significant increase in viscosity during long-term storage. Using styrene-butadiene-styrene block copolymer alone results in initial dispersion difficulties (initial viscosity as high as 210.25 mPa·s) due to the lack of strong polar anchoring, and more severe flocculation after storage.

[0050] As shown in Example 2, Comparative Example 4, and Table 1, the viscosity change rate of the carbon black dispersion for lithium-ion battery positive electrode slurry in Example 2 of this application is 19.06%, which is better than that of Comparative Example 4. This indicates that the hydrogenated nitrile butadiene rubber with a cyano content of 20-40 wt% used in this application can provide sufficient polar anchoring points to tightly bind with carbon black while avoiding intermolecular entanglement caused by excessive polarity. Compared to Example 2, the cyano content in Comparative Example 4 is too low, resulting in insufficient molecular chain polarity and an inability to form a sufficiently strong chemical anchor with the active sites on the carbon black surface. This leads to weak coating of carbon black by the main dispersant, and the hydrogenated nitrile butadiene rubber with low acrylonitrile content does not dissolve completely in the highly polar N-methylpyrrolidone, resulting in poor dispersibility. Compared to Example 2, the carbon black dispersion in Comparative Example 5 also has excellent dispersibility, but the cyano content is too high, causing the hydrogenated nitrile butadiene rubber to swell severely in the electrolyte when used as a positive electrode sheet.

[0051] As shown in Example 2, Comparative Example 7, and Table 1, the viscosity change rate of the carbon black dispersion for lithium-ion battery cathode slurry in Example 2 of this application is 19.06%, which is better than that of Comparative Example 7. This indicates that the hydrogenated nitrile rubber used in this application with a Mooney viscosity of ML(1+4) 100℃ of 30-80 can effectively construct a steric hindrance layer and achieve long-term stable dispersion. Compared with Example 2, the carbon black dispersion in Comparative Example 6 also has excellent dispersibility, but the Mooney viscosity is too low, and the hydrogenated nitrile rubber used in the cathode sheet will be severely swollen by the electrolyte. Compared with Example 2, the Mooney viscosity in Comparative Example 7 is too high, and the molecular chains of the hydrogenated nitrile rubber are too long. On the one hand, this makes it difficult for the molecular chains to dissolve and expand in the dispersion medium; on the other hand, the excessively long molecular chains are very easy to be adsorbed on the surface of multiple carbon black particles at the same time, acting as a "bridging" effect, causing severe bridging flocculation, thus resulting in poor dispersibility.

[0052] Examples 4-5 Based on Example 2, except for the weight ratio of hydrogenated nitrile rubber and styrene-butadiene-styrene block copolymer, the other components and preparation methods are the same as in Example 2, and the total weight of hydrogenated nitrile rubber and styrene-butadiene-styrene block copolymer remains unchanged.

[0053] Example 4 The difference between this embodiment and Embodiment 2 is that the weight ratio of hydrogenated nitrile rubber and styrene-butadiene-styrene block copolymer in this embodiment is 1:0.07. Specifically, the weight of hydrogenated nitrile rubber is 4.86g and the weight of styrene-butadiene-styrene block copolymer is 0.34g.

[0054] Example 5 The difference between this embodiment and Embodiment 2 is that the weight ratio of hydrogenated nitrile rubber and styrene-butadiene-styrene block copolymer in this embodiment is 1:0.1. Specifically, the weight of hydrogenated nitrile rubber is 4.727g and the weight of styrene-butadiene-styrene block copolymer is 0.473g.

[0055] Performance Test 2 The carbon black dispersions prepared in Examples 4-5 for use as positive electrode slurries in lithium-ion batteries were subjected to viscosity change rate and fineness tests. The test methods were the same as those in Performance Test 1, and the test results are shown in Table 2 below.

[0056] Table 2 Performance of carbon black dispersions for lithium-ion battery cathode slurries in Examples 2 and 4-5

[0057] As shown in Examples 2, 4-5, and Table 2, the viscosity change rate of the carbon black dispersion for lithium-ion battery cathode slurry in Example 4 of this application is 15.45%, which is significantly better than that in Examples 2 and 5. This indicates that the use of a specific weight ratio of hydrogenated nitrile rubber and styrene-butadiene-styrene block copolymer in this application can optimize the dispersibility of the two types of polymer materials on the carbon black surface and improve the dispersion stability. Compared with Example 4, although the high proportion of hydrogenated nitrile rubber in Example 2 can provide sufficient polar cyano chemical anchoring, the relatively insufficient proportion of styrene-butadiene-styrene block copolymer makes it difficult to fully fill the microscopic physical gaps generated when hydrogenated nitrile rubber coats carbon black through the π-π stacking effect. This limits the density of the coating layer, and carbon black is prone to micro-agglomeration during storage. Compared to Example 4, the high proportion of styrene-butadiene-styrene block copolymer in Example 5, while providing a stronger π-π stacking effect, also leads to excessive intermolecular entanglement and "bridging" flocculation between carbon black particles in the system due to the excessive flexible segments, resulting in an increase in the initial viscosity of the system and aggravated viscosity fluctuations during storage.

[0058] The above are all preferred embodiments of this application, and are not intended to limit the scope of protection of this application. Therefore, all equivalent changes made in accordance with the structure, shape and principle of this application should be covered within the scope of protection of this application.

Claims

1. A carbon black dispersion for lithium-ion battery cathode slurry, characterized in that, The raw materials include the following parts by weight: 8-40 parts carbon black, 1-10 parts hydrogenated nitrile butadiene rubber, 0.04-0.48 parts styrene-butadiene-styrene block copolymer, and 170-960 parts dispersion medium; the hydrogenated nitrile butadiene rubber has an acrylonitrile content of 20-40 wt% and a Mooney viscosity ML(1+4) of 30-80 at 100℃.

2. The carbon black dispersion liquid for lithium ion battery cathode slurry according to claim 1, characterized by, The weight ratio of the hydrogenated nitrile rubber and the styrene-butadiene-styrene block copolymer is 1:(0.04-0.1).

3. The carbon black dispersion liquid for lithium ion battery cathode slurry according to claim 1, characterized by, The weight-average molecular weight of the styrene-butadiene-styrene block copolymer is 100,000-200,000 g / mol.

4. The carbon black dispersion liquid for lithium ion battery cathode slurry according to claim 1, characterized by, The carbon black is at least one of Super P, Ketjen black, and acetylene black.

5. The carbon black dispersion liquid for lithium ion battery cathode slurry according to claim 1, characterized by, The carbon black has a particle size of 20-100 nm.

6. The carbon black dispersion liquid for lithium ion battery cathode slurry according to claim 1, characterized by, The hydrogenated nitrile butadiene rubber is one of the following: first hydrogenated nitrile butadiene rubber, second hydrogenated nitrile butadiene rubber, and third hydrogenated nitrile butadiene rubber. The acrylonitrile content of the first hydrogenated nitrile rubber is 20-25 wt%, and the dispersion medium is xylene; The acrylonitrile content of the second hydrogenated nitrile rubber is >25-33 wt%, and the dispersion medium is cyclohexanone; The acrylonitrile content of the third hydrogenated nitrile rubber is >33-40 wt%, and the dispersion medium is N-methylpyrrolidone.

7. A method for preparing a carbon black dispersion for lithium-ion battery cathode slurry according to any one of claims 1-6, characterized in that, Includes the following steps: S1. Divide the dispersion medium into two parts; add hydrogenated nitrile rubber and styrene-butadiene-styrene block copolymer to one part of the dispersion medium in sequence, heat and stir to obtain a premix; S2. Add carbon black to the premixed liquid, then add the remaining dispersion medium, stir evenly to obtain a carbon black dispersion for lithium-ion battery cathode slurry.

8. The method for preparing carbon black dispersion for lithium-ion battery cathode slurry according to claim 7, characterized in that, In step S1, the solid content of the premixed liquid is 4-10 wt%.

9. A lithium-ion battery cathode slurry, characterized in that, Includes the carbon black dispersion for lithium-ion battery cathode slurry as described in any one of claims 1-6.

Citation Information

Patent Citations

  • Carbon black dispersion solution and manufacturing method therefor

    CN108028091A