A metal-modified carbon current collector, its preparation method and application

By preparing a three-dimensional nano-metal array of metal-modified carbon current collector at room temperature and pressure, the problems of suppressing dendrite growth and controlling cost in metal battery anode materials have been solved, realizing the preparation of efficient and low-cost metal battery anode materials and improving battery performance and stability.

CN123120746APending Publication Date: 2026-11-17SHENZHEN TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611535554.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing metal battery anode materials suffer from low efficiency, high cost, and serious environmental pollution in suppressing metal dendrite growth. Furthermore, traditional preparation methods require sophisticated equipment, making it difficult to achieve large-scale production.

Method used

A metal-modified carbon current collector with a three-dimensional nano-metal array was prepared by using a low-concentration mixed solution of graphene oxide and carbon nanotubes to carry out a redox reaction with metal foil at room temperature and pressure, combined with plasma etching and reduction calcination, thus realizing the in-situ growth of the metal array.

Benefits of technology

It reduces safety risks in the preparation process, simplifies operation steps, reduces costs, improves the specific capacity of metal batteries, significantly inhibits the growth of metal dendrites, and improves the cycle stability and lifespan of batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120746A_ABST
    Figure CN123120746A_ABST
Patent Text Reader

Abstract

This invention relates to the field of metal battery technology, specifically to a metal-modified carbon current collector, its preparation method, and its application. The metal-modified carbon current collector is prepared according to the following steps: An aqueous solution of graphene oxide is mixed with an aqueous carbon nanotube solution. Using a metal foil as a reducing agent, a redox reaction is carried out, followed by drying to prepare a metal foil substrate-self-supporting carbon current collector. The carbon current collector is then peeled off from the metal foil substrate. The carbon current collector is subsequently subjected to plasma etching and reduction calcination treatments to obtain the metal foil-modified carbon current collector. Compared to existing technologies, the preparation method of this invention is more in line with the requirements of green manufacturing, is simple to operate, has low risk, meets personal safety requirements, and is economical in terms of low equipment and raw material costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal battery technology, specifically to a metal-modified carbon current collector, its preparation method, and its application. Background Technology

[0002] Lithium metal batteries have an ultra-high theoretical energy density of 3870 mAh / g, making them a core direction for breaking through the bottleneck of energy storage technology.

[0003] In the current energy storage technology system, ion batteries have established a dominant position in the secondary battery and large-scale energy storage market due to their excellent cycle stability and safety. However, the improvement of the energy density of ion batteries is still limited by the intrinsic properties of the anode material. Taking the most widely used commercial graphite anode as an example, its theoretical specific capacity does not exceed 400 mAh g⁻¹. -1 The current technology is insufficient to meet the demands of next-generation high-performance energy storage devices. In stark contrast, metal-based anodes (such as lithium metal / sodium metal) exhibit highly attractive application potential, with a theoretical specific capacity as high as 3860 mAh g⁻¹. -1 / 1166mAhg -1 Metal anodes, far exceeding the capacity of traditional carbon-based anodes, are considered one of the core directions for breaking through the capacity limits of ion batteries. However, in practical applications, charge accumulation and tip effects easily induce the growth of metal dendrites, severely weakening the safety performance and cycle stability of metal batteries. Therefore, suppressing the disordered growth of dendrites in metal anodes is a core research issue that urgently needs to be addressed in the field of metal batteries.

[0004] Among numerous modification strategies, constructing three-dimensional framework structures is highly favored. Existing research has confirmed that three-dimensional framework materials such as rigid matrices (foamed copper, foamed nickel), flexible substrates (carbon fiber cloth), and lightweight carbon foam can effectively alleviate the growth problem of sodium dendrites. However, current research shows that mainstream control strategies generally suffer from drawbacks such as metal waste, low specific capacity, and excessive use of organic solvents, making it difficult to balance the demands of green preparation and high performance in the new era. In addition, most of the materials prepared in this study require extremely high-end experimental equipment, resulting in low scalability. Furthermore, the preparation of some materials involves high-temperature reactions (>1000℃), increasing the risk of experimental operations. Of particular concern is that currently reported metal battery anode materials are mainly manufactured using subtractive processing, which generates a large amount of non-reusable waste solids, waste liquids, and waste gases after the preparation process, leading to material waste and hindering cost control. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this invention provides a metal-modified carbon current collector, its preparation method, and its applications. This invention uses a low-concentration mixed solution of graphene oxide and carbon nanotubes as a precursor, and metal foil as a reducing agent. A redox reaction is carried out at room temperature and pressure to prepare the carbon current collector. The carbon current collector is then subjected to plasma etching and reduction calcination treatments to achieve controllable carbon film etching and metal array construction, ultimately obtaining the metal-modified carbon current collector. Compared to existing technologies, the preparation method of this invention is simple and safe, reducing the difficulty and danger of experimental operations under high temperature and high pressure. After the redox reaction, the metal foil can be reused through simple processing, saving production costs. The prepared metal-modified carbon current collector has extremely light mass, which can significantly improve the specific capacity of metal batteries. The solvent used in the preparation process is water, achieving a balance between green preparation and high performance.

[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: The first objective of this invention is to provide a method for preparing a metal-modified carbon current collector, comprising the following steps: Graphene oxide powder and aqueous carbon nanotube dispersion are mixed and vigorously stirred to obtain a homogeneous graphene oxide / carbon nanotube mixed precursor without flocculent precipitates. The concentration of the graphene oxide / carbon nanotube mixed precursor does not exceed 2 mg / mL. The advantages of low concentration are: less raw materials are required, resulting in lower material costs; less waste products are formed (such as precursors that cannot be reused), and post-processing purification is easier. The reason for using aqueous carbon nanotubes as raw materials is that water is the solvent in the system. If non-aqueous carbon nanotubes are used, uneven mixing and precipitation are likely to occur, leading to uneven distribution of carbon nanotubes in the prepared carbon film. Ultimately, this results in poor conductivity uniformity and performance degradation of the metal-modified carbon current collector. In addition, the aqueous carbon nanotube solution of this invention uses a dispersant to disperse completely hydrophobic single-walled carbon nanotubes, rather than using hydrophilically treated carbon nanotubes.

[0007] The metal foil was cleaned with ethanol, and then the oxide layer on the surface of the metal foil was removed with a dilute acid solution. The acid treatment conditions were: dilute hydrochloric acid with a concentration of 0.01 mol / L to 1 mol / L, and deionized water was used to remove residual acid and metal ions from the surface.

[0008] The treated metal foil is immersed in a graphene oxide / carbon nanotube hybrid precursor, sealed and left to stand. During this time, the graphene oxide and the metal foil undergo a redox reaction, which drives the orderly assembly of carbon nanotubes. After the reaction is completed, the unreacted graphene oxide / carbon nanotube hybrid precursor is removed and dried in a forced-air drying oven to obtain a metal foil substrate-self-supporting carbon current collector. The carbon current collector is peeled off from the metal foil substrate. The carbon-based fluid is composed of graphene oxide, reduced graphene oxide, and carbon nanotubes, with metal ions uniformly distributed in the carbon film.

[0009] The carbon current collector is placed in a plasma cleaner and subjected to plasma etching to form a three-dimensional nano-metal array on the surface of the carbon current collector, and the metal is oxidized to obtain a metal oxide modified carbon current collector.

[0010] The metal oxide-modified carbon current collector is placed in a tube furnace and calcined in a reducing atmosphere to reduce the metal oxide to metal nanoparticles and fully reduce graphene oxide to reduced graphene oxide, thus obtaining the metal-modified carbon current collector.

[0011] Preferably, in the graphene oxide / carbon nanotube mixed precursor, the mass percentage of carbon nanotubes is 16%~48%, and the mass percentage of graphene oxide is 52%~84%, with the sum of their mass percentages being 100%. If the proportion of graphene oxide is too high, the graphene oxide / carbon nanotube mixed precursor will have high viscosity and poor flowability, affecting the redox reaction; if the proportion of graphene oxide is too low, the viscosity will be extremely low, similarly affecting the redox reaction; both situations will reduce the conductivity of the metal-modified carbon current collector.

[0012] Preferably, the dispersant is selected from sodium carboxymethyl cellulose, polylactic acid, or polyethylene oxide.

[0013] Preferably, the mass ratio of dispersant to carbon nanotubes is 1:1 to 3:2. Excessive dispersant content increases solution viscosity, reduces conductive components, and lowers the conductivity of the metal-modified carbon current collector; excessive carbon nanotube content leads to poor solution dispersibility, causing agglomeration of conductive components, resulting in an uneven surface of the metal-modified carbon current collector and a significant decrease in conductivity uniformity.

[0014] Preferably, the redox reaction time is 0.5 h to 96 h; further, the redox reaction time is 4 h to 48 h. If the time is too long, the thickness increases but the conductivity decreases; if the time is too short, the thickness is smaller but the conductivity is higher.

[0015] Preferably, the metal foil is selected from copper foil, tin foil, aluminum foil, iron foil, cobalt foil, nickel foil, or zinc foil. After the metal reacts with graphene oxide, a graphene oxide-carbon nanotube composite material coordinated with metal ions is produced; no metal nanoparticles are formed at this stage.

[0016] Preferably, the plasma etching conditions are as follows: processing at 60W~200W power for 2min~20min under an inert gas to oxygen volume ratio of 9:1~6:4. During etching, oxygen plasma continuously bombards the surface carbon film, exposing the coordinating metal ions, which then combine with the oxygen plasma to form metal oxide. As etching continues, the metal ions migrate towards the initial nucleation sites under the influence of surface energy, eventually agglomerating to form a metal oxide array structure.

[0017] Preferably, the reduction calcination conditions are: heating to 200℃~500℃ at a rate of 1℃ / min~10℃ / min, and calcining for 0.5h~4h.

[0018] A second objective of this invention is to provide a metal-modified carbon current collector, which is prepared using the above-described method.

[0019] Preferably, the surface of the metal-modified carbon current collector has a metal nanoscale array structure, and the conductivity of the metal-modified carbon current collector is 380 S / cm to 1500 S / cm.

[0020] A third objective of this invention is to provide the application of metal-modified carbon current collectors in the preparation of self-supporting anode materials for metal batteries.

[0021] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. This invention provides a method for preparing a metal-modified carbon current collector. First, a graphene oxide solution is uniformly mixed with a carbon nanotube solution dispersed in a dispersant. Then, a redox reaction is carried out between the graphene oxide and a metal foil, driving the orderly assembly of the carbon nanotubes. Next, plasma etching and calcination reduction are used to achieve in-situ growth of a metal array on the surface of the carbon current collector, ultimately producing a metal-modified carbon current collector. This preparation method significantly differs from existing vapor deposition, hydrothermal, and electrochemical deposition processes, eliminating the dependence on high-temperature and high-pressure conditions inherent in traditional methods and effectively reducing safety risks during production. Furthermore, this preparation method simplifies the operation steps through process optimization, exhibiting higher process feasibility and cost advantages while ensuring the performance of the metal-modified carbon current collector.

[0022] 2. The metal-modified carbon current collector of this invention is a nanoscale array, which differs from nanoarrays prepared by traditional vapor deposition, hydrothermal methods, and electrochemical deposition. The metal-modified carbon current collector of this invention has significant advantages in terms of high controllability and solvent-free operation. Furthermore, the carbon nanotubes in the current collector provide high conductivity while mitigating local current concentration; the defect vacancies and sodium-loving oxygen-containing groups of reduced graphene oxide provide sufficient nucleation sites for active metal deposition, inhibiting localized active ion aggregation; the nanoscale metal array forms a three-dimensional confinement effect, effectively inhibiting lithium metal growth along a single direction; the synergistic inhibition of metal dendrite growth resulting from these three factors improves the cycle stability and lifespan of the metal battery.

[0023] 3. The metal-modified carbon current collector of this invention possesses ultra-thin and ultra-light characteristics, significantly improving the problem of low specific capacity. This invention requires minimal experimental equipment, and the maximum reaction temperature is 500℃, enabling large-scale production. Attached Figure Description

[0024] Figure 1 This is a schematic diagram of the preparation process of metal-modified carbon current collectors.

[0025] Figure 2 The image shows a scanning electron microscope (SEM) image of the metal-modified carbon current collector prepared in Example 1, where a is the morphology of the sample before reduction calcination, b is the morphology of the sample after reduction calcination, and c is the nucleation overpotential of the metal-modified carbon current collector.

[0026] Figure 3 The image shows a scanning electron microscope (SEM) image of the metal-modified carbon current collector prepared in Example 2, where a is the morphology of the sample before reduction calcination, b is the morphology of the sample after reduction calcination, and c is the nucleation overpotential of the metal-modified carbon current collector.

[0027] Figure 4 The image shows a scanning electron microscope (SEM) image of the metal-modified carbon current collector prepared in Example 3, where a is the morphology of the sample before reduction calcination, b is the morphology of the sample after reduction calcination, and c is the nucleation overpotential of the metal-modified carbon current collector.

[0028] Figure 5 The image shows a scanning electron microscope (SEM) image of the metal-modified carbon current collector prepared in Example 4, where a is the morphology of the sample before reduction calcination, b is the morphology of the sample after reduction calcination, and c is the nucleation overpotential of the metal-modified carbon current collector.

[0029] Figure 6 The image shows a scanning electron microscope (SEM) image of the carbon current collector prepared in Comparative Example 1, where a represents the morphology of the sample before reduction calcination, b represents the morphology of the sample after reduction calcination, and c represents the nucleation overpotential of the carbon current collector.

[0030] Figure 7The image shows a scanning electron microscope (SEM) image of the metal-modified carbon current collector prepared in Comparative Example 2. In the image, a represents the morphology of the sample before reduction calcination, b represents the morphology of the sample after reduction calcination, and c represents the nucleation overpotential of the metal-modified carbon current collector.

[0031] Figure 8 The image shows a scanning electron microscope (SEM) image of the metal oxide-modified carbon current collector prepared in Comparative Example 3. In the image, a represents the morphology of the sample before reduction calcination, b represents the morphology of the sample after reduction calcination, and c represents the nucleation overpotential of the metal oxide-modified carbon current collector. Detailed Implementation

[0032] The technical solution of the present invention will be clearly and completely described below with reference to the data in the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0033] It should be noted that the technical terms used in this invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of this invention. Unless otherwise specified, all raw materials, reagents, instruments and equipment used in the following embodiments of this invention can be purchased on the market or prepared by existing methods.

[0034] This invention uses metal foil as a reducing agent to carry out a mild redox reaction of graphene oxide, which drives the orderly assembly of carbon nanotubes. The assembly method is to arrange them in a layer-by-layer stacking manner, namely reduced graphene oxide-carbon nanotube-reduced graphene oxide-carbon nanotube-reduced graphene oxide... While improving the electron transport capability of the carbon current collector, the thickness of the carbon current collector can be effectively controlled by controlling the reaction time, providing a flexible substrate selection for subsequent plasma etching.

[0035] The metal-modified carbon current collector prepared in this invention exhibits unique advantages due to its three-dimensional structure: its three-dimensional nano-metal array structure confines the dendrite growth in the metal battery, effectively suppressing the poor battery stability caused by dendrite growth. Thanks to the three-dimensional nano-metal array, this metal-modified carbon current collector demonstrates high stability under constant current charge-discharge testing.

[0036] In terms of fabrication process, this invention employs plasma etching technology for graphene oxide / carbon nanotube hybrid precursors under ambient pressure, eliminating the need for vapor deposition, electrochemical deposition, and high-temperature, high-pressure hydrothermal reactions required in traditional methods, thereby significantly improving operational safety. Thanks to the simplified fabrication process, the sample preparation cycle is greatly shortened while ensuring controllable sample morphology, effectively reducing time costs.

[0037] In terms of raw material utilization, this invention selects metal foil as a reducing agent. After the redox reaction is completed, the surface activity of the metal can be reset by wiping with dilute acid and rinsing with deionized water, and it can be reused. This feature significantly reduces the cost of raw materials and improves the efficiency of resource utilization.

[0038] The technical solution of the present invention will be further explained and illustrated below with examples, as detailed below: Example 1 A method for preparing a metal-modified carbon current collector includes the following steps: S1. Take 12.5 mL of graphene oxide solution and 2 mg / mL of carbon nanotube solution (the carbon nanotube solution is a mixture of carbon nanotubes and carboxymethyl cellulose with a mass ratio of carbon nanotubes to carboxymethyl cellulose of 2:3) and 10.5 mL of ultrapure water respectively, and stir vigorously to obtain a graphene oxide / carbon nanotube mixed precursor. Seal the graphene oxide / carbon nanotube mixed precursor with copper foil at 25 °C for 4 hours for redox reaction.

[0039] S2. After removing the unreacted graphene oxide / carbon nanotube mixed precursor, the mixture is dried at a constant temperature of 30°C in a forced-air drying oven for 6 hours to obtain a metal foil substrate-self-supporting carbon current collector. The carbon current collector is then peeled off from the metal foil substrate.

[0040] S3. The carbon current collector is plasma etched at 90W with a nitrogen / oxygen ratio of 7:3 for 20 minutes, and then removed to obtain a metal oxide modified carbon current collector.

[0041] S4. The metal oxide-modified carbon current collector is calcined at 500°C for 2 hours in a hydrogen / argon atmosphere to obtain the metal-modified carbon current collector.

[0042] Example 2 A method for preparing a metal-modified carbon current collector, such as... Figure 1 As shown, it includes the following steps: S1. Take 12.5 mL of graphene oxide solution and 2 mg / mL of carbon nanotube solution (the carbon nanotube solution is a mixture of carbon nanotubes and carboxymethyl cellulose with a mass ratio of carbon nanotubes to carboxymethyl cellulose of 2:3) and 10.5 mL of ultrapure water respectively, and stir vigorously to obtain a graphene oxide / carbon nanotube mixed precursor. Seal the graphene oxide / carbon nanotube mixed precursor with copper foil at 25 °C for 4 hours for redox reaction.

[0043] S2. After removing the unreacted graphene oxide / carbon nanotube mixed precursor, the mixture is dried at a constant temperature of 30°C in a forced-air drying oven for 6 hours to obtain a metal foil substrate-self-supporting carbon current collector. The carbon current collector is then peeled off from the metal foil substrate.

[0044] S3. The carbon current collector is plasma etched at 150W with a nitrogen / oxygen ratio of 7:3 for 10 minutes, and then removed to obtain a metal oxide modified carbon current collector.

[0045] S4. The metal oxide-modified carbon current collector is calcined at 500°C for 2 hours in a hydrogen / argon atmosphere to obtain the metal-modified carbon current collector.

[0046] Example 3 A method for preparing a metal-modified carbon current collector includes the following steps: S1. Take 12.5 mL of graphene oxide solution and 2 mg / mL of carbon nanotube solution (the carbon nanotube solution is a mixture of carbon nanotubes and carboxymethyl cellulose with a mass ratio of carbon nanotubes to carboxymethyl cellulose of 2:3) and 10.5 mL of ultrapure water respectively, and stir vigorously to obtain a graphene oxide / carbon nanotube mixed precursor. Seal the graphene oxide / carbon nanotube mixed precursor with copper foil at 25 °C for 4 hours for redox reaction.

[0047] S2. After removing the unreacted graphene oxide / carbon nanotube mixed precursor, the mixture is dried at a constant temperature of 30°C in a forced-air drying oven for 6 hours to obtain a metal foil substrate-self-supporting carbon current collector. The carbon current collector is then peeled off from the metal foil substrate.

[0048] S3. The carbon current collector is plasma etched at 180W with a nitrogen / oxygen ratio of 7:3 for 10 minutes, and then removed to obtain a metal oxide modified carbon current collector.

[0049] S4. The metal oxide modified carbon current collector is calcined at 500°C for 2 hours in a hydrogen / argon atmosphere to obtain the metal modified carbon current collector.

[0050] Example 4 A method for preparing a metal-modified carbon current collector, such as... Figure 1 As shown, it includes the following steps: S1. Take 12.5 mL of graphene oxide solution and 2 mg / mL of carbon nanotube solution (the carbon nanotube solution is a mixture of carbon nanotubes and carboxymethyl cellulose with a mass ratio of carbon nanotubes to carboxymethyl cellulose of 2:3) and 10.5 mL of ultrapure water respectively, and stir vigorously to obtain a graphene oxide / carbon nanotube mixed precursor. Seal the graphene oxide / carbon nanotube mixed precursor with copper foil at 25 °C for 4 hours for redox reaction.

[0051] S2. After removing the unreacted graphene oxide / carbon nanotube mixed precursor, the mixture is dried at a constant temperature of 30°C in a forced-air drying oven for 6 hours to obtain a metal foil substrate-self-supporting carbon current collector. The carbon current collector is then peeled off from the metal foil substrate.

[0052] S3. The carbon current collector is plasma etched at 150W with a nitrogen / oxygen ratio of 7:3 for 15 minutes, and then removed to obtain a metal oxide modified carbon current collector.

[0053] S4. The metal oxide-modified carbon current collector is calcined at 500°C for 2 hours in a hydrogen / argon atmosphere to obtain the metal-modified carbon current collector.

[0054] Example 5 A method for preparing a metal-modified carbon current collector, such as... Figure 1 As shown, it includes the following steps: S1. Take 12.5 mL of graphene oxide solution and 2 mg / mL of carbon nanotube solution (the carbon nanotube solution is a mixture of carbon nanotubes and polylactic acid, with a carbon nanotube:polylactic acid mass ratio of 1:1) and 10.5 mL of ultrapure water respectively, and stir vigorously to obtain a graphene oxide / carbon nanotube mixed precursor. Seal the graphene oxide / carbon nanotube mixed precursor with copper foil at 25 °C for 0.5 hours for oxidation-reduction reaction.

[0055] S2. After removing the unreacted graphene oxide / carbon nanotube mixed precursor, the mixture is dried at a constant temperature of 30°C in a forced-air drying oven for 6 hours to obtain a metal foil substrate-self-supporting carbon current collector. The carbon current collector is then peeled off from the metal foil substrate.

[0056] S3. The carbon current collector is plasma etched at 60W with a nitrogen / oxygen ratio of 7:3 for 20 minutes, and then removed to obtain a metal oxide modified carbon current collector.

[0057] S4. The metal oxide-modified carbon current collector is calcined at 200°C for 4 hours in a hydrogen / argon atmosphere to obtain the metal-modified carbon current collector.

[0058] Example 6 A method for preparing a metal-modified carbon current collector, such as... Figure 1 As shown, it includes the following steps: S1. Take 12.5 mL of graphene oxide solution and 2 mg / mL of carbon nanotube solution (the carbon nanotube solution is a mixture of carbon nanotubes and polyethylene oxide, with a carbon nanotube:polyethylene oxide mass ratio of 1:1.25) and 10.5 mL of ultrapure water respectively, and mix them vigorously to obtain a graphene oxide / carbon nanotube mixed precursor. Seal the graphene oxide / carbon nanotube mixed precursor with copper foil at 25 °C for 96 hours for redox reaction.

[0059] S2. After removing the unreacted graphene oxide / carbon nanotube mixed precursor, the mixture is dried at a constant temperature of 30°C in a forced-air drying oven for 6 hours to obtain a metal foil substrate-self-supporting carbon current collector. The carbon current collector is then peeled off from the metal foil substrate.

[0060] S3. The carbon current collector is plasma etched for 2 minutes at 200W with a nitrogen / oxygen ratio of 7:3, and then removed to obtain a metal oxide modified carbon current collector.

[0061] S4. The metal oxide-modified carbon current collector is calcined at 500°C for 0.5 hours in a hydrogen / argon atmosphere to obtain the metal-modified carbon current collector.

[0062] Comparative Example 1 A method for preparing a reduced carbon current collector, without copper foil participating in the reaction, includes the following steps: S1. Take 12.5 mL of graphene oxide solution and 2 mg / mL of carbon nanotube solution (the carbon nanotube solution is a mixture of carbon nanotubes and carboxymethyl cellulose with a mass ratio of carbon nanotubes to carboxymethyl cellulose of 2:3) and 10.5 mL of ultrapure water respectively, and mix them vigorously to obtain a graphene oxide / carbon nanotube mixed precursor. Let the graphene oxide / carbon nanotube mixed precursor stand at 25°C for 4 hours and then dry it in a forced-air drying oven.

[0063] S2. The carbon current collector is plasma etched at 150W with a nitrogen / oxygen ratio of 7:3 for 15 minutes, and then removed to obtain the plasma-treated carbon current collector.

[0064] S3. The plasma-treated carbon current collector is calcined at 500°C for 2 hours in a hydrogen / argon atmosphere to obtain a reduced carbon current collector.

[0065] Comparative Example 2 A method for preparing a metal-modified carbon current collector, without plasma etching, includes the following steps: S1. Take 12.5 mL of graphene oxide solution and 2 mg / mL of carbon nanotube solution (the carbon nanotube solution is a mixture of carbon nanotubes and carboxymethyl cellulose with a mass ratio of carbon nanotubes to carboxymethyl cellulose of 2:3) and 10.5 mL of ultrapure water respectively, and stir vigorously to obtain a graphene oxide / carbon nanotube mixed precursor. Seal the graphene oxide / carbon nanotube mixed precursor with copper foil at 25 °C for 4 hours for redox reaction.

[0066] S2. After removing the unreacted graphene oxide / carbon nanotube mixed precursor, the mixture is dried at a constant temperature of 30°C in a forced-air drying oven for 6 hours to obtain a metal foil substrate-self-supporting carbon current collector. The carbon current collector is then peeled off from the metal foil substrate.

[0067] S3. The carbon current collector is calcined at 500°C for 2 hours in a hydrogen / argon atmosphere to obtain a metal-modified carbon current collector.

[0068] Comparative Example 3 A method for preparing a plasma-treated carbon current collector, without calcination, includes the following steps: S1. Take 12.5 mL of graphene oxide solution and 2 mg / mL of carbon nanotube solution (the carbon nanotube solution is a mixture of carbon nanotubes and carboxymethyl cellulose with a mass ratio of carbon nanotubes to carboxymethyl cellulose of 2:3) and 10.5 mL of ultrapure water respectively, and stir vigorously to obtain a graphene oxide / carbon nanotube mixed precursor. Seal the graphene oxide / carbon nanotube mixed precursor with copper foil at 25 °C for 4 hours for redox reaction.

[0069] S2. After removing the unreacted graphene oxide / carbon nanotube mixed precursor, the mixture is dried at a constant temperature of 30°C in a forced-air drying oven for 6 hours to obtain a metal foil substrate-self-supporting carbon current collector. The carbon current collector is then peeled off from the metal foil substrate.

[0070] S3. The carbon current collector is plasma etched at 150W with a nitrogen / oxygen ratio of 7:3 for 10 minutes, and then removed to obtain the plasma-treated carbon current collector.

[0071] Examples 1 to 4 are preferred embodiments of the present invention. In conjunction with Comparative Example 2, it can be seen that the nano-metal array generated by plasma etching plays a key role in improving the electrochemical performance of the carbon current collector itself. Figures 2-4The comparative results show that plasma treatment can construct a three-dimensional nanoarray structure on the surface of carbon current collector, and the three-dimensional nanoarrays obtained by increasing the etching power have better dispersion and uniformity. Furthermore, it can also increase the array size, providing more surface area and effective confinement space for the nano-metal array framework, increasing the metal deposition volume and the controllable range of dendrite growth. After being assembled with lithium metal into a semi-symmetric battery, the nucleation overpotential is in the range of 20mV~41mV. Assembly method: The assembly sequence of the coin cell is: negative electrode shell - spring sheet - lithium sheet - separator - electrode sheet - gasket - positive electrode shell, where the electrolyte addition amount is 55μL, and the electrolyte is 1mol / L LiTSFI in DME / DOL=1:1 Vol% with 2% LiNO3.

[0072] Figure 5 The results show that extending the plasma etching time can further reduce the lithium metal nucleation overpotential (17mV) of the plasma-treated carbon current collector.

[0073] Figure 6 The results demonstrate the indispensability of the metal foil in this experimental process. Compared to Examples 1-4, Comparative Example 1 removed the redox step using the metal foil, thus eliminating the metal ion source in the carbon current collector, and consequently, the final product did not exhibit a nanoscale metal array structure. The nucleation overpotential after assembly with lithium metal into a semi-symmetric cell was 63 mV.

[0074] Figure 7 The results demonstrate the indispensability of plasma etching in this experimental process. Compared to Examples 1-4, Comparative Example 2 only removed the plasma etching step. The final product did not exhibit a clear nanoarray structure, but only contained some irregular metal bodies and mostly spherical particles of deeply buried carbon layers. This prevented the full utilization of the metal composition, resulting in a higher nucleation overpotential (52 mV) compared to Examples 1-4. This illustrates the crucial role of plasma etching in forming a three-dimensional nano-metal array on the carbon current collector surface.

[0075] Figure 8 The results demonstrate the indispensability of calcination reduction in this experimental process. Compared to Examples 1-4, Comparative Example 3 only removed the calcination reduction step. Although the final product also exhibited a clear nano-metal array, the poor conductivity of the metal oxides resulted in uneven local current distribution, reducing the nucleation sites for lithium metal and causing the nucleation overpotential to remain high, thus accelerating dendrite growth.

[0076] It should be noted that when numerical ranges are involved in this invention, it should be understood that both endpoints of each numerical range, as well as any value between the two endpoints, can be selected. Since the steps and methods used are the same as in the embodiments, preferred embodiments are described here to avoid redundancy. Although preferred embodiments of the invention have been described, those skilled in the art, upon learning the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments as well as all changes and modifications falling within the scope of this invention.

Claims

1. A method for producing a metal-modified carbon current collector, characterized by, Includes the following steps: Graphene oxide powder was mixed with an aqueous carbon nanotube dispersion to obtain a graphene oxide / carbon nanotube mixed precursor with uniform texture and no flocculent precipitate. The metal foil was mixed with the graphene oxide / carbon nanotube hybrid precursor, sealed and stored and left to stand. At this time, the graphene oxide and the metal foil underwent a redox reaction, which led to the orderly assembly of carbon nanotubes. After drying, the metal foil substrate-self-supporting carbon current collector was obtained. Peel the carbon current collector off the metal foil substrate; A three-dimensional nano-metal array was formed on the surface of the carbon current collector by plasma etching, resulting in a metal oxide-modified carbon current collector. The metal oxide-modified carbon current collector is calcined in a reducing atmosphere to reduce the metal oxide to metal nanoparticles and fully reduce graphene oxide to reduced graphene oxide, thus obtaining the metal-modified carbon current collector.

2. The method of producing a metal-modified carbon current collector according to claim 1, characterized by, In the graphene oxide / carbon nanotube hybrid precursor, the mass percentage of carbon nanotubes is 16%~48%, the mass percentage of graphene oxide is 52%~84%, and the sum of the mass percentages of the two is 100%.

3. The method of making a metal-modified carbon current collector of claim 1, wherein, The aqueous carbon nanotube dispersion is composed of a dispersant and carbon nanotubes, with a mass ratio of dispersant to carbon nanotubes of 5:95 to 95:

5.

4. The method of producing a metal-modified carbon current collector according to claim 3, characterized by, Carbon nanotubes are selected from single-walled carbon nanotubes, multi-walled carbon nanotubes, or functionalized carbon nanotubes.

5. The method of making a metal-modified carbon current collector of claim 3, wherein, The dispersant is selected from sodium carboxymethyl cellulose, polylactic acid, polyethylene glycol, polyethylene oxide, or polyacrylamide.

6. The method of making a metal-modified carbon current collector of claim 1, wherein, The redox reaction time is 0.5h to 96h.

7. The method of making a metal-modified carbon current collector of claim 1, wherein, The metal foil is selected from copper foil, aluminum foil, tin foil, iron foil, cobalt foil, nickel foil, or zinc foil.

8. The method for preparing the metal-modified carbon current collector according to claim 1, characterized in that, The plasma etching conditions are as follows: under an inert gas to oxygen volume ratio of 9:1 to 6:4, the process is carried out at a power of 60W to 200W for 2 to 20 minutes.

9. The method for preparing the metal-modified carbon current collector according to claim 1, characterized in that, The conditions for calcination reduction are: treatment at 200℃~500℃ for 0.5h~4h in a hydrogen atmosphere.

10. A metal-modified carbon current collector, characterized in that, It is prepared by the preparation method according to any one of claims 1 to 9.

11. The metal-modified carbon current collector according to claim 10, characterized in that, The surface of the metal-modified carbon current collector has a metal nanoscale array structure.

12. The metal-modified carbon current collector according to claim 10, characterized in that, The electrical conductivity of the metal-modified carbon current collector is 300 S / cm to 1500 S / cm.

13. The application of the metal-modified carbon current collector as described in claim 10 in the preparation of a self-supporting negative electrode material for metal batteries.