Electrode, membrane electrode assembly, electrochemical cell, battery pack, electrolysis device
By employing an alternating layered sheet and gap layer structure in the electrode, especially by adding the thickest gap layer in the first region, the problem of insufficient electrode durability is solved, achieving stable and efficient operation under high pressure and dry conditions.
Patent Information
- Application Number
- CN202610065986.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-01-19
- Publication Date
- 2026-11-17
AI Technical Summary
Existing electrochemical batteries suffer from insufficient electrode durability, especially under high pressure and dry conditions, which can easily lead to the delamination of the catalyst layer from the substrate, affecting the stability and efficiency of the battery.
An electrode structure was designed in which the catalyst layer is composed of alternating layers of sheet material and interstitial layers. The interstitial layer in the first region is thicker than that in the second region, and the thickest interstitial layer is located in the first region. This structure can effectively control the degradation when the catalyst layer cracks and reduce the separation between the substrate and the catalyst layer.
This improved electrode durability, reduced catalyst layer delamination from the substrate due to pressure differentials and dryness, and ensured battery stability and efficient operation.
Smart Images

Figure CN123120752A_ABST
Abstract
Description
[0001] References to related applications This application is based on Japanese Patent Application 2025-078853 (filed on May 9, 2025), and enjoys priority benefits from this application. This application incorporates the entire contents of that application by reference. Technical Field
[0002] The embodiments of the present invention relate to electrodes, membrane electrode assemblies, electrochemical cells, battery packs, and electrolysis devices. Background Technology
[0003] In recent years, electrochemical cells have been actively researched. Among electrochemical cells, solid polymeric water electrolyzers (PEMECs) are expected to be used for hydrogen generation in large-scale energy storage systems. To ensure sufficient durability and electrolysis characteristics, platinum (Pt) nanoparticle catalysts are generally used for the cathode of PEMECs, while noble metal catalysts such as iridium (Ir) nanoparticle catalysts are generally used for the anode. In addition, methods for obtaining hydrogen from ammonia have also been studied. Furthermore, it can also be used as the anode in electrolysis devices that electrolyze carbon dioxide to produce organic compounds such as methanol and ethylene, or carbon monoxide. Summary of the Invention
[0004] The implementation provides highly durable electrodes.
[0005] The electrode of the embodiment has a first substrate and a first catalyst layer. The first catalyst layer is alternately stacked with multiple layers of sheet layers and gap layers disposed on the first substrate. The side of the first catalyst layer opposite to the first substrate side is designated as a first region, and the area outside the first region is designated as a second region. The average thickness of the gap layer in the first region is thicker than the average thickness of the gap layer in the second region, and / or the thickest gap layer exists in the first region.
[0006] Based on the above configuration, a highly durable electrode is provided. Attached Figure Description
[0007] Figure 1 This is a schematic diagram of the electrodes in the embodiment.
[0008] Figure 2 This is a partial schematic cross-sectional view of the electrode in the embodiment.
[0009] Figure 3 This is a partial schematic cross-sectional view of the electrode in the embodiment.
[0010] Figure 4 This is the analysis point for the implementation method.
[0011] Figure 5 This is a schematic diagram of the membrane electrode assembly according to the embodiment.
[0012] Figure 6 This is a schematic cross-sectional view of the membrane electrode assembly according to the embodiment.
[0013] Figure 7 This is a schematic diagram of an electrochemical cell according to an embodiment.
[0014] Figure 8 This is a schematic diagram of the battery pack in the implementation method.
[0015] Figure 9 This is a conceptual diagram of the electrolysis apparatus for the implementation method.
[0016] Figure 10 This is a table of an example.
[0017] Explanation of reference numerals in the attached figures 1: Substrate 2: Catalyst layer 2A: Sheet layer 2B: Interstitial layer 2C: Columnar body 11: First electrode 11A: First catalyst layer 11B: First substrate 12: Second electrode 12A: Second catalyst layer 12B: Second substrate 13: Electrolyte membrane 21: Washer 22: Washer 23: Diaphragm 24: Diaphragm 31: Fastening plate 32: Fastening plate 41: Power supply 42: Gas-liquid separation device 43: Mixing tank 44: Ion exchange water production equipment 46: Pump 47: Check valve 48: Gas-liquid separation device 49: Hydrogen refining unit 50: Valve 100: Electrode 200: Membrane electrode assembly 300: Electrochemical Battery 400: Battery pack 500: Electrolysis device. Detailed Implementation
[0018] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings.
[0019] In addition, in the following descriptions, the same symbol will be used to mark the same parts, and the description of parts that have been described before should be omitted.
[0020] The physical property values in the instruction manual are those at a temperature of 25°C and a pressure of 1 atom. The thickness of each component is the average of the distances in the stacking direction.
[0021] The thickness and structure of components described in the instruction manual can be determined, for example, by images obtained from cross-sections using scanning electron microscopy (SEM), transmission electron microscopy (TEM), high-angle Annular DarkField Scanning Transmission Electron Microscopy (HAADF-STEM). Furthermore, the boundaries of components described in the instruction manual can be determined by images obtained from scanning electron microscopy or transmission electron microscopy, measurements from scanning electron microscopy with energy dispersive X-ray spectroscopy (SEM-EDS) or transmission electron microscopy with energy dispersive X-ray spectroscopy (TEM-EDX), or secondary ion mass analysis. Furthermore, the composition of the components described in the specification can be determined using methods such as secondary ion mass analysis, inductively coupled plasma mass spectrometry (ICP-MS), scanning electron microscopy with energy-dispersive X-ray spectrometry (EDX-SMS), or transmission electron microscopy with EDH-SMS. Additionally, the crystallinity of the components described in the specification can be evaluated using images obtained through X-ray diffraction (XRD), electron backscatter diffraction (EBSD), or high-angle annular dark-field scanning transmission electron microscopy, scanning electron microscopy, or transmission electron microscopy. The materials contained in the components described in the specification (crystal defects, bonding states, etc.) can be evaluated using high-angle annular dark-field scanning transmission electron microscopy, photoluminescence (PL), or X-ray photoelectron spectrophotometry (XPS). These analytical methods are examples and do not negate the specific analytical methods described in the specification.
[0022] (First Implementation) The first embodiment relates to an electrode. Figure 1 The figure shows a schematic cross-sectional view of the electrode 100 according to an embodiment. The electrode 100 has a substrate (first substrate) 1 and a catalyst layer (first catalyst layer) 2. The catalyst layer 2 is disposed on the substrate 1.
[0023] Catalyst layer 2 is used as a catalyst for electrolysis in this embodiment. The electrolysis reaction is, for example, the production of hydrogen from water or ammonia. The electrolysis reaction is, for example, the production of carbon monoxide from carbon dioxide. Catalyst layer 2 is also used as an anode catalyst in the electrolytic production of ammonia.
[0024] The electrode 100 of the first embodiment can be used, for example, as the anode of water electrolysis. If the catalyst layer 2 further includes a catalyst for a fuel cell, the electrode 100 of the embodiment can also be used as the oxygen electrode of a fuel cell. The electrode 100 of the embodiment can also be used as the anode for electrolysis to generate ammonia. The electrode of the embodiment can be used as the anode of an electrolysis apparatus for ammonia synthesis. Hereinafter, in the first embodiment and other embodiments, water electrolysis will be used as an example, but in addition to water electrolysis, the electrode 100 of the embodiment can be used, for example, as the anode of a membrane electrode assembly used in electrolysis for ammonia synthesis: ultrapure water is supplied to the anode, water is decomposed at the anode to generate protons and oxygen, and the generated protons pass through an electrolyte membrane, and nitrogen supplied to the cathode combines with protons and electrons to generate ammonia. The electrode 100 of the embodiment can also be used as the cathode for electrolysis of ammonia to generate hydrogen. The electrode of the embodiment can be used as the cathode of a hydrogen generation apparatus. Hereinafter, in the first embodiment and other embodiments, water electrolysis will be used as an example for description. However, in addition to water electrolysis, the electrode 100 of the embodiment can be used as the cathode of a membrane electrode assembly used in electrolysis for ammonia decomposition, for example: ammonia is supplied to the cathode, ammonia is decomposed at the cathode to generate protons and nitrogen, the generated protons pass through the electrolyte membrane, and at the anode, the protons combine with electrons to generate hydrogen.
[0025] As the substrate 1, a porous material with high electrical conductivity is preferably used. The substrate 1 is a porous component that allows gas and liquid to pass through.
[0026] Substrate 1 comprises metal fibers or metal particles. Substrate 1 preferably comprises metal fibers or metal particles of valve metal. The metal fibers and metal particles may also be plated.
[0027] The substrate 1 containing metal fibers is preferably a fabric containing metal fibers. The fabric containing metal fibers is preferably a web of metal fibers or a nonwoven fabric of metal fibers.
[0028] The substrate 1 containing metal particles is preferably a sintered body formed by the agglomeration of metal particles. The metal particles are preferably stacked along the thickness direction of the substrate 1.
[0029] The metal fiber preferably contains one or more metals selected from the group consisting of titanium, aluminum, tantalum, niobium, hafnium, zirconium, zinc, tungsten, bismuth and antimony, more preferably titanium, and even more preferably titanium.
[0030] The fiber diameter of the metal fiber is preferably 1 μm or more and 500 μm or less, and more preferably 1 μm or more and 100 μm or less, taking into account reactivity and charge-donating properties. The average fiber diameter of the metal fiber is preferably 1 μm or more and 500 μm or less, and more preferably 1 μm or more and 100 μm or less, taking into account reactivity and charge-donating properties.
[0031] The metal particles preferably include one or more metals selected from the group consisting of Ti, Al, Ta, Nb, Hf, Zr, Zn, W, Bi and Sb, more preferably including Ti, and even more preferably Ti.
[0032] The primary particle size (diameter) of the metal particles is preferably 1 μm or more and 500 μm or less, and more preferably 1 μm or more and 100 μm or less, taking into account reactivity and charge-donating properties. The average primary particle size (average diameter) of the metal particles is preferably 1 μm or more and 500 μm or less, and more preferably 1 μm or more and 100 μm or less, taking into account reactivity and charge-donating properties.
[0033] The substrate 1 is a conductive porous body. Considering the movement of matter, the porosity of the substrate 1 is preferably 20% or more and 95% or less, more preferably 40% or more and 90% or less.
[0034] Catalyst layer 2 is disposed on substrate 1. An intermediate layer (not shown) may also be disposed between catalyst layer 2 and substrate 1. Catalyst layer 2 is preferably in direct contact with substrate 1 (catalyst layer 2 is in direct contact with metal fibers or metal particles).
[0035] Catalyst layer 2 preferably contains one or more elements selected from the group consisting of Ir, Ru, Pt, Pd, Ni, Co, Mn, Fe, Cu, V, Au, Cr, Sr, Y, Ag, Sn, Mo, Ti, Al, Ta, Nb, Hf, Zr, Zn, W, Bi, and Sb. Catalyst layer 2 preferably contains oxides containing one or more elements selected from the group consisting of Ir, Ru, Pt, Pd, Ni, Co, Mn, Fe, Cu, V, Au, Cr, Sr, Y, Ag, Sn, Mo, Ti, Al, Ta, Nb, Hf, Zr, Zn, W, Bi, and Sb.
[0036] Catalyst layer 2 preferably contains one or more oxides of a first element selected from the group consisting of Ir, Ru, Pt, and Pd. Catalyst layer 2 preferably contains one or more first elements selected from the group consisting of Ir, Ru, Pt, and Pd. Catalyst layer 2 preferably contains Ir.
[0037] The catalyst layer 2 is preferably a porous material. The porosity of the catalyst layer 2 is preferably 10 vol% or more and 90 vol% or less, more preferably 30 vol% or more and 70 vol% or less.
[0038] The preferred amount of noble metal in catalyst layer 2 is 0.01 mg / cm³. 2 Above and 1.0 mg / cm 2 The following is more preferably 0.03 mg / cm³. 2 Above and 0.5 mg / cm 2 Hereinafter, a further preferred value is 0.04 mg / cm³. 2 Above and 0.1 mg / cm 2 The following is a summary of the mass measurements. The total mass can be determined by ICP-MS.
[0039] The thickness of the catalyst layer 2 is preferably 0.1 μm or more and 2 μm or less, more preferably 0.15 μm or more and 1 μm or less.
[0040] The side of the catalyst layer 2 opposite to the substrate 1 is designated as the first region 2X, and the area outside the first region 2X on the substrate 1 side of the catalyst layer 2 is designated as the second region 2Y.
[0041] The first region 2X and the second region 2Y are arranged in the stacking direction of the substrate 1 and the catalyst layer 2. The first region 2X is a layered region in the catalyst layer 2. The second region 2Y is a layered region in the catalyst layer 2.
[0042] The catalyst layer 2 preferably has a structure in which sheet layers 2A and interstitial layers 2B are alternately stacked. The stacked structure of the catalyst layer 2 disposed on the substrate 1 is shown in [illustration]. Figure 2 and Figure 3 The diagram shows a partial cross-sectional view of the electrodes. Sheet layer 2A and spacer layer 2B are stacked in a generally parallel arrangement. Spacer layer 2B is mostly void, but in a portion, it is connected by the protrusion of sheet layer 2A. Sheet layer 2A is connected by columnar bodies 2C present in spacer layer 2B, maintaining the stacked structure. Figure 2 Schematic diagram and Figure 3 The difference in the schematic diagram is that the layer existing on the substrate 1 side is a sheet layer 2A ( Figure 2 ), or gap layer 2B ( Figure 3 The sheet layer 2A in the attached figure is a partially interrupted, discontinuous sheet, but it can also be an uninterrupted sheet.
[0043] The structure formed by alternating layers of sheet 2A and spacer 2B can also be determined, for example, by the density of the layers in a cross-sectional SEM image of catalyst layer 2.
[0044] Sheet layer 2A is a layer composed of sheet-like aggregates of unsupported catalyst particles, such as metal oxides. Some voids also exist within sheet layer 2A. Sheet layer 2A is a dense layer containing many catalyst particles.
[0045] The sheet layer 2A preferably contains an oxide of the first element.
[0046] Interstitial layer 2B is the region sandwiched between sheet layers 2A, containing unsupported metal oxide particles, i.e., catalyst particles. Unlike sheet layers 2A, interstitial layer 2B does not have the regular structure of catalyst particles. For example, interstitial layer 2B is a region that does not contain unsupported metal oxide particles agglomerated into sheet-like structures. Interstitial layer 2B is the region located between agglomerated sheet-like metal oxide particles in sheet layer 2A. Interstitial layer 2B may sometimes have different constituent elements, but it is a region with a lower density of catalyst particles compared to sheet layer 2A. Columnar bodies 2C exist in interstitial layer 2B. In columnar bodies 2C present in interstitial layer 2B, agglomerated unsupported particles, such as metal oxide particles, extend along the stacking direction of sheet layer 2A and interstitial layer 2B, connecting sheet layer 2A.
[0047] The interstitial layer 2B preferably contains an oxide of the first element.
[0048] The thickest gap layer 2D in gap layer 2B is contained in the first region 2X. Hereinafter, the content simply referred to as gap layer 2B means the entire gap layer 2B including gap layer 2D.
[0049] The average thickness of one layer of sheet layer 2A (the average thickness of all sheet layers 2A) is preferably 10 nm or more and 200 nm or less, more preferably 10 nm or more and 100 nm or less, and even more preferably 10 nm or more and 50 nm or less.
[0050] The average porosity of the sheet layer 2A is preferably 5 vol% or more and 75 vol% or less, more preferably 10 vol% or more and 50 vol% or less, and even more preferably 10 vol% or more and 30 vol% or less.
[0051] The average thickness of the interstitial layer 2B (the average thickness of all interstitial layers 2B) is preferably 5 nm or more and 200 nm or less, more preferably 5 nm or more and 100 nm or less, even more preferably 5 nm or more and 50 nm or less, and even more preferably 5 nm or more and 24 nm or less.
[0052] The average thickness of the interstitial layer 2B in the first region 2X is preferably 1 nm or more and 25 nm or less, more preferably 2 nm or more and 15 nm or less, and even more preferably 2 nm or more and 10 nm or less.
[0053] The average thickness of the interstitial layer 2B in the second region 2Y is preferably 1 nm or more and 20 nm or less, more preferably 2 nm or more and 15 nm or less, and even more preferably 2 nm or more and 10 nm or less.
[0054] The average thickness of the gap layer 2B in the first region 2X (the average thickness of all gap layers 2B in the first region 2X) is preferably thicker than the average thickness of the gap layer 2B in the second region 2Y (the average thickness of all gap layers 2B in the second region 2Y). Preferably, the average thickness of the gap layer 2B in the first region 2X is thicker than the average thickness of the gap layer 2B in the second region 2Y, and the thickest gap layer 2D among the gap layers 2B is included in the first region 2X. The average thickness of the gap layer 2B in the first region 2X is preferably 1.1 times or more and 8 times or less, more preferably 1.5 times or more and 4 times or less, the average thickness of the gap layer 2B in the second region 2Y.
[0055] The thickness of the first region 2X of the catalyst layer 2, located on the side opposite to the substrate 1, is preferably 10% to 30% of the thickness of the first catalyst layer, more preferably 10% to 20%. Through the first region 2X and / or the interstitial layer 2D, even if degradation due to catalyst structure collapse occurs during electrolytic operation using the electrode 100, it can be controlled so that degradation occurs only in the first region 2X (e.g., the interstitial layer 2D), thus minimizing the impact of electrode 100 degradation. If the catalyst layer 2 peels off from the substrate 1 side, the surface of the substrate 1 is exposed, and sometimes the conductivity between the substrate 1 and the catalyst layer 2 decreases. During electrolytic operation, pressure is applied in the direction of contact between the catalyst layer 2 of the electrode 100 and the substrate 1, thus making the substrate 1 and the catalyst layer 2 conductive during operation. However, if the conductivity of the substrate 1 decreases, it becomes a cause of increased battery voltage. Since the catalyst layer 2 has a structure with alternating layers of sheet layer 2A and interstitial layer 2B, the catalyst layer 2 is prone to cleavage. Utilizing the properties of the catalyst layer 2 of the electrode 100, separation between the substrate 1 and the catalyst layer 2 can be suppressed. Preferably, the catalyst layer 2 includes an interstitial layer 2D that serves as an intentional stripping initiation point.
[0056] The average porosity of the interstitial layer 2B is preferably 20 vol% or more and 95 vol% or less, more preferably 30 vol% or more and 80 vol% or less, and even more preferably 40 vol% or more and 70 vol% or less.
[0057] The average porosity of the gap layer 2B is preferably more than 1.1 times and less than 3 times the average porosity of the sheet layer 2A, more preferably more than 1.3 times and less than 2.5 times, and even more preferably more than 1.5 times and less than 2 times.
[0058] The average porosity of the interstitial layer 2B in the first region 2X is preferably 20 vol% or more and 95 vol% or less, more preferably 30 vol% or more and 90 vol% or less, and even more preferably 40 vol% or more and 80 vol% or less.
[0059] Based on the above reasons, the thickness of the thickest gap layer 2D in the gap layer 2B is preferably 1.1 times to 6 times the average thickness of the gap layer 2B, more preferably 1.2 times to 3 times, and even more preferably 1.3 times to 2 times.
[0060] The gap layer 2B having a thickness of 1.3 times or more and 8 times or less than the average thickness of the gap layer 2B is preferably 1 layer (gap layer 2D only) or more and 10 layers or less, and more preferably 1 layer or more and 5 layers or less.
[0061] Based on the above reasons, the thickness of the thickest interstitial layer 2D in the interstitial layer 2B is preferably 10 nm or more and 100 nm or less, more preferably 15 nm or more and 50 nm or less, and even more preferably 20 nm or more and 40 nm or less.
[0062] The interstitial layer 2B has a thickness of 5 nm or more and 100 nm or less. Preferably, it has 1 or more layers (interstitial layer 2D only) and 12 or less, and more preferably 1 or more layers and 6 or less. The interstitial layer 2B with a thickness of 5 nm or more and 100 nm or less is preferably included in the first region 2X and not included in the second region 2Y.
[0063] Based on the above reasons, the thickest interstitial layer 2D in the interstitial layer 2B preferably exists between the interstitial layer 2B on the surface closest to the catalyst layer 2 on the side opposite to the substrate 1 and the interstitial layer 2B on the twelfth layer on the substrate 1 side, more preferably between the interstitial layers 2B in the sixth layer, and even more preferably between the interstitial layers 2B in the fourth layer.
[0064] When a crack occurs in the catalyst layer 2, the penetration depth of the electrolyte membrane varies depending on the width of the crack when bonding the electrode 100 to the electrolyte membrane. If the electrolyte membrane penetrates into the crack, the columnar body 2C at the location of the layer penetration is easily cut off and detached. Therefore, it is preferable that the thickest interstitial layer 2D in the interstitial layer 2B exists when the size and depth of the crack are matched. When a crack exists in the catalyst layer 2, it is preferable that a crack with a depth greater than or equal to the distance from the surface of the catalyst layer 2 opposite to the substrate 1 side to the thickest interstitial layer 2D in the interstitial layer 2B exists on the surface of the catalyst layer 2. In the catalyst layer 2, for example, the position of the thickest interstitial layer 2D in the interstitial layer 2B can be adjusted according to the unavoidable occurrence of cracks.
[0065] The thickness of the sheet layer 2A on the substrate 1 side that directly sandwiches the thickest gap layer 2D in the gap layer 2B is set as T1, and the thickness of the sheet layer 2A on the opposite side of the substrate 1 side that directly sandwiches the thickest gap layer 2D in the gap layer 2B is set as T2. In the gap layer 2D, from the viewpoint of easily separating the sheet layer 2A on the substrate 1 side that directly sandwiches the gap layer 2D and the sheet layer 2A on the opposite side of the substrate 1 side that directly sandwiches the gap layer 2D, it is preferable that T1 is (T1+T2) / 3 or more and 2×(T1+T2) / 3 or less ([one-third of the sum of T1 and T2] or more [[one-third of the sum of T1 and T2] twice] or less), and T2 is (T1+T2) / 3 or more and 2×(T1+T2) / 3 or less.
[0066] Furthermore, based on the above viewpoint, T1 is preferably 1 nm thicker than T2, more preferably 1 nm thicker than T2 but less than 10 nm thick, and even more preferably 1 nm thicker than T2 but less than 5 nm thick.
[0067] Furthermore, the gap layer 2B, which is close to the thickness of the gap layer 2D, may also serve as the starting point for peeling. The second thickest gap layer in the gap layer 2B is preferably present in the first region 2X, and both the second thickest and third thickest gap layers 2B are preferably present in the first region 2X. The thickness of the second thickest gap layer 2B is preferably 0.1 times or more and less than 1 times the thickness of the thickest gap layer 2D in the gap layer 2B, more preferably 0.15 times or more and less than 0.9 times, and even more preferably 0.3 times or more and less than 0.8 times.
[0068] The specific details of the sheet layer 2A and the interstitial layer 2B of the catalyst layer 2, the thickness of the interstitial layer 2B (2D), the composition of the sheet layer 2A and the interstitial layer 2B, and the shear rate of the columnar body 2C in the second embodiment are determined by observing the cross-sections of multiple analytical points using SEM-EDX (Scanning Electron Microscope-Energy Dispersive X-ray Spectroscopy) or TEM-EDX (Transmission Electron Microscope-Energy Dispersive X-ray Spectroscopy). Figure 4 As shown, with the length D1 and width D2 of electrode 100 set to (D1≥D2), imaginary lines are drawn at distances D3 (=D1 / 10) inward from each of the two opposite sides in the width direction of electrode 100, and imaginary lines are drawn at distances D4 (=D2 / 10) inward from each of the two opposite sides in the length direction of electrode 100. Then, imaginary lines parallel to the width direction and passing through the center of electrode 100 are drawn, and imaginary lines parallel to the length direction and passing through the center of electrode 100 are drawn. The region centered at the intersection point 9 of these imaginary lines is designated as analysis points A1 to A9. Each point has a square shape and a diameter of at least 1 μm. 2 The area is defined as [ ]. The image obtained by observing each point can also be a mosaic image created by combining multiple raster images (mosaic). Furthermore, the observation section using SEM-EDX or TEM-EDX is relative to [ ]. Figure 1 The plane is perpendicular to the width direction. The thickness of each sheet layer 2A and each gap layer 2B at analysis points A1~A9 is determined at 50 nm intervals along the width direction of the SEM or TEM image. The average thickness of each sheet layer 2A determined at 50 nm intervals is the thickness of one sheet layer 2A. The average thickness of each gap layer 2B determined at 50 nm intervals is the thickness of one gap layer 2B.
[0069] Next, an example of a method for fabricating electrode 100 is shown. A sheet layer precursor, which is essentially a precursor of sheet layer 2A, and a gap layer precursor, which is essentially a precursor of gap layer 2B, are alternately sputtered onto a substrate 1. The sputtering time is extended to thicken one layer (gap layer 2D) of gap layer 2B on the side opposite to the substrate 1. The sheet layer precursor and the gap layer precursor are formed in an oxidizing atmosphere. The laminate containing the alternately stacked sheet layer precursor and gap layer precursor is treated with a solution that selectively dissolves the oxides mainly contained in the precursor of gap layer 2B. The dissolving solution is, for example, sulfuric acid, hydrochloric acid, or nitric acid. After solution treatment, the electrode 100 is obtained by arbitrary heating in an oxidizing atmosphere.
[0070] In the embodiment, the electrode 100 has an average thickness of the gap layer 2B in the first region 2X that is thicker than the average thickness of the gap layer 2B in the second region 2Y, and / or the thickest gap layer 2D in the gap layer 2B exists in the first region 2X, which can suppress the deterioration of the catalyst layer 2.
[0071] (Second Implementation) The second embodiment relates to a membrane electrode assembly (MEA). Figure 5 The diagram shows a schematic of the membrane electrode assembly 200 according to an embodiment. The membrane electrode assembly 200 includes a first electrode 11, a second electrode 12, and an electrolyte membrane 13. Preferably, the first electrode 11 is an anode electrode, and the second electrode 12 is a cathode electrode. Preferably, the electrode 100 of the first embodiment is used for the first electrode 11 or the second electrode 12. The membrane electrode assembly 200 of the embodiment is preferably used in an electrochemical cell or battery pack for hydrogen or oxygen generation.
[0072] The first electrode 11 has a first substrate and a first catalyst layer. The first catalyst layer is disposed on the first substrate. The first catalyst layer is preferably in direct contact with the electrolyte membrane 13. When electrode 100 is used as the first electrode 11, the first catalyst layer is catalyst layer 2 and the first substrate is substrate 1.
[0073] When the electrode 100 of the membrane electrode assembly 200 is subjected to pressure during electrolysis operation, pressure is applied to the first electrode 11 and the second electrode 12, and the pressure is restored to atmospheric pressure when the operation stops. Sometimes, dry air is supplied to the anode via the membrane electrode assembly 200 when electrolysis operation stops. If such electrolysis operation is performed, the shape of the membrane electrode assembly 200 changes due to the pressure difference and drying, and a portion of the catalyst layer 2 peels off. Even with peeling, the peeled catalyst remains conductive to the substrate 1 due to the pressure applied during electrolysis operation. Using the electrode 100 of the embodiment, peeling at the boundary between the substrate 1 and the catalyst layer 2 caused by volume changes due to pressure difference, drying, etc., can be suppressed.
[0074] like Figure 6As shown in the schematic diagram of the membrane electrode assembly 200, when the volume of the membrane electrode assembly 200 changes, the interstitial layer 2D of the electrode 100 cleaves, suppressing the degradation of the electrode 100. In the membrane electrode assembly 200 that has undergone cycles of electrolysis operation and shutdown, the columnar sections 2C of the interstitial layer 2D are cut off. The cutting rate of the columnar section 2C of the thickest interstitial layer 2D in the interstitial layer 2B is preferably higher than the cutting rate of the columnar section 2C of the entire interstitial layer 2B, preferably 20% or more and 10000% or less of the cutting rate of the columnar section 2C of the entire interstitial layer 2B, more preferably 50% or more and 1000% or less of the cutting rate of the columnar section 2C of the entire interstitial layer 2B, and even more preferably 100% or more and 500% or less. Preferably, the shearing rate of the entire columnar body 2C of the gap layer 2B is 110% or more and 10000% or less, more preferably 120% or more and 1000% or less, and even more preferably 130% or more and 500% or less. Regarding the cutoff rate of columnar bodies 2C in the thickest gap layer 2D within gap layer 2B, observe the cross-sectional SEM image and calculate the density ρ1 of columnar bodies 2C throughout gap layer 2B (the average number of columnar bodies 2C existing within the width of gap layer 2B (width of the cross-sectional SEM image) 1 [μm)) and the density ρ2 of columnar bodies 2C in the thickest gap layer 2D (the average number of columnar bodies 2C per 1 [μm] of the width of the thickest gap layer 2D (width of the cross-sectional SEM image)). ρ1 / ρ2 represents the cutoff rate of columnar bodies 2C in the thickest gap layer 2D within gap layer 2B (at this time, the cutoff rate of columnar bodies 2C throughout gap layer 2B is set to 1).
[0075] The second electrode 12 has a second substrate 12B and a second catalyst layer 12A. The second catalyst layer 12A is disposed on the second substrate 12B. The second catalyst layer 12A is disposed on the electrolyte membrane 13 side. Preferably, the second catalyst layer 12A is in direct contact with the electrolyte membrane 13.
[0076] The second substrate 12B is preferably made of a porous material with high electrical conductivity. The second substrate 12B is a porous component that allows gas and liquid to pass through. The second substrate 12B is, for example, carbon paper or a metal mesh. As a metal mesh, a porous substrate of valve metal is preferred. As a porous substrate of valve metal, a porous substrate comprising one or more metals selected from the group consisting of titanium, aluminum, tantalum, niobium, hafnium, zirconium, zinc, tungsten, bismuth, and antimony, or a porous substrate comprising one metal selected from the group consisting of titanium, aluminum, tantalum, niobium, hafnium, zirconium, zinc, tungsten, bismuth, and antimony, is preferred. The second substrate 12B has a carbon layer (MPL layer) comprising carbon microparticles and a water-resistant resin (PTFE, Nafion, or other fluoropolymers). The carbon layer is, for example, disposed between the carbon paper and the second catalyst layer 12A.
[0077] The second catalyst layer 12A has a catalyst metal. The second catalyst layer 12A is preferably composed of catalyst metal particles supported on a carrier such as carbon. The second catalyst layer 12A is preferably a porous catalyst layer. The catalyst metal is not particularly limited, but for example, it includes one or more selected from the group consisting of Pt, Rh, Os, Ir, Pd, and Au. It is preferable to include one or more selected from the group consisting of such catalyst materials. The catalyst metal is preferably a metal, alloy, or metal oxide. The second catalyst layer 12A preferably has, for example, multiple catalyst units formed by alternating layers of sheet-like catalyst layers and interstitial layers.
[0078] The metal content per unit area of the second catalyst layer 12A is preferably 0.02 mg / cm². 2 Above and 1.0 mg / cm 2 The following is more preferably 0.05 mg / cm³. 2 Above and 0.5 mg / cm 2 The following is a summary of the mass values. The total mass can be determined using ICP-MS.
[0079] The porosity of the second catalyst layer 12A is preferably 10% or more and 90% or less, more preferably 30% or more and 70% or less.
[0080] The electrolyte membrane 13 is preferably a proton-conducting membrane. As the electrolyte membrane 13, it is preferably a fluorinated polymer or an aromatic hydrocarbon polymer selected from the group consisting of sulfonic acid groups, sulfonylimide groups, and sulfate groups. As the electrolyte membrane 13, a fluorinated polymer having sulfonic acid groups is preferred. Examples of fluorinated polymers having sulfonic acid groups include Nafion (manufactured by DuPont), Flemion (manufactured by Asahi Kasei Corporation), Selemion (manufactured by Asahi Kasei Corporation), Aquivion (manufactured by Solvay Specialty Polymers), or Aciplex (manufactured by Asahi Glass Co., Ltd.). Alternatively, the proton-conducting membrane can sometimes be replaced with anion exchange membranes, porous membranes, or other conductive membranes.
[0081] The thickness of the electrolyte membrane 13 is appropriately determined considering the membrane's permeation characteristics, durability, and other properties. From the viewpoint of strength, solvent resistance, and MEA output characteristics, the thickness of the electrolyte membrane 13 is preferably 20 μm or more and 500 μm or less, more preferably 50 μm or more and 300 μm or less, and even more preferably 80 μm or more and 200 μm or less.
[0082] The electrolyte membrane 13 preferably includes a noble metal region on the side of the first electrode 11. The noble metal region contains noble metal particles. The noble metal region is preferably present on the surface of the electrolyte membrane 13. The noble metal region is preferably composed of a single region, but it may also be composed of multiple separate regions.
[0083] The precious metal particles are preferably particles of one or more precious metals selected from the group consisting of Pt, Re, Rh, Ir, Pd, and Ru. The precious metal particles may also include particles containing alloys selected from the group consisting of Pt, Re, Rh, Ir, Pd, and Ru. The precious metal particles are preferably particles of one precious metal selected from the group consisting of Pt, Re, Rh, Ir, Pd, and Ru. Pt particles are preferred. Re particles are preferred. Rh particles are preferred. Ir particles are preferred. Pd particles are preferred. Ru particles are preferred.
[0084] The noble metal particles oxidize the hydrogen generated on the cathode side and passing through the electrolyte membrane 13. Hydrogen leakage is suppressed by the noble metal particles. Because the noble metal particles are present on the anode side, they do not readily oxidize the hydrogen discharged from the cathode side. The region containing the noble metal particles may also exist in the electrolyte membrane 13 on the second electrode 12 (cathode) side.
[0085] The average circumscribed circle diameter of the noble metal particles is preferably 0.5 nm or more and 50 nm or less, more preferably 1 nm or more and 10 nm or less, and even more preferably 1 nm or more and 5 nm or less.
[0086] By using the durable and high-performance electrode 100 as the anode of the membrane electrode assembly 200, it is possible to operate with high activity for a long time.
[0087] (Third implementation method) The third embodiment relates to an electrochemical battery. Figure 7 This is a cross-sectional view showing the electrochemical cell 300 according to the third embodiment. The electrochemical cell 300 will be described below using water electrolysis as an example, but hydrogen can also be produced by decomposing ammonia or other substances besides water.
[0088] like Figure 7 As shown, the electrochemical cell 300 of the third embodiment includes a first electrode (anode) 11, a second electrode (cathode) 12, an electrolyte membrane 13, gaskets 21 and 22, a separator 23, and a separator 24. The sealing material of the first electrode 11 can also be used as gasket 21. The sealing material of the second electrode 12 can also be used as gasket 22.
[0089] Preferably, a membrane electrode assembly 200 is used, which is formed by bonding a first electrode (anode) 11, a second electrode (cathode) 12, and an electrolyte membrane 13. Alternatively, the anode power supply and the diaphragm 23 can be disposed separately. Alternatively, the cathode power supply and the diaphragm 24 can be disposed separately.
[0090] Figure 7 In the electrochemical cell 300, a power source (not shown) is connected to membranes 23 and 24, where a reaction occurs at the first electrode 11 and the second electrode 12. For the first electrode 11, for example, water is supplied, where water is decomposed into protons, oxygen, and electrons. The electrode support and charge supply are porous materials that function as flow path plates. The generated and unreacted water is discharged, and the protons and electrons are utilized in the cathode reaction. The cathode reaction is a reaction of protons and electrons to produce hydrogen. Either or both of the generated hydrogen and oxygen can be used, for example, as fuel for fuel cells or engines.
[0091] (Fourth Implementation) The fourth embodiment relates to a battery pack. Figure 8 This is a schematic cross-sectional view showing the battery pack 400 according to the fourth embodiment. Figure 8 The battery pack 400 shown in the third embodiment has multiple MEAs 200 or electrochemical cells 300 connected in series. Fastening plates 31 and 32 are installed at both ends of the MEAs or electrochemical cells.
[0092] The amount of hydrogen generated in an electrochemical cell 300 consisting of a single MEA200 is small. Therefore, if a battery pack 400 consisting of multiple MEA200s or multiple electrochemical cells 300 connected in series is constructed, a large amount of hydrogen can be obtained.
[0093] (Fifth Implementation) The fifth embodiment relates to an electrolysis apparatus. The electrolysis apparatus is, for example, a PEM-type water electrolysis apparatus (PEMEC). Figure 9 A conceptual diagram of the electrolysis apparatus according to the fifth embodiment is shown. For the electrolysis apparatus 500, an electrochemical cell 300 or a battery pack 400 is used. Figure 9 The electrolysis apparatus is used for water electrolysis. An electrolysis apparatus for water electrolysis will be described. For example, in the case of producing hydrogen from ammonia, an apparatus with other configurations using electrode 100 is preferred. Furthermore, the electrode of the embodiment can also be used in an electrolysis apparatus for electrolyzing carbon dioxide to produce organic compounds such as methanol or ethylene, or carbon monoxide.
[0094] like Figure 9As shown, a series-cascaded water electrolysis single cell is used as a battery pack 400. A power supply 41 is installed in the battery pack 400, applying voltage between the anode and cathode. On the anode side of the battery pack 400, the generated gas is connected to a gas-liquid separator 42 and a mixing tank 43 to separate unreacted water. For the mixing tank 43, a pump 46 supplies liquid from an ion-exchange water production unit 44, circulating it from the gas-liquid separator 42 to the anode via a check valve 47. Oxygen generated at the anode is obtained by passing it through the gas-liquid separator 42. On the cathode side, a hydrogen refining unit 49 is continuously connected to the gas-liquid separator 48 to obtain high-purity hydrogen. Impurities are discharged through a path with a valve 50 connected to the hydrogen refining unit 49. To stably control the operating temperature, the heating of the battery pack and mixing tank, the current density during thermal decomposition, etc., can be controlled.
[0095] The present invention will now be described in more detail with reference to embodiments, but the present invention is not limited to the following embodiments.
[0096] (Example 1) A catalyst layer is formed on a nonwoven fabric containing titanium metal fibers as a substrate. The catalyst layer has a structure consisting of 40 alternating layers of sheet material and 40 interstitial layers. Sheet material precursors containing Ir oxide and interstitial layer precursors containing Ni oxide are alternately sputtered in an oxidizing atmosphere to form 40 alternating layers of sheet material precursors and interstitial layer precursors. The thickness of the interstitial layer precursor located on the opposite side from the substrate side in the 40 interstitial layer precursors is four times thicker than the other interstitial layer precursors. The noble metal loading density is 0.15 mg / cm³. 2 Subsequently, sulfuric acid was used to selectively dissolve most of the interstitial layer precursor to obtain the electrode of the embodiment. The obtained electrode was used as the anode.
[0097] An electrode was obtained by forming a porous catalyst layer containing Pt on carbon paper as a substrate. The resulting electrode was used as the cathode. The loading density of the noble metal was 0.2 mg / cm³. 2 ].
[0098] A Nafion membrane was sandwiched between the obtained anode and cathode as an electrolyte membrane and pressed together to obtain a membrane electrode assembly. The obtained membrane electrode assembly was then placed between two flow-pathed membranes and fixed with a gasket to obtain an electrochemical cell. An acceleration test was conducted using the obtained electrochemical cell. The measurement temperature was 80 °C, and the current density was 2 A / cm². 2The pressure difference between the anode and cathode ([pressure of the fluid flowing through the diaphragm of the cathode] - [pressure of the fluid flowing through the diaphragm of the anode]) was 8 atmospheres. Water electrolysis was performed before drying, and the battery voltage was measured. After water electrolysis, the anode and cathode were restored to atmospheric pressure. As an accelerated test, dry air (0% relative humidity, 25°C) was supplied to the anode to dry it. The battery voltage was measured approximately 100 hours, 250 hours, and 400 hours after the start of drying. Then, the rate of increase in battery voltage after each time period from the start of drying was evaluated.
[0099] In Example 1, the case where the rate of increase of battery voltage ([battery voltage after each time period] - [battery voltage at the start of operation]) / [battery voltage at the start of operation]) is 0% or more and less than 1% is evaluated as A, the case where it is 1% or more and less than 3% is evaluated as B, the case where it is 3% or more and less than 5% is evaluated as C, and the case where it is 5% or more is evaluated as D.
[0100] (Comparative Example 1) Except that the sheet layer precursor and the interstitial layer precursor are alternately laminated in such a way that all interstitial layer precursors have the same thickness, the anode is fabricated in the same manner as in Example 1, and an electrochemical cell is fabricated using the fabricated anode. The cell voltage is measured using the fabricated electrochemical cell under the same conditions as in Example 1.
[0101] Regarding the rate of increase of battery voltage in Example 1, where the comparison object is set as Comparative Example 1, the following is summarized: Figure 10 The table shows that the rate of voltage rise of the single cell in Example 1 is very low, maintaining an A rating even after a long period of time. On the other hand, the voltage rise of the battery in Comparative Example 1 after drying is shown in the table. Providing a thick interstitial layer 2D on the electrolyte membrane side suppresses the rise in battery voltage. Even changing the thickness of the interstitial layer 2D within a preferred range, the rise in battery voltage can be suppressed. Furthermore, within the first region, even changing the position of the interstitial layer 2D can suppress the rise in battery voltage.
[0102] Furthermore, unlike the accelerated test, the anodes of Example 1 and Comparative Example 1 were used in electrochemical cells, respectively. Unlike the accelerated test under the aforementioned pressurized conditions, the cells were operated under atmospheric pressure and the same conditions (current density 2 [A / cm²]). 2The electrochemical cells using the anode of Example 1 and the anode of Comparative Example 1 were evaluated after 5000 hours of continuous operation (water electrolysis operation at atmospheric pressure). The cell voltage of the electrochemical cell using the anode of Example 1 after continuous operation was lower than that of the electrochemical cell using the anode of Comparative Example 1 after continuous operation, maintaining an A rating. In contrast, the comparative example received a B rating. During normal water electrolysis operation, the durability of the anode of Example 1 also improved in the accelerated test.
[0103] The technical solutions for the implementation methods are described below.
[0104] Technical Solution 1 An electrode having: First substrate; and The first catalyst layer consists of alternating layers of sheet material and spacer material disposed on the first substrate. The side of the first catalyst layer opposite to the first substrate side is designated as the first region, and the area outside the first region is designated as the second region. The average thickness of the gap layer in the first region is greater than the average thickness of the gap layer in the second region, or / and the thickest gap layer exists in the first region.
[0105] Technical Solution 2 According to the electrode described in technical solution 1 The thickness of the first region is more than 10% and less than 30% of the thickness of the first catalyst layer.
[0106] Technical Solution 3 The electrode according to technical solution 1 or 2 The thickness of the first region is more than 10% and less than 20% of the thickness of the first catalyst layer.
[0107] Technical Solution 4 The electrode according to any one of technical solutions 1-3, The average porosity of the gap layer is more than 1.1 times and less than 3 times the average porosity of the sheet layer.
[0108] Technical Solution 5 The electrode according to any one of technical solutions 1-4, The first catalyst layer contains one or more first elements selected from the group consisting of Ir, Ru, Pt and Pd.
[0109] Technical Solution 6 The electrode according to any one of technical solutions 1-5, The average thickness of the interstitial layer is 10 nm or more and 200 nm or less. The average thickness of the interstitial layer in the first region is 1 nm or more and 25 nm or less. The average thickness of the gap layer in the second region is above 1 nm and below 20 nm.
[0110] Technical Solution 7 The electrode according to technical solution 6 The thickness of the thickest gap layer is more than 1.1 times and less than 6 times the average thickness of the gap layers.
[0111] Technical Solution 8 The electrode according to technical solution 6 or 7 The thickness of the thickest interstitial layer is 10 nm or more and 100 nm or less.
[0112] Technical Solution 9 The electrode according to any one of technical solutions 1-8, The average thickness of the gap layer in the first region is more than 1.1 times and less than 8 times the average thickness of the gap layer in the second region.
[0113] Technical Solution 10 The electrode according to any one of technical solutions 1-0, The thickest interstitial layer exists between the interstitial layer on the surface closest to the first catalyst layer on the side opposite to the first substrate and the interstitial layer on the twelfth layer located on the first substrate side.
[0114] Technical Solution 11 The electrode according to any one of technical solutions 3-10, The average porosity of the interstitial layer is above 20% and below 95%. The average porosity of the interstitial layer in the first region is above 20% and below 95%.
[0115] Technical Solution 12 The electrode according to any one of technical solutions 1-11, The thickness of the sheet layer on the first substrate side, which directly sandwiches the thickest gap layer, is defined as T1. The thickness of the sheet layer on the opposite side of the first substrate side, which directly sandwiches the thickest gap layer, is defined as T2. The T1 is greater than (T1+T2) / 3 and less than 2×(T1+T2) / 3. The T2 is greater than (T1+T2) / 3 and less than 2×(T1+T2) / 3.
[0116] Technical Solution 13 The electrode according to any one of technical solutions 1-12, The second thickest gap layer exists in the first region. The thickness of the second thickest gap layer in the gap layer is more than 0.1 times and less than 1 times the thickness of the thickest gap layer in the gap layer.
[0117] Technical Solution 14 The electrode according to any one of technical solutions 1-13, The thickness of the sheet layer on the first substrate side, which directly sandwiches the thickest gap layer, is defined as T1. The thickness of the sheet layer on the opposite side of the first substrate side, which directly sandwiches the thickest gap layer, is defined as T2. The T1 is greater than (T1+T2) / 3 and less than 2×(T1+T2) / 3. The T2 is greater than (T1+T2) / 3 and less than 2×(T1+T2) / 3. The thickness of T1 is more than 1 nm greater than that of T2.
[0118] Technical Solution 15 A membrane electrode assembly comprising an electrode as a first electrode as described in any one of technical solutions 1-14, a second electrode having a second substrate and a second catalyst layer, and an electrolyte membrane disposed between the first electrode and the second electrode.
[0119] Technical Solution 16 The membrane electrode assembly according to technical solution 15 The gap layer is sandwiched between the sheet layers. The gap layer includes columnar bodies that connect to sheet layers sandwiching the gaps. The shearing rate of the columnar part of the thickest gap layer is higher than the shearing rate of the columnar part of the entire gap layer.
[0120] Technical Solution 17 An electrochemical battery that uses the membrane electrode assembly described in technical solution 15 or 16.
[0121] Technical Solution 18 A battery pack that uses the electrochemical battery described in technical solution 17.
[0122] Technical Solution 19 An electrolysis device that uses the electrochemical cell described in technical solution 17 Technical Solution 20 A PEM-type water electrolysis device that uses the electrochemical cell of technical solution 17.
[0123] In the specification, a portion of an element is represented only by its element symbol.
[0124] While several embodiments of the invention have been described, these embodiments, presented as examples, are not intended to limit the scope of the invention. PEMEC is cited as an example of a water electrolyzer, but the invention is equally applicable to other electrolyzers. These novel embodiments described above can be implemented in various other ways, with various omissions, substitutions, and modifications possible without departing from the spirit of the invention. These embodiments and their variations are included within the scope or spirit of the invention, and within the scope of the invention as set forth in the claims and its equivalents.
Claims
1. An electrode characterized by, have: First substrate; as well as The first catalyst layer consists of alternating layers of sheet material and spacer material disposed on the first substrate. The side of the first catalyst layer opposite to the first substrate side is designated as the first region, and the area outside the first region is designated as the second region. The average thickness of the gap layer in the first region is greater than the average thickness of the gap layer in the second region, or / and the thickest gap layer exists in the first region.
2. The electrode according to claim 1, characterized in that, The thickness of the first region is more than 10% and less than 30% of the thickness of the first catalyst layer.
3. The electrode according to claim 1, characterized in that, The thickness of the first region is more than 10% and less than 20% of the thickness of the first catalyst layer.
4. The electrode according to claim 1, characterized in that, The average porosity of the gap layer is more than 1.1 times and less than 3 times the average porosity of the sheet layer.
5. The electrode according to claim 1, characterized in that, The first catalyst layer contains one or more first elements selected from the group consisting of Ir, Ru, Pt and Pd.
6. The electrode according to claim 1, characterized in that, The average thickness of the interstitial layer is greater than 5 nm and less than 200 nm. The average thickness of the interstitial layer in the first region is 1 nm or more and 25 nm or less. The average thickness of the gap layer in the second region is above 1 nm and below 20 nm.
7. The electrode according to claim 6, characterized in that, The thickness of the thickest gap layer is more than 1.1 times and less than 6 times the average thickness of the gap layers.
8. The electrode according to claim 6, characterized in that, The thickness of the thickest interstitial layer is 10 nm or more and 100 nm or less.
9. The electrode according to any one of claims 1-8, characterized in that, The average thickness of the gap layer in the first region is more than 1.1 times and less than 8 times the average thickness of the gap layer in the second region.
10. The electrode according to any one of claims 1-8, characterized in that, The thickest interstitial layer exists between the interstitial layer on the surface closest to the first catalyst layer on the side opposite to the first substrate and the interstitial layer on the first substrate side located in the twelfth layer.
11. The electrode according to any one of claims 3-8, characterized in that, The average porosity of the interstitial layer is above 20 vol% and below 95 vol%. The average porosity of the interstitial layer in the first region is 20 vol% or more and 95 vol% or less.
12. The electrode according to claim 1, characterized in that, The thickness of the sheet layer on the first substrate side, which directly sandwiches the thickest gap layer, is defined as T1. The thickness of the sheet layer on the opposite side of the first substrate side, which directly sandwiches the thickest gap layer, is defined as T2. The T1 is greater than (T1+T2) / 3 and less than 2×(T1+T2) / 3. The T2 is greater than (T1+T2) / 3 and less than 2×(T1+T2) / 3.
13. The electrode according to any one of claims 1-8, characterized in that, The second thickest gap layer exists in the first region. The thickness of the second thickest gap layer in the gap layer is more than 0.1 times and less than 1 times the thickness of the thickest gap layer in the gap layer.
14. The electrode according to claim 1, characterized in that, The thickness of the sheet layer on the first substrate side, which directly sandwiches the thickest gap layer, is defined as T1. The thickness of the sheet layer on the opposite side of the first substrate side, which directly sandwiches the thickest gap layer, is defined as T2. The T1 is greater than (T1+T2) / 3 and less than 2×(T1+T2) / 3. The T2 is greater than (T1+T2) / 3 and less than 2×(T1+T2) / 3. The thickness of T1 is more than 1 nm greater than that of T2.
15. A membrane electrode assembly, characterized by It comprises an electrode as a first electrode according to any one of claims 1-14, a second electrode having a second substrate and a second catalyst layer, and an electrolyte membrane disposed between the first electrode and the second electrode.
16. The membrane electrode assembly according to claim 15, characterized in that, The gap layer is sandwiched between the sheet layers. The gap layer includes columnar bodies that connect to sheet layers sandwiching the gaps. The shearing rate of the columnar part of the thickest gap layer is higher than the shearing rate of the columnar part of the entire gap layer.
17. An electrochemical cell characterized by It uses the membrane electrode assembly as described in claim 15.
18. A battery pack, characterized by It uses the electrochemical battery described in claim 17.
19. An electrolysis device, characterized by It uses the electrochemical battery described in claim 17.
Citation Information
Patent Citations
Rainwater drainage device, rainwater drainage system, roof, building, and pipe
JP2025078853A