C@TiN composite support, supported Pt-based catalysts, their preparation methods and applications

By coating a TiN layer onto the surface of a carbon support, the stability and mass transfer efficiency of the PEMFC cathode catalyst were solved, achieving an efficient proton conduction network and optimization of the three-phase reaction interface, thereby improving the output performance and durability of the fuel cell.

CN123120761APending Publication Date: 2026-11-17SOUTHERN UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611577485.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing platinum-carbon materials used in proton exchange membrane fuel cell (PEMFC) cathode oxygen reduction catalysts have insufficient activity and stability, the carbon support is prone to corrosion, and the mass transfer efficiency within the catalyst layer is low. This results in high platinum loading, low utilization, and high cost. Furthermore, the uneven distribution of ionomers affects the proton transport channels and the construction of the three-phase interface.

Method used

The C@TiN composite support is used to improve the corrosion resistance and anti-agglomeration stability of the support and catalyst particles by coating the surface of the carbon support with a TiN layer. Furthermore, the distribution of ionomers is regulated by the functional groups on the TiN surface, thereby optimizing the proton conduction network and the three-phase reaction interface.

Benefits of technology

It significantly improved the structural stability of the catalyst and the continuity of the proton conduction network, optimized the three-phase reaction interface, improved the output performance and durability of the membrane electrode, and reduced the platinum loading.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120761A_ABST
    Figure CN123120761A_ABST
Patent Text Reader

Abstract

This invention discloses a C@TiN composite support, a supported Pt-based catalyst, and their preparation methods and applications, relating to the fields of nanocomposite materials and electrocatalysis. Addressing the problem of uneven ionomer distribution in the membrane electrode assembly (MEA) of proton exchange membrane fuel cells (PEMFCs), this invention uses ZIF-8 as a template to prepare a C@TiN composite support through surface coating with a titanium source and programmed pyrolysis carbonization. This support comprises a carbon matrix and a TiN layer coated on its surface. By loading Pt-based active components onto the surface of this support, a supported Pt-based catalyst is obtained. This invention also provides the application of this catalyst in the MEA of a proton exchange membrane fuel cell. The C@TiN composite support exhibits adsorption regulation of ionomers, which is beneficial for promoting the continuous construction of the proton conduction network and optimizing the three-phase reaction interface, while simultaneously improving the structural stability of the catalyst particles. When this catalyst is applied to the catalytic layer of the MEA, it can improve the output performance and durability of the MEA.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of nanocomposite materials and electrocatalysis technology, specifically to a C@TiN composite support, a supported Pt-based catalyst, its preparation method, and its application. Background Technology

[0002] Proton exchange membrane fuel cells (PEMFCs), as a core technology for the efficient utilization of hydrogen energy, offer advantages such as high energy conversion efficiency and environmental friendliness, making them an important technical solution for zero-emission power in heavy-duty vehicles. However, the oxygen reduction (ORR) catalyst in PEMFC cathodes primarily uses platinum-carbon (Pt / C) materials, which suffer from insufficient activity and stability. Furthermore, the limited mass transfer efficiency within the catalyst layer results in high platinum loading and low utilization, making cost a key bottleneck restricting its large-scale application. Specifically, under strong acid and high-potential conditions, traditional Pt / C catalysts are prone to platinum particle dissolution and agglomeration, and the carbon support is also susceptible to corrosion, directly leading to a decrease in electrochemical active area and output voltage loss. Simultaneously, uneven distribution of ionomers within the catalyst layer causes discontinuous proton transport channels, resulting in low efficiency in constructing the gas-electron-proton three-phase interface, further exacerbating mass transfer resistance and reducing the effective utilization rate of platinum.

[0003] To address the aforementioned stability issues, researchers have attempted to enhance catalyst structural stability through strategies such as increasing the graphitization degree of the carbon support, heteroatom doping, or platinum coating with carbon layers. However, these methods often struggle to effectively balance improving the corrosion resistance of the support with strengthening the anchoring ability of platinum particles. For the problem of uneven ionomer distribution, existing optimization methods mainly include controlling the ionomer / carbon ratio (I / C), optimizing the solvent system and coating process to indirectly improve the ionomer dispersion, and using heteroatoms such as N and S to dope the carbon support, enhancing its interaction with the sulfonic acid groups of the ionomer. However, these methods introduce new corrosion-active sites at high potentials, making it difficult to fundamentally solve the corrosion problem of the carbon support.

[0004] In recent years, transition metal nitrides (such as TiN and VN) have attracted attention due to their excellent corrosion resistance and metalloid conductivity. To balance the high conductivity of carbon supports with the corrosion resistance of TiN, C@TiN composite supports (i.e., TiN layers coated on the surface of carbon supports) have become a more practical structural design. However, existing research is mostly limited to three-electrode activity testing of supported catalysts, lacking systematic verification of the long-term operational stability of catalysts under real membrane electrode conditions. Particularly at the catalyst layer level, the influence of C@TiN composite supports on ionomer adsorption and spatial distribution remains unclear—which directly relates to the continuity of the proton conduction network and the construction quality of the three-phase reaction interface. Therefore, elucidating the influence of C@TiN composite supports on ionomer adsorption and spatial distribution, and using this as a guide to construct efficient mass transfer catalyst layer structures, is a crucial technological bottleneck that urgently needs to be overcome in the field of low-platinum fuel cells. Summary of the Invention

[0005] The purpose of this invention is to at least solve one of the technical problems existing in the prior art, and to provide a C@TiN composite support, a supported Pt-based catalyst, and its preparation method and application. This invention improves the corrosion resistance and anti-agglomeration stability of the support and catalyst particles by growing a TiN layer on the surface of a carbon support; at the same time, it optimizes the proton conduction network and the three-phase reaction interface by regulating the uniform distribution of ionomers on the surface of the support through the functional groups on the TiN surface, thereby improving the output performance and durability of the membrane electrode.

[0006] The technical solution of the present invention is as follows: In a first aspect, the present invention provides a supported Pt-based catalyst, the supported Pt-based catalyst comprising a C@TiN composite support and a Pt-based active component supported on the C@TiN composite support; The C@TiN composite carrier includes a carbon matrix and a TiN coating layer covering the surface of the carbon matrix; In the C@TiN composite carrier, the thickness of the TiN coating layer is 5 nm to 50 nm, and the TiN loading is 5 wt% to 50 wt%. The carbon matrix is ​​formed by pyrolysis and carbonization of ZIF-8, and the particle size of ZIF-8 is 50 nm to 500 nm. The Pt-based active component is Pt nanoparticles or Pt-based intermetallic compound nanoparticles, wherein the Pt-based intermetallic compound comprises an intermetallic compound formed by Pt and at least one metal element selected from Fe, Co, Ni, Cu, Zn, Mn, Cr, and V.

[0007] In a preferred embodiment of the present invention, the loading of TiN in the C@TiN composite carrier is 5 wt% to 30 wt%.

[0008] In a preferred embodiment of the present invention, the preparation method of the C@TiN composite support includes the following steps: S1. The ZIF-8 template and titanium precursor are mixed in a solvent and reacted to obtain the ZIF-8@titanium source composite. S2. The ZIF-8@titanium source composite is subjected to programmed high-temperature pyrolysis under an inert gas atmosphere to obtain the C@TiN composite support.

[0009] In a preferred embodiment of the present invention, in step S1, the method for preparing the ZIF-8 template includes: mixing a zinc salt and 2-methylimidazole in a solvent, and reacting to obtain the ZIF-8 template; wherein the zinc salt is selected from at least one of zinc nitrate, zinc acetate, and zinc chloride; the molar ratio of 2-methylimidazole to zinc salt is 2:1 to 8:1; the solvent is selected from at least one of methanol, ethanol, N,N-dimethylformamide, and deionized water; the reaction temperature is 10°C to 60°C, and the reaction time is 0.5 hours to 24 hours.

[0010] In a preferred embodiment of the present invention, in S1, the titanium precursor is selected from at least one of tetrabutyl titanate, titanium tetrachloride, titanium isopropoxide, and titanium tetraisopropoxy; the mass ratio of the ZIF-8 template to the titanium precursor is 1:0.5 to 1:6.

[0011] In a preferred embodiment of the present invention, in S2, the temperature of the programmed high-temperature pyrolysis is 700℃~1000℃, the heating rate is 1℃ / min~10℃ / min, the holding time is 1 hour~5 hours, and the flow rate of the inert gas is 50 mL / min~500 mL / min.

[0012] In a preferred embodiment of the present invention, the loading amount of the Pt-based active component in the supported Pt-based catalyst is 10 wt% to 60 wt%, and the average particle size of the Pt-based active component is 2 nm to 6 nm.

[0013] Secondly, the present invention provides a method for preparing a supported Pt-based catalyst, comprising the following steps: The C@TiN composite support, Pt precursor, and solvent are mixed, and the Pt-based active component in the Pt precursor is loaded onto the surface of the C@TiN composite support through a reduction reaction to obtain the supported Pt-based catalyst.

[0014] In a preferred embodiment of the present invention, the Pt precursor is selected from at least one of chloroplatinic acid, potassium chloroplatinate, platinum acetylacetonate, and platinum nitrate; The reduction reaction is carried out by liquid-phase reduction, ethylene glycol reduction, or impregnation reduction.

[0015] In a preferred embodiment of the present invention, when the Pt-based active component is a Pt-based intermetallic compound, the preparation method includes the following specific steps: The C@TiN composite support, Pt precursor and solvent are mixed, and the Pt-based active component in the Pt precursor is loaded onto the surface of the C@TiN composite support by a reduction reaction to obtain the initial Pt-based catalyst. The initial Pt-based catalyst, metal salt, and solvent were mixed, rotary evaporated, and dried. The dried sample was placed in a 4%~6% H2 / Ar atmosphere and heated to 650~700℃ at a heating rate of 3℃ / min~7℃ / min and held for 1.5 hours~2 hours to obtain the supported Pt-based catalyst. The metal salt includes a salt of at least one metal selected from Fe, Co, Ni, Cu, Zn, Mn, Cr, and V.

[0016] Thirdly, the present invention provides a fuel cell catalyst layer comprising an ionomer and the supported Pt-based catalyst, wherein the ionomer is uniformly distributed on the surface of a C@TiN composite support.

[0017] This invention provides the application of supported Pt-based catalysts in the preparation of fuel cell catalyst layers, specifically the application of supported Pt-based catalysts in the preparation of fuel cell catalyst layers with uniformly distributed ionomers. The TiN layer of the C@TiN composite support in the supported Pt-based catalyst can regulate the uniform distribution of ionomers on the surface of the C@TiN composite support.

[0018] Fourthly, the present invention provides a proton exchange membrane fuel cell membrane electrode assembly, comprising the above-mentioned fuel cell catalyst layer.

[0019] This invention has at least one of the following beneficial effects: The C@TiN composite carrier of the present invention can play a synergistic role in the anchoring and stabilization of Pt particles and the regulation of ionomer distribution. On the one hand, the C@TiN composite carrier of the present invention can effectively anchor Pt particles and inhibit their migration and aggregation; on the other hand, it can regulate the adsorption and spatial distribution of ionomers. Specifically: (1) This invention utilizes the excellent corrosion resistance of TiN and the strong metal-support interaction (SMSI) between TiN and Pt to effectively suppress the electrochemical corrosion of the carbon support under strong acid and high potential conditions, as well as the dissolution and agglomeration of Pt particles, significantly improving the structural stability of the support and catalyst particles. The C@TiN composite support prepared by this invention provides uniformly dispersed anchoring points for Pt-based active components. The loaded Pt nanoparticles or Pt-based intermetallic compound nanoparticles have small particle size and high dispersion. Furthermore, the TiN coating layer can effectively suppress particle sintering of intermetallic compounds during high-temperature ordered heat treatment, which is beneficial to improving the utilization rate of Pt and reducing the platinum loading. In addition, this invention uses ZIF-8 as a template to simultaneously achieve the formation of the carbon matrix and the conversion of TiN through surface coating with a titanium source and programmed pyrolysis carbonization. The preparation method is simple, efficient, and easy to scale up.

[0020] (2) This invention utilizes the intrinsic surface chemical properties of the C@TiN composite carrier to guide the orderly adsorption and uniform distribution of ionomers on the carrier surface, which is beneficial to constructing a continuous and efficient proton conduction network, optimizing the three-phase reaction interface, and thus improving the mass transfer efficiency and output performance of the membrane electrode. Attached Figure Description

[0021] Figure 1 The image is a SEM image of ZIF-8 prepared in Example 1.

[0022] Figure 2 The XRD pattern of the C@TiN composite support prepared in Example 1.

[0023] Figure 3 SEM image of the C@TiN composite carrier prepared in Example 1.

[0024] Figure 4 STEM image and EDS surface distribution map of Ti, N and C elements of the C@TiN composite carrier prepared in Example 1.

[0025] Figure 5 The image shows the EDS surface distribution of Nafion ionomers on the C@TiN composite support prepared in Example 1.

[0026] Figure 6 TEM image and EDS surface distribution map of Pt element for the Pt / C@TiN catalyst prepared in Example 1.

[0027] Figure 7 TEM image and EDS surface distribution diagram of Pt, Co, Ti, N and C elements of the PtCo / C@TiN catalyst prepared in Example 6.

[0028] Figure 8 The graph shows the polarization performance and durability of the PtCo / C@TiN PEMFC battery in Example 8. Detailed Implementation

[0029] To make the technical problems solved, the technical solutions, and the beneficial effects of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.

[0030] One embodiment of the present invention provides a C@TiN composite support, the C@TiN composite support comprising a carbon matrix and a TiN coating layer covering the surface of the carbon matrix; In the C@TiN composite carrier, the thickness of the TiN coating layer is 5 nm to 50 nm, and the TiN loading is 5 wt% to 50 wt%.

[0031] This invention, by coating a carbon support with a TiN layer, effectively suppresses the electrochemical corrosion of the carbon support under strong acid and high potential conditions, as well as the dissolution and aggregation of Pt particles, by utilizing the excellent corrosion resistance of TiN and its strong metal-support interaction (SMSI) with Pt, thus significantly improving the structural stability of the support and catalyst particles. On the other hand, the surface groups of the C@TiN composite support can regulate the adsorption and spatial distribution of ionomers, which is beneficial for constructing a continuous and efficient proton conduction network, optimizing the three-phase reaction interface, and thus improving the mass transfer efficiency and output performance of the membrane electrode.

[0032] In some embodiments, there is a metal-support interaction between the C@TiN composite support and the Pt-based active component.

[0033] In some embodiments, the carbon matrix is ​​a carbon matrix formed by pyrolysis and carbonization of ZIF-8, wherein the particle size of ZIF-8 is 50 nm to 500 nm, preferably 100 nm to 300 nm.

[0034] In some embodiments, the loading amount of TiN in the C@TiN composite carrier is 5 wt% to 30 wt%; preferably, the loading amount of TiN is 5 wt% to 20 wt%; more preferably, the loading amount of TiN is 5 wt% to 15 wt%.

[0035] In some embodiments, the thickness of the TiN coating layer is 5 nm to 30 nm.

[0036] In some embodiments, a C@TiN composite carrier is provided, which uses ZIF-8 as a template. By dispersing ZIF-8 in a titanium compound solution, loading a titanium source onto the surface of ZIF-8, and then performing pyrolysis and carbonization, tetrabutyl titanate is converted into a TiN coating layer. At the same time, the organic ligands in ZIF-8 are carbonized into a carbon matrix to form a C@TiN composite carrier. This results in a composite carrier that combines the high conductivity of a carbon matrix with the corrosion resistance of TiN.

[0037] Another embodiment of the present invention provides a method for preparing the C@TiN composite support, comprising the following steps: S1. The ZIF-8 template and titanium precursor are mixed in a solvent and reacted to obtain the ZIF-8@titanium source composite. S2. The ZIF-8@titanium source composite is subjected to programmed high-temperature pyrolysis under an inert gas atmosphere to obtain the C@TiN composite support.

[0038] This invention uses ZIF-8 as a template to simultaneously achieve the formation of a carbon matrix and the conversion of TiN through surface coating with a titanium source and programmed pyrolysis carbonization. The preparation method is simple, efficient, and easy to scale up.

[0039] In some embodiments, in S1, the method for preparing the ZIF-8 template includes: mixing zinc salt and 2-methylimidazole in a solvent, and reacting to obtain the ZIF-8 template.

[0040] In some embodiments, in S1, the zinc salt is selected from at least one of zinc nitrate, zinc acetate, and zinc chloride, preferably zinc nitrate.

[0041] In some embodiments, in S1, the molar ratio of 2-methylimidazole to zinc salt is 2:1 to 8:1, preferably 2:1 to 6:1, and more preferably 3:1 to 5:1.

[0042] In some embodiments, in S1, the solvent is selected from at least one of methanol, ethanol, N,N-dimethylformamide and deionized water, preferably methanol.

[0043] In some embodiments, in S1, the reaction temperature is 10°C to 60°C, and the reaction time is 0.5 hours to 24 hours; preferably, the temperature is 20°C to 50°C, and the time is 4 hours to 20 hours; more preferably, the temperature is 20°C to 30°C, and the time is 8 hours to 16 hours.

[0044] In some embodiments, in S1, the titanium precursor is selected from at least one of tetrabutyl titanate, titanium tetrachloride, titanium isopropoxide, and titanium tetraisopropoxy, preferably tetrabutyl titanate.

[0045] In some embodiments, in S1, the mass ratio of the ZIF-8 template to the titanium precursor is 1:0.5 to 1:6; preferably 1:1 to 1:6; more preferably 1:2 to 1:6.

[0046] In some embodiments, in S2, the programmed high-temperature pyrolysis temperature is 700℃~1000℃, the heating rate is 1℃ / min~10℃ / min, the holding time is 1 hour~5 hours, and the inert gas flow rate is 50 mL / min~500 mL / min. Preferably, the temperature is 800℃~1000℃, the heating rate is 3℃ / min~7℃ / min, the holding time is 1 hour~4 hours, and the inert gas flow rate is 50 mL / min~400 mL / min; more preferably, the temperature is 800℃~900℃, the heating rate is 4℃ / min~6℃ / min, the holding time is 1 hour~3 hours, and the inert gas flow rate is 50 mL / min~200 mL / min.

[0047] In this invention, the titanium-containing material first reacts to generate TiO2. The Ti in TiO2 is in a stable +4 valence state, and the Ti-O bond energy is high (about 672 kJ / mol). TiO2 needs to undergo a carbothermic reduction nitridation reaction (TiO2+C+N2→TiN+CO / CO2) to generate TiN. Compared with the existing technology that uses MXene and other raw materials for direct surface nitriding, theoretically, this invention requires higher energy to break the Ti-O bond and achieve nitriding. Furthermore, according to existing records, the carbothermic reduction nitridation of TiO2 usually requires temperatures above 1200 °C to be effective. However, in this invention, the effective carbothermic reduction nitridation reaction of TiO2 can be achieved at 700 °C to 1000 °C. This is because: (1) ZIF-8 can generate a strong carbothermic reduction atmosphere during high-temperature carbonization, which can effectively reduce high-valence Ti ions. At the same time, the ligand of ZIF-8 is dimethyl-imidazole, and nitrogen-containing gases (NH3, HCN, etc.) can be released during the pyrolysis carbonization of ZIF-8. Thus, the reduction and nitridation of titanium ions are carried out simultaneously, directly yielding TiN. (2) In this invention, the high-valence Ti ions are loaded in the form of nanoscale thin layers coated on the surface of ZIF-8. After pyrolysis, the high-valence Ti ions and the ZIF-8-derived carbon matrix form an atomic-level close contact. Mechanism studies of the carbothermic reduction reaction show that when the particles are in close contact with carbon atoms, the reaction mechanism changes from a gas-solid reaction dependent on CO / CO2 mass transfer to a solid-solid reaction between carbon and titanium oxide. The mass transfer path is shorter and the reaction efficiency is higher, which can significantly reduce the reaction start temperature.

[0048] Another embodiment of the present invention provides the application of the above-described C@TiN composite support in the cathode catalyst support of a proton exchange membrane fuel cell.

[0049] Specifically, a supported Pt-based catalyst includes the C@TiN composite support and a Pt-based active component supported on the C@TiN composite support; The Pt-based active component is Pt nanoparticles or Pt-based intermetallic compound nanoparticles, wherein the Pt-based intermetallic compound comprises an intermetallic compound formed by Pt and at least one metal element selected from Fe, Co, Ni, Cu, Zn, Mn, Cr, and V.

[0050] The C@TiN composite support prepared in this invention provides uniformly dispersed anchoring points for Pt-based active components. The Pt nanoparticles or Pt-based intermetallic compound nanoparticles loaded with it have small particle size and high dispersion. Furthermore, the TiN coating layer can effectively inhibit particle sintering of intermetallic compounds during high-temperature ordered heat treatment, which is beneficial to improving the utilization rate of Pt and reducing the platinum loading.

[0051] In some embodiments, the loading of the Pt-based active component in the supported Pt-based catalyst is 10 wt% to 60 wt%, preferably 20 wt% to 50 wt%.

[0052] In some embodiments, the average particle size of the Pt-based active component is 2 nm to 6 nm.

[0053] Another embodiment of the present invention provides a method for preparing a supported Pt-based catalyst, comprising the following steps: The C@TiN composite support, Pt precursor, and solvent are mixed, and the Pt-based active component in the Pt precursor is loaded onto the surface of the C@TiN composite support through a reduction reaction to obtain the supported Pt-based catalyst.

[0054] This invention uses a C@TiN composite support as a carrier, and loads Pt-based active components onto the C@TiN composite support through a reduction reaction. The preparation method is simple, efficient, and easy to scale up.

[0055] In some embodiments, when the Pt-based active component is a Pt-based intermetallic compound, the method further includes a step of subjecting the C@TiN composite support loaded with Pt and non-Pt metal precursors to high-temperature ordered heat treatment under a reducing atmosphere; the non-Pt metal is selected from at least one of Fe, Co, Ni, Cu, Zn, Mn, Cr, and V, and the specific preparation method is as follows: The C@TiN composite support, Pt precursor and solvent are mixed, and the Pt-based active component in the Pt precursor is loaded onto the surface of the C@TiN composite support by a reduction reaction to obtain the initial Pt-based catalyst. The initial Pt-based catalyst, metal salt, and solvent were mixed, rotary evaporated, and dried. The dried sample was placed in a 4%~6% H2 / Ar atmosphere and heated to 650~700℃ at a heating rate of 3℃ / min~7℃ / min and held for 1.5 hours~2 hours to obtain the supported Pt-based catalyst. The metal salt includes a salt of at least one metal selected from Fe, Co, Ni, Cu, Zn, Mn, Cr, and V.

[0056] In some embodiments, the Pt precursor is selected from at least one of chloroplatinic acid, potassium chloroplatinate, platinum acetylacetonate, and platinum nitrate.

[0057] In some embodiments, the reduction reaction is performed using a liquid-phase reduction method, an ethylene glycol reduction method, or an impregnation reduction method.

[0058] In some embodiments, the reduction reaction method includes: reflux reduction in an oil bath at 120°C to 140°C for 2 to 4 hours.

[0059] Another embodiment of the present invention provides the application of the above-mentioned supported Pt-based catalyst in the catalyst layer of a fuel cell or in the membrane electrode of a proton exchange membrane fuel cell.

[0060] Specifically, a fuel cell catalyst layer includes an ionomer and the supported Pt-based catalyst, wherein the ionomer is uniformly distributed on the surface of a C@TiN composite support.

[0061] A proton exchange membrane fuel cell membrane electrode assembly includes the aforementioned fuel cell catalyst layer.

[0062] This invention utilizes the intrinsic surface chemical properties of the C@TiN composite support to guide the orderly adsorption and uniform distribution of ionomers on the support surface, which is beneficial for constructing a continuous and efficient proton conduction network, optimizing the three-phase reaction interface, and thus improving the mass transfer efficiency and output performance of the membrane electrode.

[0063] The present invention will be further described in detail below with reference to specific embodiments, but the present invention is not limited to the following specific embodiments.

[0064] Raw materials: All chemical reagents used in the following examples are commercially available analytical grade, including zinc nitrate hexahydrate (Zn(NO3)2·6H2O, ≥99.9%), 2-methylimidazole (C4H6N2, ≥99%), and tetrabutyl titanate (C 16 H 36 O4Ti (≥99%) was purchased from Aladdin Reagent Co., Ltd.; chloroplatinic acid (H2PtCl6·6H2O, Pt content ≥37.5%) was purchased from Sinopharm Chemical Reagent Co., Ltd.; ferric chloride (FeCl3·6H2O, ≥99%) was purchased from Xilong Scientific Co., Ltd.; Nafion solution (5 wt%) was purchased from DuPont; commercial Pt / C catalyst (40 wt% Pt) was purchased from Johnson Matthey. The gas diffusion layer (SGL 39BB) was purchased from SGL Carbon; the Nafion® NR211 membrane was purchased from DuPont. All solvents (methanol, ethanol, ethylene glycol, etc.) were commercially available analytical grade reagents and used directly without further purification. The resistivity of deionized water used in the experiment was 18.2 MΩ·cm.

[0065] Part 1: Materials Level (Three-Electrode Testing) Examples and Comparative Cases Example 1 In this embodiment, a C@TiN composite support (TiN coating amount 10 wt%) was prepared and used to load Pt nanoparticles. The specific preparation steps are as follows: (1) Preparation of ZIF-8 template: 2.5 mmol zinc nitrate hexahydrate and 10 mmol 2-methylimidazole were dissolved in 50 mL methanol respectively. The latter was quickly poured into the former and the mixture was stirred at room temperature for 12 hours. The product was centrifuged, washed three times with methanol, and dried under vacuum at 60 °C for 12 hours to obtain ZIF-8 template with a particle size of about 150 nm.

[0066] (2) Titanium source loading: 1 g of ZIF-8 template obtained in step (1) was dispersed in 50 mL of ethanol, 0.2 mL of tetrabutyl titanate was added, and the mixture was stirred and adsorbed for 6 hours. The product was dried in an oven to obtain ZIF-8@titanium source composite.

[0067] (3) Programmed high-temperature pyrolysis: The ZIF-8@titanium source composite obtained in step (2) was placed in a tube furnace and heated to 800 ℃ at a heating rate of 5 ℃ / min under an argon atmosphere (gas flow rate 100 mL / min). The temperature was held for 2 hours and then naturally cooled to room temperature to obtain C@TiN composite support (TiN coating amount 10 wt%). Elemental scanning was used to determine the adsorption and distribution regulation of the ionomer on the support.

[0068] (4) Pt nanoparticle loading: 50 mg of the C@TiN composite support obtained in step (3) was dispersed in 50 mL of ethylene glycol, 88 mg of chloroplatinic acid (Pt loading was 30 wt%) was added, the pH was adjusted to 10 with NaOH, and the mixture was refluxed in an oil bath at 130 °C for 3 hours. The product was centrifuged, washed three times with deionized water, and dried under vacuum at 60 °C to obtain the Pt / C@TiN catalyst. The average particle size of the Pt nanoparticles was 3.5 nm.

[0069] (5) Preparation of working electrode and electrochemical performance test: 2 mg of the catalyst obtained in step (4) was dispersed in 1 mL of Nafion / ethanol solution (Nafion content 0.05 wt%), ultrasonically dispersed for 30 min, and 5 μL was dropped onto the surface of the rotating disk electrode and dried at room temperature. In 0.1 M HClO4 electrolyte, with Ag / AgCl electrode as reference electrode and platinum wire as counter electrode, cyclic voltammetry was performed in N2 saturated electrolyte at a scan rate of 10 mV / s, and linear scan voltammetry was performed in O2 saturated electrolyte at a scan rate of 10 mV / s and a rotation speed of 1600 rpm. The electrochemical active area (ECSA) and mass activity (MA) were calculated respectively. Accelerated durability testing (ADT) was performed in an O2-saturated 0.1 M HClO4 solution, with 5000 cyclic voltammetric scans in the potential range of 0.6 V to 1.0 V at a scan rate of 100 mV / s. Changes in electrochemical active area and mass activity before and after ADT were recorded.

[0070] Example 2 In this embodiment, a C@TiN composite support (TiN coating amount 20 wt%) was prepared and used to load Pt nanoparticles. The specific preparation steps are as follows: (1) Preparation of ZIF-8 template: Same as step (1) in Example 1.

[0071] (2) Titanium source loading: 1 g of ZIF-8 template obtained in step (1) was dispersed in 50 mL of ethanol, and 0.4 mL of tetrabutyl titanate was added. The mixture was hydrolyzed and deposited at 40 °C for 8 hours. The product was centrifuged, washed and dried to obtain ZIF-8@titanium source composite.

[0072] (3) Programmed high-temperature pyrolysis: Same as step (3) in Example 1, to obtain C@TiN composite carrier (TiN coating amount 20wt%).

[0073] (4) Pt nanoparticle loading: Same as step (4) in Example 1, to obtain Pt / C@TiN catalyst. The average particle size of Pt nanoparticles is 3.8 nm.

[0074] (5) Preparation of working electrode and electrochemical performance test: Same as step (5) in Example 1.

[0075] Example 3 In this embodiment, a C@TiN composite support (TiN coating amount 30 wt%) was prepared and used to load Pt nanoparticles. The specific preparation steps are as follows: (1) Preparation of ZIF-8 template: Same as step (1) in Example 1.

[0076] (2) Titanium source loading: 1 g of ZIF-8 template obtained in step (1) was dispersed in 50 mL of ethanol, and 0.6 mL of tetrabutyl titanate was added. The mixture was subjected to hydrolysis deposition reaction at 40 °C for 12 hours. The product was centrifuged, washed and dried to obtain ZIF-8@titanium source composite.

[0077] (3) Programmed high-temperature pyrolysis: Same as step (3) in Example 1, to obtain C@TiN composite carrier (TiN coating amount 30wt%).

[0078] (4) Pt nanoparticle loading: Same as step (4) in Example 1, to obtain Pt / C@TiN catalyst. The average particle size of Pt nanoparticles is 4.0 nm.

[0079] (5) Preparation of working electrode and electrochemical performance test: Same as step (5) in Example 1.

[0080] Example 4 In this embodiment, a C@TiN composite support (pyrolysis temperature 700 ℃) was prepared and used to load Pt nanoparticles. The specific preparation steps are as follows: (1) Preparation of ZIF-8 template: Same as step (1) in Example 1.

[0081] (2) Titanium source loading: Same as step (2) in Example 2.

[0082] (3) Programmed high-temperature pyrolysis: The ZIF-8@titanium source composite obtained in step (2) was placed in a tube furnace and heated to 700 ℃ at a heating rate of 5 ℃ / min under an argon atmosphere (gas flow rate 100 mL / min). The temperature was held for 2 hours and then naturally cooled to room temperature to obtain the C@TiN composite support.

[0083] (4) Pt nanoparticle loading: Same as step (4) in Example 1, to obtain Pt / C@TiN catalyst.

[0084] (5) Preparation of working electrode and electrochemical performance test: Same as step (5) in Example 1.

[0085] Example 5 In this embodiment, a C@TiN composite support (pyrolysis temperature 900℃) was prepared and Pt nanoparticles were loaded onto it. The specific preparation steps are as follows: (1) Preparation of ZIF-8 template: Same as step (1) in Example 1.

[0086] (2) Titanium source loading: Same as step (2) in Example 2.

[0087] (3) Programmed high-temperature pyrolysis: The ZIF-8@titanium source composite obtained in step (2) was placed in a tube furnace and heated to 900 ℃ at a heating rate of 5 ℃ / min under an argon atmosphere (gas flow rate 100 mL / min). The temperature was held for 2 hours and then naturally cooled to room temperature to obtain the C@TiN composite support.

[0088] (4) Pt nanoparticle loading: Same as step (4) in Example 1, to obtain Pt / C@TiN catalyst.

[0089] (5) Preparation of working electrode and electrochemical performance test: Same as step (5) in Example 1.

[0090] Example 6 This embodiment prepared a C@TiN composite support and loaded PtCo intermetallic compound nanoparticles onto it. The specific preparation steps are as follows: (1) Preparation of ZIF-8 template: Same as step (1) in Example 1.

[0091] (2) Titanium source loading: Same as step (2) in Example 2.

[0092] (3) Programmed high-temperature pyrolysis: Same as step (3) in Example 1, to obtain C@TiN composite carrier.

[0093] (4) PtCo intermetallic compound loading: Following step (4) of Example 1, a Pt / C@TiN catalyst was obtained. 100 mg of Pt / C@TiN was dispersed in 50 mL of ethanol, and 30 mg of cobalt chloride (Pt to Co molar ratio of 1:1) was added. The mixture was stirred for 12 hours, rotary evaporated, and vacuum dried at 60 °C. The dried sample was placed in a tube furnace and heated to 700 °C at a heating rate of 5 °C / min under a 5% H2 / Ar atmosphere for 2 hours to perform high-temperature ordering heat treatment, thus obtaining the PtCo / C@TiN catalyst. The average particle size of the PtCo intermetallic compound nanoparticles was 5 nm, the Pt loading was 27 wt%, and the Co loading was 7.5 wt%.

[0094] (5) Preparation of working electrode and electrochemical performance test: Same as step (5) in Example 1.

[0095] Comparative Example 1 In this comparative example, a pure carbon support (C support) without TiN coating was prepared and Pt nanoparticles were loaded onto it. The specific preparation steps are as follows: (1) Preparation of ZIF-8 template: Same as step (1) in Example 1.

[0096] (2) Programmed pyrolysis: The ZIF-8 template obtained in step (1) is placed in a tube furnace and heated to 800°C at a heating rate of 5°C / min under an argon atmosphere. It is held for 2 hours and then naturally cooled to room temperature to obtain a pure carbon support (C support).

[0097] (3) Pt nanoparticle loading: Same as step (4) in Example 1, to obtain the Pt / C catalyst. The average particle size of the Pt nanoparticles is 4.5 nm.

[0098] (4) Preparation of working electrode and electrochemical performance test: Same as step (5) in Example 1.

[0099] Comparative Example 2 This comparative example prepared a pure TiN support (carbon-free matrix) and loaded Pt nanoparticles onto it. The specific preparation steps are as follows: (1) Preparation of TiO2 nanoparticles: 2 mL of tetrabutyl titanate was slowly added dropwise to 50 mL of deionized water and stirred for 4 hours for hydrolysis. The product was centrifuged, washed and dried to obtain TiO2 nanoparticles.

[0100] (2) Programmed high-temperature pyrolysis: The titanium source nanoparticles obtained in step (1) are placed in a tube furnace and heated to 800 °C at a heating rate of 5 °C / min under an ammonia atmosphere. The temperature is held for 2 hours and then naturally cooled to room temperature to obtain pure TiN support.

[0101] (3) Pt nanoparticle loading: Same as step (4) in Example 1, to obtain Pt / TiN catalyst. The average particle size of Pt nanoparticles is 5.2 nm.

[0102] (4) Preparation of working electrode and electrochemical performance test: Same as step (5) in Example 1.

[0103] Comparative Example 3 In this comparative example, a commercial Pt / C catalyst (Johnson Matthey, 40 wt% Pt) was used as the reference sample. The preparation of the working electrode and the electrochemical performance test were the same as in step (5) of Example 1.

[0104] Examples 1 to 6 and Comparative Examples 1 to 3 were characterized and tested: I. Characterization: 1. Figure 1 The image shows a SEM image of ZIF-8 prepared in Example 1. As can be seen from the image, ZIF-8 is a carbon precursor with single particles dispersed in size between 100 nm and 200 nm.

[0105] 2. Figure 2 The XRD pattern of the C@TiN composite support prepared in Example 1 is shown below. Figure 3 The image shows a SEM image of the C@TiN composite carrier prepared in Example 1. Figures 2-3 It can be concluded that ZIF-8 can achieve the preparation of TiN during the pyrolysis and carbonization process, while maintaining the monodisperse state of ZIF-8 particles to facilitate the subsequent dispersion of the support and the loading of the catalyst particles.

[0106] 3. Figure 4 The image shows the TEM and elemental distribution of the C@TiN composite support prepared in Example 1. As can be seen from the image, the TiN phase is uniformly dispersed on the surface of the carbon support.

[0107] 4. Figure 5 The image shows the EDS surface distribution of Nafion ionomers on the C@TiN composite support prepared in Example 1. As can be seen from the image, F element (the marker element of Nafion ionomers) is uniformly distributed on the surface of the support, indicating that the support uniformly adsorbs the ionomers, which is beneficial for the construction of proton transport networks.

[0108] 5. Figure 6 The image shows a TEM image and an EDS surface distribution diagram of Pt element prepared in Example 1. As can be seen from the image, Pt particles are uniformly grown on the surface of C@TiN composite support.

[0109] 6. Figure 7The image shows a TEM image of the PtCo / C@TiN catalyst prepared in Example 6 and an EDS surface distribution diagram of Pt, Co, Ti, N, and C elements. As can be seen from the image, the PtCo alloy was successfully prepared on the surface of this support.

[0110] II. Test The electrochemical performance test results of the catalysts prepared in Examples 1 to 6 and Comparative Examples 1 to 3 are shown in Table 1.

[0111] Table 1. Comparison of catalyst performance between Examples 1-6 and Comparative Examples 1-3 After undergoing a durability test of 30,000 accelerated cycles at 0.6 V to 1.0 V, the ECSA retention rate of the catalysts in Examples 1 to 6 reached 80% to 95%, which is much higher than that of Pt / C in Comparative Example 1 (59%), Pt / TiN in Comparative Example 2 (65%), and commercial Pt / C in Comparative Example 3 (57%). This indicates that the supported catalyst prepared in this invention has significant advantages in terms of overall structural stability, and that the strong metal-support interaction (SMSI) between TiN and Pt enhances the anchoring of Pt particles by the support, inhibits the dissolution and agglomeration of Pt, thereby significantly improving the structural stability of the catalyst particles.

[0112] Part Two: Device Level (Membrane Electrode) Examples and Comparative Examples Based on the RDE tests conducted in Examples 1 to 6 above, the Pt / C@TiN catalyst prepared in Example 1 (with a TiN loading of approximately 10 wt% and a pyrolysis temperature of 800 °C) is the optimal formulation. To further verify the performance of this catalyst under real fuel cell operating conditions, Example 7 below describes its application to the membrane electrode assembly and single-cell testing.

[0113] Example 7 In this embodiment, the Pt / C@TiN catalyst prepared in Example 1 is used for the fabrication of the membrane electrode and single-cell testing to evaluate its performance under real fuel cell operating conditions. The specific preparation and testing steps are as follows: (1) Membrane electrode preparation: The Pt / C@TiN catalyst prepared in Example 1 was mixed with Nafion ionomer (5 wt% solution) at a ionomer / carbon (I / C) mass ratio of 0.8:1. Propanol and water (mass ratio of 1:1) were added, and the mixture was ultrasonically dispersed to prepare a catalyst slurry. The slurry was uniformly coated onto the gas diffusion layer (SGL 39BB) using ultrasonic spraying, and the cathode Pt loading was controlled to be 0.3 mgPt / cm. 2 The anode uses a commercial Pt / C catalyst (Johnson Matthey, 40 wt%). Pt Pt loading: 0.1 mg Pt / cm³2 The heat-pressed transfer was applied to a Nafion NR211 film to prepare an effective area of ​​4 cm². 2 The membrane electrode.

[0114] (2) Single-cell test: The membrane electrode assembly was placed in a single-cell test fixture and tested under the conditions of a cell temperature of 80 ℃, anode relative humidity of 100%, cathode relative humidity of 100%, and back pressure of 150 kPa. H2 was introduced into the anode (flow rate of 200 sccm), and air was introduced into the cathode (flow rate of 500 sccm). The polarization curve and power density curve were recorded.

[0115] (3) Accelerated Durability Test (ADT): Perform 30,000 cycles of triangular wave scanning within the potential range of 0.6 V to 1.0 V at a scanning rate of 100 mV / s. After ADT, test the polarization curve again and record the performance degradation.

[0116] (4) Membrane electrode disassembly and ionomer distribution characterization: After the ADT test, the membrane electrode was disassembled, and the cathode catalyst layer sample was taken for ionomer distribution characterization. Scanning electron microscopy combined with energy dispersive spectroscopy (SEM-EDS) was used to analyze the surface distribution of F element (F is the characteristic element of sulfonate in ionomers) on the cross-section of the catalyst layer to evaluate the spatial uniformity of ionomer distribution in the catalyst layer. At the same time, transmission electron microscopy combined with energy dispersive spectroscopy (TEM-EDS) was used to observe the coverage state and distribution characteristics of ionomers on the catalyst support surface.

[0117] Example 8 In this embodiment, the PtCo / C@TiN catalyst prepared in Example 6 is used for the fabrication of a membrane electrode and single-cell testing to verify the membrane electrode performance of the C@TiN composite support of the present invention when loaded with Pt-based intermetallic compounds. The specific preparation and testing steps are as follows: (1) Membrane electrode preparation: The PtCo / C@TiN catalyst prepared in Example 6 was mixed with Nafion ionomer (5 wt% solution) at a ionomer / carbon (I / C) mass ratio of 0.8:1. Propanol and water (mass ratio of 1:1) were added, and the mixture was ultrasonically dispersed to prepare a catalyst slurry. The slurry was uniformly coated onto the gas diffusion layer (SGL 39BB) using ultrasonic spraying, and the cathode Pt loading was controlled to be 0.1 mgPt / cm³. 2 (Based on Pt mass), the anode uses a commercial Pt / C catalyst (Johnson Matthey, 40 wt%). Pt Pt loading 0.1 mg Pt / cm 2 The heat-pressed transfer was applied to a Nafion® NR211 film to prepare an effective area of ​​4 cm². 2 The membrane electrode.

[0118] Subsequent single-cell testing, accelerated durability testing, and membrane electrode disassembly and ionomer distribution characterization: same as steps (2) to (4) in Example 7.

[0119] Comparative Example 4 This comparative example uses a commercial Pt / C catalyst (Johnson Matthey, 40 wt%). Pt Assemble the membrane electrode and compare it with Example 7. The specific preparation and testing steps are as follows: (1) Preparation of membrane electrode: A commercial Pt / C catalyst and Nafion ionomer (5 wt% solution) were mixed at an I / C mass ratio of 0.8:1, and isopropanol and water (mass ratio of 1:1) were added. The mixture was then ultrasonically dispersed to prepare a catalyst slurry. The same coating and transfer process as in Example 7 was used to control the Pt loading at the cathode to be 0.3 mg. Pt / cm 2 The anode was prepared using a commercial Pt / C catalyst (Pt loading 0.1 mgPt / cm²), which was hot-pressed onto a Nafion® NR211 membrane to create an effective area of ​​4 cm². 2 The membrane electrode.

[0120] (2) Single cell test: The test conditions are the same as step (2) in Example 7. Record the polarization curve and power density curve.

[0121] (3) Accelerated durability test (ADT): The test conditions are the same as step (3) in Example 7.

[0122] (4) Membrane electrode disassembly and ionomer distribution characterization: Same as step (4) in Example 7.

[0123] Characterization and testing: I. Characterization Figure 8 The graph shows the polarization performance and durability of the PtCo / C@TiN PEMFC battery in Example 8. As can be seen from the graph, the obtained catalyst possesses excellent activity (Pt mass activity 0.71 A / mg). Pt ) and stability (800 mA / cm 2 The current decayed by only 11 mV after aging cycles.

[0124] II. Test Table 2 shows the comparison results of the membrane electrode performance of Examples 7-8 and Comparative Example 4.

[0125] Table 2 Comparison of membrane electrode performance between Examples 7-8 and Comparative Example 4 As shown in Table 2, the current density (900 mA / cm²) of the Pt / C@TiN catalyst film electrode prepared in Example 7 of this invention at 0.7 V is... 2 The efficiency was significantly higher than that of the commercial Pt / C film electrode in Comparative Example 4 (800 mA / cm). 2 Furthermore, after accelerated durability testing, the current density decay of Example 7 (10%) was significantly lower than that of Comparative Example 4 (16%).

[0126] Furthermore, the current density (1200 mA / cm²) of the PtCo / C@TiN catalyst film electrode prepared in Example 8 at 0.7 V was... 2 The degradation rate (current density decay) after ADT is better than that of the Pt / C@TiN catalyst in Example 7. This is consistent with the activity advantage of the alloy catalyst in RDE test (Examples 6 and Example 1), and also verifies the membrane electrode performance of the C@TiN composite support of the present invention when loaded with Pt-based intermetallic compounds.

[0127] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. A supported Pt-based catalyst, characterized in that, The supported Pt-based catalyst includes a C@TiN composite support and a Pt-based active component supported on the C@TiN composite support; The C@TiN composite support comprises a carbon matrix and a TiN coating layer covering the surface of the carbon matrix; in the C@TiN composite support, the thickness of the TiN coating layer is 5 nm to 50 nm, and the TiN loading is 5 wt% to 50 wt%; the carbon matrix is ​​a carbon matrix formed by pyrolysis and carbonization of ZIF-8, and the particle size of the ZIF-8 is 50 nm to 500 nm; The Pt-based active component is Pt nanoparticles or Pt-based intermetallic compound nanoparticles, wherein the Pt-based intermetallic compound comprises an intermetallic compound formed by Pt and at least one metal element selected from Fe, Co, Ni, Cu, Zn, Mn, Cr, and V.

2. The supported Pt-based catalyst according to claim 1, characterized in that, The preparation method of the C@TiN composite support includes the following steps: S1. The ZIF-8 template and titanium precursor are mixed in a solvent and reacted to obtain the ZIF-8@titanium source composite. S2. The ZIF-8@titanium source composite is subjected to programmed high-temperature pyrolysis under an inert gas atmosphere to obtain the C@TiN composite support.

3. The supported Pt-based catalyst according to claim 2, characterized in that, In S1, the method for preparing the ZIF-8 template includes: mixing zinc salt and 2-methylimidazole in a solvent, and reacting to obtain the ZIF-8 template; wherein the zinc salt is selected from at least one of zinc nitrate, zinc acetate, and zinc chloride; the molar ratio of 2-methylimidazole to zinc salt is 2:1 to 8:1; the solvent is selected from at least one of methanol, ethanol, N,N-dimethylformamide, and deionized water; the reaction temperature is 10℃ to 60℃, and the reaction time is 0.5 hours to 24 hours.

4. The supported Pt-based catalyst according to claim 2, characterized in that, In S1, the titanium precursor is selected from at least one of tetrabutyl titanate, titanium tetrachloride, titanium isopropoxide, and titanium tetraisopropoxy; the mass ratio of the ZIF-8 template to the titanium precursor is 1:0.5 to 1:

6.

5. The supported Pt-based catalyst according to claim 2, characterized in that, In S2, the temperature of the programmed high-temperature pyrolysis is 700℃~1000℃, the heating rate is 1℃ / min~10℃ / min, the holding time is 1 hour~5 hours, and the flow rate of the inert gas is 50 mL / min~500 mL / min.

6. The supported Pt-based catalyst according to claim 1, characterized in that, In the supported Pt-based catalyst, the loading of the Pt-based active component is 10 wt% to 60 wt%, and the average particle size of the Pt-based active component is 2 nm to 6 nm.

7. The method for preparing the supported Pt-based catalyst according to any one of claims 1 to 6, characterized in that, Includes the following steps: The C@TiN composite support, Pt precursor, and solvent are mixed, and the Pt-based active component in the Pt precursor is loaded onto the surface of the C@TiN composite support through a reduction reaction to obtain the supported Pt-based catalyst.

8. The preparation method according to claim 7, characterized in that, When the Pt-based active component is a Pt-based intermetallic compound, the preparation method includes the following specific steps: The C@TiN composite support, Pt precursor and solvent are mixed, and the Pt-based active component in the Pt precursor is loaded onto the surface of the C@TiN composite support by a reduction reaction to obtain the initial Pt-based catalyst. The initial Pt-based catalyst, metal salt, and solvent were mixed, rotary evaporated, and dried. The dried sample was placed in a 4%~6% H2 / Ar atmosphere and heated to 650~700℃ at a heating rate of 3℃ / min~7℃ / min and held for 1.5 hours~2 hours to obtain the supported Pt-based catalyst. The metal salt includes a salt of at least one metal selected from Fe, Co, Ni, Cu, Zn, Mn, Cr, and V; The Pt precursor is selected from at least one of chloroplatinic acid, potassium chloroplatinate, and platinum acetylacetonate; The reduction reaction is carried out by liquid-phase reduction, ethylene glycol reduction, or impregnation reduction.

9. A catalyst layer for a fuel cell, characterized in that, The catalyst includes an ionomer and the supported Pt-based catalyst according to any one of claims 1 to 6, wherein the ionomer is uniformly distributed on the surface of the C@TiN composite support.

10. A membrane electrode assembly for a proton exchange membrane fuel cell, characterized in that, Includes the fuel cell catalyst layer as described in claim 9.