A halide oxide solid electrolyte, its preparation method and application

The preparation of zirconium-based halide oxide solid electrolytes with doped elements by a one-step ball milling method solves the problems of low ionic conductivity and poor air stability of halide electrolytes, enabling the application of all-solid-state batteries with high energy density and long cycle life, which are suitable for new energy vehicles, aerospace and other fields.

CN123120844APending Publication Date: 2026-11-17ZHEJIANG UNIV +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611330134.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing halide solid electrolytes suffer from low ionic conductivity, poor air stability, and high cost, which affect the rate performance and energy utilization of lithium-ion batteries.

Method used

Zirconium-based halide oxide solid electrolytes are prepared by a one-step ball milling method. By doping with inexpensive and abundant elements such as Tb, Y, Gd, Ce, La, Ta, W or Er, a stable halide oxide system is formed. Combining forward and reverse ball milling techniques simplifies the preparation process and reduces costs.

Benefits of technology

The ionic conductivity of halide oxide solid electrolytes has been improved, and air and chemical stability have been enhanced, resulting in high energy density and long cycle life of all-solid-state batteries, which are suitable for new energy vehicles, aerospace and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120844A_ABST
    Figure CN123120844A_ABST
Patent Text Reader

Abstract

This invention discloses a halogen oxide solid electrolyte, wherein the halogen oxide solid electrolyte is Li a Zr 1‑x‑y M x N y Cl b O c The present invention discloses a method for preparing the above-mentioned halide oxide solid electrolyte: under oxygen-free and anhydrous conditions, lithium chloride, lithium oxide, zirconium chloride, and metal or non-metal chlorides are prepared by one-step ball milling in a sealed ball mill jar, wherein the metal or non-metal in the metal or non-metal chloride is independently selected from M or N. The present invention also discloses the application of the above-mentioned halide oxide solid electrolyte in lithium-ion all-solid-state batteries. The present invention improves electronic conductivity while reducing cost, and can be prepared by one-step ball milling. When applied to lithium-ion all-solid-state batteries, it can achieve excellent rate performance and long cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium-ion battery materials, and specifically relates to a halide oxide solid electrolyte, its preparation method, and its application. Background Technology

[0002] With the rapid development of energy storage materials, lithium-ion batteries are widely used in new energy vehicles, aerospace, energy storage systems, and other fields. However, traditional liquid lithium-ion batteries suffer from safety hazards such as flammability, leakage, and high risk of thermal runaway, and their energy density has reached its theoretical limit. These problems seriously hinder the development of the energy storage battery industry. All-solid-state batteries, with their safety, high energy density, and long cycle life, have become excellent candidates for the next generation of energy storage batteries. The evolution of batteries from liquid to solid state is an inevitable trend in the technological iteration of lithium-ion batteries, and solid electrolytes are key to breakthroughs in solid-state battery technology.

[0003] Currently, the mainstream solid electrolytes in the research field include polymers, oxides, halides, and sulfides. Among them, polymer electrolytes are flexible and easy to process, making them the easiest to mass-produce, but they suffer from low ionic conductivity. Oxide electrolytes have excellent thermal and oxidative stability, but their rigid structure makes them difficult to process, limiting their industrialization. Sulfides currently have the highest ionic conductivity among electrolytes (e.g., Li6PS5Cl > 10 × 10⁻⁶). -3 While halogenated electrolytes have a wide electrochemical window, deformability, and low cost, they exhibit poor chemical stability during application, easily releasing toxic H2S gas, severely polluting the air, and posing a safety risk. Halogenated electrolytes, on the other hand, possess advantages such as a wide electrochemical window, deformability, and low cost, showing promising development prospects. However, halide electrolytes are extremely sensitive to moisture, especially chloride and bromine salt systems, which readily deliquesce in air, releasing hydrogen halide gas and causing electrolyte failure. Furthermore, halide ions have low conductivity (e.g., Li2ZrCl6 approximately 5 × 10⁻⁶ at room temperature). -4 The ratio of S / cm affects the rate performance and energy utilization of the battery.

[0004] To address the issues of low ionic conductivity and poor air stability in halide solid electrolytes, Zhaozhe Yu's group (Journal of Energy Storage 89 (2024) 111700) modified traditional Li₂ZrCl₆ using oxygen ion substitution and lithium enrichment strategies. This optimized the crystal structure of the electrolyte material, forming a stable halide oxide system and thus improving ionic conductivity. The halide oxides, through the introduction of oxygen ions, cause local structural distortion, disrupting the long-range order of pure halides and inducing the formation of amorphous structures, thereby broadening the lithium-ion transport channels. Furthermore, Chinese patent CN121601756A discloses a halide oxide solid electrolyte, its preparation method, and its applications. Using fluorocarbon calcium neodymium ore as raw material, a two-step method is employed to extract rare earth oxides from neodymium ore and synthesize a halide oxide solid electrolyte with a low degree of crystallinity through high-energy ball milling. Its general chemical formula is: [Li (6ac3b) M a Nd b ]6+[O y X (62y) ]6, wherein: M is at least one element selected from Ti, Zr, Hf, V, Nb, and Ta; and X is at least one element selected from F, Cl, Br, and I.

[0005] However, these electrolytes still have problems and technical bottlenecks, such as insufficient ionic conductivity, high cost, and large solid-solid interface contact resistance.

[0006] In summary, given the technical limitations and scientific challenges faced by solid-state electrolytes, it is of paramount importance to develop a halide oxide solid-state electrolyte that combines high ionic conductivity, a wide electrochemical window, and a simple preparation process, and to apply it to all-solid-state batteries to achieve high energy density and long cycle life. Summary of the Invention

[0007] The purpose of this invention is to provide a halide oxide solid electrolyte, its preparation method and application; it can improve electronic conductivity while reducing cost, and can be prepared by a one-step ball milling method. When applied to lithium-ion all-solid-state batteries, it can achieve excellent rate performance and long cycle performance.

[0008] To achieve the above-mentioned objectives, the present invention is implemented through the following technical solution: A first aspect of the present invention provides a halide oxide solid electrolyte, wherein the halide oxide solid electrolyte is Li a Zr 1-x-y M x N y Cl b O cWhere M and N are at least one of the elements Tb, Y, Gd, Ce, La, Ta, W, or Er, and M and N can be the same element or different elements; the values ​​of a, b, and c are in the range of: 2≤a≤3.5, 4.5≤b<6, 0<c≤1.5, and the values ​​of x and y are in the range of: 0<x+y<1. Within this range, the ionic conductivity, air stability, and chemical stability of the halide oxide solid electrolyte reach their optimal values.

[0009] Optionally, the chemical valence states of M and N are between +3 and +5.

[0010] The halide oxide solid electrolyte is Li 3.5 Zr 0.9 Gd 0.1 Cl 4.6 O 1.4 Li 3.45 Zr 0.95 Gd 0.05 Cl 4.6 O 1.4 Li 2.8 Zr 0.9 Gd 0.1 Cl 5.2 O 0.75 Li 2.8 Zr 0.9 Gd 0.1 Cl 5.1 O 0.8 Li 3.4 Zr 0.8 W 0.1 Gd 0.1 Cl 4.6 O 1.4 Li 3.4 Zr 0.8 W 0.1 Y 0.1 Cl 4.6 O 1.4 Or Li 2.8 Zr 0.8 W 0.1 Gd 0.1 Cl 5.2 O 0.8 .

[0011] A second aspect of the present invention provides a method for preparing the above-mentioned halide oxide solid electrolyte, comprising: directly preparing lithium chloride, lithium oxide, zirconium chloride, and metal or non-metal chlorides by one-step ball milling in a sealed ball mill jar under oxygen-free and anhydrous conditions (water content ≤ 0.01 ppm, oxygen content ≤ 0.01 ppm), wherein the metal or non-metal in the metal or non-metal chloride is independently selected from M or N.

[0012] Unlike other methods for preparing halide oxides, the oxygen element in the halide oxides prepared by the present invention is entirely derived from Li2O (99.99%).

[0013] The one-step ball milling method includes: a ball milling speed of 400~600 r / min, a ball milling method of clockwise ball milling for 10~30 minutes, stopping ball milling for 5~15 minutes, and counterclockwise ball milling for 10~30 minutes; the total ball milling time is 10~50 hours, which reduces the impact of side reactions caused by overheating on the electrolyte.

[0014] Preferably, the one-step ball milling method includes: a ball milling speed of 500~580 r / min, a ball milling method of clockwise milling for 15~25 minutes, stopping the ball milling for 5~10 minutes, and then ball milling counterclockwise for 15~25 minutes; the total ball milling time is 24~28 hours. This process condition can further reduce the impact of side reactions caused by overheating on the electrolyte.

[0015] The grinding balls used in the one-step ball milling method are made of ZrO2 material, with a size of 5-15 mm and a ball-to-material ratio of 80:1-150:1. Preferably, the ZrO2 grinding balls have diameters of 10 mm, 8 mm, and 5 mm, with a ratio of large, medium, and small grinding balls of 2:3:5 and a ball-to-material ratio of 100:1, 120:1, and 125:1.

[0016] Unlike other methods for preparing halide oxides, this invention uses a one-step ball milling method, without changing the ball milling speed and ball-to-material ratio midway. By combining forward and reverse rotation, it saves energy and time, and is simple to operate. Furthermore, it eliminates the need for solid-state high-temperature sintering to modify the halide oxide solid electrolyte, significantly reducing the operational difficulty of the preparation process.

[0017] This invention reduces the application cost of halide oxide solid electrolytes by doping with inexpensive and abundant elements, and can be prepared by a one-step ball milling method, saving ball milling time.

[0018] The method for measuring the ionic conductivity of halide oxide solid electrolytes under different conditions provided by this invention is as follows: The powder obtained from ball milling is placed in an electrolyte mold and cold-pressed using a tablet press to obtain electrolyte tablets. This operation is performed in a glove box free of water and oxygen (water content ≤ 0.01 ppm, oxygen content ≤ 0.01 ppm). After cold pressing, the mold is placed in an electrochemical workstation, and the EIS test temperature is between 15 ℃ and 85 ℃. High temperatures intensify lattice vibrations, expand ion migration channels, thereby reducing the migration barrier. Simultaneously, thermal excitation of numerous intrinsic defects affects the magnitude of ionic conductivity.

[0019] Optionally, the mass of the cold-pressed powder is between 100 and 300 mg, and more preferably 150 mg.

[0020] Optionally, the cold pressing pressure of the tablet press is between 100 and 800 MPa, and more preferably 625 MPa. After cold pressing, the thickness of the electrolyte tablet is between 0.5 and 2.0 mm.

[0021] Optionally, the tablet press holding time is between 3 and 6 minutes, and more preferably 5 minutes.

[0022] Optionally, single-sided carbon-coated aluminum foil, double-sided carbon-coated aluminum foil, indium foil, or other separator materials can be placed at both ends of the electrolyte sheet. The carbon-coated aluminum foil is used as a blocking electrode, which can improve the solid-solid contact between the electrode and the electrolyte and reduce the interfacial impedance.

[0023] A third aspect of the present invention provides the application of the above-described halide oxide solid electrolyte or the halide oxide solid electrolyte obtained by the above preparation method in a lithium-ion all-solid-state battery.

[0024] The lithium-ion all-solid-state battery includes a negative electrode, a positive electrode, a halide oxide solid electrolyte film, and a sulfide interlayer film.

[0025] The halide oxide solid electrolyte film is cold-pressed using the method described above. The sulfide interlayer uses common interlayer materials such as Li6PS5Cl or Li. 10 GeP2S 12 .

[0026] Compared with the prior art, the advantages of the present invention are: using zirconium-based chloro-halide electrolyte as the main body, designing anion and cation dual doping to prepare new solid electrolytes with different proportions, realizing phase transformation and amorphization transformation, and forming new stable chemical structures. Compared with traditional halide electrolytes, the prepared halide oxide electrolyte achieves an improvement in the key parameter ionic conductivity while reducing costs. Unlike other electrolyte preparation methods that require multiple ball milling and high-temperature solid-state sintering, the preparation method of this invention is simple and time-saving, requiring only one-step ball milling to obtain the target electrolyte, without the need for solid-state sintering. This method is simple, efficient, energy-saving, emission-reducing, and has low preparation costs, making it suitable for industrial-scale production. In terms of full-cell applications, the electrolyte of this invention is compatible with positive electrode active materials such as lithium cobalt oxide, NCM811, and lithium-rich manganese-based materials, exhibiting good compatibility and stable chemical properties, and can achieve excellent rate performance and long-cycle performance. Through the development and adaptation of this type of novel solid-state electrolyte, the high energy density and long-cycle performance of all-solid-state batteries can be effectively improved. This is not only a key breakthrough in the current technical bottlenecks in the field of energy storage batteries, but also provides important technical support for the large-scale and industrial upgrading of the new energy industry and the optimization and transformation of the national energy structure. Attached Figure Description

[0027] Figure 1 The Li obtained in Example 1 of this invention 2.8 Zr0.9 Gd 0.1 Cl 5.2 O 0.75 and Li 2.8 Zr 0.9 Gd 0.1 Cl 5.1 O 0.8 X-ray diffraction pattern; Figure 2 The Li obtained in Example 2 of this invention 3.4 Zr 0.8 W 0.1 Gd 0.1 Cl 4.6 O 1.4 X-ray diffraction pattern; Figure 3 The X-ray diffraction pattern of Li2ZrCl6 prepared in Comparative Example 1 of this invention; Figure 4 The Li obtained in Example 1 of this invention 3.5 Zr 0.9 Gd 0.1 Cl 4.6 O 1.4 Li 3.45 Zr 0.95 Gd 0.05 Cl 4.6 O 1.4 Li 2.8 Zr 0.9 Gd 0.1 Cl 5.2 O 0.75 Li 2.8 Zr 0.9 Gd 0.1 Cl 5.1 O 0.8 EIS impedance spectrum and ionic conductivity plot; Figure 5 The Li obtained in Example 2 of this invention 3.4 Zr 0.8 W 0.1 Gd 0.1 Cl 4.6 O 1.4 Li 3.4 Zr 0.8 W 0.1 Y 0.1 Cl 4.6 O 1.4 Li 2.8 Zr 0.8 W 0.1 Y 0.1 Cl 5.2 O 0.8 EIS impedance spectrum and ionic conductivity plot; Figure 6 The ionic and electronic conductivity diagrams of Li₂ZrCl₆ prepared in Comparative Example 1 are shown. Figure 7 The Li obtained in Example 1 of this invention 2.8 Zr 0.9 Gd 0.1 Cl 5.2 O 0.75 Li 2.8 Zr 0.9 Gd 0.1 Cl 5.1 O 0.8 Electron conductivity diagram; Figure 8 The Li obtained in Example 1 of this invention 3.5 Zr 0.9 Gd 0.1 Cl 4.6 O 1.4 Li 2.8 Zr 0.9 Gd 0.1 Cl 5.2 O 0.75 Li 2.8 Zr 0.9 Gd 0.1 Cl 5.1 O 0.8 The first charge-discharge cycle voltage curve; Figure 9 The Li obtained in Example 2 of this invention 2.8 Zr 0.8 W 0.1 Gd 0.1 Cl 5.2 O 0.8 The first charge-discharge cycle voltage curve; Figure 10 The Li obtained in Example 1 of this invention 2.8 Zr 0.9 Gd 0.1 Cl 5.2 O 0.75 Long-cycle charge-discharge curves and rate performance curves of full batteries using lithium cobalt oxide as the active material. Detailed Implementation

[0028] To make the technical problems solved by the present invention, the technical solutions, and the beneficial effects clearer, the following specific embodiments provide a further detailed description of the present invention. It should be understood that the specific embodiments described herein are merely illustrative and are not intended to limit the scope of the invention.

[0029] Example 1 The halide oxide solid electrolyte in this embodiment is prepared by doping Li₂ZrCl₆ with Gd and O as doping elements, and the specific preparation method is as follows: Raw materials were weighed separately in a glove box in an anhydrous and oxygen-free environment (water content ≤ 0.01 ppm, oxygen content ≤ 0.01 ppm). The purity of the following reagents was all above 99.9 wt%.

[0030] Sample ①: 0.096 g LiCl, 0.682 g ZrCl4, 0.136 g Li2O, 0.086 g GdCl3; Sample ②: 0.108 g LiCl, 0.592 g ZrCl4, 0.132 g Li2O, 0.168 g GdCl3; Sample ③: 0.176 g LiCl, 0.669 g ZrCl4, 0.072 g Li2O, 0.084 g GdCl3; Sample ④: 0.164 g LiCl, 0.675 g ZrCl4, 0.077 g Li2O, 0.085 g GdCl3; The raw materials in the above proportions were poured into 100 mL ZrO2 vacuum ball mill jars. The diameters of the ZrO2 grinding beads were 10 mm, 8 mm, and 5 mm, respectively, with a ratio of 2:3:5, i.e., the weights of the grinding beads were 25 g, 37.5 g, and 62.5 g, respectively, for a total grinding bead weight of 125 g. The ball-to-material ratio was 125:1. After sealing, the jar was removed from the glove box and ball-milled using a planetary ball mill at a speed of 500 rpm. The milling method was clockwise for 25 minutes, followed by a 10-minute pause, then counterclockwise for 25 minutes, repeated 24 times. The total milling time was 28 hours. After milling, the ZrO2 grinding jar was returned to the glove box, and the electrolyte powder was removed and placed in a dry, clean sample bottle, completing the preparation of the halide oxide solid electrolyte.

[0031] The chemical formulas of the halide oxide electrolytes prepared in this embodiment are as follows: Sample ①: Li 3.5 Zr 0.9 Gd 0.1 Cl 4.6 O 1.4 ; Sample ②: Li 3.45 Zr 0.95 Gd 0.05 Cl 4.6 O 1.4 ; Sample ③: Li 2.8 Zr 0.9 Gd 0.1 Cl5.2 O 0.75 ; Sample ④: Li 2.8 Zr 0.9 Gd 0.1 Cl 5.1 O 0.8 .

[0032] Example 2 The halide oxide solid electrolyte in this embodiment is prepared by doping Li₂ZrCl₆ with W, Gd, Y, and O as doping elements. The specific preparation method is as follows: Raw materials were weighed separately in a glove box in an anhydrous and oxygen-free environment (water content ≤ 0.01 ppm, oxygen content ≤ 0.01 ppm). The purity of the following reagents was all above 99.9 wt%.

[0033] Sample ①: 0.0804 g LiCl, 0.5897 g ZrCl4, 0.1323 g Li2O, 0.0834 g GdCl3, 0.1142 g WCl5 Sample ②: 0.0822 g LiCl, 0.6025 g ZrCl4, 0.1352 g Li2O, 0.0634 g YCl3, 0.1167 g WCl5 Sample ③: 0.1572 g LiCl, 0.5760 g ZrCl4, 0.0739 g Li2O, 0.0814 g GdCl3, 0.1116 g WCl5 The raw materials in the above proportions were poured into 100 mL ZrO2 vacuum ball mill jars. The diameters of the ZrO2 grinding balls were 10 mm, 8 mm, and 5 mm, respectively, with a ratio of 2:3:5, meaning the mass of the grinding balls was 25 g, 37.5 g, and 62.5 g, respectively, for a total grinding ball mass of 125 g. The ball-to-material ratio was 125:1. After sealing, the jar was removed from the glove box and ball-milled using a planetary ball mill at 580 rpm. The milling process consisted of 15 minutes clockwise, a 5-minute pause, and 15 minutes counterclockwise, repeated 36 times. The total milling time was 24 hours. After milling, the ZrO2 grinding jar was returned to the glove box, and the electrolyte powder was removed and placed in a dry, clean sample vial, completing the preparation of the halide oxide solid electrolyte.

[0034] The chemical formulas of the prepared halide oxide electrolytes are as follows: Sample ①: Li 3.4 Zr 0.8 W 0.1 Gd 0.1 Cl 4.6 O 1.4 ; Sample ②: Li 3.4 Zr 0.8 W 0.1 Y 0.1 Cl 4.6 O 1.4 ; Sample ③: Li 2.8 Zr 0.8 W 0.1 Gd 0.1 Cl 5.2 O 0.8 .

[0035] Comparative Example 1 This comparative example provides a conventional halide electrolyte, Li₂ZrCl₆, and the specific preparation method is as follows: 0.267 g LiCl and 0.733 g ZrCl4 were weighed in a glove box under anhydrous and oxygen-free conditions (water content ≤ 0.01 ppm, oxygen content ≤ 0.01 ppm) and placed in a 100 mL ZrO2 vacuum-sealed ball mill jar. The ball milling beads, their material, mass, and ratio were consistent with those in the examples, with a ball-to-bead ratio of 125:1. The ball milling method and time were also consistent with those in the examples. The final product was a Li2ZrCl6 halide solid electrolyte.

[0036] The performance of the halide oxide electrolyte prepared in the examples and the halide solid electrolyte prepared in the comparative examples was tested using the following methods: (1) X-ray diffraction: 200 mg of sample halide oxide solid electrolyte was weighed in a glove box in an anhydrous and oxygen-free environment (water content ≤ 0.01 ppm, oxygen content ≤ 0.01 ppm) and placed in a sealed sample cell (20 mm × 20 mm) for XRD. The powder was compacted with a custom glass slide. The sample stage was sealed with a sealing tape to isolate oxygen and moisture. X-ray diffraction was used to characterize the diffraction peaks and other information of the solid electrolyte. The test range was 10-80 °, and the scanning speed was 8 ° / min.

[0037] (2) Ionic conductivity test: 150 mg of the prepared solid electrolyte was weighed in a glove box in an anhydrous and oxygen-free environment (water content ≤ 0.01 ppm, oxygen content ≤ 0.01 ppm) and placed in a zirconia pore solid battery mold with an inner diameter of 10 mm. The mold was pressed with a tablet press at a pressure of 625 MPa for 5 min. The height difference of the solid battery mold before and after placing the electrolyte was recorded as d, which is the thickness of the solid electrolyte sheet. The mold was left to stand in a constant temperature oven at 25 ℃ for 20 min. Then, the impedance was tested by AC impedance method using an electrochemical workstation. The test range was 0.01~1000000 Hz, and the obtained impedance value was recorded as R. Finally, the ionic conductivity was calculated by the formula σ=d / R·S, with the unit being S·cm. -1S is the contact area between the blocking electrode and the electrolyte sheet.

[0038] (3) Electronic conductivity test: 150 mg of the prepared solid electrolyte was weighed in a glove box in an anhydrous and oxygen-free environment (water content ≤ 0.01 ppm, oxygen content ≤ 0.01 ppm). The mold was assembled and pressed according to the same method as the electronic conductivity test. The mold was left to stand in a constant temperature chamber at 25 ℃ for 20 min. Then, the electronic conductivity was tested by DC polarization method using an electrochemical workstation. The constant DC voltage was U = 0.4 V, the high voltage was 0.2 V, the low voltage was 0.6 V, the pulse width was 300 s, the sample interval was 10 s, and the standing time was 30 s. The stable current I was obtained, and the total resistance of the system was calculated using the formula R = U / I. Finally, the electronic conductivity was calculated using the formula σ = d / R·S, with the unit being S·cm. -1 S is the contact area between the blocking electrode and the electrolyte sheet.

[0039] (4) All-solid-state battery and long-cycle test: Lithium cobalt oxide was used as the active material for the positive electrode. 200 mg of LCO positive electrode powder and 85.71 mg of solid electrolyte powder (LCO:electrolyte = 7:3) were weighed in a glove box under anhydrous and oxygen-free conditions (water content ≤ 0.01 ppm, oxygen content ≤ 0.01 ppm), placed in a centrifuge tube, and several ZrO2 milling beads with a diameter of 5 mm were added. The centrifuge tube was placed in a high-speed vibratory ball mill and milled at 5000 r / min for 1 min to obtain a composite positive electrode through uniform mixing. 80 mg of the prepared solid electrolyte was placed in a mold, and the mold was pressed using a tablet press at a pressure of 375 MPa for 5 min. 10 mg of composite positive electrode powder was added to one side of the electrolyte sheet in the mold, and the mold was pressed at a pressure of 125 MPa for 5 min. Next, 80 mg of intermediate layer material, Li6PS5Cl, was added to the other side of the mold to prevent direct contact between the halide electrolyte and the lithium indium sheet, which could lead to rapid lithium dendrite growth and battery failure. The mold was pressed at 375 MPa for 5 min. Finally, a 0.25 mm lithium indium alloy sheet was placed on the sulfide side of the mold, and the mold was pressed at 125 MPa for 5 min. This yielded an all-solid-state battery with a LiIn alloy-LPSC-halo electrolyte-LCO composite cathode structure. The resulting all-solid-state battery was then placed in a Blue Electric system for constant charge-discharge current cycling tests at 0.1 C, with a voltage range of 2.3 V to 3.6 V and a voltage protection range of -5 V to 5 V.

[0040] The test results are as follows: like Figure 1 As shown, Li 2.8 Zr0.9 Gd 0.1 Cl 5.2 O 0.75 and Li 2.8 Zr 0.9 Gd 0.1 Cl 5.1 O 0.8 The X-ray diffraction pattern of Li3ScCl6 was obtained, revealing its crystal structure. Characteristic diffraction peaks of Li3ScCl6 appear at 2θ=30°, 2θ=35°, and 2θ=51°, indicating a monoclinic phase (C2 / m) forming a stable oxychloride framework. Furthermore, the diffraction peaks weaken, suggesting that the synthesized Li... 2.8 Zr 0.9 Gd 0.1 Cl 5.2 O 0.75 and Li 2.8 Zr 0.9 Gd 0.1 Cl 5.1 O 0.8 It exhibits a high amorphous phase content.

[0041] In comparison, such as Figure 3 The image shows the X-ray diffraction pattern of Li₂ZrCl₆. It reveals the crystal structure of Li₃YCl₆. Characteristic diffraction peaks of Li₃YCl₆ appear at 2θ=16°, 2θ=32°, 2θ=41.5°, and 2θ=50°, indicating a hexagonal close-packed (HCP) triangular structure similar to space group P₃m₁. The peaks are strong and sharp, typical of a crystalline structure. This suggests that with the development of Gd... 3+ and O 2- The introduction of ion doping causes a phase transition in halide electrolytes, changing from a hexagonal phase to a monoclinic phase, while simultaneously increasing the degree of amorphous phase. Microscopically, O... 2- Smaller radius, enhanced electrostatic repulsion, and larger overall lattice size prevent blockage at high lithium content, lowering the migration barrier. The transformation from Zr-Cl bonds to Zr-O / Cl and Gd-O / Cl bonds leads to octahedral contraction, widening the lithium-ion transport pathways. Increased amorphization transforms the lithium-ion transport pathway from a confined two-dimensional conduction to a continuous three-dimensional conduction, making the transport channels open and continuous, lowering the transport barrier, and further improving lithium-ion transport efficiency. This is one of the reasons for the increased ionic conductivity of halide oxide electrolytes.

[0042] Zr 4+ The radius of the ion is around 0.72 Å, while the radius of rare earth ions (such as Gd) is much larger. 3+The ion radius is between 0.9 Å and 1.03 Å. The introduction of rare earth element ions with larger radii expands the lattice volume, widening the lithium-ion transport channels. At the same time, it also reduces the risk of transport channel blockage caused by high lithium content, which is one of the reasons for the improved ionic conductivity of halide oxide solid electrolytes.

[0043] like Figure 2 As shown, Li 2.8 Zr 0.8 W 0.1 Gd 0.1 Cl 5.2 O 0.8 The X-ray diffraction pattern shows a similarity to Li. 2.8 Zr 0.9 Gd 0.1 Cl 5.2 O 0.75 and Li 2.8 Zr 0.9 Gd 0.1 Cl 5.1 O 0.8 Similar diffraction peaks were observed. Characteristic diffraction peaks of Li3ScCl6 appeared at 2θ=30°, 2θ=35°, and 2θ=51°, indicating a monoclinic phase (C2 / m). Simultaneously, the lower diffraction peak intensities reflected increased amorphization. In contrast, W... 5+ Gd 3+ Dual-doped Gd 3+ The single-doped diffraction peaks shift to lower angles, the lattice spacing increases further, and the lattice expands further, widening the channels for lithium-ion transport.

[0044] like Figure 4 As shown, this is the synthesized Li. 3.5 Zr 0.9 Gd 0.1 Cl 4.6 O 1.4 Li 3.45 Zr 0.95 Gd 0.05 Cl 4.6 O 1.4 Li 2.8 Zr 0.9 Gd 0.1 Cl 5.2 O 0.75 Li 2.8 Zr 0.9 Gd 0.1 Cl 5.1 O 0.8 The EIS impedance spectra and ionic conductivity plots are shown. The conductivity of these halide oxide solid electrolytes is 0.301 mS·cm. -1 0.311 mS·cm -11.039 mS·cm -1 0.934 mS·cm -1 In comparison, the Li₂ZrCl₆ electrolyte has a capacity of only 0.500 mS·cm. -1 (like Figure 6 As shown in the figure, the ionic conductivity is relatively high (1.039 mS·cm) when the Li content is around 6.2 wt% and the O content is 3.83 wt%. -1 The conductivity is twice that of traditional Li₂ZrCl₆. This invention not only investigates the ionic conductivity performance of halide oxides under lithium-rich conditions but also explores their performance under low lithium contents.

[0045] like Figure 5 As shown, this is the synthesized Li. 3.4 Zr 0.8 W 0.1 Gd 0.1 Cl 4.6 O 1.4 Li 3.4 Zr 0.8 W 0.1 Y 0.1 Cl 4.6 O 1.4 Li 2.8 Zr 0.8 W 0.1 Gd 0.1 Cl 5.2 O 0.8 The EIS impedance spectra and ionic conductivity plots are shown. The ionic conductivity of these halide oxide solid electrolytes is 0.151 mS·cm. -1 0.159 mS·cm -1 0.544 mS·cm -1 In comparison, the conductivity of Li₂ZrCl₆ electrolyte is 0.500 mS·cm. -1 (like Figure 6 As shown), the conductivity is slightly improved, but using W 5+ Gd 3+ Replace part of Zr 4+ Such systems with higher entropy are more thermodynamically stable, thus improving air stability. In addition, they also enhance thermal and cycling stability, suppressing structural collapse and cracking during battery charge-discharge cycles.

[0046] like Figure 7 As shown, Li 2.8 Zr 0.9 Gd 0.1 Cl 5.2 O 0.75 Li 2.8 Zr 0.9Gd 0.1 Cl 5.1 O 0.8 A schematic diagram of electronic conductivity. All electronic conductivities are above 10. -7 ~10 -9 S·cm -1 This value is on the order of magnitude lower than that of ionic conductivity, indicating that the electrolyte has excellent properties as an ionic conductor and an electronic insulator, eliminating self-discharge and leakage, while also suppressing lithium dendrite penetration and internal short circuits.

[0047] Figure 8 and Figure 9 This study demonstrates the excellent compatibility and chemical stability of the halide oxide electrolyte with the lithium cobalt oxide cathode. A full cell assembly was performed using LiCoO2 as the positive electrode active material, lithium indium alloy as the negative electrode, and Li6PS5Cl as an interlayer to prevent direct contact between the negative electrode and the halide oxide electrolyte material. Charge-discharge tests were conducted at a 0.1 C rate. 2.8 Zr 0.9 Gd 0.1 Cl 5.2 O 0.75 Li 2.8 Zr 0.9 Gd 0.1 Cl 5.1 O 0.8 and Li 2.8 Zr 0.8 W 0.1 Gd 0.1 Cl 5.2 O 0.8 The performance was 169.06 mAh·g -1 146.65mAh·g -1 , 149.53 mAh·g -1 High specific capacity (the nominal specific capacity of lithium cobalt oxide is approximately 160 mAh·g) -1 Furthermore, the coulombic efficiency of the first charge and discharge both reached over 90%, proving that the synthesized halide electrolyte has excellent compatibility and chemical stability with lithium cobalt oxide, and can be applied to high energy density cathode materials without electrolyte failure caused by problems such as poor solid-solid contact, charge and discharge volume changes, and lithium dendrite growth. Figure 10 Li was showcased 2.8 Zr 0.9 Gd 0.1 Cl 5.2 O 0.75 The full battery exhibits excellent rate performance and charge / discharge performance after 300 cycles at 1C rate, with a capacity retention rate of up to 68.4%, and meets the cycling requirements at high rates. The assembled full battery demonstrates superior rate performance and cycle life.

Claims

1. A halide oxide solid electrolyte, characterized in that, The halide oxide solid electrolyte is Li a Zr 1-x- y M x N y Cl b O c M and N are at least one of the elements Tb, Y, Gd, Ce, La, Ta, W or Er, and M and N are the same element or different elements; wherein 2≤a≤3.5, 4.5≤b<6, 0<c≤1.5, and 0<x+y<1.

2. The halide oxide solid electrolyte according to claim 1, characterized in that, The chemical valence states of M and N are between +3 and +5.

3. The halide oxide solid electrolyte according to claim 1, characterized in that, The halide oxide solid electrolyte is Li 3.5 Zr 0.9 Gd 0.1 Cl 4.6 O 1.4 Li 3.45 Zr 0.95 Gd 0.05 Cl 4.6 O 1.4 Li 2.8 Zr 0.9 Gd 0.1 Cl 5.2 O 0.75 Li 2.8 Zr 0.9 Gd 0.1 Cl 5.1 O 0.8 Li 3.4 Zr 0.8 W 0.1 Gd 0.1 Cl 4.6 O 1.4 Li 3.4 Zr 0.8 W 0.1 Y 0.1 Cl 4.6 O 1.4 Or Li 2.8 Zr 0.8 W 0.1 Gd 0.1 Cl 5.2 O 0.8 .

4. A method for preparing a halide oxide solid electrolyte according to any one of claims 1-3, characterized in that, include: Under anaerobic and anhydrous conditions, lithium chloride, lithium oxide, zirconium chloride, and metal or non-metal chlorides are directly prepared by one-step ball milling in a sealed ball mill jar, wherein the metal or non-metal in the metal or non-metal chloride is independently selected from M or N.

5. The method for preparing a halide oxide solid electrolyte according to claim 4, characterized in that, The one-step ball milling method includes: a ball milling speed of 400~600 r / min, a ball milling method of clockwise ball milling for 10~30 minutes, stopping ball milling for 5~15 minutes, and counterclockwise ball milling for 10~30 minutes; the total ball milling time is 10~50 hours.

6. The method for preparing halide oxide solid electrolyte according to claim 4, characterized in that, The grinding balls used in the one-step ball milling method are made of ZrO2 material, with a size of 5~15 mm and a ball-to-material ratio of 80:1~150:

1.

7. The application of a halide oxide solid electrolyte according to any one of claims 1-3 or a halide oxide solid electrolyte obtained by the preparation method according to any one of claims 4-6 in a lithium-ion all-solid-state battery.

8. The application according to claim 7, characterized in that, The lithium-ion all-solid-state battery includes a negative electrode, a positive electrode, a halide oxide solid electrolyte film, and a sulfide interlayer film.

9. The application according to claim 8, characterized in that, The material of the sulfide interlayer film is Li6PS5Cl or Li 10 GeP2S 12 .

10. The application according to claim 8, characterized in that, The cathode material is lithium cobalt oxide, NCM811, or lithium-rich manganese-based material.

Citation Information

Patent Citations

  • Oxidation halide solid electrolyte as well as preparation method and application thereof

    CN121601756A