A wide-temperature-range copper ion hydrogel electrolyte based on multi-component synergistic regulation, its preparation method and application
By using a multi-component synergistically regulated copper ion hydrogel electrolyte, a cross-linked network is formed between copper salts and high-valence metal salts and sodium alginate. Combined with sugar additives and polyols to regulate the moisture state, the stability and transport performance of copper ion hydrogel electrolyte in a wide temperature range are solved, achieving stable operation in the range of -20 to 60 °C.
Patent Information
- Application Number
- CN202611619362.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing copper-ion hydrogel electrolytes suffer from poor cycle performance, freezing at low temperatures, and water loss at high temperatures in a wide temperature range, making it difficult to balance antifreeze performance and high-temperature stability, thus affecting the stable operation of the battery.
A multi-component synergistic regulation method was adopted, in which copper salt and high-valence metal salt were combined with sodium alginate to form a multi-ion cross-linked gel network, and sugar auxiliaries and polyols were used to regulate the moisture state, thereby improving the wide temperature range stability and ion transport performance of the gel.
Stable operation of copper ion hydrogel electrolyte was achieved in the range of -20~60 ℃, maintaining good ionic conductivity and cycling performance, and solving the problems of freezing at low temperature and water loss at high temperature of traditional electrolytes.
Smart Images

Figure CN123120924A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of aqueous battery technology, and in particular to a wide-temperature-range copper ion hydrogel electrolyte based on multi-component synergistic regulation, its preparation method, and its application. Background Technology
[0002] Aqueous batteries currently hold great promise. At present, aqueous metal-ion batteries mainly include zinc-ion, aluminum-ion, magnesium-ion, and copper-ion systems. While the zinc-ion system offers advantages such as low cost and high safety, it is prone to dendrite growth, corrosion, and hydrogen evolution reactions during cycling. In contrast, copper ions possess a higher redox potential, effectively suppressing hydrogen evolution reactions and exhibiting a higher theoretical specific capacity. Furthermore, copper ions have strong interactions with water molecules and polar groups in the gel network, facilitating the construction of a stable ion transport environment, making it more suitable as a research system for wide-temperature-range aqueous gel electrolytes. With the increasing application scenarios of batteries, there is a need to design a wide-temperature-range copper-ion gel electrolyte applicable to various temperature environments. The design of wide-temperature-range gel electrolytes presents several challenges. At low temperatures, free water in the gel easily freezes to form ice crystals, hindering ion migration and reducing ionic conductivity. Simultaneously, it damages the gel network structure, causing the material to harden and become embrittled. At high temperatures, water evaporation leads to gel dehydration, structural shrinkage, and decreased ion transport performance, while also exacerbating side reactions at the copper-electrode interface, reducing battery cycle stability. Therefore, how to balance antifreeze performance, high-temperature water retention performance, and ion transport capacity to achieve stable operation of copper ion hydrogels in a wide temperature range is a key technical problem that urgently needs to be solved in this field. Summary of the Invention
[0003] The purpose of this invention is to provide a wide-temperature-range copper ion hydrogel electrolyte based on multi-component synergistic regulation, its preparation method, and its application, so as to solve the problems existing in the prior art. Specifically, the existing copper ion hydrogel electrolyte system mainly has the following problems: (1) Poor battery cycle performance: Copper ion aqueous batteries may have problems such as uneven copper deposition, dendrite growth, and side reactions during cycling, resulting in reduced cycle stability. The existing copper ion hydrogel electrolyte has poor low-temperature performance. Some studies have tried to use copper perchlorate (Cu(ClO4)2) as a copper ion source, mainly because ClO4 - It possesses weak coordination properties, making it difficult to form a strong hydrogen bond network with water molecules. Therefore, it can reduce ice crystal formation at low temperatures while maintaining good ion migration capabilities. However, ClO4... -It belongs to the high oxidation state anion and has potential thermal decomposition behavior during the heating process, thus posing a safety hazard and may promote the occurrence of side reactions at the electrode interface. In the application of wide temperature range energy storage devices, the high temperature environment will further accelerate the reaction at the electrode and electrolyte interface and the water decomposition process, thereby affecting the long-term stability of the electrolyte system. (2) The design of wide temperature range copper ion hydrogel electrolyte is challenging and insufficiently studied: At present, the research on copper ion aqueous batteries mainly focuses on room temperature performance optimization or low temperature antifreeze performance improvement, and the research on electrolyte stability under wide temperature range operating conditions is still insufficient. The design of wide temperature range hydrogel electrolyte faces the problem of difficulty in balancing low temperature and high temperature performance: at low temperature, the free water in the gel is easy to freeze to form ice crystals, which hinders ion migration and reduces flexibility; at high temperature, water volatilization leads to gel dehydration and structural degradation, while aggravating the side reactions at the electrode and electrolyte interface. Therefore, the development of a wide temperature range copper ion hydrogel electrolyte with both low temperature antifreeze and high temperature stability is still a great challenge. Based on the above problems, the main purpose of this invention is to: (1) enhance battery cycle performance: suppress dendrite and by-product generation and improve cycle stability without using high-risk salts. (2) Enhance performance over a wide temperature range: improve ionic conductivity at low temperatures and enhance water retention at high temperatures to ensure that copper-ion batteries can be used in a wide temperature range of scenarios.
[0004] To achieve the above objectives, the present invention provides the following solution: One of the technical solutions of the present invention is a wide-temperature-range copper ion hydrogel electrolyte based on multi-component synergistic regulation, the raw materials of which include sodium alginate, copper salt, high-valence metal salt, sugar additives, polyol and water; The carbohydrate adjuvant includes one or more of disaccharides and polysaccharides; The high-valence metal salts include one or more of aluminum (+3 valence) salts, zirconium (+4 valence) salts, lanthanum (+3 valence) salts, and iron (+3 valence) salts.
[0005] In the raw material system of this invention: Copper salts and high-valence metal salts provide copper ions (Cu). 2+ The copper ions and high-valence metal ions participate in the ionic crosslinking of the carboxyl groups in the sodium alginate molecular chain. Through the synergistic coordination between metal ions of different valence states, multiple ionic connection nodes are formed between the sodium alginate molecular chains, forming a multi-metal ion synergistic crosslinking gel network. This network structure has higher crosslinking density and structural stability, which can effectively improve the stability of gel ion transport and the ability to maintain structure under wide temperature range. Sugar-based additives are used to adjust the moisture state in gel systems and improve water retention performance under high temperature conditions; Polyols are used as co-solvents to adjust the hydrogen bond structure in the system, reduce the tendency of water to freeze, and improve the ion transport performance under low temperature conditions. Through the synergistic effect of the above components, the copper ion hydrogel electrolyte maintains stable operation over a wide temperature range.
[0006] Furthermore, the copper salt includes one or more of copper sulfate, copper acetate, copper chloride, and copper nitrate.
[0007] Optionally, the copper salt may contain bound water or not, that is, the copper salt includes one or more of copper sulfate, copper acetate, copper chloride and copper nitrate, which may or may not contain bound water.
[0008] Furthermore, the aluminum salt includes aluminum chloride; the zirconium salt includes zirconium chloride; the lanthanum salt includes lanthanum chloride; and the iron salt includes ferric chloride.
[0009] Furthermore, the aluminum salt may or may not contain bound water; the zirconium salt may or may not contain bound water; the lanthanum salt may or may not contain bound water; and the iron salt may or may not contain bound water.
[0010] Furthermore, the disaccharide includes trehalose; the polysaccharide includes one or more of dextran, hydroxyethyl cellulose, starch, xanthan gum, and guar gum.
[0011] Furthermore, the polyol includes one or more of ethylene glycol, glycerol, propylene glycol, diethylene glycol, and triethylene glycol.
[0012] Further, the mass ratio of sodium alginate to the saccharide auxiliaries is 1:1 to 7, preferably 1:5.8; the molar ratio of the copper salt to the high-valence metal salt is 8 to 20:1, preferably 10 to 17:1; the dosage ratio of sodium alginate to the copper salt is 1 g: 5 to 20 mmol, preferably 1 g: 5 to 17 mmol; the ratio of the sum of the masses of sodium alginate, the copper salt, the high-valence metal salt, and the saccharide auxiliaries to the volume of water is 1 g: 1 to 8 mL, preferably 1 g: 3 to 6 mL; and the volume ratio of the polyol to the water is 1:3 to 8, preferably 1:5.
[0013] The second technical solution of the present invention: A method for preparing the above-mentioned wide-temperature-range copper ion hydrogel electrolyte based on multi-component synergistic regulation, comprising the following steps: mixing sodium alginate, sugar auxiliaries, polyol and a portion of water to obtain a gel precursor solution; mixing copper salt, high-valence metal salt and remaining water to obtain a composite metal salt solution; pouring the gel precursor solution into a mold, adding the composite metal salt solution to perform a cross-linking reaction (causing copper ions and high-valence metal ions to undergo ionic cross-linking reaction with the carboxyl groups in the sodium alginate molecular chain, and fixing the morphology through the mold), to obtain the wide-temperature-range copper ion hydrogel electrolyte based on multi-component synergistic regulation.
[0014] Furthermore, the ratio of sodium alginate to water in the gel precursor solution is 1 g: 20~30 mL.
[0015] Furthermore, the crosslinking reaction is carried out at a temperature of 20-30 °C (i.e., room temperature) for 12-48 h.
[0016] Furthermore, the crosslinking reaction is carried out under static conditions.
[0017] Optionally, before pouring the gel precursor liquid into the mold, the process further includes a step of letting it stand at room temperature (i.e., 20~30 ℃) for 6~12 h to remove air bubbles from the gel precursor liquid.
[0018] Optionally, after pouring the gel precursor liquid into the mold, before adding the composite metal salt solution, the process further includes a step of letting it stand at room temperature (i.e., 20~30 ℃) for 1~3 h to further remove air bubbles.
[0019] Optionally, after the crosslinking reaction is completed, the step of pouring out and removing the unreacted residual solution is further included.
[0020] Optionally, sodium alginate, sugar additives, polyols and a portion of water are mixed and stirred at room temperature (i.e., 20-30 °C) for 6-12 h.
[0021] Optionally, the copper salt, high-valence metal salt and remaining water are mixed by stirring at room temperature (i.e., 20~30 °C) for 0.5~2 h.
[0022] The third technical solution of the present invention: the application of the above-mentioned wide-temperature-range copper ion hydrogel electrolyte based on multi-component synergistic regulation in the preparation of aqueous copper ion batteries.
[0023] The fourth technical solution of the present invention: an aqueous copper-ion battery, wherein the raw materials of the aqueous copper-ion battery include the above-mentioned wide-temperature-range copper-ion hydrogel electrolyte based on multi-component synergistic regulation.
[0024] This invention prepares a copper ion hydrogel electrolyte with wide temperature range adaptability by ion crosslinking copper ions and high-valence metal ions with sodium alginate. Specifically, a composite metal ion system composed of copper ions and high-valence metal ions is introduced to form a stable ion-crosslinked gel structure with sodium alginate. Furthermore, the addition of saccharide auxiliaries (disaccharides and / or polysaccharides) and polyols to the sodium alginate system can regulate the state of water molecules through hydrogen bonding, reducing free water content and improving the gel's water retention capacity under high-temperature conditions, while simultaneously enhancing its antifreeze properties at low temperatures. Through multi-component synergistic regulation, stable operation of the copper ion hydrogel electrolyte is achieved under wide temperature range conditions. The performance improvement is not simply achieved by increasing the number of components, but rather by producing a synergistic effect across a wide temperature range within a specific ratio range.
[0025] The present invention discloses the following technical effects: The copper ion hydrogel electrolyte of this invention, based on multi-component synergistic regulation, achieves stable ion transport capability and electrochemical performance over a wide temperature range. It maintains good operational stability at temperatures ranging from -20 to 60 °C, with ionic conductivity reaching 1.6–2.1 mS / cm at 30 °C, 2.5–3.3 mS / cm at 60 °C, and maintaining 0.25–0.34 mS / cm at -20 °C. Furthermore, it achieves long-term stable operation at these temperatures, effectively solving the performance degradation problem faced by traditional aqueous gel electrolytes under low-temperature freezing and high-temperature dehydration conditions. Attached Figure Description
[0026] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0027] Figure 1 The ionic conductivity of the wide-temperature-range copper ion hydrogel electrolyte prepared in Example 1 based on multi-component synergistic regulation is measured in a wide temperature range (-20~60 °C).
[0028] Figure 2 Cycling performance of the wide-temperature-range copper ion hydrogel electrolyte prepared in Example 1 based on multi-component synergistic regulation at 30 °C.
[0029] Figure 3 Cycling performance of the wide-temperature-range copper ion hydrogel electrolyte prepared in Example 1 based on multi-component synergistic regulation at 60 °C.
[0030] Figure 4 Cycling performance of the wide-temperature-range copper ion hydrogel electrolyte prepared in Example 1 based on multi-component synergistic regulation at -20℃.
[0031] Figure 5 The cycling performance of the copper ion hydrogel electrolyte prepared in Comparative Example 1 at -20 °C was measured.
[0032] Figure 6 The cycling performance of the copper ion hydrogel electrolyte prepared in Comparative Example 2 at 60 °C was measured.
[0033] Figure 7 The cycling performance of the copper ion hydrogel electrolyte prepared in Comparative Example 3 at 60 °C was measured.
[0034] Figure 8 The cycling performance of the copper ion hydrogel electrolyte prepared in Comparative Example 4 at 60 °C was measured.
[0035] Figure 9 The cycling performance of the copper ion hydrogel electrolyte prepared in Comparative Example 5 at -20 °C was measured.
[0036] Figure 10 The cycling performance of the copper ion hydrogel electrolyte prepared in Comparative Example 6 at -20 °C was measured. Detailed Implementation
[0037] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0038] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Any stated value or intermediate value within a stated range, as well as each smaller range between any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.
[0039] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.
[0040] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be apparent to those skilled in the art. This specification and embodiments are merely exemplary.
[0041] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.
[0042] It should be noted that any aspects not described in detail in this invention are conventional practices in the field and are not the focus of this invention.
[0043] Unless otherwise specified, room temperature or ambient temperature refers to 20~30℃ in the following embodiments, comparative examples and test examples of this invention.
[0044] Unless otherwise specified, all raw materials used in the following embodiments, comparative examples and test examples of this invention are commercially available products.
[0045] Example 1 A wide-temperature-range copper ion hydrogel electrolyte based on multi-component synergistic regulation is prepared as follows: 1.2 g of sodium alginate and 7 g of trehalose were weighed and added to 30 mL of deionized water, along with 10 mL of ethylene glycol. The mixture was stirred at room temperature for 8 h to ensure complete dissolution of all components, resulting in a homogeneous gel precursor solution. The solution was then allowed to stand for 8 h to remove air bubbles. 4.98 g (20 mmol) of copper sulfate pentahydrate (CuSO4·5H2O) and 0.482 g (2 mmol) of aluminum chloride hexahydrate (AlCl3·6H2O) were weighed and dissolved in 20 mL of deionized water. The mixture was stirred at room temperature for 1 h to obtain a homogeneous composite metal salt solution. The defoamed gel precursor solution was poured into a mold (the mold dimensions were: outer diameter 120 mm, inner diameter 110 mm, height 20 mm; the mold dimensions used in all embodiments and comparative examples of this invention were consistent), and allowed to stand at room temperature for 2 h to further remove air bubbles. The aforementioned composite metal salt solution was then added, and the mixture was allowed to stand at room temperature for 24 h to allow the Cu... 2+ And Al 3+ An ionic crosslinking reaction (i.e., gelation) occurs with the carboxyl groups in the sodium alginate molecular chain. After the reaction is complete, the unreacted residual solution (composite metal salt solution) is decanted to obtain a wide-temperature-range copper ion hydrogel electrolyte based on multi-component synergistic regulation.
[0046] Example 2 A wide-temperature-range copper ion hydrogel electrolyte based on multi-component synergistic regulation is prepared as follows: 1.2 g of sodium alginate and 7 g of trehalose were weighed and added to 30 mL of deionized water, along with 10 mL of ethylene glycol. The mixture was stirred at room temperature for 8 h to ensure complete dissolution of all components, resulting in a homogeneous gel precursor solution. The solution was then allowed to stand for 8 h to remove air bubbles. 4.98 g of copper sulfate pentahydrate and 0.325 g (1.2 mmol) of ferric chloride hexahydrate (FeCl3·6H2O) were weighed and dissolved in 20 mL of deionized water. The mixture was stirred at room temperature for 1 h to obtain a homogeneous composite metal salt solution. The defoamed gel precursor solution was poured into a mold and allowed to stand at room temperature for 2 h to further remove air bubbles. The composite metal salt solution was then added, and the mixture was allowed to stand at room temperature for 24 h to initiate the cross-linking reaction. After the reaction, the unreacted residual solution was discarded to obtain a wide-temperature-range copper ion hydrogel electrolyte based on multi-component synergistic regulation.
[0047] Example 3 A wide-temperature-range copper ion hydrogel electrolyte based on multi-component synergistic regulation is prepared as follows: 1.2 g of sodium alginate and 7 g of trehalose were weighed and added to 30 mL of deionized water, along with 10 mL of ethylene glycol. The mixture was stirred at room temperature for 8 h to ensure complete dissolution of all components, resulting in a homogeneous gel precursor solution. The solution was then allowed to stand for 8 h to remove air bubbles. 1.2 g (6 mmol) of copper acetate monohydrate (Cu(CH3COO)2·H2O) and 0.121 g (0.5 mmol) of aluminum chloride hexahydrate were weighed and dissolved in 20 mL of deionized water. The mixture was stirred at room temperature for 1 h to obtain a homogeneous composite metal salt solution. The defoamed gel precursor solution was poured into a mold and allowed to stand at room temperature for 2 h to further remove air bubbles. The composite metal salt solution was then added, and the mixture was allowed to stand at room temperature for 24 h to initiate the cross-linking reaction. After the reaction, the unreacted residual solution was discarded to obtain a wide-temperature-range copper ion hydrogel electrolyte based on multi-component synergistic regulation.
[0048] Comparative Example 1 1.2 g of sodium alginate and 7 g of trehalose were weighed and added to 30 mL of deionized water, followed by 10 mL of ethylene glycol. The mixture was stirred at room temperature for 8 h to ensure complete dissolution of all components, resulting in a homogeneous gel precursor solution. The solution was then allowed to stand for 8 h to remove air bubbles. 4.98 g of copper sulfate pentahydrate was weighed and dissolved in 20 mL of deionized water. The solution was stirred at room temperature for 1 h to obtain a homogeneous metal salt solution. The defoamed gel precursor solution was poured into a mold and allowed to stand at room temperature for 2 h to further remove air bubbles. The aforementioned metal salt solution was then added, and the mixture was allowed to stand at room temperature for 24 h to initiate the cross-linking reaction. After the reaction was complete, the unreacted residual solution was discarded to obtain a copper ion hydrogel electrolyte.
[0049] Comparative Example 2 1.2 g of sodium alginate was weighed and added to 30 mL of deionized water, followed by 10 mL of ethylene glycol. The mixture was stirred at room temperature for 8 h to obtain a homogeneous gel precursor solution. The solution was then allowed to stand for 8 h to remove air bubbles. 4.98 g of copper sulfate pentahydrate and 0.482 g of aluminum chloride hexahydrate were weighed and dissolved in 20 mL of deionized water. The mixture was stirred at room temperature for 1 h to obtain a homogeneous composite metal salt solution. The defoamed gel precursor solution was poured into a mold and allowed to stand at room temperature for 2 h to further remove air bubbles. The composite metal salt solution was then added, and the mixture was allowed to stand at room temperature for 24 h to initiate the cross-linking reaction. After the reaction, the unreacted residual solution was discarded to obtain a copper ion hydrogel electrolyte.
[0050] Comparative Example 3 1.2 g of sodium alginate and 7 g of trehalose were weighed and added to 30 mL of deionized water, followed by 15 mL of ethylene glycol. The mixture was stirred at room temperature for 8 h to ensure complete dissolution of all components, resulting in a homogeneous gel precursor solution. The solution was then allowed to stand for 8 h to remove air bubbles. 4.98 g of copper sulfate pentahydrate and 0.482 g of aluminum chloride hexahydrate were weighed and dissolved in 20 mL of deionized water. The mixture was stirred at room temperature for 1 h to obtain a homogeneous composite metal salt solution. The defoamed gel precursor solution was poured into a mold and allowed to stand at room temperature for 2 h to further remove air bubbles. The composite metal salt solution was then added, and the mixture was allowed to stand at room temperature for 24 h to initiate the cross-linking reaction. After the reaction, the unreacted residual solution was discarded to obtain a wide-temperature-range copper ion hydrogel electrolyte.
[0051] Comparative Example 4 1.2 g of sodium alginate and 7 g of trehalose were weighed and added to 30 mL of deionized water, followed by 10 mL of ethylene glycol. The mixture was stirred at room temperature for 8 h to ensure complete dissolution of all components, resulting in a homogeneous gel precursor solution. The solution was then allowed to stand for 8 h to remove air bubbles. 4.98 g of copper sulfate pentahydrate and 1.2 g (5 mmol) of aluminum chloride hexahydrate were weighed and dissolved in 20 mL of deionized water. The mixture was stirred at room temperature for 1 h to obtain a homogeneous composite metal salt solution. The defoamed gel precursor solution was poured into a mold and allowed to stand at room temperature for 2 h to further remove air bubbles. The composite metal salt solution was then added, and the mixture was allowed to stand at room temperature for 24 h to initiate the cross-linking reaction. After the reaction, the unreacted residual solution was discarded to obtain a wide-temperature-range copper ion hydrogel electrolyte.
[0052] Comparative Example 5 1.2 g of sodium alginate and 10.2 g of trehalose were weighed and added to 30 mL of deionized water, along with 10 mL of ethylene glycol. The mixture was stirred at room temperature for 8 h to ensure complete dissolution of all components, resulting in a homogeneous gel precursor solution. The solution was then allowed to stand for 8 h to remove air bubbles. 4.98 g of copper sulfate pentahydrate and 0.482 g of aluminum chloride hexahydrate were weighed and dissolved in 20 mL of deionized water. The mixture was stirred at room temperature for 1 h to obtain a homogeneous composite metal salt solution. The defoamed gel precursor solution was poured into a mold and allowed to stand at room temperature for 2 h to further remove air bubbles. The composite metal salt solution was then added, and the mixture was allowed to stand at room temperature for 24 h to initiate the cross-linking reaction. After the reaction, the unreacted residual solution was discarded to obtain a copper ion hydrogel electrolyte.
[0053] Comparative Example 6 Same as Example 1, except that equimolar amounts of aluminum chloride hexahydrate are replaced with zinc sulfate heptahydrate.
[0054] Test Example 1 Ionic conductivity testing over a wide temperature range The ionic conductivity of the copper ion hydrogel electrolytes prepared in each embodiment and comparative example was tested over a wide temperature range (-20~60 °C). Electrochemical impedance spectroscopy (EIS) was used for testing. The copper ion hydrogel electrolytes were cut into uniformly sized discs or thin film samples, placed between stainless steel blocking electrodes to assemble symmetrical test cells, and subjected to isothermal equilibration at different temperatures (-20 °C, 0 °C, 25 °C, 40 °C, 60 °C) before measuring the AC impedance spectra. The bulk resistance of the sample was obtained from the high-frequency intercept of the Nyquist curve, and the ionic conductivity was calculated using the following formula: In the formula: : Ionic conductivity (S / cm); L : Thickness of hydrogel electrolyte membrane (cm); R The bulk resistance (Ω) of the hydrogel electrolyte is determined by the intersection of the high-frequency region and the real axis in the Nyquist curve. S Conductive area (cm²) in actual tests 2 ).
[0055] Test results are as follows Figure 1 As shown in Table 1, where, Figure 1 The ionic conductivity of the wide-temperature-range copper ion hydrogel electrolyte prepared in Example 1 based on multi-component synergistic regulation is measured in a wide temperature range (-20~60 °C).
[0056] Table 1. Ionic conductivity (mS / cm) of the products of each embodiment and comparative example over a wide temperature range (-20~60 °C) From Table 1 and Figure 1 It can be seen that the copper ion hydrogel electrolytes prepared in Examples 1-3, based on multi-component synergistic regulation, all exhibit good ionic conductivity over a wide temperature range (-20~60 °C). A comparison between Example 1 and Comparative Example 1 shows that although Comparative Example 1, which omits aluminum chloride hexahydrate, exhibits ionic conductivity similar to the system containing high-valence aluminum ions at both room temperature and high temperature (60 °C), the lack of Al... 3+ The synergistic cross-linking effect reduces the stability of the gel network and the ability to regulate the water structure at low temperatures, resulting in a significant decrease in ion transport performance at low temperatures (-20 °C). The ionic conductivity of Comparative Examples 2-6 is also lower than that of Example 1 over a wide temperature range (-20~60 °C).
[0057] Test Example 2 Cyclic performance test The copper-ion hydrogel electrolytes prepared in each embodiment and comparative example were assembled into aqueous copper-ion batteries, and their cycle performance was tested. Wherein: The assembly method for aqueous copper-ion batteries is as follows: A standard CR2032 button cell was used, and Cu||Cu symmetric cells were assembled in ambient air at room temperature. Specifically, in the Cu||Cu symmetric cells, copper foil (12 mm in diameter and 100 μm in thickness) was used for both the positive and negative electrodes. During battery assembly, the copper-ion hydrogel electrolyte prepared in each embodiment or comparative example was used as the electrolyte.
[0058] Cyclic performance testing conditions: ambient temperature 30℃, current density 1 mA / cm² 2 At a high temperature of 60℃, the current density is 1 mA / cm². 2 At a low temperature of -20°C, the current density is 0.25 mA / cm². 2 .
[0059] Test results are as follows Figures 2-10 As shown, where: Figures 2-4 The cycling performance of the wide-temperature-range copper ion hydrogel electrolyte based on multi-component synergistic regulation prepared in Example 1 is shown at 30 ℃, 60 ℃, and -20 ℃. It can be seen that it can achieve good cycling performance in a wide temperature range of -20~60 ℃.
[0060] Figure 5 The cycling performance of the copper ion hydrogel electrolyte (without aluminum chloride hexahydrate) prepared in Comparative Example 1 at -20 ℃ was compared. It can be seen that the copper ion hydrogel electrolyte prepared without aluminum chloride hexahydrate has poor cycling performance at -20 ℃, with a high initial polarization voltage, and significant performance degradation after less than 10 h of operation, indicating that the copper ion hydrogel electrolyte has failed.
[0061] Figure 6 The cycling performance of the copper ion hydrogel electrolyte (without trehalose) prepared in Comparative Example 2 at 60 °C was compared. It can be seen that the copper ion hydrogel electrolyte prepared without trehalose has poor cycling performance at 60 °C. The initial cycling is normal, but the polarization voltage increases significantly after only 33 h of operation, and the copper ion hydrogel electrolyte fails.
[0062] Figure 7The cycling performance of the copper ion hydrogel electrolyte prepared in Comparative Example 3 (with a volume ratio of ethylene glycol to deionized water of 1:2 in the gel precursor solution, which is an increase in ethylene glycol content compared to Example 1) at 60 °C was compared. It can be seen that the copper ion hydrogel electrolyte prepared by increasing the ethylene glycol content in the gel precursor solution has poor cycling performance at 60 °C. The initial cycle is normal, but the polarization voltage fluctuates after only 10 h of operation, and the polarization voltage increases significantly after 20 h, indicating that the copper ion hydrogel electrolyte has failed.
[0063] Figure 8 The cycling performance of the copper ion hydrogel electrolyte (copper sulfate pentahydrate and aluminum chloride hexahydrate molar ratio of 4:1, with an increased aluminum chloride hexahydrate content compared to Example 1) prepared in Comparative Example 4 at 60 °C was compared. It can be seen that the copper ion hydrogel electrolyte prepared with increased aluminum chloride hexahydrate content has poor cycling performance at 60 °C. The initial cycle is normal, but the polarization voltage increases significantly after only 5 h of operation, and the copper ion hydrogel electrolyte fails.
[0064] Figure 9 The cycling performance of the copper ion hydrogel electrolyte (the mass ratio of trehalose to sodium alginate was 8.5:1, which was higher than that of Example 1) prepared in Comparative Example 5 was compared at -20 °C. It can be seen that the copper ion hydrogel electrolyte prepared with increased trehalose content had poor cycling performance at -20 °C and failed after running for 1 hour.
[0065] Figure 10 The cycling performance of the copper ion hydrogel electrolyte (using two divalent metal ions) prepared in Comparative Example 6 at -20 ℃ is shown. It can be seen that the copper ion hydrogel electrolyte prepared using two divalent metal ions has poor cycling performance at -20 ℃ and fails after running for 38 hours.
Claims
1. A multi-component synergistically regulated wide-temperature-range copper-ion hydrogel electrolyte, characterized in that, The raw materials include sodium alginate, copper salt, high-valent metal salt, sugar additives, polyols, and water; The carbohydrate adjuvant includes one or more of disaccharides and polysaccharides; The high-valence metal salts include one or more of aluminum salts, zirconium salts, lanthanum salts, and iron salts; The mass ratio of sodium alginate to the saccharide auxiliaries is 1:1~7; the molar ratio of copper salt to the high-valence metal salt is 8~20:1; the dosage ratio of sodium alginate to copper salt is 1 g:5~20 mmol; the ratio of the sum of the masses of sodium alginate, copper salt, high-valence metal salt and saccharide auxiliaries to the volume of water is 1 g:1~8 mL; and the volume ratio of polyol to water is 1:3~8.
2. The multi-component synergistically regulated wide-temperature-range copper ion hydrogel electrolyte according to claim 1, wherein, The copper salt includes one or more of copper sulfate, copper acetate, copper chloride, and copper nitrate.
3. The wide-temperature-range copper ion hydrogel electrolyte based on multi-component synergistic regulation as described in claim 1, characterized in that, The disaccharide includes trehalose; the polysaccharide includes one or more of dextran, hydroxyethyl cellulose, starch, xanthan gum, and guar gum.
4. The wide-temperature-range copper ion hydrogel electrolyte based on multi-component synergistic regulation as described in claim 1, characterized in that, The polyols include one or more of ethylene glycol, glycerol, propylene glycol, diethylene glycol, and triethylene glycol.
5. A method for preparing a wide-temperature-range copper ion hydrogel electrolyte based on multi-component synergistic regulation as described in any one of claims 1 to 4, characterized in that, Includes the following steps: Sodium alginate, sugar additives, polyols, and some water are mixed to obtain a gel precursor solution; copper salt, high-valence metal salt, and remaining water are mixed to obtain a composite metal salt solution; the gel precursor solution is poured into a mold, and the composite metal salt solution is added to carry out a cross-linking reaction to obtain the wide-temperature-range copper ion hydrogel electrolyte based on multi-component synergistic regulation.
6. The preparation method of the wide-temperature-range copper ion hydrogel electrolyte based on multi-component synergistic regulation as described in claim 5, characterized in that, The ratio of sodium alginate to water in the gel precursor solution is 1 g: 20~30 mL.
7. The preparation method of the wide-temperature-range copper ion hydrogel electrolyte based on multi-component synergistic regulation as described in claim 5, characterized in that, The cross-linking reaction is carried out at a temperature of 20-30 °C for 12-48 h.
8. The application of a wide-temperature-range copper-ion hydrogel electrolyte based on multi-component synergistic regulation as described in any one of claims 1 to 4 in the preparation of aqueous copper-ion batteries.
9. An aqueous copper-ion battery, characterized in that, The raw materials for the aqueous copper-ion battery include the wide-temperature-range copper-ion hydrogel electrolyte based on multi-component synergistic regulation as described in any one of claims 1 to 4.