Lithium-ion cells, batteries and electrical devices

By controlling the SEI and CEI interface composition and gas composition of lithium-ion cells, the problems of low-temperature cold start and high-temperature gas generation stability in the high-nickel cathode and silicon-carbon anode combination system are solved, and the cells achieve both low-temperature polarization improvement and high-temperature gas generation stability.

CN123121067APending Publication Date: 2026-11-17JIANGSU RELIANCE ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611516489.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve low-temperature cold start and high-temperature gas generation stability in lithium-ion cells, especially in the combination system of high-nickel cathode and silicon-carbon anode. The problems of electrolyte oxidation, side reaction gas generation, and transition metal dissolution caused by interface state sensitivity are difficult to solve effectively.

Method used

By controlling the ratio of inorganic lithium salt to organic lithium salt in the negative electrode SEI, a stable SEI film is formed. By controlling the P-containing, F-containing, and B-containing species in the positive electrode CEI, and combining the interface impedance and gas composition, a combined relationship between interface formation traces and performance stability is constructed, thereby achieving low-temperature cold start and high-temperature gas generation stability of the battery cell.

Benefits of technology

It achieves good polarization performance of lithium-ion cells at low temperatures and stability of gas generation at high temperatures, avoiding excessive interface impedance or abnormal gas generation, and ensuring the safety and performance stability of the cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123121067A_ABST
    Figure CN123121067A_ABST
Patent Text Reader

Abstract

This invention discloses lithium-ion battery cells, batteries, and electrical devices, relating to the field of lithium-ion batteries. This invention controls the ratio of inorganic lithium salt to organic lithium salt in the negative electrode SEI through RSEI, ensuring that the SEI film has sufficient electron blocking capability without significantly hindering LiF due to excessive LiF enrichment. + Migration improves polarization performance during low-temperature cold starts; controlling P-, F-, and B-containing species in the cathode CEI through RCEI enables the formation of a more stable protective layer on the surface of the high-nickel cathode, reducing the risks of electrolyte oxidation, side reaction gas generation, and transition metal dissolution at high temperatures; correlating interface composition, interface impedance, and gas composition through Rint, Gint, and Kif, and forming a combined window of traces at the finished interface, enables the cell to have both low-temperature cold start capability and high-temperature gas generation stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery technology, and more specifically, to lithium-ion cells, batteries, and electrical devices. Background Technology

[0002] The combination of high-nickel cathodes and silicon-carbon anodes can improve the capacity and energy density of cylindrical lithium-ion cells, but this system is more sensitive to the interface state of the finished product. High-nickel cathode surfaces are prone to electrolyte oxidation, side reaction gas generation, and transition metal dissolution under high SOC, high temperature, or high potential conditions. Silicon-carbon anodes undergo volume changes during lithium insertion / extraction, which can easily lead to SEI film rupture, regeneration, and impedance growth. These factors further affect polarization during low-temperature cold starts, gas generation during high-temperature cycling or storage, and safety and stability.

[0003] In existing technologies, some solutions directly specify electrolyte additive formulations, injection volumes, formation currents, formation temperatures, or settling times to improve the interfacial state of high-nickel silicon-carbon systems. However, for commercially available or uncirculated cylindrical cells, process parameters such as formation current, formation temperature, and settling time cannot usually be directly obtained from the finished product; even if residual electrolyte components can be detected, it is difficult to prove that they correspond to the final effective interfacial state. For reverse protection, a more stable technical approach is to start from the detectable SEI / CEI composition, interfacial impedance, gas composition, and low-temperature and gas generation performance under fixed conditions in the finished cell, and construct a correlation between interfacial formation traces and performance stability.

[0004] Therefore, there is an urgent need to provide lithium-ion cells that can simultaneously support low-temperature cold start and high-temperature gas production stability, and whose finished products can be reverse tested by XPS, TOF-SIMS, EIS and gas analysis.

[0005] In view of this, the present invention is proposed. Summary of the Invention

[0006] The purpose of this invention is to provide lithium-ion cells, batteries, and electrical devices that can achieve low-temperature cold start while also possessing high-temperature gas generation stability.

[0007] This invention is implemented as follows: In a first aspect, the present invention provides a lithium-ion battery cell, comprising a cylindrical shell, a core housed within the cylindrical shell, and an electrolyte impregnating the core. The core includes a positive electrode, a negative electrode, and a separator disposed between the positive and negative electrode. The positive electrode comprises a high-nickel layered lithium transition metal oxide with a nickel molar ratio of 88% to 93% in the transition metal elements. The negative electrode comprises graphite material and silicon-carbon material. The lithium-ion battery cell, after formation and capacity testing, meets the conditions for interface formation traces and low-temperature gas generation stability. The conditions for the formation of traces at the interface include features A1 to F1: Feature A1: The negative electrode interface film is a SEI reaction product layer that remains on the surface of the negative electrode active particles after the finished battery cell has been disassembled and treated with dimethyl carbonate to remove free electrolyte, and can be detected by XPS or TOF-SIMS. The ratio of the equivalent content of LiF to the equivalent content of organic lithium salt in the negative electrode interface film, RSEI, is 0.70~2.60. Feature B1: The positive electrode interface film is a CEI reaction product layer that remains on the surface of the positive electrode active particles after the finished battery cell has been disassembled and treated with dimethyl carbonate to remove the free electrolyte, and can be detected by XPS or TOF-SIMS. The ratio of the total equivalent content of interface species containing at least one of P, F and B in the positive electrode interface film to the equivalent content of lattice oxygen on the surface of the transition metal oxide is 0.16~0.90. Feature C1: The interface impedance Rint obtained by fitting the EIS equivalent circuit after standing at 25℃, 50% SOC for 2 hours is 8mΩ~42mΩ.

[0008] In an optional implementation, the lithium-ion battery also meets the following conditions: After storing fully charged finished battery cells at 60℃ for 7 days, headspace gas was collected. The ratio of the sum of the volume fractions of CO2 and CO in the gas to the sum of the volume fractions of CH4, C2H4, C2H6 and H2, Git, was 1.8~12.0. The interface stability coupling coefficient Kif of lithium-ion cells is 0.16~1.60. The formula for calculating Kif is: Kif=RSEI×RCEI×ln(1+Gint) / (Rint / 10); Low-temperature gas production stability conditions include: the lowest discharge voltage V at a constant current of 15A when discharging at -40℃ and 100% SOC. min The lithium-ion cell did not experience casing rupture due to gas generation inside the casing after 80 cycles at 60℃, 8A charging and 20A discharging conditions with a voltage not lower than 1.60V.

[0009] In an optional implementation, the RSEI is 0.90~2.10, preferably 1.05~1.65; The equivalent LiF content in RSEI was calculated by converting the LiF peak area in the range of 684.5 eV to 685.8 eV in the XPS F1s spectrum; the equivalent organic lithium salt content in RSEI was calculated by converting the corresponding peak areas of ROCO2Li, ROLi and carbonyl-containing organic lithium salts in the C1s and O1s spectra.

[0010] In an optional implementation, the RCEI is 0.24~0.72, preferably 0.32~0.58; At least one of the P-containing interface species, F-containing interface species, and B-containing interface species includes LiPxOyFz, LixPOy, LixBOy, BOF species, and LiF; RCEI is calculated based on the equivalent content after sensitivity factor correction of XPS spectral peaks on the surface of positive electrode active particles; TOF-SIMS depth profiling is used to confirm that the corresponding interface species are located in the interface layer on the surface of positive electrode active particles and to verify their distribution along the depth direction.

[0011] In an optional implementation, Rint is 12mΩ to 32mΩ, preferably 15mΩ to 26mΩ; Rint is obtained by fitting an equivalent circuit consisting of an ohmic internal resistance unit, a parallel unit of SEI film impedance and its constant phase element, a parallel unit of charge transfer impedance and its constant phase element, and a Warburg diffusion unit connected in series. Rint = Rsei + Rct, the EIS test frequency is 100kHz~10mHz, and the AC disturbance is 5mV. And / or, the Git is 2.5 to 8.5, preferably 3.2 to 6.5; Git is calculated from the volume fractions of CO2, CO, CH4, C2H4, C2H6 and H2, and the volume fraction of H2 in the headspace gas is not higher than 18%; And / or, Kif is 0.25~1.20, preferably 0.35~0.85.

[0012] In an optional embodiment, in TOF-SIMS analysis, the LiF secondary ion signal integrated area in the range of 0nm~80nm from the surface of the negative electrode particle accounts for 18%~48% of the secondary ion signal integrated area of ​​the lithium-containing interface species, and the LiF signal attenuation half-height depth from the surface to a depth of 80nm is 12nm~45nm. And / or, in TOF-SIMS analysis, the positive electrode interface film contains PO2. - PO3 - PF2 - BO2 - and LiF2 - The total signal forms a continuous interface signal layer on the surface of the positive electrode particle in the range of 0nm~60nm, and the thickness of the continuous interface signal layer is 8nm~55nm.

[0013] In an optional implementation, the minimum discharge voltage at a constant current of 10A under conditions of -40°C and 100% SOC is not less than 2.15V, and the discharge capacity at a constant current of 15A is not less than 4.20Ah. And / or, after storage at 60℃ and 100% SOC for 28 days, the volume expansion rate of the lithium-ion cell is no greater than 8.0%, the capacity recovery rate is no less than 90%, and the total headspace gas volume is no greater than 0.75 mL / Ah.

[0014] In an optional embodiment, the areal density of the positive electrode sheet on one side is 11.5 mg / cm³. 2 ~14.5mg / cm 2 The areal density of the negative electrode sheet on one side is 4.8 mg / cm³. 2 ~6.4mg / cm 2 ; And / or, the lithium-ion cell is a fully tabbed cylindrical lithium-ion cell, and the internal resistance of the lithium-ion cell at 25℃ and 30% SOC is 2.3mΩ~3.3mΩ.

[0015] Secondly, the present invention provides a battery comprising a lithium-ion cell according to any of the foregoing embodiments.

[0016] Thirdly, the present invention provides an electrical device including the battery of the aforementioned embodiments.

[0017] This invention has the following beneficial effects: By controlling the ratio of inorganic lithium salt to organic lithium salt in the negative electrode SEI through RSEI, this invention ensures that the SEI film has sufficient electron blocking capability without significantly hindering Li due to excessive LiF enrichment. + Migration improves polarization performance during low-temperature cold starts. This invention controls P-, F-, and B-containing species in the positive electrode CEI through RCEI, forming a more stable protective layer on the high-nickel positive electrode surface, reducing the risks of electrolyte oxidation, side reaction gas generation, and transition metal dissolution at high temperatures. This invention correlates interface composition, interface impedance, and gas composition through Rint, Gint, and Kif, avoiding the excessive interface impedance, low-temperature performance degradation, or abnormal gas generation ratios that can result from solely pursuing SEI inorganicization or CEI passivation. This invention, through a combined window of finished interface formation traces including negative electrode SEI, positive electrode CEI, interface impedance, and gas composition, enables the cell to possess both low-temperature cold start capability and high-temperature gas generation stability. Attached Figure Description

[0018] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0019] Figure 1 The schematic spectrum of the negative electrode F1s XPS (RSEI gradient) is shown. Figure 2 The schematic XPS spectrum of the negative electrode (organic lithium salt); Figure 3 This is a schematic XPS spectrum of the negative electrode O1s; Figure 4 The schematic spectrum of the positive electrode P2p XPS (RCEI gradient) is shown. Figure 5 This is a schematic diagram of the F1s XPS spectrum at the positive electrode. Figure 6 This is a schematic XPS spectrum of the positive electrode B1s; Figure 7 The negative electrode LiF2-TOF-SIMS depth distribution (RSEI gradient); Figure 8 The total signal depth distribution (RCEI gradient) for the positive electrode PO2- / PO3- / PF2- / BO2- / LiF2- is shown. Detailed Implementation

[0020] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0021] This invention provides a lithium-ion battery cell, specifically a high-nickel silicon-carbon cylindrical lithium-ion battery cell that synergistically combines interface formation traces with low-temperature gas generation stability. For example, it can be a 5Ah high-nickel positive / silicon-carbon negative cylindrical lithium-ion battery cell. This lithium-ion battery cell does not rely on formation process parameters that cannot be directly obtained from the finished product as product limitations. Instead, it achieves both low-temperature cold start capability and high-temperature gas generation stability through a combined window of finished product interface formation traces, such as the negative electrode SEI, positive electrode CEI, interface impedance, and gas composition.

[0022] The structure of a lithium-ion battery cell includes a cylindrical shell, a core housed within the cylindrical shell, and an electrolyte impregnating the core. The core includes a positive electrode, a negative electrode, and a separator disposed between the positive and negative electrode.

[0023] The positive electrode sheet includes a positive current collector and a positive active coating attached to the current collector. The positive active material in the positive active coating is a high-nickel layered lithium transition metal oxide. The molar percentage of nickel in the transition metal elements such as Ni, Co, Mn, and Al is 88% to 93%, such as 88%, 89%, 90%, 91%, 92%, 93%, or any value between these adjacent values. The type and content of other components in the positive active coating, such as conductive agents and binders, are not limited. The positive active material can be NCMA, NCM, or NCA type materials.

[0024] The negative electrode sheet includes a negative current collector and a negative active coating attached to the negative current collector. The negative active coating includes graphite materials and silicon-carbon materials. The silicon-carbon composite material can be silicon-carbon, silicon-suboxide composite material, porous silicon-carbon, or a combination thereof. The type and content of other components in the negative active coating, such as conductive agents and binders, are not limited.

[0025] The material of the separator is not limited; commonly used lithium-ion battery separators are all within the scope of protection of this invention.

[0026] The electrolyte contains lithium salts, carbonate solvents, and film-forming aids. The content of intact molecules or identifiable residues of the film-forming aids in the finished product residue is not limited; however, the SEI / CEI interface traces after formation are used as the product criterion for lithium-ion cells. Carbonate solvents can include ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC), etc. Film-forming aids can include vinylene carbonate (VC), fluoroethylene carbonate (FEC), ethylene ethylene carbonate (VEC), etc.

[0027] After formation and capacity testing, the battery cell exhibits detectable SEI / CEI interface formation traces in its finished product state. The lithium-ion battery cell provided in this embodiment of the invention simultaneously satisfies both the combined condition for interface formation traces and the low-temperature gas generation stability condition in its finished product state after formation and capacity testing. The combined condition for interface formation traces and the low-temperature gas generation stability condition are explained below: [Conditions for Interface Formation Traces] The conditions for interface formation traces are that the following conditions must be met simultaneously: (1) The ratio of the equivalent content of LiF to the equivalent content of organic lithium salt in the negative electrode interface film, RSEI, is 0.70~2.60, such as 0.70, 0.90, 1.05, 1.10, 1.20, 1.30, 1.40, 1.50, 1.60, 1.65, 1.80, 2.00, 2.10, 2.30, 2.60, etc., or any value between the above adjacent values. RSEI is preferably 0.90~2.10, more preferably 1.05~1.65. Specifically, "negative electrode interface film" is a solid or quasi-solid SEI reaction product layer that remains on the surface of the negative electrode active particles after the finished battery cell is disassembled and the free electrolyte is removed by light washing with dimethyl carbonate, and can be detected by XPS or TOF-SIMS. The ratio of the equivalent content of LiF to the equivalent content of organic lithium salt in the negative electrode interface film, RSEI, is 0.70~2.60.

[0028] The equivalent LiF content in RSEI was calculated by converting the LiF peak area in the range of 684.5 eV to 685.8 eV in the XPS F1s spectrum; the equivalent organic lithium salt content in RSEI was calculated by converting the corresponding peak areas of ROCO2Li, ROLi and carbonyl-containing organic lithium salts in the C1s and O1s spectra.

[0029] This invention controls the ratio of inorganic lithium salt to organic lithium salt in the negative electrode SEI through RSEI, so that the SEI film has sufficient electron blocking capability without significantly hindering Li due to excessive LiF enrichment. + Migration, thereby improving polarization performance during low-temperature cold starts.

[0030] (2) The ratio of the total equivalent content of at least one of P-type, F-type, and B-type interfacial species in the positive electrode interface film to the equivalent content of lattice oxygen on the surface of the transition metal oxide, RCEI, is 0.16 to 0.90. For example, it can be 0.16, 0.20, 0.24, 0.32, 0.40, 0.45, 0.50, 0.58, 0.65, 0.72, 0.90, etc., or any value between the above adjacent values. RCEI is preferably 0.24 to 0.72, and more preferably 0.32 to 0.58. Specifically, "positive electrode interface film" is a solid or quasi-solid CEI reaction product layer that remains on the surface of the positive electrode active particles after the finished battery cell has been disassembled and the free electrolyte has been removed by light washing with dimethyl carbonate, and can be detected by XPS or TOF-SIMS.

[0031] Specifically, at least one of the P-containing, F-containing, and B-containing interface species includes LiPxOyFz, LixPOy, LixBOy, BOF species, and LiF. RCEI is calculated based on the equivalent content of XPS peaks on the surface of the positive electrode active particles after sensitivity factor correction. TOF-SIMS depth profiling is used for interface layer localization and continuity verification: sputtering time is converted to depth using a standard SiO2 film, and the interface layer boundary is defined as the position where the combined signal of P-, F-, and B-containing secondary ions decays to 50% from its peak and the matrix metal oxide signal enters the stable region; the TOF-SIMS signal is not directly added to the XPS peak area.

[0032] This invention controls the P-, F-, and B-containing species in the cathode CEI through RCEI, thereby forming a more stable protective layer on the surface of the high-nickel cathode and reducing the risks of electrolyte oxidation, side reaction gas generation, and transition metal dissolution at high temperatures.

[0033] (3) The interface impedance Rint obtained by fitting the battery cell through the EIS equivalent circuit after it has been at 25℃, 50% SOC and left to stand for 2 hours is 8mΩ~42mΩ. For example, it can be 8mΩ, 10mΩ, 12mΩ, 15mΩ, 18mΩ, 20mΩ, 23mΩ, 26mΩ, 28mΩ, 32mΩ, 35mΩ, 38mΩ, 40mΩ, 42mΩ, etc., or any value between the above adjacent values. Rint is preferably 12mΩ~32mΩ, and more preferably 15mΩ~26mΩ.

[0034] Specifically, 50% SOC refers to the current remaining usable capacity of the battery cell being 50% of its rated full-charge capacity. Rint is obtained by fitting an equivalent circuit consisting of an ohmic internal resistance unit, a parallel unit of the SEI film impedance and its constant-phase element, a parallel unit of the charge transfer impedance and its constant-phase element, and a Warburg diffusion unit connected in series. Rint = Rsei + Rct, the EIS test frequency is 100kHz~10mHz, and the AC disturbance is 5mV. This equivalent circuit can be simplified as Rs - (Rsei / / CPEsei) - (Rct / / CPEct) - W, where Rs is the ohmic internal resistance, Rsei is the SEI film impedance, CPEsei is the constant-phase element corresponding to the SEI film, Rct is the charge transfer impedance, CPEct is the constant-phase element corresponding to the double layer, and W is the Warburg diffusion element. Nonlinear least squares fitting is used, and this fitting result is adopted when the normalized residual is no greater than 5%.

[0035] (4) After storing the fully charged finished battery cell at 60°C for 7 days, collect the headspace gas. The ratio of the sum of the volume fractions of CO2 and CO in the gas to the sum of the volume fractions of CH4, C2H4, C2H6 and H2, Gint, is 1.8 to 12.0. It can be 1.8, 2.0, 2.5, 3.2, 4.0, 4.8, 5.0, 6.0, 6.5, 7.0, 8.0, 8.5, 9.0, 10.0, 11.0, 12.0, etc., or any value between the above adjacent values. Gint is preferably 2.5 to 8.5, and more preferably 3.2 to 6.5. CH4, C2H4 and C2H6 are collectively referred to as low-carbon hydrocarbon gases.

[0036] Gint is calculated from the volume fractions of CO2, CO, CH4, C2H4, C2H6, and H2, and the volume fraction of H2 in the headspace gas is no higher than 18%, such as 18%, 15%, 10%, 5%, 3%, 1%, etc.

[0037] (5) The formula for calculating the interface stability coupling coefficient Kif of the lithium-ion battery cell is: RSEI×RCEI×ln(1+Gint) / (Rint / 10). The value range of Kif is 0.16~1.60, such as 0.16, 0.20, 0.25, 0.30, 0.35, 0.40, 0.50, 0.60, 0.70, 0.85, 1.00, 1.20, 1.40, 1.60, etc., or any value between the above adjacent values. Kif is preferably 0.25~1.20, and more preferably 0.35~0.85. Kif represents the coupling relationship between the above interface components, gas composition and interface impedance.

[0038] This invention correlates the interfacial components, interfacial impedance, and gas composition through Rint, Gint, and Kif, avoiding excessive interfacial impedance, decreased low-temperature performance, or abnormal gas production ratio caused by solely pursuing SEI inorganicization or CEI passivation.

[0039] [Low Temperature - Stable Gas Production Conditions] Low-temperature gas production stability conditions include: the lowest discharge voltage V at a constant current of 15A when discharging at -40℃ and 100% SOC. min The lithium-ion cell did not experience casing rupture due to gas generation inside the casing after 80 cycles at 60℃ and under conditions of 8A charging / 20A discharging, with a voltage not lower than 1.60V.

[0040] It should be noted that, by limiting RSEI to 0.70 to 2.60, RCEI to 0.16 to 0.90, Rint to 8 mΩ to 42 mΩ, Gint to 1.8 to 12.0, and ensuring Kif satisfies 0.16 to 1.60, this invention enables the formation of an SEI film on the negative electrode side that combines electron blocking and lithium-ion migration capabilities, and a CEI film on the positive electrode side that suppresses continuous electrolyte oxidation, while avoiding excessively high interface impedance leading to increased low-temperature polarization. Furthermore, this invention further defines the low-temperature gas generation stability window corresponding to the interface traces through the minimum low-temperature voltage and the shell integrity after high-temperature cycling.

[0041] In some embodiments, during TOF-SIMS depth profiling, the LiF secondary ion signal integrated area in the range of 0nm~80nm from the surface of the negative electrode particle to the secondary ion signal integrated area of ​​the lithium-containing interface species is 18%~48% (e.g., 18%, 25%, 33%, 40%, 48%, etc.), and the LiF signal attenuation half-height depth from the surface to a depth of 80nm is 12nm~45nm, e.g., 12nm, 20nm, 28nm, 36nm, 45nm, etc.

[0042] In some embodiments, the positive electrode interface film in TOF-SIMS depth profiling, PO2 - PO3 - PF2 - BO2 - and LiF2 - The total signal forms a continuous interface signal layer on the surface of the positive electrode particle in the range of 0nm~60nm, and the thickness of the continuous interface signal layer is 8nm~55nm, such as 8nm, 20nm, 32nm, 44nm, 55nm, etc., or any value between the above adjacent values.

[0043] In some embodiments, the minimum discharge voltage at a constant current of 10A under conditions of -40°C and 100% SOC is not less than 2.15V, and the discharge capacity at a constant current of 15A is not less than 4.20Ah. After storage at 60°C and 100% SOC for 28 days, the volume expansion rate of the lithium-ion cell is not greater than 8.0%, the capacity recovery rate is not less than 90%, and the total headspace volume is not greater than 0.75mL / Ah.

[0044] In some embodiments, the areal density of the positive electrode sheet on one side is 11.5 mg / cm³. 2 ~14.5mg / cm 2 For example, it can be 11.5 mg / cm³ 2 12.0 mg / cm 2 13.0 mg / cm 214.0 mg / cm 2 14.5 mg / cm 2 The areal density of the negative electrode sheet on one side is 4.8 mg / cm³. 2 ~6.4mg / cm 2 For example, it could be 4.8 mg / cm³ 2 5.2 mg / cm 2 5.6 mg / cm 2 6.0 mg / cm 2 6.4 mg / cm 2 wait.

[0045] Furthermore, the lithium-ion cell is a fully tabbed cylindrical lithium-ion cell, and the internal AC resistance of the lithium-ion cell at 25℃ and 30% SOC is 2.3mΩ~3.3mΩ, such as 2.3mΩ, 2.5mΩ, 2.8mΩ, 3.0mΩ, 3.3mΩ, etc.

[0046] This invention also provides a battery, including the lithium-ion battery cell provided in this invention. The form of the battery is not limited, and it can also be a battery module, battery pack, etc.

[0047] This invention also provides an electrical device, including the battery provided in this invention, which is used to supply power. The specific form of the electrical device is not limited.

[0048] This invention can obtain core parameters from finished battery cells in the same batch using conventional characterization methods such as XPS, TOF-SIMS, EIS, and GC / GC-MS, and has strong reverse detection capability and feasibility.

[0049] The features and performance of the present invention will be further described in detail below with reference to embodiments.

[0050] I. The testing process for each parameter in the following embodiments and comparative examples is as follows: (1) RSEI: RSEI is the ratio of the equivalent LiF content to the equivalent organic lithium salt content in the negative electrode interface film. The pretreated negative electrode sample was transferred to an XPS device in an inert atmosphere, and F1s, C1s, O1s, and Li1s spectra were acquired. The equivalent LiF content was obtained by correcting the LiF peak area in the F1s spectrum from 684.5 eV to 685.8 eV using a sensitivity factor; the equivalent organic lithium salt content was obtained by correcting the corresponding peak areas of ROCO2Li, ROLi, and carbonyl-containing organic lithium salts in the C1s and O1s spectra using a sensitivity factor. RSEI was calculated using the following formula: RSEI=C LiF / C org-Li Among them, C LiF For the equivalent content of LiF, Corg-Li This represents the equivalent content of organic lithium salts.

[0051] (2) RCEI: RCEI is the ratio of the total equivalent content of at least one of the P-containing, F-containing, and B-containing interfacial species in the cathode interfacial film to the equivalent content of lattice oxygen on the transition metal oxide surface. XPS testing was performed on the cathode sample. Shirley background was subtracted from the P2p, F1s, B1s, and O1s peaks, and peak fitting was performed and corrected according to the relative sensitivity factor. TOF-SIMS was used to confirm that the corresponding species were located in the interfacial layer and was not directly added to the XPS peak area. RCEI was calculated using the following formula: RCEI=(C P-interface +C F-interface +C B-interface ) / O lattice Among them, C P-interface C F-interface and C B-interface The equivalent contents of interfacial species containing P, F, and B are respectively, and O lattice It represents the equivalent content of lattice oxygen on the positive electrode surface.

[0052] (3) Rint: Rint is the interface impedance. The finished cell is adjusted to 50% SOC and left to stand for 2 hours at 25℃ before EIS testing. The frequency range is 100kHz to 10mHz, and the AC disturbance is 5mV. The equivalent circuit fitting is Rs-(Rsei / / CPEsei)-(Rct / / CPEct)-W, Rint=Rsei+Rct, and the unit is mΩ.

[0053] (4) Git: Git is the headspace gas ratio after high-temperature storage. After storing fully charged finished cells at 60℃ for 7 days, the headspace gas is collected by puncturing or disassembling under an inert atmosphere. The volume fractions of CO2, CO, CH4, C2H4, C2H6, and H2 are determined by GC or GC-MS and calculated using the following formula: Gint=(V CO2 +V CO ) / (V CH4 +V C2H4 +V C2H6 +V H2 ).

[0054] (5) Kif: Kif is the interface stability coupling coefficient, calculated by the following formula: Kif=RSEI×RCEI×ln(1+Gint) / (Rint / 10); Rint is expressed in mΩ; Kif is used to characterize the comprehensive matching relationship between the degree of inorganicization of the negative electrode SEI, the degree of protection of the positive electrode CEI, the composition of gas production, and the interfacial impedance.

[0055] (6) Lowest discharge voltage at low temperature V min After placing the fully charged battery cell in a -40℃ environment for 6 hours, discharge it at a constant current of 15A at -40℃ until the cutoff voltage or protection termination. Record the lowest voltage during the discharge process as V. min .

[0056] II. Preparation of Reference Materials, Electrodes, and Cells (1) Preparation of positive electrode slurry LiNi was selected 0.90 Co 0.05 Mn 0.04 Al 0.01 O2 is used as the positive electrode active material, in which nickel accounts for 90% of the molar proportion of the transition metal elements. Polyvinylidene fluoride is pre-dissolved in N-methylpyrrolidone, followed by pre-dispersion with conductive carbon black and carbon nanotube dispersions. Then, the high-nickel positive electrode active material is added, and the mixture is vacuum-stirred and degassed to obtain the positive electrode slurry. Based on a total mass of 100% for the positive electrode active material, conductive agent, and binder, the positive electrode active material accounts for 97.5% of the mass, the conductive agent accounts for 1.3%, and the binder accounts for 1.2%. The conductive agent consists of conductive carbon black and carbon nanotubes in a 3:1 mass ratio.

[0057] (2) Preparation of positive electrode sheet A 12μm thick aluminum current collector was selected, and the positive electrode slurry was coated on both sides of the aluminum current collector surface. After drying, rolling, and slitting, the positive electrode sheet was obtained. In Example 1, the areal density of the positive electrode on one side was 12.7 mg / cm³. 2 The positive electrode compaction density is 3.48 g / cm³. 3 The thickness of the positive electrode sheet is 87 μm. The discharge capacity of the positive electrode active material was approximately 201.2 mAh / g after 0.1C coin cell testing.

[0058] (3) Preparation of negative electrode slurry Artificial graphite and silicon carbide were selected as the negative electrode active materials. Sodium carboxymethyl cellulose was dissolved in deionized water, and Super P, artificial graphite, and silicon carbide were added and dispersed. Then, styrene-butadiene rubber emulsion was added, and the mixture was vacuum stirred and degassed to obtain the negative electrode slurry. Based on the total solid mass of the negative electrode slurry as 100%, the mass percentages of artificial graphite, silicon carbide, Super P, sodium carboxymethyl cellulose, and styrene-butadiene rubber were 67.9%, 29.1%, 1.0%, 0.8%, and 1.2%, respectively. The mass ratio of artificial graphite to silicon carbide was 7:3, the C / Si mass ratio of the silicon carbide was 5:4, and the lithium removal capacity of the negative electrode active material was 515 mAh / g.

[0059] (4) Preparation of negative electrode sheet A copper current collector with a thickness of 8 μm was selected. The negative electrode slurry was coated on both sides of the copper current collector surface. After drying, rolling, and slitting, the negative electrode sheet was obtained. In Example 1, the areal density of the negative electrode on one side was 5.46 mg / cm³. 2 The negative electrode compaction density is 1.53 g / cm³. 3 The thickness of the negative electrode sheet is approximately 87 μm.

[0060] (5) Preparation of diaphragm, electrolyte and core A single-sided ceramic-coated polyolefin separator was selected, with a total separator thickness of 11 μm. The electrolyte consisted of 1.0 mol / L LiPF6, EC, EMC, and DMC in a volume ratio of 2:5:3, as well as FEC, VC, LiPO2F2, and LiDFOB; based on the total mass of the electrolyte, the mass percentages of FEC, VC, LiPO2F2, and LiDFOB were 5.0%, 1.0%, 0.5%, and 0.5%, respectively. The positive electrode, separator, and negative electrode were wound into a cylindrical core with the negative electrode covering the positive electrode. The core was then installed in a cylindrical shell, connected to the current collector, and then grooved, injected with electrolyte, and sealed.

[0061] (6) Liquid injection, pre-formation, formation, venting and volume division After electrolyte injection, the cell was left to stand at 35°C for 24 hours to allow the electrolyte to fully wet the positive electrode, negative electrode, and separator pores. Pre-formation and formation were then performed. In Example 1, pre-formation used a low-current stage to form an initial SEI film on the negative electrode surface; subsequently, within a formation range that gradually increased the state of charge (SOC), a CEI film was formed on the positive electrode surface, and some initial side reaction gases were removed through aging, venting, and capacity testing.

[0062] It should be noted that the product of this invention is not limited by pre-formation current, formation temperature, resting time, or venting time; the above process is only used to illustrate the preparation method that can obtain the interface traces of the finished product of this invention. The finished battery cell is ultimately defined by detectable traces such as RSEI, RCEI, Rint, Gint, and Kif.

[0063] Example 1 Example 1 was prepared according to the above-described reference materials, electrode, and cell preparation methods. The finished cell was a 21700 approximately 5Ah high-nickel silicon-carbon all-tab cylindrical lithium-ion cell. Interface trace testing showed an RSEI of 1.30, an RCEI of 0.42, a Rint of 18mΩ, a Gint of 4.8, and a Kif of 0.53. Low-temperature testing showed a minimum discharge voltage of 1.95V at -40℃, 100% SOC, and 15A. After 80 cycles at 60℃ and 8A / 20A, no casing rupture due to internal gas generation occurred.

[0064] Example 2 The difference between this embodiment and Embodiment 1 is that the FEC mass ratio is reduced from 5.0% to 2.0%, the 0% to 10% SOC range is pre-formed at 0.02C and no 10% SOC holding voltage is set; the equivalent LiF content on the surface of the finished negative electrode is 18%, and the RSEI changes from 1.30 to 0.75; the rest is the same as in Embodiment 1.

[0065] Example 3 The difference between this embodiment and Embodiment 1 is that the FEC mass ratio is increased from 5.0% to 8.0%, the 0% to 20% SOC range is pre-formulated at 0.05C, and the voltage is maintained at 20% SOC for 120 minutes; the equivalent LiF content on the surface of the finished negative electrode is 44%, and the RSEI changes from 1.30 to 2.35; the rest is the same as in Embodiment 1.

[0066] Example 4 The difference between this embodiment and Embodiment 1 is that the mass percentages of LiPO2F2 and LiDFOB are reduced from 0.5% to 0.1%, and the 80% SOC holding voltage is eliminated; the total equivalent content of P, F and B interface species on the surface of the finished cathode is 0.18 times the equivalent content of lattice oxygen, and the RCEI changes from 0.42 to 0.18; everything else is the same as in Embodiment 1.

[0067] Example 5 The difference between this embodiment and Embodiment 1 is that the mass percentages of LiPO2F2 and LiDFOB are both increased from 0.5% to 1.0%, and the pressure is maintained at 80% SOC for 120 min; the total equivalent content of P, F and B interface species on the surface of the finished cathode is 0.82 times the equivalent content of lattice oxygen, and the RCEI changes from 0.42 to 0.82; everything else is the same as in Embodiment 1.

[0068] Example 6 The difference between this embodiment and Embodiment 1 is that the mass ratio of FEC is adjusted to 3.0%, and the mass ratios of LiPO2F2 and LiDFOB are both adjusted to 0.2%. After formation, the product is aged at 25°C for 24 hours. The Rint obtained by EIS fitting of the finished product changes from 18mΩ to 9mΩ. Everything else is the same as in Embodiment 1.

[0069] Example 7 The difference between this embodiment and Embodiment 1 is that the mass ratio of FEC is adjusted to 8.0%, and the mass ratios of LiPO2F2 and LiDFOB are both adjusted to 1.0%. After formation, the product is aged at 45°C for 72 hours. The Rint obtained by EIS fitting of the finished product changes from 18mΩ to 39mΩ. Everything else is the same as in Embodiment 1.

[0070] Example 8 The difference between this embodiment and Embodiment 1 is that the mass percentage of FEC is adjusted to 3.0%, the mass percentage of VC is adjusted to 2.0%, and after formation, it is aged at 45°C for 48 hours; after storage at 60°C for 7 days, the total volume fraction of CO2 and CO in the headspace gas is measured to be 42%, the total volume fraction of CH4, C2H4, C2H6 and H2 is 19%, and Gint is changed from 4.8 to 2.2; everything else is the same as in Embodiment 1.

[0071] Example 9 The difference between this embodiment and Embodiment 1 is that the mass ratios of FEC, LiPO2F2, and LiDFOB are adjusted to 6.0%, 0.7%, and 0.7%, respectively, and the pressure is maintained at 20% SOC and 80% SOC for 60 minutes. The measured RSEI, RCEI, Rint, and Gint of the finished product are 1.65, 0.58, 16 mΩ, and 6.3, respectively, and Kif changes from 0.53 to 1.19. Everything else is the same as in Embodiment 1.

[0072] The structure and interface parameters of each embodiment are summarized in Table 1: Table 1 Summary of structural and interface parameters for each embodiment

[0073] Comparative Example 1 The difference between this comparative example and Example 1 is that the FEC mass ratio is reduced to 0.5%, and the 0% to 10% SOC range is pre-formed at 0.1C without voltage holding; the equivalent LiF content on the surface of the finished negative electrode is 10%, and the RSEI changes from 1.30 to 0.42; the rest is the same as Example 1.

[0074] Comparative Example 2 The difference between this comparative example and Example 1 is that the FEC mass ratio is increased to 12.0%, the 0% to 20% SOC range is pre-formulated at 0.03C, and the voltage is maintained at 20% SOC for 180 min; the equivalent LiF content on the surface of the finished negative electrode is 58%, and the RSEI changes from 1.30 to 3.10; the rest is the same as Example 1.

[0075] Comparative Example 3 The difference between this comparative example and Example 1 is that LiPO2F2 and LiDFOB are not added, and the 80% SOC holding pressure is cancelled; the RCEI of the finished product is changed from 0.42 to 0.08; otherwise, it is the same as Example 1.

[0076] Comparative Example 4 The difference between this comparative example and Example 1 is that the mass percentage of FEC was reduced to 1.0%, the mass percentage of VC was increased to 3.0%, and the mixture was aged at 45°C for 72 hours after formation. After storage at 60°C for 7 days, the total volume fraction of H2 and low-carbon hydrocarbon gases was measured to be 48%, the total volume fraction of CO2 and CO was 38%, and Gint was changed from 4.8 to 0.79. Other aspects are the same as in Example 1.

[0077] Comparative Example 5 The difference between this comparative example and Example 1 is that the mass percentage of FEC is increased to 12.0%, and the mass percentages of LiPO2F2 and LiDFOB are both increased to 1.5%, and the product is aged at 45°C for 120 hours; the Rint obtained by EIS fitting of the finished product changes from 18mΩ to 58mΩ; everything else is the same as in Example 1.

[0078] Comparative Example 6 The difference between this comparative example and Example 1 is that the mass ratios of FEC, LiPO2F2, and LiDFOB were adjusted to 1.0%, 0.1%, and 0.1%, respectively. The product was pre-formulated at 0.1°C and aged at 45°C for 96 hours. The measured values ​​of the finished product were RSEI 0.55, RCEI 0.12, Rint 45mΩ, Gint 1.1, and Kif changed from 0.53 to 0.01. The rest were the same as in Example 1.

[0079] Comparative Example 7 The difference between this comparative example and Example 1 is that the mass ratio of LiPO2F2 and LiDFOB is increased to 1.8%, and the pressure is maintained at 80% SOC for 180 min; the RCEI of the finished product is 1.05, and the rest is the same as in Example 1.

[0080] Comparative Example 8 The difference between this comparative example and Example 1 is that FEC, LiPO2F2 and LiDFOB are not added, rapid pre-formulation at 0.2C is used and no SOC holding pressure is set; the finished product is fitted by EIS and the Rint is 6mΩ, and other aspects are the same as in Example 1.

[0081] Comparative Example 9 The difference between this comparative example and Example 1 is that the mass percentage of LiPO2F2 was increased to 1.5%, the mass percentage of FEC was reduced to 1.0%, and the sample was aged at 45°C for 96 hours under full charge. After storage at 60°C for 7 days, the Gint value was measured to be 14.0. Other aspects are the same as in Example 1.

[0082] Comparative Example 10 The difference between this comparative example and Example 1 is that the mass ratios of FEC, LiPO2F2, and LiDFOB were adjusted to 8.0%, 1.2%, and 1.2%, respectively, and the pressure was maintained at 20% SOC and 80% SOC for 120 min. The measured RSEI, RCEI, Rint, and Gint of the finished product were 2.60, 0.90, 16 mΩ, and 2.6, respectively. The Kif value was calculated to be 1.87 according to the formula. Other parameters were the same as in Example 1.

[0083] The values ​​of each proportional variable are shown in Table 2: Table 2 Values ​​of each proportional variable

[0084] Performance tests were conducted on each embodiment and comparative example, and the test methods are as follows: (1) XPS test SEI / CEI composition The finished battery cell was discharged to 2.5V to 3.0V and left to stand for 2 hours. It was then disassembled in an Ar glove box where H2O and O2 were both no higher than 1ppm. Samples from the rolled-up areas of the negative and positive electrodes were taken and gently washed with DMC for 10 to 30 seconds to remove free electrolyte. The samples were then vacuum dried in the transition chamber of the glove box for 30 minutes. The samples were transferred to the XPS equipment using a sealed transfer device to avoid air exposure. The XPS test used Al Kα rays with a test area of ​​no less than 200μm×200μm. Li1s, C1s, O1s, F1s, P2p, B1s and Ni2p spectra were collected. The F1s, C1s, O1s, P2p and B1s peaks were subjected to Shirley background subtraction and peak separation fitting. RSEI and RCEI were calculated after correction by sensitivity factor. (2) TOF-SIMS in-depth analysis TOF-SIMS in-depth profiling was performed on the same batch of positive and negative electrode interface samples. Samples were transferred under low temperature and inert atmosphere before testing. LiF2 was monitored in the negative electrode sample. - F - CH3OCO2 - ROCO2Li-related fragments and SiO- signals; monitoring PO2 in cathode samples - PO3 - PF2 - BO2 - LiF2 - NiO - and MnO - Signal. Sputtering depth was calibrated using a standard SiO2 film. Negative electrode profiling depths ranged from 0 nm to 120 nm, and positive electrode profiling depths ranged from 0 nm to 100 nm. Interface signal layer thickness, integral area ratio, and half-height depth were calculated.

[0085] (3) EIS interface impedance fitting The finished battery cells were charged or discharged at 0.5C at 25℃ to adjust to 50% SOC, and then allowed to stand for 2 hours before EIS testing. The test frequency was 100kHz to 10mHz, and the AC disturbance was 5mV. An equivalent circuit fitting was used: Rs-(Rsei / / CPEsei)-(Rct / / CPEct)-W, where Rint=Rsei+Rct. If the fitting residual of samples in the same group is greater than 5%, the test should be repeated or samples with abnormal contact should be removed.

[0086] (4) Headspace gas GC / GC-MS detection Fully charged finished battery cells were stored at 60°C for 7 days, then cooled to 25°C and transferred to an inert atmosphere device. Headspace gas inside the casing was collected using either sealed puncture sampling or sealed disassembly sampling. H2, CO, and CO2 were detected using GC-TCD, and CH4, C2H4, and C2H6 were detected using GC-FID or GC-MS. Calibration curves were established using standard gases, and the volume fraction of each gas was calculated according to Gint=(V CO2 +V CO ) / (V CH4 +V C2H4 +V C2H6 +V H2 Calculate Gint.

[0087] (5) Low temperature DCR and cold start test The finished battery cells were charged to 100% SOC and left to stand at -40℃ for 6 hours. First, they were discharged at a constant current of 10A to a predetermined time or cutoff voltage, and the lowest voltage, capacity, and temperature rise were recorded. After returning to 100% SOC, they were discharged again at a constant current of 15A, and the lowest discharge voltage V was recorded. min Discharge capacity. Low-temperature DCR tests were conducted at -20℃, -15℃, -10℃, 0℃, and 25℃, with the cells left to stand for at least 4 hours at each temperature. The DCR was calculated using the 10s pulse current method. All samples used the same fixture, the same sampling frequency, and the same cutoff voltage.

[0088] (6) High-temperature storage and high-temperature circulating gas generation test In the high-temperature storage test, fully charged finished battery cells were stored in a 60℃ environment for 7, 14, and 28 days, and their mass, dimensions, open-circuit voltage, volume expansion rate, capacity retention rate, capacity recovery rate, and headspace gas composition were recorded. In the high-temperature cycling test, the finished battery cells were cycled at 60℃ with 8A charging and 20A discharging for 80 cycles, and the cycle capacity retention rate, casing condition, and whether casing rupture or significant pressure leakage occurred were recorded. After the test, the gas composition was determined according to the headspace gas detection method.

[0089] (7) Calculation formula RSEI=C LiF / C org-Li.

[0090] RCEI=(C P-interface +C F-interface +C B-interface ) / O lattice .

[0091] Rint = Rsei + Rct.

[0092] Gint=(V CO2 +V CO ) / (V CH4 +V C2H4 +V C2H6 +V H2 ).

[0093] Kif=RSEI×RCEI×ln(1+Gint) / (Rint / 10).

[0094] (8) The test conditions are fixed as shown in Table 3: Table 3 Test conditions for each parameter

[0095] The test results of each embodiment and comparative example are as follows: Figures 1-8 As shown in Table 4: Figure 1 The schematic spectrum of the negative electrode F1s XPS (RSEI gradient) is shown. Figure 2 The schematic XPS spectrum of the negative electrode (organic lithium salt); Figure 3 This is a schematic XPS spectrum of the negative electrode O1s; Figure 4 The schematic spectrum of the positive electrode P2p XPS (RCEI gradient) is shown. Figure 5 This is a schematic diagram of the F1s XPS spectrum at the positive electrode. Figure 6 This is a schematic XPS spectrum of the positive electrode B1s; Figure 7 The negative electrode LiF2-TOF-SIMS depth distribution (RSEI gradient); Figure 8 The total signal depth distribution (RCEI gradient) for the positive electrode PO2- / PO3- / PF2- / BO2- / LiF2- is shown.

[0096] Table 4 Performance test results of each embodiment and comparative example

[0097] To demonstrate the existence and quantification of the interface species corresponding to features A1, B1, and Gint as defined in this invention, eight typical samples from Examples 1 to 5 and Comparative Examples 1 to 3 were selected from the examples and comparative examples. XPS peak fitting and TOF-SIMS depth analysis were performed on the negative and positive electrode interface samples from the same batch. Each spectral peak was fitted after Shirley background subtraction and charge correction using C1s 284.8 eV, and quantified according to the relative sensitivity factor. P-containing, F-containing, and B-containing interface species were assigned according to their principal elements. LiPxOyFz was included in the CP-interface, and F was not repeatedly included in the CF-interface; the same species was not repeatedly included. The TOF-SIMS sputtering depth was calibrated using a standard SiO2 film. The interface layer boundary was determined by the position where the combined signal of P-, F-, and B-containing secondary ions decayed from its peak to 50% and the matrix metal oxide signal entered the stable region.

[0098] The XPS peak assignments, substance identification criteria, and quantitative results of Example 1 for typical samples are shown in Table 5.

[0099] Table 5. XPS peak assignments of typical samples and quantitative results from Example 1.

[0100] As shown in Table 5, LiF in the negative electrode interface film corresponds to a single component in the F1s spectrum from 684.5 eV to 685.8 eV, which can be separately fitted with fluorine-containing inorganic interface species such as LiPOxFy at F1s 686.8 eV and PVDF binder at F1s 688.2 eV; the organic lithium salts correspond to ROCO2Li at 289.0 eV, carbonyl-containing organic lithium salts at 288.3 eV, and ROLi at 286.5 eV in the C1s spectrum. The three can be integrated separately and the corresponding oxygen-containing groups can be found in the O1s spectrum. The fluorine-containing interfacial species such as LiPxOyFz, LixPOy, LiF, and LiPFxOy in the positive electrode interface film, as well as LixBOy and BOF, correspond to P2p 133.6 eV, P2p 134.5 eV, F1s 685.2 eV, F1s 686.5 eV, B1s 192.1 eV, and B1s 193.0 eV, respectively. Together with the lattice oxygen on the surface of the transition metal oxide (O1s 529.2 eV), they form the basis for RCEI calculations. Therefore, it can be confirmed that the interfacial species in features A1 and B1 defined in this invention are specific substances that can be identified and quantified.

[0101] The XPS quantitative results of 8 typical samples are shown in Table 6, and the TOF-SIMS depth analysis results are shown in Table 7.

[0102] Table 6. XPS Quantitative Results of Typical Samples

[0103] Table 7. TOF-SIMS depth profiling results of typical samples

[0104] As shown in Tables 6 and 7, the RSEI of Examples 1 to 5 ranges from 0.75 to 2.35, and the RCEI ranges from 0.18 to 0.82, all falling within the range of 0.70 to 2.60 for characteristic A1 and 0.16 to 0.90 for characteristic B1. The LiF secondary ion signal integrated area ratio of the negative electrode interface film in the range of 0 nm to 80 nm is 22.5% to 44.0%, and the LiF signal attenuation half-height depth is 18 nm to 40 nm. The PO2 in the positive electrode interface film... - PO3 - PF2 - BO2 - and LiF2 - The total signal formation resulted in a continuous interface signal layer with a thickness ranging from 14 nm to 48 nm, all falling within the scope defined by this invention. The LiF secondary ion signal integral area ratio and attenuation half-height depth of Comparative Examples 1 and 2 were below the lower limit and above the upper limit, respectively, while Comparative Example 3 did not form a continuous interface signal layer, all falling outside the scope defined by this invention. These results demonstrate that the interface species corresponding to each characterization limitation exist, can be quantified, and their boundaries are necessary.

[0105] The XPS peak assignments and TOF-SIMS in-depth analysis data mentioned above can be obtained from the same batch of finished cells and can be used to verify the limited content of this invention.

[0106] Data Analysis: (1) Single-factor influence of RSEI Comparing Examples 1 to 3 with Comparative Examples 1 and 2, it can be seen that RSEI is used to limit the balance between inorganic components such as LiF and organic lithium salt components in the negative electrode SEI. When RSEI is low to 0.42, the equivalent LiF content on the negative electrode surface is insufficient, the electron blocking ability of the SEI film decreases, and silicon carbon particles are still prone to continuous electrolyte reduction under low temperature and high SOC conditions, resulting in increased interfacial polarization during low-temperature discharge and the generation of more reducing gases during high-temperature storage or cycling. This is manifested in Comparative Example 1, where the minimum voltage at -40℃ and 15A drops to 1.54V, and the total headspace gas volume increases to 0.95mL / Ah. Conversely, when RSEI is high to 3.10, the LiF enrichment layer is too thick or too dense. Although electron blocking is enhanced, Li... +The increased energy barrier across the SEI leads to a significant rise in interfacial impedance, resulting in a rapid voltage drop during cold start at low temperatures. Therefore, limiting the RSEI to 0.70 to 2.60, especially 0.90 to 2.10, can suppress side reactions and maintain Li... + A balance must be struck between migrations.

[0107] (2) Single-factor effects of RCEI Comparing Examples 1, 4, and 5 with Comparative Example 3, it can be seen that RCEI is used to limit the protection level of P-, F-, and B-containing interface species in the CEI on the surface of high-nickel cathode particles. High-nickel cathodes exhibit strong oxidation activity at high SOC and high temperatures. If the RCEI is only 0.08, it indicates insufficient formation of P / F / B interface species on the cathode surface. The CEI's ability to inhibit lattice oxygen release, electrolyte oxidation, and transition metal dissolution is weak. During high-temperature storage, the increase in CO2, CO, and other side reaction gases further promotes the increase in interfacial impedance and a decrease in capacity recovery. If the RCEI is in the range of 0.16 to 0.90, P-, F-, and B-containing interface species can form a continuous but not excessively thick passivation layer on the cathode particle surface, reducing continuous electrolyte oxidation while avoiding excessive coverage that would hinder charge transfer. Examples 4 and 5 correspond to low and high RCEI boundaries, respectively, yet the shell remains intact and exhibits acceptable low-temperature performance, indicating that this range can balance high-temperature gas generation stability and low-temperature polarization control.

[0108] (3) Single-factor influence of Rint Comparing Examples 1, 6, and 7 with Comparative Example 5, it can be seen that Rint reflects the interfacial charge transfer and film impedance level after the combined action of the negative electrode SEI and the positive electrode CEI. A low Rint may indicate an insufficient interfacial film or defects in the local protective layer. Although the impedance is low at low temperatures in the short term, side reactions continue to occur during long-term storage or cycling at high temperatures, increasing the risk of gas generation. A high Rint indicates that the SEI or CEI is too thick or too dense, and the Li... + The migration path within the interfacial film becomes longer, limiting diffusion and charge transfer at low temperatures, and significantly reducing the minimum voltage during cold start. In Comparative Example 5, with Rint increased to 58 mΩ, the minimum voltage at -40°C and 15A was only 1.30 V, indicating that simply enhancing the interfacial film does not achieve comprehensive performance. Limiting Rint to 8 mΩ to 42 mΩ, preferably 12 mΩ to 32 mΩ, allows the interfacial film to provide sufficient protection without significantly sacrificing low-temperature ion transport and charge transfer kinetics.

[0109] (4) Single-factor influence of Gint Comparing Examples 1 and 8 with Comparative Example 4, it can be seen that Git is used to characterize the degree to which the gas composition shifts from a relatively mild CO2 / CO combination to an abnormal gas production direction of H2 and low-carbon hydrocarbons after high-temperature storage. CO2 and CO are usually related to the oxidation of the positive electrode surface, the decomposition of electrolyte carbonates, and the reforming of the interfacial film; an abnormally high proportion of H2 and low-carbon hydrocarbons often indicates that the reduction side reactions, water trace side reactions, or the continuous rupture and regeneration of SEI on the negative electrode side are more serious. In Comparative Example 4, Git decreased to 0.79, indicating that the proportion of H2 and low-carbon hydrocarbons was too high, the total headspace gas volume increased to 1.05 mL / Ah, and obvious gas expansion occurred. In Example 8, Git was 2.2, which is still within the scope of this invention, indicating that although the gas composition is close to the lower limit, it does not show abnormal reduction gas production as the main factor. Limiting Git to 1.8 to 12.0, especially 2.5 to 8.5, is beneficial to exclude the interfacial instability state of abnormal gas production composition and to characterize the stability of the interface after formation together with RSEI and RCEI.

[0110] (5) Single-factor influence of Kif Comparing Examples 1 and 9 with Comparative Example 6, it can be seen that Kif does not evaluate the content of a single interfacial species in isolation, but rather couples the inorganic / organic balance of the negative electrode SEI, the degree of protection of the positive electrode CEI, gas composition, and interfacial impedance. If only RSEI is adequate but RCEI is insufficient, high-temperature positive electrode side reactions will still cause gas production; if both RSEI and RCEI are high but Rint is too large, low-temperature Li + Migration is hindered, and the cold start voltage decreases. If Gint is abnormally low, it indicates a shift in the interfacial gas side reaction path, which also fails to reflect a stable interface. In Comparative Example 6, deviations in multiple interfacial parameter combinations caused Kif to drop to 0.01, manifested as a decrease in the minimum low-temperature voltage, an increase in the total headspace gas volume, and shell depressurization. In Example 9, Kif was 1.19, and RSEI, RCEI, Rint, and Gint remained within their respective acceptable ranges, maintaining good low-temperature and gas production performance. Therefore, limiting Kif to 0.16 to 1.60 can avoid the problem of seemingly acceptable individual parameters leading to an overall unbalanced interfacial state, thus improving the ability of this invention to characterize the stability of the actual finished product interface.

[0111] Comparative Examples 7 to 10 cover cases of excessively high RCEI, excessively low Rint, excessively high Gint, and Kif exceeding 1.60, respectively. Excessively high RCEI leads to interfacial layer thickening and increased low-temperature polarization; excessively low Rint reflects insufficient film formation, resulting in continued side reactions and pressure relief at high temperatures; excessively high Gint indicates an abnormally high proportion of oxidative decomposition gases; and excessively high Kif corresponds to a mismatch between interfacial composition, impedance, and gas composition. These results, along with the lower-side comparative examples for each parameter, illustrate the upper and lower boundaries of the simultaneous window.

[0112] The method for detecting various parameters of lithium-ion battery products provided in this embodiment of the invention: (1) Initial record and performance retest of complete battery cell Take a finished cylindrical lithium-ion cell of unknown origin and record its appearance, dimensions, weight, open-circuit voltage, terminal structure, and nominal information. Perform a 0.2C capacity test on the cell at 25°C to confirm its capacity plateau; adjust the cell to 30% SOC to test its AC internal resistance, and adjust it to 50% SOC for EIS testing; perform a -40°C cold start test on another cell from the same batch or the same cell after recovery. If the sample quantity is limited, prioritize reserving one cell for disassembly and characterization, and use the other cell from the same batch for retesting its low-temperature and high-temperature gas generation performance.

[0113] (2) SOC protection, pretreatment and inert disassembly For interface characterization, the battery cell is preferably discharged to 2.5V to 3.0V and allowed to stand for 2 hours to reduce disassembly risks and minimize further interfacial reactions. The cell is then transferred to an Ar glove box, where both H2O and O2 concentrations are no higher than 1 ppm. After opening the casing, the core is removed, and the positions of the positive and negative terminals, the beginning of the roll, the middle of the roll, and the end of the roll are marked. The positive and negative electrode plates from the middle of the roll are taken as interface samples, avoiding areas with obvious mechanical damage, welding heat effects, or electrode edge contamination.

[0114] (3) Sample classification and preservation Negative electrode samples were categorized into three types: Type A (original interface sample), Type B (lightly washed interface sample), and Type C (powder verification sample). Type A samples were not washed and were used for TOF-SIMS in-depth analysis; Type B samples were lightly washed with DMC for 10 to 30 seconds and vacuum dried for XPS quantification; Type C samples had powder scraped off and were used for SEM / EDS and auxiliary material identification. Positive electrode samples were similarly categorized into Types A, B, and C. Headspace gas samples were collected using sealed puncture or closed disassembly methods and transferred to airtight syringes or gas bags for GC / GC-MS analysis. Residual liquid samples could be stored separately but were not used for calculating the core parameters exclusive to this case.

[0115] (4) RSEI detection and calculation XPS analysis was performed on the negative electrode type B interface sample, and Li1s, C1s, O1s, and F1s spectra were acquired. The C1s concentration was calculated using the LiF characteristic peak in the F1s region. LiF C was calculated using the characteristic peaks of ROCO2Li, ROLi, and carbonyl-containing organolithium salts in C1s and O1s. org-Li Press RSEI=C LiF / C org-Li Calculations were performed. TOF-SIMS in-depth profiling was conducted on the negative electrode type A sample to verify LiF2. - The distribution of organic lithium salt-related fragments in the range of 0 nm to 80 nm was studied to rule out false positives caused by surface contamination or over-cleaning.

[0116] (5) RCEI detection and calculation XPS analysis was performed on the cathode type B interface sample, acquiring O1s, F1s, P2p, B1s, Ni2p, Co2p, and Mn2p spectra. The equivalent contents of P-, F-, and B-containing interface species were obtained through peak separation, and the relative crystalline oxygen content (RCEI) was calculated using the equivalent surface lattice oxygen content as the denominator. TOF-SIMS depth profiling was performed on the cathode type A sample to confirm PO2 content. - PO3 - PF2 - BO2 - and LiF2 - Whether a continuous interface signal layer is formed in the range of 0nm to 60nm.

[0117] (6) Rint detection and calculation Finished cells from the same batch were adjusted to 50% SOC at 25℃ and left to stand for 2 hours before EIS testing. The test frequency was 100kHz to 10mHz, with an AC disturbance of 5mV. An equivalent circuit fitting was used: Rs-(Rsei / / CPEsei)-(Rct / / CPEct)-W, where Rint=Rsei+Rct. If only a single cell before disassembly can be tested for EIS, the EIS test should be completed first before disassembly and sampling.

[0118] (7) Gint detection and calculation Fully charged finished battery cells from the same batch were stored at 60℃ for 7 days, then cooled to 25℃ before headspace gas was collected in a sealed device. The volume fractions of CO2, CO, CH4, C2H4, C2H6, and H2 were measured using GC-TCD and GC-FID or GC-MS, respectively, and calculated according to Gint=(V CO2 +V CO ) / (V CH4 +V C2H4 +V C2H6 +V H2 ) Calculation. If the total headspace gas volume is too low, it should be diluted with a known volume of inert gas and a blank correction should be performed.

[0119] (8) Kif calculation and combination determination Substitute the aforementioned RSEI, RCEI, Rint, and Gint into Kif = RSEI × RCEI × ln(1 + Gint) / (Rint / 10) to calculate Kif. If the tested product simultaneously satisfies RSEI of 0.70 to 2.60, RCEI of 0.16 to 0.90, Rint of 8 mΩ to 42 mΩ, Gint of 1.8 to 12.0, and Kif of 0.16 to 1.60, and meets the minimum discharge voltage at low temperature and the stable gas production conditions at high temperature, then it can be preliminarily determined that it meets the limitations of this invention.

[0120] This invention provides a high-nickel silicon-carbon cylindrical lithium-ion battery cell that synergistically combines interface formation traces with low-temperature gas generation stability. The cell comprises a high-nickel positive electrode, a silicon-carbon negative electrode, a separator, an electrolyte, and a cylindrical shell. In its finished state after formation and capacity testing, it satisfies a combined window of the following parameters: LiF / organic lithium salt ratio (RSEI) in the negative electrode SEI, P / F / B interfacial species ratio (RCEI) in the positive electrode CEI, interfacial impedance (Rint), headspace gas ratio (Gint), and interfacial stability coupling coefficient (Kif). It also satisfies low-temperature cold start and high-temperature gas generation stability conditions. This invention does not use formation current, formation temperature, or settling time—which cannot be directly obtained from the finished product—as core product limitations. Instead, it characterizes the effective interfacial state after formation using interface traces detectable by XPS, TOF-SIMS, EIS, and GC / GC-MS, thereby improving the low-temperature polarization, interfacial side reactions, and high-temperature gas generation stability of the high-nickel silicon-carbon cylindrical battery cell, and facilitating identification from unknown finished cells.

[0121] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A lithium-ion battery cell, characterized in that, The device includes a cylindrical shell, a core housed within the cylindrical shell, and an electrolyte impregnating the core. The core includes a positive electrode, a negative electrode, and a separator disposed between the positive and negative electrode. The positive electrode includes a high-nickel layered lithium transition metal oxide with a nickel molar ratio of 88% to 93% in the transition metal elements. The negative electrode includes graphite material and silicon-carbon material. The lithium-ion battery cell, after formation and capacity testing, meets the conditions for interface formation traces and low-temperature gas generation stability. The conditions for the formation of traces at the interface include features A1 to C1: Feature A1: The negative electrode interface film is a SEI reaction product layer that remains on the surface of the negative electrode active particles after the finished battery cell has been disassembled and treated with dimethyl carbonate to remove the free electrolyte, and can be detected by XPS or TOF-SIMS. The ratio of the equivalent content of LiF to the equivalent content of organic lithium salt in the negative electrode interface film, RSEI, is 0.70~2.

60. Feature B1: The positive electrode interface film is a CEI reaction product layer that remains on the surface of the positive electrode active particles after the finished battery cell has been disassembled and treated with dimethyl carbonate to remove the free electrolyte, and can be detected by XPS or TOF-SIMS. The ratio of the total equivalent content of interface species containing at least one of P, F and B in the positive electrode interface film to the equivalent content of lattice oxygen on the surface of the transition metal oxide, RCEI, is 0.16~0.

90. Feature C1: The interface impedance Rint obtained by fitting the EIS equivalent circuit after standing at 25℃, 50% SOC for 2 hours is 8mΩ~42mΩ.

2. The lithium-ion battery cell according to claim 1, characterized in that, Lithium-ion batteries also meet the following conditions: After storing fully charged finished battery cells at 60℃ for 7 days, headspace gas was collected. The ratio of the sum of the volume fractions of CO2 and CO in the gas to the sum of the volume fractions of CH4, C2H4, C2H6 and H2, Git, was 1.8~12.

0. The interface stability coupling coefficient Kif of the lithium-ion battery cell is 0.16~1.

60. The formula for calculating Kif is: Kif=RSEI×RCEI×ln(1+Gint) / (Rint / 10); The low-temperature gas production stability conditions include: the lowest discharge voltage V when discharging at a constant current of 15A under conditions of -40℃ and 100% SOC. min The lithium-ion cell does not experience casing rupture due to gas generation inside the casing after 80 cycles at 60°C, under conditions of not less than 1.60V and charging at 8A and discharging at 20A, with a voltage not lower than 1.60V.

3. The lithium-ion battery cell according to claim 1, characterized in that, The RSEI is 0.90~2.10, preferably 1.05~1.65; The equivalent LiF content in RSEI was calculated by converting the LiF peak area in the range of 684.5 eV to 685.8 eV in the XPS F1s spectrum; the equivalent organic lithium salt content in RSEI was calculated by converting the corresponding peak areas of ROCO2Li, ROLi and carbonyl-containing organic lithium salts in the C1s and O1s spectra.

4. The lithium-ion battery cell according to claim 1, characterized in that, The RCEI is 0.24~0.72, preferably 0.32~0.58; At least one of the P-containing interface species, F-containing interface species, and B-containing interface species includes LiPxOyFz, LixPOy, LixBOy, BOF species, and LiF; the RCEI is calculated based on the equivalent content after the XPS spectrum peaks on the surface of the positive electrode active particles are corrected by the sensitivity factor; TOF-SIMS depth profiling is used to confirm that the corresponding interface species are located in the interface layer on the surface of the positive electrode active particles and to verify their distribution along the depth direction.

5. The lithium-ion battery cell according to claim 1, characterized in that, Rint is 12mΩ~32mΩ, preferably 15mΩ~26mΩ; Rint is obtained by equivalent circuit fitting, where Rint=Rsei+Rct, the EIS test frequency is 100kHz~10mHz, and the AC disturbance is 5mV. And / or, the Gint is 2.5~8.5, preferably 3.2~6.5; the Gint is calculated from the volume fractions of CO2, CO, CH4, C2H4, C2H6 and H2, and the volume fraction of H2 in the headspace gas is not higher than 18%; And / or, Kif is 0.25~1.20, preferably 0.35~0.

85.

6. The lithium-ion battery cell according to claim 1, characterized in that, In TOF-SIMS analysis, the LiF secondary ion signal integrated area in the range of 0nm~80nm from the surface of the negative electrode particles accounts for 18%~48% of the secondary ion signal integrated area of ​​the lithium-containing interface species, and the LiF signal attenuation half-height depth from the surface to a depth of 80nm is 12nm~45nm. And / or, in TOF-SIMS analysis, the positive electrode interface film contains PO2 - PO3 - PF2 - BO2 - and LiF2 - The total signal forms a continuous interface signal layer on the surface of the positive electrode particle in the range of 0nm~60nm, and the thickness of the continuous interface signal layer is 8nm~55nm.

7. The lithium-ion battery cell according to claim 1, characterized in that, The minimum discharge voltage at 10A constant current discharge under -40℃ and 100% SOC conditions is not less than 2.15V, and the discharge capacity at 15A constant current discharge is not less than 4.20Ah. And / or, after storage at 60°C and 100% SOC for 28 days, the volume expansion rate of the lithium-ion cell is not greater than 8.0%, the capacity recovery rate is not less than 90%, and the total headspace gas volume is not greater than 0.75 mL / Ah.

8. The lithium-ion battery cell according to claim 1, characterized in that, The areal density of the positive electrode sheet is 11.5 mg / cm³. 2 ~14.5mg / cm 2 The areal density of the negative electrode sheet on one side is 4.8 mg / cm³. 2 ~6.4mg / cm 2 ; And / or, the lithium-ion cell is a full-tab cylindrical lithium-ion cell, and the internal resistance of the lithium-ion cell at 25°C and 30% SOC is 2.3mΩ~3.3mΩ.

9. A battery, characterized in that, The lithium-ion battery cell includes any one of claims 1 to 8.

10. An electrical appliance, characterized in that, Includes the battery as described in claim 9.