Lithium-ion battery separators, preparation methods and applications

By introducing a blend of polyethylene and polybutene into the lithium battery separator, the grain boundary distribution and stress transmission path are optimized, solving the problems of high pore temperature and insufficient needle penetration strength in the early stage of thermal runaway of the lithium battery separator, and achieving faster safety response and higher mechanical stability.

CN123121069APending Publication Date: 2026-11-17LIYANG YUEQUAN ELECTRIC ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611365424.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-04
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium battery separators have high pore-closing temperatures in the early stages of thermal runaway, making it difficult to respond quickly and cut off ion conduction. They also lack sufficient needle penetration strength, making it unable to effectively prevent short circuits and mechanical damage.

Method used

A polyethylene and polybutene blend membrane is used. By introducing 10%-30% polybutene into the membrane, combined with appropriate grain boundary distribution and stress transmission path, the thermal stability and mechanical reliability of the membrane are optimized, the pore-closing temperature is reduced and the needle-punching strength is improved.

Benefits of technology

It achieves a reduction in pore temperature and an increase in needle penetration strength without sacrificing the film rupture temperature, ensuring that the battery cuts off the current in time at the initial stage of abnormal temperature rise, enhancing the resistance to dendrite puncture, and improving the safety response speed and mechanical stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123121069A_ABST
    Figure CN123121069A_ABST
Patent Text Reader

Abstract

This invention discloses a lithium-ion battery separator, its preparation method, and its application. The lithium-ion battery separator comprises polyethylene and polybutene, wherein the mass fraction of polybutene in the separator is 10%-30%. In the XRD pattern of the separator, a characteristic peak appears at 2θ of 21.3°-21.5°, and the full width at half maximum (FWHM) of the characteristic peak is 0.65°~0.76°, corresponding to a crystal size of 10.7nm~12.4nm. By introducing 10%-30% polybutene by mass, and with appropriate grain boundary distribution and stress transmission paths, the thermal stability and mechanical reliability of the lithium-ion battery separator in this application are synergistically optimized, achieving the goal of reducing the pore-closing temperature and improving the needle-punching strength without sacrificing the membrane rupture temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery technology, and more specifically, to separators for lithium batteries, their preparation methods, and their applications. Background Technology

[0002] Lithium-ion battery separators are crucial basic materials in power batteries and energy storage batteries, possessing both functionality and safety. Their core functions are: firstly, to physically isolate the positive and negative electrodes to prevent short circuits; and secondly, to construct ion transport channels, ensuring efficient and stable migration of lithium ions. The thermal shutdown performance (i.e., low-temperature pore-closing capability) and mechanical puncture strength of the separator directly determine the battery's safe operating boundaries and the yield rate of mass production.

[0003] Currently, the mainstream commercial separators are polyethylene (PE) / polypropylene (PP) bilayer or multilayer polyolefin microporous membranes. This system achieves a rapid response to the initial stage of thermal runaway by melting and closing the pores of the PE component at a relatively low temperature; at the same time, relying on the high melting point and structural rigidity of the PP component, it maintains the integrity of the membrane at high temperatures, forming the first passive safety barrier for preventing battery thermal runaway.

[0004] However, in response to increasingly stringent battery safety and manufacturing requirements, the industry's technical requirements for separators include: low-temperature rapid pore closure to promptly block ion conduction and inhibit the spread of chain reactions during the thermal runaway initiation stage; high membrane rupture temperature to delay separator failure time and reserve sufficient buffer space for system-level thermal management; and high needle penetration strength to resist lithium dendrite puncture and assembly mechanical damage.

[0005] Therefore, a diaphragm that can achieve low pore closure temperature and high membrane rupture temperature has significant engineering application value. Summary of the Invention

[0006] The purpose of this invention is to provide a separator for lithium batteries, a preparation method thereof, and an application thereof, which is beneficial to achieving a balance between low pore closure temperature, high membrane rupture temperature, and high needle penetration strength.

[0007] This invention is implemented as follows: In a first aspect, the present invention provides a separator for lithium batteries, comprising polyethylene and polybutene, wherein the mass fraction of polybutene in the separator is 10%-30%; In the XRD pattern of the diaphragm, a characteristic peak appears at 2θ of 21.3°-21.5°, and the full width at half maximum (FWHM) of the characteristic peak is 0.65°~0.76°, corresponding to a crystal size of 10.7nm~12.4nm.

[0008] In an optional embodiment, the diaphragm further includes polypropylene.

[0009] In an optional embodiment, the mass fraction of polypropylene in the diaphragm is 7%-15%.

[0010] In an optional embodiment, the molecular weight of the polyethylene is 50-150W; And / or, the molecular weight of the polybutene is 5w-15w; And / or, the isotacticity of the polybutene is 96%-97%; And / or, the molecular weight of the polypropylene is 20w-60w; And / or, the isotacticity of the polypropylene is 97.0%-97.5%.

[0011] In an optional embodiment, the thickness of the diaphragm is 3μm-10μm.

[0012] In an optional embodiment, the diaphragm is subjected to a first heating, a cooling, and a second heating in sequence; the second heating process is analyzed by differential scanning calorimetry. During the second heating process, a second melting endothermic peak is obtained in the temperature range of 80℃-100℃, and the crystallinity of polybutene in the second melting endothermic peak is 2%-6%; wherein the first heating is carried out to a temperature greater than 90℃.

[0013] In a second aspect, the present invention provides a method for preparing a lithium battery separator as described in the foregoing embodiments, comprising: mixing a mixture of a polymer raw material for preparing the separator and a pore-forming agent and molding it to obtain a substrate; The substrate is subjected to biaxial stretching, extraction, and heat setting in sequence to obtain the diaphragm.

[0014] In an optional embodiment, the pore-forming agent in the mixture has a mass fraction of 70-80%; And / or, the mixing temperature is 170℃-190℃, and the time is 8min-12min; And / or, the biaxial stretching ratios are each independently selected from 10 to 20 times; And / or, the heat setting temperature is 120℃-130℃, and the time is 50min-70min; And / or, it also includes heat-treating the heat-set substrate to obtain the heat-treated diaphragm; the heat treatment temperature is greater than 90°C.

[0015] In an optional embodiment, the heat treatment temperature is 120℃-130℃ and the time is 50min-70min.

[0016] Thirdly, the present invention provides a lithium-ion battery, including the lithium battery separator described in any one of the foregoing embodiments.

[0017] The present invention has the following beneficial effects: This application's lithium battery separator incorporates 10%-30% polybutene by mass, along with appropriate grain boundary distribution and stress transmission paths, synergistically optimizing the separator's thermal stability and mechanical reliability. This achieves the goal of reducing the pore-closing temperature and increasing the needle penetration strength without sacrificing the membrane rupture temperature. Specifically, the membrane rupture temperature is ≥146℃, indicating that it maintains physical integrity at high temperatures, delaying thermal runaway propagation; the pore-closing temperature is ≤135℃, ensuring timely current cutoff in the early stages of abnormal battery temperature rise, improving safety response speed; and the needle penetration strength per unit thickness is ≥72 gf / μm, reflecting a significantly enhanced resistance to internal dendrite penetration, helping to suppress short-circuit risks and achieving a synergistic improvement in thermal turn-off performance and mechanical robustness. Attached Figure Description

[0018] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0019] Figure 1 The images show the XRD patterns of the lithium battery separators prepared in Example 1 and the comparative example. Figure 2 The image shows the DSC test results of the lithium battery separator sample from Example 1 after heat treatment at T=200. Figure 3 The image shows the DSC test results of the lithium battery separator sample from Example 1 after heat treatment at T=130. Figure 4 The image shows the DSC test results of the lithium battery separator sample from Example 1 after heat treatment at T=110. Figure 5 The image shows the DSC test results of the lithium battery separator sample from Example 1 after heat treatment at T=100. Figure 6 The image shows the DSC test results of the lithium battery separator sample from Example 1 after heat treatment at T=90°C. Figure 7 This is a temperature impedance test diagram of the closed-cell membrane before heat treatment of the lithium battery separator sample in Example 1. Figure 8 The image shows the temperature impedance test result of the closed-cell membrane after heat treatment at 130°C for the lithium battery separator sample in Example 1. Detailed Implementation

[0020] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0021] The applicant's research found that although adding low-melting-point polyethylene can reduce the closed-cell temperature, a large amount of low-melting-point polyethylene needs to be added, otherwise the reduction in closed-cell temperature will be limited; and a high amount of addition will significantly reduce the mechanical properties of the base film, such as the needle penetration strength and tensile strength.

[0022] This invention provides a separator for lithium batteries, comprising polyethylene and polybutene, wherein the mass fraction of polybutene in the separator is 10%-30%, for example 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, 28%, or 30%. In the XRD pattern of the diaphragm, a characteristic peak appears at 2θ of 21.3°-21.5°, and the full width at half maximum (FWHM) of the characteristic peak is 0.65°~0.76°, corresponding to a crystal size of 10.7nm~12.4nm.

[0023] The membrane of this application incorporates 10%-30% by mass of polybutene. Simultaneously, the XRD pattern of the membrane satisfies the following condition: a characteristic peak appears at 2θ of 21.3°-21.5°, and the full width at half maximum (FWHM) of the characteristic peak is 0.65°~0.76°, for example, 0.650°, 0.662°, 0.674°, 0.686°, 0.698°, 0.710°, 0.722°, 0.734°, 0.746°, 0.758°, and 0.760°. The corresponding crystal size is 10.7nm~12.4nm, for example, 10.70nm, 10.89nm, 11.08nm, 11.27nm, 11.46nm, 11.65nm, 11.84nm, 12.03nm, 12.22nm, and 12.40nm. The aforementioned technical measures synergistically optimize the thermal stability and mechanical reliability of the separator, reducing the pore-closing temperature and increasing the needle penetration strength without sacrificing the membrane rupture temperature. This achieves the following: a membrane rupture temperature ≥146℃, indicating that it can still maintain physical integrity at high temperatures and delay the spread of thermal runaway; a pore-closing temperature ≤135℃, ensuring that the current can be cut off in time at the initial stage of abnormal battery temperature rise, improving the safety response speed; and a needle penetration strength per unit thickness ≥72 gf / μm, reflecting its significantly enhanced resistance to internal dendrite puncture, which helps to suppress short-circuit risks and achieve a synergistic improvement in thermal turn-off performance and mechanical robustness.

[0024] In this application, if the amount of PB added is too small, the closing temperature will not decrease significantly, and no PB component will appear in the secondary melting. This may be because PB is dispersed and wrapped by PE and cannot form an isolated dispersed phase. If the amount added is too large, PB and PP are a partially compatible system. If the critical addition ratio is exceeded, phase separation will occur. Neither of these conditions is conducive to achieving a balance between low closing temperature, high film breaking temperature and high needle penetration strength.

[0025] In this application, the XRD pattern of the diaphragm shows a characteristic peak at 2θ of 21.3°-21.5°, and the full width at half maximum (FWHM) of the characteristic peak is 0.65°~0.76°, corresponding to a crystal size of 10.7nm~12.4nm. This is beneficial for optimizing the grain boundary distribution and stress transmission path, and is the common structural basis for achieving high membrane breakage temperature, high tensile strength and good needle penetration resistance. With the addition of PB, a balance of low pore closure temperature, high membrane breakage temperature and high needle penetration strength is achieved.

[0026] In an optional embodiment, the diaphragm further includes polypropylene. Polypropylene can complement the crystallization behavior of polyethylene, and its higher melting point and rigid segments can enhance the high-temperature dimensional stability of the diaphragm and suppress thermal shrinkage; at the same time, it can synergistically construct a multiphase interface with polybutene, optimize the pore uniformity and mechanical transmission path, and achieve a balance between improving the membrane rupture temperature and the needle penetration strength.

[0027] In an optional embodiment, the mass fraction of polypropylene in the diaphragm is 7%-15%, for example 7.0%, 7.9%, 8.8%, 9.7%, 10.6%, 11.5%, 12.4%, 13.3%, 14.2%, and 15.0%. If the amount of polypropylene added is too small, the increase in membrane breaking temperature will not be significant; if the amount added is too large, the strength will be reduced significantly. Neither of these is conducive to achieving a balance between high membrane breaking temperature and high needle punching strength.

[0028] In an optional embodiment, the mass ratio of PE:PP:PB in the diaphragm is 55-83:7-15:10-30, preferably 60-78:7-10:15-30.

[0029] In an optional embodiment, the molecular weight of the polyethylene is 50-150W, such as 50W, 61W, 72W, 83W, 94W, 105W, 116W, 127W, 138W, 149W, and 150W. The high molecular weight of polyethylene is beneficial to the entanglement density and melt strength of the polyethylene main phase, giving the diaphragm excellent film-forming integrity and high-temperature creep resistance, which is the basis for achieving high film-breaking temperature and structural stability under thin profile.

[0030] In an optional embodiment, the molecular weight of the polypropylene is 20w-60w, such as 20W, 24W, 28W, 32W, 36W, 40W, 44W, 48W, 52W, 56W, and 60W, and the isotacticity is 97.0%-97.5%, such as 97.00%, 97.06%, 97.11%, 97.17%, 97.22%, 97.28%, 97.33%, 97.39%, 97.44%, and 97.50%. The moderate molecular weight of the polypropylene balances processability and mechanical contribution; high isotacticity is beneficial for the regularity and density of the crystallization micro-regions, enhancing local rigidity.

[0031] In an optional embodiment, the polybutene has a molecular weight of 5w-15w, such as 5W, 6W, 7W, 8W, 9W, 10W, 11W, 12W, 13W, 14W, or 15W, and an isotacticity of 96%-97%, such as 96.0%, 96.1%, 96.2%, 96.3%, 96.4%, 96.5%, 96.6%, 96.7%, 96.8%, 96.9%, or 97.0%. It combines good compatibility with moderate chain flexibility, which is beneficial for forming stable dispersed microregions in the polyethylene matrix, playing a toughening and interface regulation role, without interfering with the crystallization of the main phase, and ensuring comprehensive performance.

[0032] In an optional embodiment, the thickness of the separator is 3μm-10μm, for example 3.0μm, 3.8μm, 4.6μm, 5.4μm, 6.2μm, 7.0μm, 7.8μm, 8.6μm, 9.4μm, and 10.0μm. This aims to shorten the lithium-ion transport path as much as possible while ensuring mechanical integrity, thereby improving rate performance.

[0033] In an optional embodiment, the diaphragm is subjected to a first heating, a cooling, and a second heating in sequence; the second heating process is analyzed by differential scanning calorimetry. During the second heating process, a second melting endothermic peak is obtained in the temperature range of 80℃-100℃. The crystallinity of polybutene in the second melting endothermic peak is 2%-6%, for example, 2.0%, 2.4%, 2.8%, 3.2%, 3.6%, 4.0%, 4.4%, 4.8%, 5.2%, 5.6%, and 6.0%; wherein the first heating is performed to a temperature greater than 90℃.

[0034] In the lithium battery separator of this application, polyethylene and polybutene can undergo phase separation during the melting and cooling process to form a blended structure with polyethylene as the continuous phase and polybutene as the dispersed micro-regions. The first heating to above 90°C melts the two components, and the cooling process determines the nucleation and crystallization behavior of the polybutene micro-regions. The endothermic peak that appears at 80–100°C during the second heating corresponds to the melting of polybutene microcrystals. The 2%–6% crystallinity of the separator after the first heating indicates that the polybutene is arranged in a highly amorphous or weakly crystalline state in the polyethylene matrix with a very low degree of order.

[0035] In an optional embodiment, the crystallinity of the polybutene in the diaphragm is 2%-6%, for example 2.0%, 2.4%, 2.8%, 3.2%, 3.6%, 4.0%, 4.4%, 4.8%, 5.2%, 5.6%, 6.0%.

[0036] Low-crystallinity polybutene microregions can serve as a flexible interface phase to alleviate stress concentration and improve membrane ductility and needle penetration resistance. Furthermore, due to their lower melting point than the polyethylene main phase, they soften earlier during heating and promote pore closure, synergistically achieving a lower pore-closing temperature. Simultaneously, this weakly crystalline structure does not significantly weaken the high-temperature strength of the polyethylene skeleton, thus ensuring that the membrane rupture temperature is not lowered. Therefore, a polybutene crystallinity of 2%-6% is the structural basis for achieving synergistic optimization of pore-closing temperature, membrane rupture temperature, and needle penetration strength.

[0037] In an optional embodiment, the membrane rupture temperature is 146°C to 179°C, for example 146°C, 150°C, 154°C, 158°C, 162°C, 166°C, 170°C, 174°C, 178°C, 179°C; preferably greater than 160°C.

[0038] In an optional embodiment, the pore-closing temperature of the diaphragm is 132℃~134.5℃, for example 132.0℃, 132.3℃, 132.6℃, 132.9℃, 133.2℃, 133.5℃, 133.8℃, 134.1℃, 134.4℃, 134.5℃; In an optional embodiment, the pore-closing speed of the diaphragm is 29852Ω / ℃ to 42010Ω / ℃, for example, 29852Ω / ℃, 31200Ω / ℃, 32548Ω / ℃, 33896Ω / ℃, 35244Ω / ℃, 36592Ω / ℃, 37940Ω / ℃, 39288Ω / ℃, 40636Ω / ℃, 41984Ω / ℃, and 42010Ω / ℃. The pore-closing speed of the diaphragm is significantly accelerated after adding PB.

[0039] In an optional embodiment, the needle penetration strength per unit thickness of the diaphragm is 72 gf / μm to 79.3 gf / μm, for example 72.0 gf / μm, 72.8 gf / μm, 73.6 gf / μm, 74.4 gf / μm, 75.2 gf / μm, 76.0 gf / μm, 76.8 gf / μm, 77.6 gf / μm, 78.4 gf / μm, and 79.3 gf / μm; In an optional embodiment, the MD tensile strength of the diaphragm is 2600 kgf / cm²-3200 kgf / cm², for example 2600, 2667, 2733, 2800, 2867, 2933, 3000, 3067, 3133, 3200 kgf / cm². In an optional embodiment, the TD tensile strength of the diaphragm is 2700 kgf / cm²-3100 kgf / cm², for example 2700, 2744, 2789, 2833, 2878, 2922, 2967, 3011, 3056, 3100 kgf / cm².

[0040] The present invention also provides a method for preparing the lithium battery separator described in the foregoing embodiments, comprising: mixing a mixture of polymer raw materials for preparing the separator and a pore-forming agent and molding it to obtain a substrate; The substrate is subjected to biaxial stretching, extraction, and heat setting in sequence to obtain the diaphragm.

[0041] In the preparation method of this application, biaxial stretching can induce the formation of polyethylene microfiber network and improve orientation; extraction to remove pore-forming agent can construct through-pores; heat setting locks the crystal structure and pore morphology, together completing the preparation of a membrane with high mechanical strength, uniform pore size distribution and stable thermal response characteristics.

[0042] In an optional embodiment, the mass fraction of the pore-forming agent in the mixture is 70-80%, for example 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%; while ensuring sufficient porosity and ion flux, excessive phase separation or residual defects are avoided, and the mechanical integrity of the membrane and the electrochemical performance are balanced.

[0043] In an optional embodiment, the pore-forming agent is selected from at least one of paraffin oil, soybean oil, dioctyl phthalate, dibutyl phthalate, fatty oil, and liquid paraffin; the selected pore-forming agent has moderate compatibility with the polymer and a matching boiling point / solubility, which is conducive to uniform dispersion in the mixture and can be completely extracted by the extractant, reducing the residual dense layer and improving the pore connectivity and pore uniformity.

[0044] In an optional embodiment, the mixing temperature is 170℃-190℃, for example 170℃, 172℃, 174℃, 176℃, 178℃, 180℃, 182℃, 184℃, 186℃, 188℃, or 190℃, and the time is 8min-12min, for example 8.0min, 8.4min, 8.8min, 9.2min, 9.6min, 10.0min, 10.4min, 10.8min, 11.2min, 11.6min, or 12.0min; this facilitates the full melting and blending of each component and microscopic homogenization, avoiding degradation or localized unmelted areas.

[0045] In an optional embodiment, the biaxial stretching ratio is independently selected from 10 to 20 times, for example 10 times, 11 times, 12 times, 13 times, 14 times, 15 times, 16 times, 17 times, 18 times, 19 times, and 20 times; giving the diaphragm a high degree of biaxial orientation and balanced mechanical strength.

[0046] In an optional embodiment, the extractant used for extraction is selected from dichloromethane, which has strong dissolving ability for the selected pore-forming agent and low residue.

[0047] In an optional embodiment, the extraction time is 10-30 min, for example 10 min, 12 min, 14 min, 16 min, 18 min, 20 min, 22 min, 24 min, 26 min, 28 min, or 30 min; to reduce pore-forming agent residue.

[0048] In an optional embodiment, the heat setting temperature is 120℃-130℃, for example 120℃, 121℃, 122℃, 123℃, 124℃, 125℃, 126℃, 127℃, 128℃, 129℃, or 130℃, and the time is 50min-70min, for example 50min, 52min, 54min, 56min, 58min, 60min, 62min, 64min, 66min, 68min, or 70min. This process relaxes internal stress below the melting point of polyethylene, achieving heat setting and appropriately improving crystallization, thereby enhancing heat shrinkage suppression and film rupture temperature stability.

[0049] In an optional embodiment, the heat-set substrate is further subjected to heat treatment to obtain the heat-treated diaphragm. The heat treatment temperature is greater than 90°C, preferably 120°C-130°C, such as 120°C, 121°C, 122°C, 123°C, 124°C, 125°C, 126°C, 127°C, 128°C, 129°C, or 130°C, for a time of 50-70 minutes, such as 50 minutes, 52 minutes, 54 minutes, 56 minutes, 58 minutes, 60 minutes, 62 minutes, 64 minutes, 66 minutes, 68 minutes, or 70 minutes. The heat treatment further regulates the micro-crystallization state of the polybutene, improving safety performance.

[0050] The present invention also provides a lithium-ion battery, including the lithium battery separator described in any one of the foregoing embodiments.

[0051] The features and performance of the present invention will be further described in detail below with reference to embodiments.

[0052] Example 1 This application provides a separator for lithium batteries. The separator is a blend of polyethylene (Daehan Oil Chemical, molecular weight 100W), polypropylene (Daehan Oil Chemical, molecular weight 40W, isotacticity 97.16%) and polybutene (Shandong Dongfang Hongye New Material Technology Co., Ltd., molecular weight 10W, isotacticity 96.23%), with a thickness of 5.5μm.

[0053] The method for preparing the separator for lithium batteries in this embodiment includes the following steps: S1. Polyethylene, polypropylene, polybutene (78:7:15) and pore-forming agent paraffin oil are thoroughly mixed at a mass ratio of 25:75 and then kneaded at 180°C for 10 minutes. Then, the mixture is extruded, cooled and cast to obtain a substrate. S2. The substrate is subjected to biaxial stretching at 120°C (stretching ratio of 15 times in both directions), then extracted in dichloromethane for 20 min, and finally heat-set at 129°C for 1 h to obtain a separator for lithium batteries.

[0054] Example 2 The preparation method of the lithium battery separator provided in this embodiment is basically the same as that in Example 1, except that the mass ratio of polyethylene, polypropylene and polybutene is 85:0:15.

[0055] Example 3 The preparation method of the lithium battery separator provided in this embodiment is basically the same as that in Example 1, except that the mass ratio of polyethylene, polypropylene and polybutene is 83:7:10.

[0056] Example 4 The preparation method of the lithium battery separator provided in this embodiment is basically the same as that in Example 1, except that the mass ratio of polyethylene, polypropylene and polybutene is 63:7:30.

[0057] Example 5 The preparation method of the lithium battery separator provided in this embodiment is basically the same as that in Example 1, except that the mass ratio of polyethylene, polypropylene and polybutene is 75:10:15.

[0058] Example 6 The preparation method of the lithium battery separator provided in this embodiment is basically the same as that in Example 1, except that the mass ratio of polyethylene, polypropylene and polybutene is 70:15:15.

[0059] Comparative Example 1 The preparation method of the lithium battery separator provided in this embodiment is basically the same as that in Example 1, except that polypropylene and polybutene are not added.

[0060] Comparative Example 2 The preparation method of the lithium battery separator provided in this embodiment is basically the same as that in Example 1, except that the mass ratio of polyethylene, polypropylene and polybutene is 93:7:0.

[0061] Comparative Example 3 The preparation method of the lithium battery separator provided in this embodiment is basically the same as that in Example 1, except that the mass ratio of polyethylene, polypropylene and polybutene is 86:7:7.

[0062] The performance of the lithium battery separators prepared in the above embodiments and comparative examples was tested. The testing methods are shown in Table 1, and the test results are shown in Table 2.

[0063] Table 1

[0064] Table 2

[0065] 1. The XRD patterns of the lithium battery separators prepared in Example 1 and Comparative Example 1 are shown below. Figure 1 As shown in Example 1, PB acts as a heterogeneous nucleating agent, disrupting the entanglement of PE macromolecular chains and reducing the size of PE spherulites. The fine-grained structure increases the number of grain boundaries and distributes stress more evenly, avoiding intergranular cracks that are prone to occur in large spherulites. During needle punching, cracks do not propagate rapidly, resulting in an increase in needle punching strength on a macroscopic scale. Figure 1 The PE diffraction peak has a full width at half maximum (FWHM) of 0.58° and a grain size of 14.3 nm, while the PE+PB+PP diffraction peak has a FWHM of 0.73° and a grain size of 11.3 nm. The decrease in grain size confirms the existence of the grain refinement effect.

[0066] Note: The formula for calculating grain size is D. hkl =K*λ / (β*cosθ) Among them, D hkl : Lamellar size perpendicular to the direction of the diffraction plane (hkl); K: Scherrer constant (shape factor), which is a dimensionless constant. In this invention, K = 0.94. λ: Wavelength of the incident X-ray; β: Physical broadening of the diffraction peak (hkl), β = FWHM × (π / 180); θ: Bragg angle of the diffraction peak (hkl).

[0067] 2. Five lithium battery separator samples prepared in Example 1 were taken and tested using a differential scanning calorimeter (DSC3). The samples were first heated from 25°C to T°C at a rate of 5°C / min, then cooled to 25°C at a rate of -5°C / min, and finally heated to 200°C at a rate of 5°C / min. The temperature changes during this process were analyzed using differential scanning calorimetry to obtain the DSC test results, as shown below. Figure 2-6 As shown, where Figure 2-6 The corresponding T values ​​are 200, 130, 110, 100, and 90, respectively. Figure 2-5 The crystallinity of polybutene in the secondary melting endothermic peaks was 4.11%, 3.1%, 2.95%, and 2.66%, respectively. Figure 6 No melting endothermic peak was observed in the 80-100℃ temperature range. The presence of a melting endothermic peak in this temperature range can reduce the closed-cell temperature, which is beneficial to battery safety.

[0068] DSC method for calculating crystallinity: Crystallinity (%) = (Sample melting enthalpy ΔHm / Theoretical melting enthalpy ΔH° of fully crystallized polymer) × 100%.

[0069] 3. The lithium battery separator prepared in Example 1 was subjected to heat treatment, that is, the lithium battery separator was placed in an oven at 130°C and heated for 60 minutes. The closed-cell rupture temperature impedance test diagrams of the lithium battery separator before and after heat treatment are shown in the figure below. Figure 7 and Figure 8 As shown, the pore-closing temperature of the lithium battery separator after heat treatment is 132℃, and the membrane rupture temperature is 169.8℃, resulting in higher safety.

[0070] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A separator for lithium batteries, characterized by, The membrane comprises polyethylene and polybutene, wherein the mass fraction of polybutene in the membrane is 10%-30%. In the XRD pattern of the diaphragm, a characteristic peak appears at 2θ of 21.3°-21.5°, and the full width at half maximum (FWHM) of the characteristic peak is 0.65°~0.76°, corresponding to a crystal size of 10.7nm~12.4nm.

2. The separator for lithium batteries according to claim 1, characterized by The diaphragm also includes polypropylene.

3. The separator for lithium batteries according to claim 2, characterized by The mass fraction of polypropylene in the diaphragm is 7%-15%.

4. The separator for lithium batteries according to claim 2, characterized by The molecular weight of the polyethylene is 50-150W; And / or, the molecular weight of the polybutene is 5w-15w; And / or, the isotacticity of the polybutene is 96%-97%; And / or, the molecular weight of the polypropylene is 20w-60w; And / or, the isotacticity of the polypropylene is 97.0%-97.5%.

5. The separator for lithium batteries according to claim 1, characterized by The thickness of the diaphragm is 3μm-10μm.

6. The separator for lithium batteries according to claim 1 or 2, characterized by The diaphragm was subjected to a first heating, a cooling, and a second heating in sequence. The second heating process was analyzed by differential scanning calorimetry. During the second heating process, a second melting endothermic peak was obtained in the temperature range of 80℃-100℃. The crystallinity of polybutene in the second melting endothermic peak was 2%-6%. The first heating was carried out to a temperature greater than 90℃.

7. A method for producing the separator for lithium batteries as claimed in any one of claims 1 to 6, characterized by, include: The polymer raw material used to prepare the diaphragm is mixed with a pore-forming agent and then molded to obtain a substrate; The substrate is subjected to biaxial stretching, extraction and heat setting in sequence to obtain the diaphragm.

8. The method for producing a separator for lithium batteries according to claim 7, characterized by, The mass fraction of the pore-forming agent in the mixture is 70-80%; And / or, the mixing temperature is 170℃-190℃, and the time is 8min-12min; And / or, the biaxial stretching ratios are each independently selected from 10 to 20 times; And / or, the heat setting temperature is 120℃-130℃, and the time is 50min-70min; And / or, it further includes heat-treating the heat-set substrate to obtain the heat-treated diaphragm; the heat treatment temperature is greater than 90°C.

9. The method for producing a separator for lithium batteries according to claim 8, characterized by, The heat treatment temperature is 120℃-130℃, and the time is 50min-70min.

10. A lithium-ion battery, characterized by, Includes the lithium battery separator as described in any one of claims 1-6.