Laser-modified high-adhesion DPC ceramic substrates and low-temperature preparation process

By constructing a uniform honeycomb texture on the surface of a ceramic substrate through laser micro-modification and HPPMS high-power pulsed magnetron sputtering technology, combined with the high kinetic energy deposition of high ionization metal particles of HPPMS, the problems of bonding force dispersion, microcracks, warping deformation and environmental protection of traditional DPC ceramic substrates are solved, and high reliability and high precision DPC ceramic substrate preparation is achieved.

CN123124202APending Publication Date: 2026-11-17JIANGXI LATTICE GRAND ADVANCED MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611499114.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing DPC ceramic substrate manufacturing processes have significant bottlenecks in terms of bonding consistency, substrate integrity, circuit accuracy, energy consumption, and environmental protection. Traditional high-temperature acid and alkali strong corrosion roughening processes result in high bonding dispersion, easy generation of microcracks in the substrate, insufficient seed layer step coverage, high-temperature warping deformation, and serious chemical waste pollution, making it difficult to meet the requirements for large-scale mass production of ultra-high reliability and high precision DPC ceramic substrates.

Method used

A uniform nano-micro composite honeycomb micro-interlocking texture layer was constructed using laser micro-modification technology, and a titanium-copper composite seed layer was prepared by combining HPPMS high-power pulsed magnetron sputtering and ion-assisted deposition. This replaced the traditional high-temperature chemical roughening process, enabling the preparation of DPC ceramic substrates with low-temperature processing and environmental friendliness.

Benefits of technology

It achieves improved uniform bonding force of ceramic substrates, preservation of substrate integrity, improved circuit accuracy and enhanced environmental friendliness, meets the high reliability packaging requirements of automotive and aerospace grades, reduces energy consumption and production cycle, and realizes large-scale and green mass production of high-end DPC ceramic substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124202A_ABST
    Figure CN123124202A_ABST
Patent Text Reader

Abstract

This invention discloses a laser-modified high-adhesion DPC ceramic substrate and its low-temperature preparation process, belonging to the field of ceramic substrate technology. The substrate comprises a ceramic matrix, a laser-modified textured layer, a low-temperature seed layer, and a DPC precision copper circuit layer. A cold-processing laser scans the surface of the ceramic matrix to construct a nano-micro composite honeycomb micro-interlocking textured layer. After plasma activation, a titanium-copper composite low-temperature seed layer is prepared using HPPMS high-power pulsed magnetron sputtering / ion-assisted deposition. Utilizing the high kinetic energy and directional scattering of high-ionization metal particles, excellent step coverage and dense filling of the honeycomb pits are achieved. Subsequently, low-temperature pulsed electroplating is used to prepare the precision copper circuit, resulting in high adhesion and good consistency of the plating layer. The entire process temperature is below 200℃. The low-temperature treatment throughout suppresses substrate warping and deformation, resulting in high circuit precision. There is no corrosive chemical waste discharge, making it environmentally friendly and suitable for the mass production of automotive-grade and aerospace-grade high-end DPC ceramic substrates.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of ceramic substrate technology, and in particular to a laser-modified high-adhesion DPC ceramic substrate and a low-temperature preparation process, which is suitable for ultra-high reliability power semiconductors, aerospace and military applications, and high-end optoelectronic device packaging. Background Technology

[0002] Direct Plated Copper (DPC) ceramic substrates have become core interconnect materials in high-end electronic packaging fields such as IGBT power modules, LiDAR, and 5G RF devices due to their advantages of high thermal conductivity, high insulation, and high circuit precision. In the DPC process, the bonding force between the ceramic substrate and the copper metal layer is a key indicator determining the reliability of the substrate, and the ceramic surface pretreatment process before metallization directly determines the adhesion performance of subsequent plating layers.

[0003] Traditional surface pretreatment of DPC ceramic substrates commonly employs high-temperature acid-base strong etching roughening processes. This process involves immersing the ceramic substrate in a high-concentration hydrofluoric acid-nitric acid mixture, high-temperature high-concentration phosphoric acid or hydrochloric acid, or high-temperature alkaline etching solution, utilizing chemical etching to form a micron-level uneven structure on the ceramic surface, thereby providing a mechanical interlocking interface for subsequent sputtering or chemical plating seed layers. However, this chemical roughening method has several insurmountable drawbacks: First, chemical etching is an isotropic etching process, and its corrosion rate is affected by multiple factors such as solution concentration, temperature, stirring conditions, and the crystal phase distribution of the ceramic substrate, resulting in extremely poor uniformity of the roughened microstructure. Significant differences in surface roughness between different batches and even different areas of the same substrate lead to large fluctuations in the actual contact area between the subsequent metal plating and the ceramic substrate, resulting in high dispersion in plating adhesion. Under harsh conditions such as thermal cycling and power cycling, this easily leads to failures such as localized plating peeling and circuit breaks, making it difficult to meet the high reliability requirements of automotive-grade and aerospace-grade packaging applications.

[0004] Secondly, strong acids and alkalis selectively erode ceramic grain boundaries under high-temperature conditions, easily introducing microcracks or even surface peeling into the matrix, directly weakening the mechanical strength of the ceramic substrate. Simultaneously, the high-temperature processing itself induces thermal stress accumulation within the ceramic, leading to irreversible warping deformation in thin substrates (≤0.5mm). The substrate warping often exceeds 0.2%, severely restricting the alignment accuracy of subsequent precision circuitry processes such as photolithography and electroplating, and limiting the fabrication capability of fine-line, narrow-pitch DPC products.

[0005] Furthermore, the traditional process involves multiple high-temperature steps (usually >200℃) from roughening and activation to seed layer sputtering and high-temperature annealing. This not only results in high energy consumption and long production cycles, but also exacerbates the mismatch in thermal expansion coefficients between the substrate and the metal layer due to the high-temperature environment, further increasing the interfacial thermal stress.

[0006] Furthermore, in terms of seed layer preparation, traditional DC magnetron sputtering is a line-of-sight deposition, where metal particles fly in a straight line. When there are micro-pits or textures on the ceramic surface, the particle incident angles on the sidewalls and bottom of the pits are different, the step coverage is insufficient, the bottom film is thin, and even pinholes and discontinuities appear. The mechanical interlocking effect of the micro-texture cannot be fully utilized. Although the chemical plating seed layer has isotropic filling capability, its metal atoms have almost no kinetic energy and are only adsorbed to the ceramic interface by van der Waals forces. The intrinsic interface bonding is weak, and the chemical plating process has problems such as hydrogen evolution, hydrogen-induced micropores, and complex chemical control.

[0007] Finally, the large amounts of wastewater generated by chemical coarsening, containing fluorine, phosphorus, nitrogen, and heavy metals, are highly corrosive and biotoxic, resulting in high treatment costs and increasingly stringent environmental regulations. As the electronics manufacturing industry shifts towards green and low-carbon practices, the sustainable development potential of traditional, highly polluting DPC processes has been significantly reduced.

[0008] In summary, existing DPC ceramic substrate manufacturing processes have significant bottlenecks in terms of bonding consistency, substrate integrity, circuit accuracy, energy consumption, and environmental protection, which severely restrict the large-scale mass production of ultra-reliable and high-precision DPC ceramic substrates. The industry urgently needs a new surface modification technology that can achieve uniform micro-coarsening, low-temperature processing throughout the process, green environmental protection, and excellent bonding. Summary of the Invention

[0009] In view of this, the present invention addresses the shortcomings of the existing technology, and its main objective is to provide a laser-modified DPC ceramic substrate with high adhesion and a low-temperature preparation process. The laser micro-modification replaces the traditional high-temperature acid and alkali strong corrosion roughening process, and HPPMS high-power pulsed magnetron sputtering combined with ion-assisted deposition is used to prepare the seed layer. This solves the problems of high adhesion dispersion of existing DPC ceramic substrates, easy formation of microcracks in the substrate, insufficient step coverage of the seed layer, high-temperature warping deformation, and serious chemical waste pollution.

[0010] To achieve the above objectives, the present invention adopts the following technical solution: A laser-modified high-adhesion DPC ceramic substrate includes a ceramic substrate, a laser-modified textured layer, a low-temperature seed layer, and a DPC precision copper circuit layer. The laser-modified textured layer is formed on the surface of the ceramic substrate by laser etching. The low-temperature seed layer densely fills and covers the laser-modified textured layer. The DPC precision copper circuit layer is formed on the surface of the low-temperature seed layer.

[0011] As a preferred embodiment, the laser-modified textured layer is a nano-micro composite honeycomb micro-interlocking textured layer.

[0012] As a preferred embodiment, the depth of the laser micro-modified texture layer is 0.8–1.5 μm, and the laser source used for the laser micro-modified texture layer is a nanosecond, picosecond, or femtosecond cold processing laser source.

[0013] As a preferred embodiment, the low-temperature seed layer is a titanium-copper composite layer deposited by HPPMS high-power pulsed magnetron sputtering / ion-assisted deposition, which includes a titanium bonding layer bonded to the ceramic substrate interface and a copper conductive layer covering the surface of the titanium bonding layer.

[0014] As a preferred embodiment, the thickness of the low-temperature seed layer is 0.3–0.6 μm, wherein the thickness of the titanium bonding layer is 0.05–0.1 μm, and the thickness of the copper conductive layer is 0.25–0.5 μm.

[0015] As a preferred embodiment, the thickness of the ceramic matrix is ​​0.2 to 0.5 mm.

[0016] As a preferred embodiment, the ceramic matrix is ​​made of aluminum nitride or aluminum oxide.

[0017] A low-temperature fabrication process for laser-modified high-adhesion DPC ceramic substrates includes the following steps: S1. Precision cleaning of the substrate: The ceramic substrate is treated with ultrasonic degreasing, deionized water rinsing and cold air drying to ensure that the surface of the ceramic substrate is clean and free of impurities. S2. Laser microtexture modification: A cold-processing laser light source is used to perform full-area scanning etching on the surface of the ceramic substrate. The laser power and scanning speed are controlled to construct a uniform nano-micro composite honeycomb micro-interlocking texture to form a laser micro-modified texture layer. S3. Low-temperature plasma activation: The surface of the laser micro-modified textured layer is activated by room-temperature argon-oxygen plasma to improve the surface energy and wettability of the ceramic substrate. S4. Low-temperature HPPMS seed layer deposition: Using HPPMS high-power pulsed magnetron sputtering combined with ion-assisted deposition process, a titanium bonding layer and a copper conductive layer are sequentially deposited on the surface of the laser micro-modified texture layer. By utilizing the high kinetic energy and large-angle scattering characteristics of high ionization metal particles, excellent step coverage and dense filling of the pits inside the honeycomb micro-texture are achieved, so as to form a continuous and complete low-temperature seed layer as a conductive substrate. S5. Low-temperature electroplating forming circuit: Low-temperature pulse electroplating is used to thicken the copper layer on the surface of the low-temperature seed layer, and photolithography is used to etch the DPC precision copper circuit layer. S6. Room temperature passivation test: The coating adhesion, circuit accuracy and conductivity are tested by using room temperature passivation treatment.

[0018] As a preferred embodiment, the power of the cold processing laser source in step S2 is 5-30W, and the scanning speed is 200-6000mm / s.

[0019] As a preferred embodiment, the process parameters for HPPMS high-power pulsed magnetron sputtering in step S4 are as follows: peak pulse power density 1–3 kW / cm², pulse frequency 50–200 Hz, pulse width 50–200 μs, substrate negative bias voltage -50–-150 V, argon working pressure 0.3–0.8 Pa, and deposition temperature ≤150 °C; ion-assisted deposition is performed using argon ion beam assistance, with ion beam energy of 100–300 eV and ion beam current density of 0.1–0.5 mA / cm².

[0020] Compared with the prior art, the present invention has obvious advantages and beneficial effects. Specifically, as can be seen from the above technical solution: Firstly, this invention completely abandons the traditional high-temperature acid-base chemical roughening process and uses laser micro-modification technology to construct a uniform and controllable honeycomb interlocking texture on the surface of the ceramic substrate. The entire pretreatment process does not involve any chemical corrosion liquid, and does not corrode the ceramic substrate or damage the grain boundaries. It fundamentally eliminates the problem of microcracks in the substrate caused by selective grain boundary corrosion in traditional processes, and fully preserves the original mechanical strength and thermal conductivity of the ceramic substrate, thus greatly improving the overall reliability of the substrate.

[0021] Secondly, this invention employs HPPMS high-power pulsed magnetron sputtering combined with ion-assisted deposition to prepare a titanium-copper composite seed layer. The ionization rate of metal particles generated by the HPPMS process is as high as 60%–90%, far exceeding the 1%–5% of traditional DC magnetron sputtering. These highly ionized metal particles gain high kinetic energy under the negative bias of the substrate and are accompanied by large-angle scattering, enabling them to effectively penetrate the pits within the honeycomb microstructure, achieving excellent step coverage and dense filling. This overcomes the defects of traditional DC magnetron sputtering line-of-sight deposition, which results in thin films at the bottom of pits, numerous pinholes, and insufficient mechanical interlocking. Simultaneously, ion-assisted deposition continuously bombards the growing film with an argon ion beam during the deposition process, further densifying the film, improving film-substrate bonding, and releasing internal stress.

[0022] Thirdly, under the action of HPPMS high-kinetic-energy particles, the titanium bonding layer of this invention undergoes atomic-level mixing and diffusion at the ceramic substrate interface. Titanium atoms react with oxygen elements on the alumina / aluminum nitride ceramic surface to generate Ti-O chemical bonds, forming a strong chemical bonding interface. Simultaneously, the honeycomb-like microtexture is densely filled by the titanium-copper composite layer, forming a mechanically interlocked anchoring structure with controllable depth. The synergistic effect of the dual interface strengthening mechanism of chemical bonding and mechanical interlocking makes the coating adhesion significantly better than that of traditional chemical roughening processes, and the uniformity within and between batches is greatly improved, effectively reducing the risk of failure such as coating peeling and localized detachment, which can meet the application requirements of high-reliability packaging scenarios such as automotive and aerospace grades.

[0023] Fourth, the invention employs a low-temperature processing technology throughout the entire process. Laser modification is carried out at room temperature, the HPPMS seed layer deposition temperature is ≤150℃, and the copper circuit fabrication adopts low-temperature pulse electroplating. The entire process temperature is below 200℃, which completely eliminates the problems of thermal stress accumulation and substrate warping caused by traditional multi-stage high-temperature processes. The substrate has excellent flatness, and the alignment accuracy and dimensional consistency of the circuit can meet the requirements for the fabrication of precision miniaturized DPC products. At the same time, it significantly reduces energy consumption and production cycle costs.

[0024] Fifth, the entire preparation process of this invention produces no fluorine- or heavy metal-containing chemical wastewater discharge. HPPMS is a vacuum physical deposition process, which eliminates the consumption of chemical plating solutions and the risks of hydrogen evolution and hydrogen-induced micropores, making it green and environmentally friendly. Furthermore, both the laser process and HPPMS process parameters are digitally controllable, and the consistency and stability of mass production are superior to the traditional chemical roughening and chemical plating routes that rely on manual experience for control. This provides a practical and feasible technical path for the large-scale and green mass production of high-end DPC ceramic substrates.

[0025] To more clearly illustrate the structural features and effects of the present invention, the present invention will be described in detail below with reference to the accompanying drawings and specific embodiments. Attached Figure Description

[0026] Figure 1 This is an exploded view of the present invention; Figure 2 This invention relates to a diagram of the honeycomb microstructure after laser modification. Figure 3 This is a flowchart of the low-temperature preparation process of the present invention.

[0027] Explanation of reference numerals in the attached diagram: 10. Ceramic substrate; 20. Laser-modified textured layer 30. Low-temperature seed layer; 40. DPC precision copper circuit layer. Detailed Implementation

[0028] Please refer to Figure 1 and Figure 2 As shown, it illustrates the specific structure of a laser-modified high-adhesion DPC ceramic substrate according to the present invention, including a ceramic substrate 10, a laser-modified textured layer 20, a low-temperature seed layer 30, and a DPC precision copper circuit layer 40.

[0029] The ceramic substrate 10 has a thickness of 0.2 to 0.5 mm and is made of aluminum nitride or aluminum oxide.

[0030] The laser-modified textured layer 20 is formed on the surface of the ceramic substrate 10 by laser etching. The laser-modified textured layer 20 is a nano-micro composite honeycomb micro-interlocking textured layer, and the depth of the laser-modified textured layer 20 is 0.8-1.5 μm. The laser light source used for the laser-modified textured layer 20 is a nanosecond, picosecond, femtosecond, or other cold-processing laser light source. The texture is uniformly distributed and free from microcracks in the substrate and surface damage.

[0031] The low-temperature seed layer 30 densely fills and covers the laser-modified textured layer 20. The low-temperature seed layer 30 is a titanium-copper composite layer deposited by HPPMS high-power pulsed magnetron sputtering / ion-assisted deposition, comprising a titanium bonding layer bonded to the ceramic substrate 10 and a copper conductive layer covering the surface of the titanium bonding layer. Furthermore, the thickness of the low-temperature seed layer 30 is 0.3–0.6 μm, with the titanium bonding layer having a thickness of 0.05–0.1 μm and the copper conductive layer having a thickness of 0.25–0.5 μm. It is prepared entirely at low temperatures, without high-temperature thermal deformation.

[0032] The DPC precision copper circuit layer 40 is formed on the surface of the low-temperature seed layer 30, forming a mechanically interlocked high-strength bonding structure.

[0033] This invention also discloses a low-temperature preparation process for laser-modified high-adhesion DPC ceramic substrates, as described above. Figure 3 As shown, it includes the following steps: S1. Precision cleaning of the substrate: The ceramic substrate 10 is subjected to ultrasonic degreasing, deionized water rinsing and cold air drying to ensure that the surface of the ceramic substrate 10 is clean and free of impurities.

[0034] S2. Laser Microtexture Modification: A cold-processing laser source (nanosecond, picosecond, femtosecond, or other cold-processing laser sources) is used to perform full-area scanning etching on the surface of the ceramic substrate 10. The laser power and scanning speed are controlled to construct a uniform nano-micro composite honeycomb micro-interlocking texture to form a laser-modified texture layer 20. The power of the cold-processing laser source is 5–30W, and the scanning speed is 200–6000 mm / s.

[0035] S3. Low-temperature plasma activation: The surface of the laser micro-modified texture layer 20 is activated by room-temperature argon-oxygen plasma to improve the surface energy and wettability of the ceramic substrate 10.

[0036] S4. Low-Temperature HPPMS Seed Layer Deposition: A titanium bonding layer and a copper conductive layer are sequentially deposited on the surface of the laser-modified textured layer 20 using HPPMS high-power pulsed magnetron sputtering combined with ion-assisted deposition. Utilizing the high kinetic energy and wide-angle scattering characteristics of highly ionized metal particles, excellent step coverage and dense filling of the pits within the honeycomb microtexture are achieved, forming a continuous and complete low-temperature seed layer 30 as the conductive substrate. The process parameters for HPPMS high-power pulsed magnetron sputtering are: peak pulse power density 1–3 kW / cm², pulse frequency 50–200 Hz, pulse width 50–200 μs, substrate negative bias -50–-150 V, argon working pressure 0.3–0.8 Pa, and deposition temperature ≤150℃. Ion-assisted deposition uses an argon ion beam with an ion beam energy of 100–300 eV and an ion beam current density of 0.1–0.5 mA / cm².

[0037] S5. Low-temperature electroplating forming circuit: Low-temperature pulse electroplating is used to thicken the copper layer on the surface of the low-temperature seed layer 30, and photolithography is used to etch the DPC precision copper circuit layer 40.

[0038] S6. Room temperature passivation test: The coating adhesion, circuit accuracy and conductivity are tested by using room temperature passivation treatment.

[0039] The above preparation process involves no high-temperature processes or chemical corrosion roughening.

[0040] The present invention will be further described in detail below with reference to several embodiments: Example 1: A 0.3 mm thick aluminum nitride was selected as the ceramic substrate 10. After ultrasonic cleaning and drying of the ceramic substrate 10 with ethanol and deionized water, nanosecond laser full-domain scanning etching was used to form a laser micro-modified texture layer 20 with a depth of 1.2 μm.

[0041] The laser-modified textured layer 20 was activated for 5 min using room-temperature argon-oxygen plasma. Subsequently, a low-temperature seed layer 30 was prepared using HPPMS high-power pulsed magnetron sputtering combined with ion-assisted deposition: first, a titanium bonding layer was deposited with a peak pulse power density of 2 kW / cm², a pulse frequency of 100 Hz, a pulse width of 100 μs, a substrate negative bias of -100 V, an argon working pressure of 0.5 Pa, a deposition temperature of 120 °C, an argon ion beam assist energy of 200 eV, and a beam current density of 0.3 mA / cm², resulting in a titanium bonding layer thickness of 0.08 μm; then, a copper conductive layer was deposited with a peak pulse power density of 1.5 kW / cm², a pulse frequency of 80 Hz, a pulse width of 150 μs, a substrate negative bias of -80 V, an argon working pressure of 0.6 Pa, and a deposition temperature of 120 °C, resulting in a copper conductive layer thickness of 0.42 μm. The total thickness of the low-temperature seed layer 30 was 0.5 μm, with dense, full-coverage, and uninterrupted honeycomb texture.

[0042] A 40μm thick copper layer was prepared on the surface of the low-temperature seed layer 30 by low-temperature pulse electroplating, and a high-precision DPC circuit was formed by photolithography etching. The DPC precision copper circuit layer 40 was then prepared by room temperature passivation treatment.

[0043] Tests showed that the coating adhesion of the DPC ceramic substrate in this embodiment reached 35 N / mm, with no microcracks in the substrate, substrate warpage ≤0.1%, and no coating peeling or circuit failure after 1000 cycles of thermal cycling. Its precision and reliability far exceed those of products made with traditional processes.

[0044] Example 2: A 0.2 mm thick alumina was selected as the ceramic substrate 10. After ultrasonic cleaning and drying of the ceramic substrate 10 with ethanol and deionized water, a picosecond laser was used for full-area scanning etching with a laser power of 6 W and a scanning speed of 1500 mm / s to form a laser micro-modified texture layer 20 with a depth of 0.8 μm.

[0045] The laser-modified textured layer 20 was activated for 3 min using room-temperature argon-oxygen plasma. Subsequently, a low-temperature seed layer 30 was prepared using HPPMS high-power pulsed magnetron sputtering combined with ion-assisted deposition: first, a titanium bonding layer was deposited with a peak pulse power density of 1 kW / cm², a pulse frequency of 50 Hz, a pulse width of 50 μs, a substrate negative bias of -50 V, an argon working pressure of 0.3 Pa, a deposition temperature of 100 °C, an argon ion beam assist energy of 100 eV, and a beam current density of 0.1 mA / cm², resulting in a titanium bonding layer thickness of 0.05 μm; then, a copper conductive layer was deposited with a peak pulse power density of 1 kW / cm², a pulse frequency of 50 Hz, a pulse width of 100 μs, a substrate negative bias of -50 V, an argon working pressure of 0.4 Pa, and a deposition temperature of 100 °C, resulting in a copper conductive layer thickness of 0.25 μm. The total thickness of the low-temperature seed layer 30 was 0.3 μm, with dense, full-coverage, and uninterrupted honeycomb texture.

[0046] A 30μm thick copper layer was prepared on the surface of the low-temperature seed layer 30 by low-temperature pulse electroplating, and a high-precision DPC circuit was formed by photolithography etching. The DPC precision copper circuit layer 40 was then prepared by room temperature passivation treatment.

[0047] Tests showed that the coating adhesion of the DPC ceramic substrate in this embodiment reached 34 N / mm, with no microcracks in the substrate, substrate warpage ≤0.1%, and no coating peeling or circuit failure after 1000 cycles of thermal cycling. Its precision and reliability far exceed those of products made with traditional processes.

[0048] Example 3: A 0.4 mm thick aluminum nitride was selected as the ceramic substrate 10. After ultrasonic cleaning and drying of the ceramic substrate 10 with ethanol and deionized water, a femtosecond laser full-domain scanning etching was performed with a laser power of 5 W and a scanning speed of 2400 mm / s to form a laser micro-modified texture layer 20 with a depth of 1.4 μm.

[0049] The laser-modified textured layer 20 was activated for 8 min using room-temperature argon-oxygen plasma. Subsequently, a low-temperature seed layer 30 was prepared using HPPMS high-power pulsed magnetron sputtering combined with ion-assisted deposition: first, a titanium bonding layer was deposited with a peak pulse power density of 3 kW / cm², a pulse frequency of 200 Hz, a pulse width of 200 μs, a substrate negative bias of -150 V, an argon working pressure of 0.8 Pa, a deposition temperature of 150 °C, an argon ion beam assist energy of 300 eV, and a beam current density of 0.5 mA / cm², resulting in a titanium bonding layer thickness of 0.1 μm; then, a copper conductive layer was deposited with a peak pulse power density of 2.5 kW / cm², a pulse frequency of 150 Hz, a pulse width of 200 μs, a substrate negative bias of -120 V, an argon working pressure of 0.7 Pa, and a deposition temperature of 150 °C, resulting in a copper conductive layer thickness of 0.5 μm. The total thickness of the low-temperature seed layer 30 was 0.6 μm, with dense, full-coverage, and uninterrupted honeycomb texture.

[0050] A 50μm thick copper layer was prepared on the surface of the low-temperature seed layer 30 by low-temperature pulse electroplating, and a high-precision DPC circuit was formed by photolithography etching. The DPC precision copper circuit layer 40 was then prepared by room temperature passivation treatment.

[0051] Tests showed that the coating adhesion of the DPC ceramic substrate in this embodiment reached 36 N / mm, with no microcracks in the substrate, substrate warpage ≤0.1%, and no coating peeling or circuit failure after 1000 cycles of thermal cycling. Its precision and reliability far exceed those of products made with traditional processes.

[0052] Example 4: A 0.5 mm thick alumina was selected as the ceramic substrate 10. After ultrasonic cleaning and drying of the ceramic substrate 10 with ethanol and deionized water, a nanosecond laser full-area scanning etching was performed with a laser power of 10 W and a scanning speed of 500 mm / s to form a laser micro-modified texture layer 20 with a depth of 1.5 μm.

[0053] The laser-modified textured layer 20 was activated for 6 min using room-temperature argon-oxygen plasma. Subsequently, a low-temperature seed layer 30 was prepared using HPPMS high-power pulsed magnetron sputtering combined with ion-assisted deposition: first, a titanium bonding layer was deposited with a peak pulse power density of 2.5 kW / cm², a pulse frequency of 150 Hz, a pulse width of 150 μs, a substrate negative bias of -120 V, an argon working pressure of 0.6 Pa, a deposition temperature of 130 °C, an argon ion beam assist energy of 250 eV, and a beam current density of 0.4 mA / cm², resulting in a titanium bonding layer thickness of 0.09 μm; then, a copper conductive layer was deposited with a peak pulse power density of 2 kW / cm², a pulse frequency of 120 Hz, a pulse width of 180 μs, a substrate negative bias of -100 V, an argon working pressure of 0.5 Pa, and a deposition temperature of 130 °C, resulting in a copper conductive layer thickness of 0.31 μm. The total thickness of the low-temperature seed layer 30 was 0.4 μm, with dense, full-coverage, and uninterrupted honeycomb texture.

[0054] A 35μm thick copper layer was prepared on the surface of the low-temperature seed layer 30 by low-temperature pulse electroplating, and a high-precision DPC circuit was formed by photolithography etching. The DPC precision copper circuit layer 40 was then prepared by room temperature passivation treatment.

[0055] Tests showed that the coating adhesion of the DPC ceramic substrate in this embodiment reached 35 N / mm, with no microcracks in the substrate, substrate warpage ≤0.1%, and no coating peeling or circuit failure after 1000 cycles of thermal cycling. Its precision and reliability far exceed those of products made with traditional processes.

[0056] Example 5: A 0.25 mm thick aluminum nitride was selected as the ceramic substrate 10. After ultrasonic cleaning and drying of the ceramic substrate 10 with ethanol and deionized water, a picosecond laser was used for full-area scanning etching with a laser power of 9 W and a scanning speed of 1200 mm / s to form a laser micro-modified texture layer 20 with a depth of 0.9 μm.

[0057] The laser-modified textured layer 20 was activated for 7 min using room-temperature argon-oxygen plasma. Subsequently, a low-temperature seed layer 30 was prepared using HPPMS high-power pulsed magnetron sputtering combined with ion-assisted deposition: first, a titanium bonding layer was deposited with a peak pulse power density of 1.8 kW / cm², a pulse frequency of 120 Hz, a pulse width of 120 μs, a substrate negative bias of -90 V, an argon working pressure of 0.45 Pa, a deposition temperature of 110 °C, an argon ion beam assist energy of 180 eV, a beam current density of 0.25 mA / cm², and a titanium bonding layer thickness of 0.06 μm; then, a copper conductive layer was deposited with a peak pulse power density of 1.6 kW / cm², a pulse frequency of 100 Hz, a pulse width of 140 μs, a substrate negative bias of -70 V, an argon working pressure of 0.55 Pa, a deposition temperature of 110 °C, and a copper conductive layer thickness of 0.29 μm. The total thickness of the low-temperature seed layer 30 was 0.35 μm, with dense, full-coverage, and uninterrupted honeycomb texture.

[0058] A 45μm thick copper layer was prepared on the surface of the low-temperature seed layer 30 by low-temperature pulse electroplating, and a high-precision DPC circuit was formed by photolithography etching. The DPC precision copper circuit layer 40 was then prepared by room temperature passivation treatment.

[0059] Tests showed that the coating adhesion of the DPC ceramic substrate in this embodiment reached 38 N / mm, with no microcracks in the substrate, substrate warpage ≤0.1%, and no coating peeling or circuit failure after 1000 cycles of thermal cycling. Its precision and reliability far exceed those of products made with traditional processes.

[0060] Example 6: A 0.35 mm thick aluminum nitride was selected as the ceramic substrate 10. After ultrasonic cleaning and drying of the ceramic substrate 10 with ethanol and deionized water, a femtosecond laser full-domain scanning etching was performed with a laser power of 12 W and a scanning speed of 3000 mm / s to form a laser micro-modified texture layer 20 with a depth of 1.0 μm.

[0061] The laser-modified textured layer 20 was activated for 4 min using room-temperature argon-oxygen plasma. Subsequently, a low-temperature seed layer 30 was prepared using HPPMS high-power pulsed magnetron sputtering combined with ion-assisted deposition: first, a titanium bonding layer was deposited with a peak pulse power density of 2.2 kW / cm², a pulse frequency of 130 Hz, a pulse width of 110 μs, a substrate negative bias of -110 V, an argon working pressure of 0.55 Pa, a deposition temperature of 125 °C, an argon ion beam assist energy of 220 eV, a beam current density of 0.35 mA / cm², and a titanium bonding layer thickness of 0.07 μm; then, a copper conductive layer was deposited with a peak pulse power density of 1.8 kW / cm², a pulse frequency of 110 Hz, a pulse width of 160 μs, a substrate negative bias of -90 V, an argon working pressure of 0.5 Pa, a deposition temperature of 125 °C, and a copper conductive layer thickness of 0.38 μm. The total thickness of the low-temperature seed layer 30 was 0.45 μm, with dense, full-coverage, and uninterrupted honeycomb texture.

[0062] A 40μm thick copper layer was prepared on the surface of the low-temperature seed layer 30 by low-temperature pulse electroplating, and a high-precision DPC circuit was formed by photolithography etching. The DPC precision copper circuit layer 40 was then prepared by room temperature passivation treatment.

[0063] Tests showed that the coating adhesion of the DPC ceramic substrate in this embodiment reached 36 N / mm, with no microcracks in the substrate, substrate warpage ≤0.1%, and no coating peeling or circuit failure after 1000 cycles of thermal cycling. Its precision and reliability far exceed those of products made with traditional processes.

[0064] The key design focus of this invention is that it completely abandons the traditional high-temperature acid-base chemical roughening process. Instead, it employs laser micro-modification technology to construct a uniform and controllable honeycomb interlocking texture on the surface of a ceramic substrate. The entire pretreatment process does not involve any chemical etching solutions, causing no corrosion or grain boundary damage to the ceramic substrate. This fundamentally eliminates the microcrack problem introduced by selective grain boundary corrosion in traditional processes, fully preserving the original mechanical strength and thermal conductivity of the ceramic substrate, and significantly improving the overall reliability of the substrate. Simultaneously, this invention uses HPPMS high-power pulsed magnetron sputtering combined with ion-assisted deposition to prepare a titanium-copper composite seed layer. Utilizing the high kinetic energy and wide-angle scattering of the high-ionization metal particles in HPPMS, it achieves excellent step coverage and dense filling within the honeycomb micro-texture pits, overcoming the defect of discontinuous film layers at the bottom of pits caused by traditional DC magnetron sputtering line-of-sight deposition. The titanium bonding layer forms a Ti-O chemical bond with the ceramic interface, superimposed with mechanical interlocking of the honeycomb texture, achieving dual interface strengthening. The coating has high adhesion and good consistency, meeting the requirements of high-reliability packaging scenarios such as automotive and aerospace applications. Furthermore, this invention employs a low-temperature processing technique throughout, with seed layer deposition and copper circuit fabrication both completed below 200°C. This eliminates the thermal stress accumulation and substrate warping issues caused by traditional multi-stage high-temperature processes, resulting in excellent substrate flatness and achieving the precision and dimensional consistency required for the fabrication of miniaturized DPC products. Finally, the entire fabrication process of this invention generates no fluorine- or heavy metal-containing chemical wastewater. HPPMS is a vacuum physical deposition process, eliminating the consumption of chemical plating solutions and the risk of hydrogen evolution, making it environmentally friendly. Moreover, both the laser process and HPPMS process parameters are digitally controllable, resulting in superior mass production consistency and stability compared to traditional chemical coarsening routes. This provides a practical and feasible technical path for the large-scale, green mass production of high-end DPC ceramic substrates.

[0065] The technical principles of the present invention have been described above with reference to specific embodiments. These descriptions are merely for explaining the principles of the invention and should not be construed as limiting the scope of protection of the invention in any way. Based on this explanation, those skilled in the art can readily conceive of other specific embodiments of the invention without inventive effort, and these embodiments will all fall within the scope of protection of the present invention.

Claims

1. A laser-modified DPC ceramic substrate with high adhesion, characterized in that: It includes a ceramic substrate, a laser-modified texture layer, a low-temperature seed layer, and a DPC precision copper circuit layer; the laser-modified texture layer is formed on the surface of the ceramic substrate by laser etching; the low-temperature seed layer densely fills and covers the laser-modified texture layer; and the DPC precision copper circuit layer is formed on the surface of the low-temperature seed layer.

2. The laser-modified high-adhesion DPC ceramic substrate according to claim 1, characterized in that: The laser-modified textured layer is a nano-micro composite honeycomb micro-interlocking textured layer.

3. The laser-modified high-adhesion DPC ceramic substrate according to claim 1, characterized in that: The depth of the laser-modified texture layer is 0.8–1.5 μm, and the laser source used for the laser-modified texture layer is a nanosecond, picosecond, or femtosecond cold processing laser source.

4. The laser-modified high-adhesion DPC ceramic substrate according to claim 1, characterized in that: The low-temperature seed layer is a titanium-copper composite layer deposited by HPPMS high-power pulsed magnetron sputtering / ion-assisted deposition, which includes a titanium bonding layer bonded to the ceramic substrate interface and a copper conductive layer covering the surface of the titanium bonding layer.

5. The laser-modified high-adhesion DPC ceramic substrate according to claim 4, characterized in that: The thickness of the low-temperature seed layer is 0.3–0.6 μm, wherein the thickness of the titanium bonding layer is 0.05–0.1 μm and the thickness of the copper conductive layer is 0.25–0.5 μm.

6. The laser-modified high-adhesion DPC ceramic substrate according to claim 1, characterized in that: The thickness of the ceramic matrix is ​​0.2 to 0.5 mm.

7. The laser-modified high-adhesion DPC ceramic substrate according to claim 1, characterized in that: The ceramic matrix is ​​made of aluminum nitride or aluminum oxide.

8. A low-temperature preparation process for laser-modified high-adhesion DPC ceramic substrates as described in any one of claims 1-7, characterized in that: Includes the following steps: S1. Precision cleaning of the substrate: The ceramic substrate is treated with ultrasonic degreasing, deionized water rinsing and cold air drying to ensure that the surface of the ceramic substrate is clean and free of impurities. S2. Laser microtexture modification: A cold-processing laser light source is used to perform full-area scanning etching on the surface of the ceramic substrate. The laser power and scanning speed are controlled to construct a uniform nano-micro composite honeycomb micro-interlocking texture to form a laser micro-modified texture layer. S3. Low-temperature plasma activation: The surface of the laser micro-modified textured layer is activated by room-temperature argon-oxygen plasma to improve the surface energy and wettability of the ceramic substrate. S4. Low-temperature HPPMS seed layer deposition: Using HPPMS high-power pulsed magnetron sputtering combined with ion-assisted deposition process, a titanium bonding layer and a copper conductive layer are sequentially deposited on the surface of the laser micro-modified texture layer. By utilizing the high kinetic energy and large-angle scattering characteristics of high ionization metal particles, excellent step coverage and dense filling of the pits inside the honeycomb micro-texture are achieved, so as to form a continuous and complete low-temperature seed layer as a conductive substrate. S5. Low-temperature electroplating forming circuit: Low-temperature pulse electroplating is used to thicken the copper layer on the surface of the low-temperature seed layer, and photolithography is used to etch the DPC precision copper circuit layer. S6. Room temperature passivation test: The coating adhesion, circuit accuracy and conductivity are tested by using room temperature passivation treatment.

9. The low-temperature preparation process of laser-modified high-adhesion DPC ceramic substrate according to claim 8, characterized in that: In step S2, the power of the cold processing laser source is 5-30W, and the scanning speed is 200-6000mm / s.

10. The low-temperature preparation process of laser-modified high-adhesion DPC ceramic substrate according to claim 8, characterized in that: The process parameters for HPPMS high-power pulsed magnetron sputtering in step S4 are as follows: peak pulse power density 1-3 kW / cm², pulse frequency 50-200 Hz, pulse width 50-200 μs, substrate negative bias voltage -50 to -150 V, argon working pressure 0.3-0.8 Pa, and deposition temperature ≤150 °C; ion-assisted deposition is performed using argon ion beam assistance, with ion beam energy of 100-300 eV and ion beam current density of 0.1-0.5 mA / cm².