A vacuum two-fluid PCB fine circuit etching method

By employing a vacuum two-fluid PCB fine circuit etching method, which combines the fluid coupling balance of vacuum negative pressure and two-fluid jet with chemical bonding treatment, the problems of fine circuit etching and high-frequency signal transmission in high-frequency and high-speed PCBs have been solved, achieving copper circuit etching effects with high uniformity and low loss.

CN123124221APending Publication Date: 2026-11-17PUTIAN HANJIANG YD PCB CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611018187.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for etching fine lines on high-frequency, high-speed printed circuit boards (PCBs) suffer from a contradiction between insufficient microfluidic penetration and macro-fluid exchange obstruction, leading to lateral etching and uniformity degradation of the lines. At the same time, high-frequency signal transmission faces a process paradox between skin effect loss and lamination bonding force, making it difficult to achieve highly uniform fine lines and low-loss transmission.

Method used

The vacuum two-fluid PCB fine line etching method is adopted. By utilizing the fluid coupling balance between vacuum negative pressure and the mixed micro-droplets sprayed by the two-fluid nozzle during horizontal transmission, the etching solution is effectively replaced. Then, a metal bridging layer and an organosilane coupling agent are chemically deposited on the copper line surface to form a copper line with low surface roughness.

Benefits of technology

A highly uniform and fine circuit without side etching was obtained, and the surface roughness of the copper was controlled within the range of 0.1μm~0.3μm. A non-discontinuous and dense cladding of the nanoscale thick metal bridging layer was achieved, which improved the interlayer adhesion strength and the low-loss transmission of high-frequency signals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124221A_ABST
    Figure CN123124221A_ABST
Patent Text Reader

Abstract

This invention relates to the field of printed circuit board manufacturing technology, specifically to a vacuum two-fluid PCB fine line etching method, comprising the following steps: S100, providing a copper-clad laminate and fabricating a dry film mask pattern on the surface of the copper-clad laminate; S200, sending the copper-clad laminate with the dry film mask pattern into an etching chamber for horizontal transport, applying a vacuum negative pressure above the transport area of ​​the copper-clad laminate, and using a two-fluid nozzle below to spray mixed micro-droplets containing etching solution and gas for etching; This invention constructs a fluid dynamic coupling mechanism of upper vacuum negative pressure suction and lower two-fluid mixed micro-droplet spraying in a horizontal etching chamber, utilizing the upward negative pressure to overcome the surface tension of the liquid film retained on the board surface, while simultaneously giving the micro-droplets sufficient vertical kinetic energy to penetrate deep and narrow mask trenches with an aspect ratio greater than 1.0, thereby obtaining highly uniform fine lines without side etching, and strictly controlling the micro-roughness of the copper surface within an extremely low range of 0.1μm~0.3μm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of printed circuit board manufacturing technology, specifically to a vacuum two-fluid PCB fine line etching method. Background Technology

[0002] As high-frequency, high-speed printed circuit boards (PCBs) evolve towards high-density interconnects, extremely high demands are placed on the precision of metal traces (e.g., 30μm~50μm line width / spacing) and the low-loss performance of high-frequency signal transmission. Current horizontal transfer etching processes mainly face the following two core technological shortcomings: First, in the fine-line etching process, there is a contradiction between insufficient micro-fluid penetration and macro-fluid exchange obstruction. On the one hand, the etching droplets generated by traditional single-fluid nozzles are usually larger than 50μm in diameter. Due to the surface tension of the liquid, large-diameter droplets lack sufficient vertical penetration energy and cannot penetrate to the bottom of fine dry film mask trenches with an aspect ratio greater than 1.0, resulting in delayed reaction at the bottom of the deep trench and severe lateral etching of the lines. On the other hand, during horizontal transmission, reaction waste liquid inevitably accumulates in the central area of ​​the copper-clad laminate, forming a stagnant liquid film that prevents fresh etching liquid from contacting the copper surface. This leads to a significant difference in etching rate between the central and edge areas, which in turn causes a deterioration in the linewidth uniformity of the entire board and makes it impossible to stably obtain fine lines with vertical cross-sections.

[0003] Secondly, high-frequency signal transmission suffers from a process paradox between skin effect loss and lamination bonding strength. At high frequencies (above 10 GHz), high-frequency alternating current primarily transmits within the extremely shallow skin depth of the copper trace surface. Traditional processes, to ensure interlayer peel strength during multilayer PCB lamination, commonly employ micro-etching to achieve high surface roughness (typically Ra > 1.0 μm) on the copper trace surface to generate mechanical anchoring force. However, the high roughness micro-ripples significantly lengthen the actual transmission path of high-frequency signals, leading to severe signal insertion loss. Although the industry has attempted to introduce non-roughening chemical adhesion promotion processes (such as depositing extremely thin metal layers), these nanoscale chemical layers have extremely stringent requirements on substrate morphology. Traditional etching processes cannot consistently provide a substrate with extremely low and uniform surface roughness, causing micro-fractures and structural tears in the extremely thin chemically adhered layer at roughness peaks and valleys, resulting in chemical bonding failure and ultimately lamination delamination defects. Summary of the Invention

[0004] To achieve the above objectives, the present invention provides the following technical solution: This invention provides a vacuum two-fluid PCB fine line etching method, including the following steps: S100, providing a copper-clad laminate and forming a dry film mask pattern on the surface of the copper-clad laminate; S200: The copper-clad laminate with the dry film mask pattern is fed into the etching chamber for horizontal transport. A vacuum negative pressure is applied above the transport area of ​​the copper-clad laminate, and a mixed micro-droplet containing etching solution and gas is sprayed from below using a two-fluid nozzle for etching. The fluid coupling balance between the upward suction force of the vacuum negative pressure and the downward penetration kinetic energy of the mixed micro-droplet is used to displace the etching solution in the gap of the dry film and control the copper line after etching to be in a low surface roughness state. S300: Peel off the residual dry film on the copper circuit and clean it; S400. For the copper circuit in the low surface roughness state, perform non-roughening surface treatment: chemically deposit a metal bridging layer on the surface of the copper circuit, and then coat the surface of the metal bridging layer with an organosilane coupling agent so that one end of the organosilane coupling agent is chemically bonded to the metal bridging layer, and the other end is used to crosslink with the resin medium to be subsequently pressed.

[0005] Furthermore, step S100 specifically includes the following sub-steps: S110. Provide a high-frequency, high-speed copper-clad laminate substrate, and perform a micro-roughening pretreatment on the copper surface of the substrate; S120. Under vacuum conditions, a photoresist dry film is laminated onto the pretreated copper surface, wherein the photoresist dry film is a dry film with a resolution of less than 50 μm. S130. The photoresist dry film is aligned and exposed using a preset fine line mask. S140. Develop the exposed photoresist dry film to remove the dry film in the unexposed areas, so as to expose the trenches to be etched on the copper surface and form the dry film mask pattern.

[0006] Further, in step S140, the opening width of the trench to be etched exposed after development is 30μm~50μm, and the aspect ratio of the depth of the trench to the opening width is greater than or equal to 1.0; the trench to be etched allows the mixed microdroplets in step S200 to penetrate. When providing the copper-clad laminate, the thickness of the initial thick copper layer to be patterned on the outer layer of the copper-clad laminate is greater than or equal to 18 μm.

[0007] Furthermore, in step S200, the specific method for horizontal transport and differentiated spraying of the copper-clad laminate is as follows: Along the transmission width direction of the copper-clad laminate, the etching area is divided into a central spray area and edge spray areas located on both sides of the central spray area; the two-fluid nozzles disposed below the etching chamber are correspondingly divided into a central nozzle group and an edge nozzle group. During the etching process, by independently adjusting the gas-liquid mixing ratio of the central nozzle group, the spraying pressure of the mixed micro-droplets ejected by the central nozzle group is 15% to 25% higher than that of the edge nozzle group, in order to compensate for the slowdown in etching rate caused by the accumulation of liquid film on the board surface in the central spray area.

[0008] Furthermore, in step S200, the fluid coupling balance between the vacuum negative pressure and the downward penetration kinetic energy of the mixed microdroplets is achieved through the following dynamic feedback control logic: A pressure sensor is installed inside the etching chamber to monitor the fluctuation of the vacuum negative pressure in real time. When the absolute value of the vacuum negative pressure increases to a set threshold, causing some of the mixed microdroplets to rise and escape, the control system proportionally increases the opening of the compressed air inlet valve of the two-fluid nozzle according to the fluctuation value, so as to increase the downward vertical penetration kinetic energy of the mixed microdroplets until the mixed microdroplets return to the state of penetrating the gap of the dry film mask pattern downward.

[0009] Furthermore, in step S200, the relevant fluid dynamic parameters are strictly controlled within the following window: The absolute pressure of the vacuum negative pressure is controlled to be between 5 kPa and 20 kPa; the gas-liquid mass ratio of the mixed microdroplets ejected by the two-fluid nozzle is controlled to be between (0.5~1.5):1, and the velocity of the mixed microdroplets impacting the copper-clad laminate surface vertically downward is controlled to be between 20 m / s and 40 m / s.

[0010] Furthermore, in step S200, the microstructure of the etched copper circuit meets the following requirements: The surface roughness Ra of the top surface, sidewalls and base copper surface of the copper circuit is 0.1μm~0.3μm, and the included angle between the sidewall of the copper circuit and the surface of the copper clad laminate substrate is controlled between 88° and 90° to form a fine circuit with a vertical cross-section without side etching.

[0011] Further, step S300 specifically includes: After the residual dry film is peeled off with an alkaline stripping solution, the following steps are performed in sequence: initial pure water rinsing, non-micro-corrosion deoxidation and activation treatment, and secondary pure water rinsing. The non-micro-etching deoxidation activation treatment uses a dilute acid solution with a volume fraction of 3% to 5% to remove copper surface oxides and expose fresh pure copper crystal surfaces for chemical deposition in step S400 without increasing the surface roughness of the copper circuit and maintaining the low surface roughness state. During the initial and secondary pure water cleaning processes, megasonic waves are introduced to assist in the pure water spraying. The frequency of the megasonic waves is controlled between 0.8MHz and 1.2MHz. This is to utilize the high-frequency micro cavitation effect to remove organic residues at the bottom of the gaps in the fine lines and to avoid physical impact damage to the sidewalls of the copper lines with vertical cross-sections.

[0012] Furthermore, in step S400, the specific process conditions and composition of the chemical deposition of the continuous tin alloy layer are limited as follows: The temperature of the deposition solution is controlled at 60℃~80℃, and the immersion time of the copper-clad laminate is controlled at 1min~3min; The continuous tin alloy layer is a microalloy layer containing tin and silver elements, wherein the mass fraction of silver is controlled between 1% and 3% to further suppress the growth of tin whiskers on the surface of the metal bridging layer and reduce the surface resistance of the conductor under the skin effect while achieving contour wrapping.

[0013] Furthermore, in step S400, the specific material matching for the 5G high-frequency signal transmission scenario is limited as follows: The organosilane coupling agent is selected from one or more end-group silane coupling agents containing epoxy, amino, or vinyl groups; The low dielectric constant resin medium is selected from polytetrafluoroethylene, polyphenylene ether, or liquid crystal polymer, and the organic active functional groups extended outward by the organosilane coupling agent undergo matched crosslinking with the low dielectric constant resin medium. The key heat treatment process for achieving interfacial chemical bonding is: The conditions for baking and drying after coating with the organosilane coupling agent are set as follows: baking at a temperature of 100℃~150℃ for 10min~30min; The heat treatment process provides the activation energy required for the dehydration condensation reaction, driving the complete evaporation of water molecules at the interface and ensuring the irreversible compaction of the tin-oxygen-silicon inorganic covalent bonds. Beneficial effects

[0014] This invention constructs a fluid dynamic coupling mechanism within a horizontal etching chamber, combining upper vacuum negative pressure suction with lower two-fluid mixing microdroplet spraying. The upward negative pressure overcomes the surface tension of the liquid film remaining on the board surface, while simultaneously providing sufficient vertical kinetic energy to the microdroplets to penetrate deep, narrow mask trenches with an aspect ratio greater than 1.0. This results in highly uniform and fine lines without lateral etching, and strictly controls the micro-roughness of the copper surface within an extremely low range of 0.1 μm to 0.3 μm. Furthermore, using this low-roughness, smooth morphology as a physical substrate, it achieves seamless, dense encapsulation of a nanoscale thick metal bridging layer and effective chemical bonding with an organosilane coupling agent. This constructs a high-peel-strength interlayer adhesion structure under the premise of zero micro-etching coarsening, resolving the technical contradiction between the difficulty of micro-fluid displacement in deep trenches and the transmission loss due to the skin effect of high-frequency signals. Attached Figure Description

[0015] Figure 1 This is a general process flow diagram of the present invention; Figure 2 These are comparative images of the microscopic cross-sections of the ultra-low roughness interface chemical bonding of the present invention. Figure 3 This is a flowchart of the vacuum two-fluid fluid coupling closed-loop control of the present invention; Figure 4 This is a flowchart of the low-loss surface interface chemical bonding process of the present invention. Detailed Implementation

[0016] To enable those skilled in the art to better understand the present invention, the technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of the present invention.

[0017] It should be noted that the terms "first," "second," etc., in the specification, claims, and accompanying drawings of this invention are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments of the invention described herein can be implemented in orders other than those illustrated or described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover a non-exclusive inclusion; for example, a process, method, system, product, or apparatus that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but includes other steps or units not explicitly listed or inherent to such processes, methods, products, or apparatus.

[0018] The present invention will now be described in further detail with reference to the accompanying drawings: Example

[0019] like Figures 1-4 As shown, a vacuum two-fluid PCB fine circuit etching method includes the following steps: S100: Provide a copper-clad laminate and fabricate a dry film mask pattern on the surface of the copper-clad laminate; S200: The copper-clad laminate with the dry film mask pattern is sent into the etching chamber for horizontal transport. A vacuum negative pressure is applied above the copper-clad laminate transport area, and a two-fluid nozzle is used below to spray mixed micro-droplets containing etching solution and gas for etching. The fluid coupling balance between the upward suction force of the vacuum negative pressure and the downward penetration kinetic energy of the mixed micro-droplets is used to replace the etching solution in the gap of the dry film and control the copper line after etching to be in a low surface roughness state. S300: Remove residual dry film from copper traces and clean. S400. Non-roughening surface treatment for copper circuits in a low surface roughness state: chemically deposit a metal bridging layer on the surface of the copper circuit, and then coat the surface of the metal bridging layer with an organosilane coupling agent so that one end of the organosilane coupling agent is chemically bonded to the metal bridging layer, and the other end is used to crosslink with the resin medium of subsequent lamination.

[0020] Furthermore, the specific implementation process of step S100 is as follows: A copper-clad laminate is provided, and a dry film mask pattern with a feature pitch of 30μm to 50μm is formed on the surface of the copper-clad laminate. Step S100 specifically includes pretreatment, vacuum lamination, exposure, and development and forming steps for high aspect ratio trenches on a high-frequency, high-speed copper-clad laminate substrate.

[0021] High-frequency, high-speed copper-clad laminate (CCL) substrates are provided, such as double-sided CCLs using polytetrafluoroethylene (PTFE), polyphenylene ether (PPE), or liquid crystal polymer (LCP) resin systems. The initial thick copper layer to be patterned on the outer layer of the CCL has a thickness greater than or equal to 18 μm, preferably between 18 μm and 35 μm. A micro-roughening pretreatment is performed on the surface of the initial thick copper layer of the CCL. The CCL is fed into a horizontal conveyor processing line, and the surface is chemically micro-etched using a mixed micro-etching solution containing hydrogen peroxide and sulfuric acid. The temperature range of the mixed micro-etching solution is controlled between 30°C and 35°C, and the processing time is set to 1 to 2 minutes. After chemical micro-etching, a multi-stage countercurrent rinsing with pure water and forced hot air drying are performed sequentially to achieve a copper surface roughness Ra value of 0.2 μm to 0.4 μm, forming a pure copper crystal surface with microscopic geometric irregularities.

[0022] In a vacuum environment, a photoresist dry film is laminated onto the pretreated copper surface. A fine-line dry film with a resolution of less than 50 μm and a thickness parameter set to 35 μm to 50 μm is selected. The copper-clad laminate is fed into the operating chamber of the vacuum laminator, and the vacuum pump is started to evacuate the operating chamber to a vacuum level of -90 kPa to -98 kPa. After reaching the preset vacuum level, the heating and lamination components are started, controlling the surface temperature of the lamination rollers to 100℃ to 115℃, the lamination line pressure to 0.3 MPa to 0.5 MPa, and the lamination drive speed to 1.5 m / min to 2.5 m / min. The lamination operation under vacuum negative pressure forces out the tiny air residues between the dry film and the slightly roughened copper surface, achieving tight filling of the micro-geometric unevenness of the dry film resin under hot pressing.

[0023] A pre-set fine-line photomask is used to align and expose the laminated photoresist dry film. A laser direct imaging (LDI) system is used as the exposure light source, selecting an ultraviolet laser source with a peak wavelength of 355nm or 405nm. An optical target on the edge of the copper-clad laminate is captured by a CCD vision alignment system to align the photomask pattern data with the physical position of the copper-clad laminate. The exposure energy received on the surface of the photoresist dry film is controlled to be between 150mJ / cm² and 250mJ / cm², causing the dry film in the light-receiving area to undergo a polymerization and cross-linking reaction, forming a polymer insoluble in the developer.

[0024] The exposed photoresist dry film is developed to remove unexposed areas, exposing the trenches to be etched on the copper surface, ultimately forming the dry film mask pattern. The developing solution is a 0.8% to 1.2% (w / w) anhydrous sodium carbonate aqueous solution. The operating temperature of the developing solution is controlled between 28°C and 32°C, and the nozzle spray pressure in the developing chamber is set between 0.15 MPa and 0.25 MPa. Development and rinsing dissolve and remove areas where no cross-linking reaction has occurred. After development, the aforementioned trenches to be etched expose the underlying pure copper substrate. The opening width of the trenches to be etched is measured, with the value controlled between 30 μm and 50 μm. Combined with the selected photoresist dry film with a thickness of 35μm to 50μm, the thickness of the cross-linked dry film retained on the surface of the copper clad laminate and the width of the trench opening to be etched constitute a deep and narrow geometric structure. The aspect ratio of the depth of the trench to be etched to the opening width is calculated to be strictly greater than or equal to 1.0, and the angle between the sidewall of the trench to be etched and the bottom copper surface presents a vertical rectangular or trapezoidal cross section, which is used for subsequent steps to mix microdroplets for deep hole penetration.

[0025] Specific experimental scenario: Experimental materials and equipment preparation: A Rogers RO4350B high-frequency copper-clad laminate substrate with dimensions of 18 inches × 24 inches and a dielectric layer thickness of 0.508 mm was selected, with electrolytic copper foil of initial thickness of 18 μm attached to both outer layers. A special high-resolution photoresist dry film with a nominal thickness of 50 μm and a nominal resolution of 25 μm, manufactured by DuPont, was used.

[0026] Implementation process parameter record: A 500L micro-etching solution was prepared, with sulfuric acid concentration maintained at 20g / L and hydrogen peroxide concentration maintained at 30g / L. The copper-clad laminate was horizontally conveyed through the micro-etching tank at a speed controlled at 1.2m / min, the solution temperature was kept constant at 32℃, and the actual contact reaction time was measured to be 90 seconds. Random sampling using a coordinate measuring machine (CMM) showed that the average surface roughness Ra of the center and edge areas of the board was 0.28μm.

[0027] The micro-etched copper-clad laminate is fed into the CSUN vacuum laminator. After being evacuated to -95kPa and stabilized for 3 seconds, the cylinder is pressed down. The infrared monitoring value of the surface temperature of the hot roller is 110℃. A lamination pressure of 0.4MPa is applied, and the 50μm thick dry film is laminated at a constant linear speed of 2.0m / min.

[0028] The copper-clad laminate was transferred to the Orbotech LDI laser direct imaging system, and the preset test pattern data of 50μm linewidth / 40μm line spacing was read. The dominant exposure wavelength was set to 405nm, and the total exposure energy was set to 200mJ / cm² to complete the double-sided parallel exposure.

[0029] After exposure and settling for 15 minutes, the sample is fed into the horizontal developing line. A 1.0% sodium carbonate developer solution is prepared, and the developing tank temperature is heated to 30°C. The pressure gauge readings of the upper and lower spray lines are adjusted to 0.2 MPa, the conveyor speed is set to 1.5 m / min, and the measured developing points are controlled within 50% to 60% of the total developing chamber length. After rinsing with pure water and drying with hot air at 80°C, samples are taken for testing.

[0030] Experimental Results Measurement and Cross-Sectional Analysis: Metallurgical microscopy combined with scanning electron microscopy (SEM) was used to perform cross-sectional measurements on the developed board surface. Measurement data showed that the average opening width of the trenches exposed on the copper surface was 40.2 μm, the dry film in the unexposed areas was completely dissolved, and there was no residual adhesive on the bottom copper surface. The measured retained thickness of adjacent cross-linked dry films was 48.5 μm. The calculated actual aspect ratio of the trenches in this experimental scenario was 1.206 (greater than the standard of 1.0). The measured verticality of the dry film development sidewalls was 89.2 degrees, exhibiting a standard vertical geometric cavity structure.

[0031] Furthermore, the specific implementation process of step S200 is as follows: The copper-clad laminate with the dry film mask pattern is fed into the etching chamber for horizontal transport. A vacuum negative pressure is applied above the copper-clad laminate transport area, and a two-fluid nozzle is used below to spray mixed micro-droplets containing etching solution and compressed air for etching.

[0032] The copper-clad laminate, after the aforementioned development steps, is placed on the conveyor rollers of the horizontal etching line. The conveyor roller speed is set to 1.0 m / min to 3.0 m / min. Along the conveying width direction of the copper-clad laminate, the etching area is physically divided proportionally into a central spray area and edge spray areas located on both sides of the central spray area. The width of the central spray area is set to account for 40% of the total conveying width, and the width of each edge spray area accounts for 30% of the total conveying width. The two-fluid nozzles located below the etching chamber are correspondingly divided into a central nozzle group and an edge nozzle group, and the central nozzle group and the edge nozzle group are respectively connected to an independent gas-liquid mixing control valve array.

[0033] Start the etching solution supply pump and air compressor. Supply the acidic etching solution, composed of copper chloride, hydrochloric acid, and hydrogen peroxide, to the two-fluid nozzle, maintaining the temperature of the etching solution entering the nozzle between 45°C and 55°C. Simultaneously introduce compressed air into the two-fluid nozzle, controlling the gas-liquid mass ratio of the mixed microdroplets ejected from the nozzle to be between (0.5~1.5):1 by adjusting the gas-liquid mixing control valve array. The compressed air mechanically shears the etching solution inside the nozzle, generating mixed microdroplets with a particle size distribution between 10μm and 30μm. Adjust the gas-liquid mixing ratio parameters of the central nozzle group, setting the input air pressure and hydraulic parameters of the central nozzle group so that the final spray pressure of the ejected mixed microdroplets is 15%~25% higher than that of the edge nozzle group. Adjust the installation angle of all two-fluid nozzles to vertically upward, and control the speed at which the mixed micro-droplets impact the bottom surface of the copper-clad laminate vertically upward to reach 20m / s~40m / s, so that the mixed micro-droplets in the particle size range of 10μm~30μm can penetrate the deep and narrow grooves to be etched on the bottom surface of the copper-clad laminate with an aspect ratio greater than 1.0.

[0034] While spraying the etching solution upwards, a vacuum suction hood is activated inside the etching chamber, above the copper-clad laminate transfer area. The vacuum pump speed is adjusted to apply and maintain a vacuum pressure of -5 kPa to -20 kPa in the space above the copper-clad laminate. The upward suction force generated by the vacuum pressure overcomes the surface tension of the waste liquid accumulated on the bottom surface of the copper-clad laminate, forcibly removing the etching solution that has lost its activity due to reaction consumption from the central spray area of ​​the board surface.

[0035] The closed-loop feedback control system integrated inside the etching chamber is activated. A pressure sensor located in the upper region of the etching chamber is invoked to collect real-time data on vacuum pressure fluctuations below the vacuum suction hood. A vacuum threshold range is set. When the pressure sensor detects a sudden increase in the absolute value of the vacuum pressure exceeding the set upper threshold, the programmable logic controller (PLC) of the control system generates a linkage control signal. Based on the detected vacuum pressure overshoot, a pulse width modulation (PWM) command is sent to the intake solenoid valves of the central and edge nozzle groups, proportionally increasing the opening of the compressed air intake valves of the two-fluid nozzles. This instantaneous increase in air intake enhances the upward vertical penetration kinetic energy of the mixed microdroplets, counteracting the droplet escape caused by excessive vacuum suction from above, until the pressure sensor feedback value falls back within the threshold range. The hydrodynamic balance formed between the negative pressure suction action and the microdroplet penetration action forcibly displaces the etching solution at the bottom of the gaps in the dry film mask pattern. After the reaction, the etching process yields a fine copper circuit structure.

[0036] Specific experimental scenario: Experimental materials and equipment preparation: The copper-clad laminate (with dry film trenches of 40.2μm aperture width and aspect ratio of 1.206) developed in experiment number Exp-S100-A01 was used. The equipment was a custom-modified horizontal conveyor vacuum etching machine, with Japanese Ikeuchi BIM series micro-atomizing two-fluid nozzles added to the lower spray line, and a titanium alloy negative pressure suction hood driven by a variable frequency Roots vacuum pump installed above.

[0037] Implementation process parameter record: An acidic copper chloride etching solution was prepared, in which the Cu²⁺ concentration was controlled at 130 g / L, the hydrochloric acid (HCl) equivalent concentration was maintained at 2.0 mol / L, and the oxidation potential (ORP) was maintained at 580 mV by automatically adding hydrogen peroxide. The bath temperature was heated and kept constant at 50°C.

[0038] The copper-clad laminate enters the etching chamber at a speed of 2.2 m / min. The upper Roots vacuum pump is turned on, and the pressure gauge reading inside the suction hood stabilizes at -15 kPa.

[0039] Activate the lower two-fluid spray system. Adjust the compressed air input pressure of the edge nozzle group to 0.30 MPa and the etching solution input pressure to 0.15 MPa; adjust the compressed air input pressure of the center nozzle group to 0.36 MPa and the etching solution input pressure to 0.18 MPa (the center spray pressure is approximately 20% higher than the edge pressure). Offline calibration using a laser particle size analyzer verifies that, under the current gas-liquid parameters, the median D50 diameter of the generated droplets is 18.5 μm, and the initial ejection velocity is 28 m / s.

[0040] Within 120 seconds of the copper-clad laminate passing through the etching chamber, the PLC control panel showed two transient fluctuations of -18 kPa from the upper air pressure sensor. The air intake solenoid valve responded and increased the input air pressure by 0.02 MPa instantaneously, maintaining the continuous impact of the atomized droplets on the 50 μm deep trenches, and no backflow of water on the board surface occurred.

[0041] Experimental Results Measurement and Cross-Section Analysis: After the copper-clad laminate (CCL) was produced, it underwent three stages of water washing and drying. Samples were taken for metallographic section analysis. Measurement data showed that the etching uniformity of the central and edge regions was extremely high. The actual measured linewidth of the designed 50μm line was 48.5μm at the top and 50.1μm at the bottom, with an etch factor (EtchFactor) greater than 8.0. The measured angle between the copper circuit sidewall and the CCL substrate surface was 89.5 degrees, exhibiting an almost perpendicular sidewall cross-section. Atomic force microscopy (AFM) was used to measure the top surface and sidewalls of the formed copper circuit within a 5μm × 5μm scanning range. The measured surface roughness Ra was 0.18μm, meeting the technical requirements of being controlled between 0.1μm and 0.3μm, providing a smooth crystalline substrate for subsequent nanoscale chemical processing.

[0042] Furthermore, the specific implementation process of step S300 is as follows: The residual dry film on the copper circuit after etching is peeled off and then cleaned. Step S300 includes a series of operations such as residual dry film peeling, initial pure water rinsing, non-micro-etching deoxidation and activation treatment, and secondary pure water rinsing.

[0043] The copper-clad laminate etched in step S200 is fed into the conveyor track of the horizontal stripping line. An alkaline stripping solution, specifically a 3% to 5% (w / w) sodium hydroxide (NaOH) aqueous solution, is sprayed into the stripping chamber. The heating temperature of the alkaline stripping solution is controlled at 45°C to 55°C, the total spray pressure is set at 0.2 MPa to 0.3 MPa, and the dwell time of the copper-clad laminate in the stripping chamber is controlled at 60 to 90 seconds. The alkaline stripping solution reacts with the residual cross-linked dry film on the copper trace surface through saponification and swelling, causing the residual cross-linked dry film to rupture and detach from the top of the copper trace.

[0044] After the residual dry film detaches, the copper-clad laminate enters the initial pure water cleaning chamber. Deionized pure water is sprayed into the chamber, and a megasonic generator integrated into the spray pipeline is simultaneously activated. The output frequency of the megasonic generator is controlled between 0.8MHz and 1.2MHz, and the megasonic power density is set to 0.5W / cm² to 1.5W / cm². The pure water is heated to 30℃ to 40℃, and a micro-cavitation effect is generated under the high-frequency excitation of the megasonic waves. The pure water spray pressure is set to 0.1MPa to 0.15MPa. The micro-cavitation bubbles collapse at high frequency at the bottom of the fine line gaps at the 50μm level, using micro-jets to physically remove the organic colloidal residue remaining at the bottom of the deep trench. The high-frequency megasonic waves controlled at 0.8MHz to 1.2MHz, due to their extremely short wavelength and uniform distribution of micro-cavitation energy, avoid physical impact deformation or mechanical damage to the sidewalls of the copper lines with vertical cross-sections.

[0045] After the initial pure water cleaning, the copper-clad laminate is transferred to the activation treatment chamber for non-micro-etching oxidation removal activation treatment. A 3%–5% (v / v) dilute sulfuric acid solution is sprayed into the activation treatment chamber. The operating temperature of the dilute sulfuric acid solution is controlled at 20°C to 25°C (room temperature), the spray pressure is set at 0.05 MPa to 0.1 MPa, and the treatment time is strictly controlled between 20 and 40 seconds. The dilute sulfuric acid solution only reacts with the copper oxide (CuO) or cuprous oxide (Cu2O) passivation layer on the surface of the copper circuit to form soluble copper sulfate, which is discharged with the water flow. The low-concentration room-temperature dilute sulfuric acid does not have the redox potential to etch pure copper metal, thus strictly maintaining the low surface roughness state established after etching in step S200 while removing the oxides on the copper surface.

[0046] After undergoing non-micro-etching oxidation activation treatment, the copper-clad laminate enters the secondary pure water cleaning chamber. The megasonic pure water spray system within the secondary pure water cleaning chamber is activated, with the secondary megasonic frequency set to 0.8MHz~1.2MHz. The secondary pure water cleaning removes residual acid and free copper sulfate ions adhering to the copper circuit surface, ultimately exposing a fresh, pure copper crystal surface that has not been damaged by micro-etching and maintains extremely low roughness parameters. The laminate then enters the hot air drying section for forced drying, providing a clean chemical deposition substrate for step S400.

[0047] Specific experimental scenario: Experimental materials and equipment preparation: The high-frequency copper-clad laminate etched with residual dry film as per experiment number Exp-S200-A02 was used. The equipment used was a custom-designed horizontal stripping and cleaning line from Aerospace PCB, with a 1.0MHz megaacoustic transducer array manufactured by Honda Electric Corporation of Japan installed in both the primary and secondary pure water cleaning tanks.

[0048] Implementation process parameter record: Prepare an alkaline stripping solution with a capacity of 300L, adding NaOH to achieve a mass fraction of 4.0%. Set the target temperature of the stripping tank heating system to 50℃. Set the horizontal conveyor roller linear speed to 1.5m / min, and adjust the upper and lower spray pressure gauges to 0.25MPa.

[0049] The copper-clad laminate enters the initial pure water cleaning stage, with the water temperature set at 35℃. A 1.0MHz megasonic generator is turned on, and the power meter displays an output power of 800W. Deionized water performs high-frequency cleaning on the fine circuit gaps under megasonic excitation, with a residence time of 40 seconds.

[0050] The copper-clad laminate was placed into the activation tank. A 4% (v / v) dilute sulfuric acid activation solution was prepared, and heating was not turned on (measured temperature 23°C). The spray pipeline pressure was set to an extremely low 0.08 MPa, and the contact time of the copper-clad laminate in this range was measured to be 30 seconds.

[0051] The copper-clad laminate enters the secondary pure water cleaning section, where a 1.0MHz mega-sonic wave is activated again for final cleaning. Afterward, it is dried by a 100℃ high-pressure air knife before being removed from the board.

[0052] Experimental Results Measurement and Cross-Sectional Analysis: Scanning electron microscopy (SEM) at 5000x magnification was used to observe the resin substrate area at the bottom of the copper trace. The results showed that the copper trace root and substrate surface were extremely clean, without any dry film debris or organic residue, demonstrating the excellent penetration cleaning capability of 1.0MHz mega-sonic cleaning for deep and narrow trenches. A single copper trace was extracted and scanned using atomic force microscopy (AFM), and the surface roughness Ra value of its top and sidewalls was read as 0.182 μm. Compared with the original data of 0.18 μm output in step S200 (Exp-S200-A02), the roughness value did not change significantly, verifying the non-micro-corrosion characteristics of 4% room-temperature dilute sulfuric acid. No microscopic defects were observed on the sidewalls of the copper trace, and the remeasured sidewall angle was 89.5 degrees, maintaining a standard vertical geometry. Furthermore, the specific implementation process of step S400 is as follows: For copper circuits that have undergone step S300 and are in a low surface roughness state, a non-roughening surface treatment is performed. First, a metal bridging layer is chemically deposited on the surface of the copper circuit. The copper-clad laminate with fresh pure copper crystal faces is immersed in a pre-prepared chemical deposition solution. The deposition solution is set to an aqueous solution containing stannous ions, silver ions, thiourea complexing agents, and sodium hypophosphite promoter. The temperature of the deposition solution is adjusted to between 60°C and 80°C. The time for the copper-clad laminate to be completely immersed in the deposition solution is controlled to be between 1 minute and 3 minutes. Under the set temperature and time parameters, stannous ions and silver ions undergo a displacement reduction reaction on the pure copper crystal faces, precipitating on the top and sidewall surfaces of the copper circuit and forming a continuous tin alloy layer, which serves as a physical bridging metal medium.

[0053] The concentration ratio of silver ions in the deposition solution was adjusted to ensure that the precipitated continuous tin alloy layer contained both tin and silver elements, with the silver mass fraction controlled between 1% and 3%. The thickness of the resulting continuous tin alloy layer was strictly controlled to be between 0.05 μm and 0.2 μm. Utilizing the extremely low surface roughness of the copper circuit (Ra = 0.1 μm to 0.3 μm), the replacement-generated ultrathin continuous tin alloy layer conformed to the microscopic undulations, achieving a dense, contour-following encapsulation without physical breaks or pinhole defects that would expose the underlying pure copper.

[0054] After the continuous tin alloy layer is deposited, it is cleaned with deionized water in two stages and dried with cold air. An organosilane coupling agent is then uniformly coated onto the surface of the continuous tin alloy layer. A silane coupling agent containing epoxy, amino, or vinyl groups is selected and dissolved in an alcohol-water mixture to prepare a working solution with a mass concentration of 0.5% to 2.0%. Horizontal dip coating or ultrasonic atomization spraying is used to ensure that the organosilane coupling agent molecules are uniformly adhered to the outer side of the continuous tin alloy layer.

[0055] After coating, the copper-clad laminate is placed in a hot air circulating tunnel oven for baking, drying, and interfacial reaction heat treatment. The thermodynamic baking temperature is set to 100℃ to 150℃, and the baking time is controlled between 10 and 30 minutes. Under the set high-temperature activation conditions, the siloxane groups at one end of the organosilane coupling agent attached to the surface undergo hydrolysis to generate silanol groups. The generated silanol groups then undergo a dehydration condensation reaction with the naturally generated metal hydroxyl groups on the surface of the continuous tin alloy layer. The high temperature provided by the tunnel oven continuously drives the complete evaporation of water molecules at the interface, promoting the irreversible densification of the "tin-oxygen-silicon" inorganic covalent bonds, completing the first-level chemical bonding.

[0056] The organic active functional groups at the other end of the organosilane coupling agent extend radially outward. A low-dielectric-constant resin dielectric prepreg is provided, composed of polytetrafluoroethylene (PTFE), polyphenylene ether (PPE), or liquid crystal polymer (LCP). The copper-clad laminate is stacked with the low-dielectric-constant resin dielectric prepreg and placed in a vacuum press. During the high-temperature, high-pressure pressing process, the outwardly extending organic active functional groups undergo ring-opening or addition reactions with the polymer macromolecular chains inside the low-dielectric-constant resin dielectric, completing the second-level chemical crosslinking. Through the tandem bonding mechanism of inorganic covalent bonds and organic crosslinking, a high-peel-strength interlayer adhesion structure is constructed while maintaining the physical premise of zero coarsening morphology of the underlying pure copper circuitry.

[0057] Specific experimental scenario: Experimental Materials and Equipment Preparation: A high-frequency copper-clad laminate (CCL) that underwent mega-sonic cleaning and activation (as per experiment number Exp-S300-A03) was used (the surface roughness Ra of the copper circuit was measured to be 0.182 μm). A commercially available tin-silver immersion solution was selected, primarily composed of stannous methanesulfonate and silver nitrate. KH-550 (γ-aminopropyltriethoxysilane) was used as the organosilane coupling agent. Rogers RO4450F (a high-frequency, low-loss prepreg based on hydrocarbon resin / ceramic fillers) was used as the lamination substrate.

[0058] Implementation process parameter record: Prepare a 200L immersion tin-silver bath solution, and maintain the bath temperature at a constant 70℃ using the heating system. Vertically immerse the activated copper-clad laminate into the bath solution, and activate the mechanical oscillation device (frequency 15 times / minute). The immersion time is precisely timed to 120 seconds. After removal from the bath, rinse with pure water and dry with cold air.

[0059] The coating parameters were measured using an X-ray fluorescence thickness gauge (XRF). The average thickness of the precipitated alloy layer was determined to be 0.12 μm. Energy dispersive spectroscopy (EDS) was used to analyze the film composition, revealing a silver mass fraction of 1.8% and the remainder being tin. Under a metallographic microscope, the alloy layer exhibited a dense, silvery-white, specular reflective surface with no exposed crystal faces.

[0060] The KH-550 coupling agent stock solution was dissolved in a mixed solvent of deionized water and anhydrous ethanol at a volume ratio of 1:1 to prepare a 1.0% (w / w) silane aqueous solution. The copper-clad laminate was passed through the silane immersion coating tank at a speed of 1.0 m / min, and then fed into a conveyor-type infrared drying oven. The infrared heating tube was set to a temperature of 120℃, and the conveyor belt time was set to 20 minutes to complete dehydration condensation curing.

[0061] The copper-clad laminate coated with silane and the RO4450F prepreg were stacked in a Class 10,000 cleanroom. The laminates were then fed into a vacuum hot press, with the maximum pressing temperature set to 190℃, the main pressure section pressure set to 2.5MPa, and the high-temperature, high-pressure holding time set to 90 minutes. After natural cooling to below 60℃, the laminates were removed from the press.

[0062] Experimental Results Measurement and Performance Analysis: Following the IPC-TM-650 standard peel strength test method, copper circuit samples with a width of 10mm were cut and subjected to a 90-degree pull-out test. The measured peel strength reached 0.85 N / mm (far exceeding the 0.6 N / mm acceptable standard for high-frequency boards). The pull-out fracture occurred within the high-frequency resin medium, indicating that the chemical bonding force at the interface is greater than the cohesive force of the resin itself.

[0063] A 50mm transmission line segment was connected to a vector network analyzer (VNA) for S-parameter loss testing. At a test frequency of 20GHz, the insertion loss per unit length was measured to be -0.62dB / inch. Compared to a reference board of the same specifications prepared using a traditional micro-etching and browning process (Ra = 1.2μm) (test value -0.95dB / inch), this embodiment shows a reduction of approximately 34.7% in signal insertion loss at high frequencies, fully verifying the superior technical effect of ultra-low roughness superimposed with chemical bonding in overcoming skin effect loss.

[0064] Comparative Example 1 (Disruption of fluid coupling: No effective vacuum negative pressure) The developed copper-clad laminate is fed into the horizontal etching line. The lower two-fluid nozzle is turned on, and the mixed microdroplet particle size is controlled to be 18.5 μm. The downward penetration kinetic energy parameters are exactly the same as those in Example Exp-S200-A02. The upper vacuum negative pressure suction hood is turned off (or the negative pressure is set to an invalid -1 kPa).

[0065] Results: Due to the lack of effective upward suction, the high-pressure sprayed etching solution rapidly accumulated in the central spray area, creating a severe puddle effect due to surface tension. The penetrating kinetic energy of the microdroplets was completely absorbed by the accumulated water layer, preventing them from reaching the bottom of the deep, narrow trenches. Metallographic section measurements showed that the copper-clad laminate edge area was over-etched (sidewall angle was only 75 degrees), while the central area contained a large amount of residual copper, with an etching factor of only 3.2 and an extremely low etching yield.

[0066] Comparative Example 2 (Destructive Microscopic Penetration Size: Traditional Large Droplets) The developed copper-clad laminate is fed into the horizontal etching line. The operating parameters of the upper vacuum suction hood are maintained at -15 kPa. The lower part is replaced with a conventional single-fluid spray system, with compressed air assistance turned off, and spraying is done solely by pressurizing the liquid pump. The median D50 diameter of the droplets produced by the single-fluid nozzle is measured to be 65 μm using a laser particle size analyzer.

[0067] Results: Although the vacuum suction above eliminated the puddle effect, the physical size of the single-fluid droplet (65μm) was larger than the opening gap of the dry film mask pattern (40μm). Most droplets were blocked at the top of the dry film, and the reaction could only proceed through natural liquid penetration. Cross-section results showed extremely delayed reaction at the bottom of the trenches. To etch through to the bottom, the etching time had to be extended, leading to catastrophic lateral etching of the upper lines. The top linewidth was reduced to 32μm, completely losing the rectangular cross-sectional morphology of the 50μm fine lines.

[0068] Comparative Example 3 (Destructive Uniformity of Topographic Anchor Points: Traditional High-Roughness Micro-Etching) Fine etching was performed using the vacuum two-fluid parameters of Example Exp-S200-A02 to obtain vertical rectangular lines. However, a conventional sodium persulfate micro-etching roughening process was inserted before proceeding to step S400. The micro-etching depth was controlled at 1.5 μm, which forcibly increased the surface roughness Ra of the copper lines from 0.18 μm to 1.2 μm. Subsequently, the non-roughening surface treatment of S400 was performed, depositing a 0.12 μm thick tin alloy layer and coating it with a silane coupling agent.

[0069] Results: Cross-sectional scanning electron microscopy (SEM) confirmed that, due to the much larger surface roughness of the copper substrate (Ra 1.2 μm) than the deposition thickness of the tin alloy layer (0.12 μm), the extremely thin tin alloy layer experienced severe fracturing and tearing at the roughness peaks and valleys, making dense encapsulation impossible. Subsequent peel strength tests showed a drop to 0.45 N / mm (unacceptable), and due to the rough morphology combined with interface porosity, the signal insertion loss at the 20 GHz band deteriorated to -0.92 dB / inch, completely losing low-loss transmission performance.

[0070] To visually demonstrate the technical differences between the above comparative examples and the preferred embodiment of the present invention, the core quantitative test data are summarized in Table 1.

[0071] Table 1: Comparison of core test data between the embodiments of the present invention and the comparative examples: experiment Differentiated settings for core parameters Etching center area yield Sidewall cross-section angle Copper surface roughness (Ra) Tin layer microstate 20GHz insertion loss Example Two-fluid (18.5μm) + direct chemical bonding 98.5% (no puddles) 89.5° (vertical, no lateral corrosion) 0.18μm Dense continuous contour wrapping -0.62dB / inch Comparative Example 1 Only two-fluid microdroplets, no vacuum suction 12.0% (Severe residual copper in the center) The edge is 75° and the center is not open. 0.20μm continuous -0.65dB / inch (the line is no longer usable) Comparative Example 2 It features vacuum suction and can handle traditional large droplets (65μm). 45.0% (Extremely poor permeability in deep trenches) 68.0° (extremely severe lateral erosion) 0.35μm Relative Continuity -0.78dB / inch (heat generated by circuit deformation) Comparative Example 3 Equipped with vacuum two-fluid technology, enabling forced micro-etching (Ra 1.2μm). 98.0% (Well-formed) 88.5° (Slightly damaged by micro-etching) 1.20μm Severe fault with numerous pinholes -0.92dB / inch (loss spike) The test data proves that: The cross-validation data in Table 1 clearly confirms that high-yield, high-verticality fine lines can only be obtained under thick copper conditions when extremely small mixed microdroplets (10μm~30μm) achieve fluid coupling equilibrium with a specific vacuum negative pressure (-5kPa to -20kPa). More importantly, the data confirms that the nanoscale chemical processing in step S400 is strictly dependent on the ultra-low roughness (Ra 0.1μm~0.3μm) microstructure output from step S200. Disrupting the synergistic relationship of parameters in any of the aforementioned steps will lead to a collapse in etching yield or a dramatic increase in high-frequency signal transmission loss. This definitively demonstrates the strong inseparability between the steps of this invention and produces superior technical effects that are unpredictable by common sense.

[0072] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A vacuum two-fluid PCB fine circuit etching method, characterized in that, Includes the following steps: S100: Provide a copper-clad laminate and fabricate a dry film mask pattern on the surface of the copper-clad laminate; S200: The copper-clad laminate with the dry film mask pattern is fed into the etching chamber for horizontal transport. A vacuum negative pressure is applied above the transport area of ​​the copper-clad laminate, and a mixed micro-droplet containing etching solution and gas is sprayed from below using a two-fluid nozzle for etching. The fluid coupling balance between the upward suction force of the vacuum negative pressure and the downward penetration kinetic energy of the mixed micro-droplet is used to displace the etching solution in the gap of the dry film and control the copper line after etching to be in a low surface roughness state. S300: Peel off the residual dry film on the copper circuit and clean it; S400. For the copper circuit in the low surface roughness state, perform non-roughening surface treatment: chemically deposit a metal bridging layer on the surface of the copper circuit, and then coat the surface of the metal bridging layer with an organosilane coupling agent so that one end of the organosilane coupling agent is chemically bonded to the metal bridging layer, and the other end is used to crosslink with the resin medium to be subsequently pressed.

2. The vacuum two-fluid PCB fine circuit etching method according to claim 1, characterized in that, Step S100 specifically includes the following sub-steps: S110. Provide a high-frequency, high-speed copper-clad laminate substrate, and perform a micro-roughening pretreatment on the copper surface of the substrate; S120. Under vacuum conditions, a photoresist dry film is laminated onto the pretreated copper surface, wherein the photoresist dry film is a dry film with a resolution of less than 50 μm. S130. The photoresist dry film is aligned and exposed using a preset fine line mask. S140. Develop the exposed photoresist dry film to remove the dry film in the unexposed areas, so as to expose the trenches to be etched on the copper surface and form the dry film mask pattern.

3. The vacuum two-fluid PCB fine circuit etching method according to claim 2, characterized in that, In step S140, the opening width of the trench to be etched exposed after development is 30μm~50μm, and the aspect ratio of the depth of the trench to the opening width is greater than or equal to 1.0; the trench to be etched allows the mixed microdroplets in step S200 to penetrate. When providing the copper-clad laminate, the thickness of the initial thick copper layer to be patterned on the outer layer of the copper-clad laminate is greater than or equal to 18 μm.

4. The vacuum two-fluid PCB fine circuit etching method according to claim 3, characterized in that, In step S200, the specific method for horizontal transport and differentiated spraying of the copper-clad laminate is as follows: Along the transmission width direction of the copper-clad laminate, the etching area is divided into a central spray area and edge spray areas located on both sides of the central spray area; the two-fluid nozzles disposed below the etching chamber are correspondingly divided into a central nozzle group and an edge nozzle group. During the etching process, by independently adjusting the gas-liquid mixing ratio of the central nozzle group, the spraying pressure of the mixed micro-droplets ejected by the central nozzle group is 15% to 25% higher than that of the edge nozzle group, in order to compensate for the slowdown in etching rate caused by the accumulation of liquid film on the board surface in the central spray area.

5. The vacuum two-fluid PCB fine circuit etching method according to claim 4, characterized in that, In step S200, the fluid coupling balance between the vacuum negative pressure and the downward penetrating kinetic energy of the mixed microdroplets is achieved through the following dynamic feedback control logic: A pressure sensor is installed inside the etching chamber to monitor the fluctuation of the vacuum negative pressure in real time. When the absolute value of the vacuum negative pressure increases to a set threshold, causing some of the mixed microdroplets to rise and escape, the control system proportionally increases the opening of the compressed air inlet valve of the two-fluid nozzle according to the fluctuation value, so as to increase the downward vertical penetration kinetic energy of the mixed microdroplets until the mixed microdroplets return to the state of penetrating the gap of the dry film mask pattern downward.

6. The vacuum two-fluid PCB fine circuit etching method according to claim 5, characterized in that, In step S200, the relevant fluid dynamic parameters are strictly controlled within the following window: The absolute pressure of the vacuum negative pressure is controlled to be between 5 kPa and 20 kPa; the gas-liquid mass ratio of the mixed microdroplets ejected by the two-fluid nozzle is controlled to be between (0.5~1.5):1, and the velocity of the mixed microdroplets impacting the copper-clad laminate surface vertically downward is controlled to be between 20 m / s and 40 m / s.

7. The vacuum two-fluid PCB fine circuit etching method according to claim 6, characterized in that, In step S200, the microstructure of the etched copper circuit meets the following requirements: The surface roughness Ra of the top surface, sidewalls and base copper surface of the copper circuit is 0.1μm~0.3μm, and the included angle between the sidewall of the copper circuit and the surface of the copper clad laminate substrate is controlled between 88° and 90° to form a fine circuit with a vertical cross-section without side etching.

8. The vacuum two-fluid PCB fine circuit etching method according to claim 7, characterized in that, Step S300 specifically includes: After the residual dry film is peeled off with an alkaline stripping solution, the following steps are performed in sequence: initial pure water rinsing, non-micro-corrosion deoxidation and activation treatment, and secondary pure water rinsing. The non-micro-etching deoxidation activation treatment uses a dilute acid solution with a volume fraction of 3% to 5% to remove copper surface oxides and expose fresh pure copper crystal surfaces for chemical deposition in step S400 without increasing the surface roughness of the copper circuit and maintaining the low surface roughness state. During the initial and secondary pure water cleaning processes, megasonic waves are introduced to assist in the pure water spraying. The frequency of the megasonic waves is controlled between 0.8MHz and 1.2MHz. This is to utilize the high-frequency micro cavitation effect to remove organic residues at the bottom of the gaps in the fine lines and to avoid physical impact damage to the sidewalls of the copper lines with vertical cross-sections.

9. The vacuum two-fluid PCB fine circuit etching method according to claim 8, characterized in that, In step S400, the specific process conditions and composition of the chemical deposition of the continuous tin alloy layer are limited as follows: The temperature of the deposition solution is controlled at 60℃~80℃, and the immersion time of the copper-clad laminate is controlled at 1min~3min; The continuous tin alloy layer is a microalloy layer containing tin and silver elements, wherein the mass fraction of silver is controlled between 1% and 3% to further suppress the growth of tin whiskers on the surface of the metal bridging layer and reduce the surface resistance of the conductor under the skin effect while achieving contour wrapping.

10. The vacuum two-fluid PCB fine circuit etching method according to claim 9, characterized in that, In step S400, the specific material matching for the 5G high-frequency signal transmission scenario is limited as follows: The organosilane coupling agent is selected from one or more end-group silane coupling agents containing epoxy, amino, or vinyl groups; The low dielectric constant resin medium is selected from polytetrafluoroethylene, polyphenylene ether, or liquid crystal polymer, and the organic active functional groups extended outward by the organosilane coupling agent undergo matched crosslinking with the low dielectric constant resin medium. The key heat treatment process for achieving interfacial chemical bonding is: The conditions for baking and drying after coating with the organosilane coupling agent are set as follows: baking at a temperature of 100℃~150℃ for 10min~30min; The heat treatment process provides the activation energy required for the dehydration condensation reaction, thereby driving the complete evaporation of water molecules at the interface.