Memory and its Formation Method
By using chemical vapor deposition (CVD) to generate a capping layer in memory manufacturing to suppress the etching reaction, the problem of uneven grooves caused by wet etching is solved, thereby improving the electrical performance and yield of the memory.
Patent Information
- Application Number
- CN202610191203.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-02-09
- Publication Date
- 2026-11-17
AI Technical Summary
In the manufacturing process of memory with a three-dimensional stacked structure, wet etching is difficult to control in high aspect ratio and complex topology, resulting in uneven formation of grooves at the interface between the protective material layer and the insulating dielectric layer, which affects the morphology and electrical performance of the storage capacitor and reduces the performance and yield of the memory.
Chemical vapor deposition (CVD) is used to remove the protective material layer. By generating a thicker byproduct capping layer at the junction, the etching reaction rate is suppressed, depression formation is avoided, and the consistency of the thickness between the insulating dielectric layer and the protective material layer is ensured.
This improves the electrical performance and product yield of the memory, ensures the shape regularity and size consistency of the storage capacitors, and enhances the overall performance of the memory.
Smart Images

Figure CN123124345A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor manufacturing, and more particularly to a random access memory and a method for forming the same. Background Technology
[0002] With the continuous advancement of semiconductor technology, memory devices are facing physical limits in their pursuit of higher integration density and smaller feature sizes. To perpetuate Moore's Law, the industry has shifted its research focus from traditional planar structures to three-dimensional stacked device architectures. These architectures, by stacking multiple layers of memory cells vertically, can significantly increase storage capacity per unit area, and have become an important direction for the evolution of memory technologies such as dynamic random access memory (DRAM). Meanwhile, novel functional media such as magnetic tunnel junction materials, ferroelectric materials, phase change materials, and resistive switching materials, due to their superior physical properties, are increasingly being researched and applied in these three-dimensional stacked structures, providing a new material foundation for improving device performance.
[0003] In the fabrication of 3D stacked structures, it is typically necessary to define intricate vertical columnar structures within the formed stack and form protective material layers on their sidewalls. Subsequent processes require the selective removal of some dielectric material to create cavities for filling functional materials. When removing the exposed protective dielectric layer through these cavities, the uniformity and topography control of the process are crucial, directly impacting the consistency of the final memory cell's electrical characteristics. While current semiconductor manufacturing methods such as wet etching offer selective advantages in certain scenarios, their performance is significantly influenced by structural geometry and reaction kinetics when dealing with high aspect ratios and complex topologies in 3D structures, making uniformity control a widespread challenge.
[0004] Currently, the performance and product yield of memory still need to be improved. Summary of the Invention
[0005] The problem solved by the embodiments of the present invention is to provide a memory and a method for forming the same, which improves the performance and product yield of the memory.
[0006] To address the aforementioned problems, embodiments of the present invention provide a method for forming a memory, comprising: providing a stacked structure, the stacked structure including a dielectric stacked structure, a pillar structure extending longitudinally through the dielectric stacked structure, and a protective material layer located between the dielectric stacked structure and the pillar structure and surrounding and covering the pillar structure, the dielectric stacked structure including a sacrificial layer and an insulating dielectric layer alternately stacked longitudinally, the insulating dielectric layer and the protective material layer comprising the same material; removing the sacrificial layer to form an opening exposing a portion of the sidewall of the protective material layer; performing a chemical vapor deposition (CVD) process through the opening to remove the exposed protective material layer and a portion of the thickness of the insulating dielectric layer, wherein, before the exposed protective material layer is completely removed, byproducts of the CCVD process cover the protective material layer, and the thickness of the byproducts at the junction of the protective material layer and the insulating dielectric layer is greater than the thickness of the byproducts on the surface of the protective material layer.
[0007] Accordingly, embodiments of the present invention also provide a memory, which is formed using the memory formation method provided by the present invention.
[0008] Compared with the prior art, the technical solution of the embodiments of the present invention has the following advantages: The memory formation method provided in this invention uses a chemical vapor deposition (CVD) process to remove the exposed protective material layer. During the etching process, byproducts generated cover the surface of the protective material layer. Since the thickness of the byproducts at the junction of the protective material layer and the insulating dielectric layer is greater than the thickness of the byproducts on the surface of the protective material layer, this thickness difference plays a crucial role in the etching process. The thicker byproducts effectively suppress the etching rate at the junction, thereby significantly reducing over-etching of the protective material layer at the junction while removing the exposed layer. This avoids the risk of forming depressions at the junction and improves the consistency of the thickness between the insulating dielectric layer and the remaining protective material layer. Consequently, the electrode plates and storage dielectric layers subsequently formed in the space released by the sacrificial layer and the protective material layer have more regular shapes, thus improving the memory's performance and product yield. Attached Figure Description
[0009] Figures 1 to 3 A schematic diagram of the structure corresponding to each step of a method for forming a memory is shown; Figures 4 to 8 The diagram shows the structural schematics corresponding to each step of the memory formation method in an embodiment of the present invention. Detailed Implementation
[0010] Currently, the performance and product yield of memory still need to be improved. This paper analyzes the reasons why the performance and product yield of memory still need to be improved by combining a memory manufacturing method.
[0011] in, Figures 1 to 3 A schematic diagram of the structure corresponding to each step of a method for forming a memory is shown.
[0012] refer to Figure 1 A stack structure 80 is provided, which includes a dielectric stack structure 10, a column structure 20 extending longitudinally through the dielectric stack structure 10, and a protective material layer 30 located between the dielectric stack structure 10 and the column structure 20 and surrounding and covering the column structure 20. The dielectric stack structure 10 includes a sacrificial layer 101 and an insulating dielectric layer 102 that are alternately stacked in the longitudinal direction.
[0013] refer to Figure 2 Remove the sacrificial layer 101 to form an opening 103 that exposes part of the sidewall of the protective material layer 30.
[0014] refer to Figure 3 The exposed portion of the protective material layer 30 is removed via opening 103 using a wet chemical etching process.
[0015] The space freed by the removed protective material layer 30 serves as a cavity. The cavity and opening 103 are connected to form a filling tank. In subsequent processes, a storage material layer and an electrode plate are sequentially deposited on the inner surface of the filling tank. The pillar structure 20 can be an electrode pillar. The storage material layer can be a variable resistance layer that stores data through resistance changes under the action of current or voltage, such as a magnetic tunnel junction material layer, a phase change material layer, or a resistive switching material layer. The storage material layer can also be a polarization layer that stores data through polarization state changes under the action of voltage, such as a ferroelectric material layer. Thus, the storage material layer between the electrode pillar and the electrode plate, as well as the corresponding portions of the electrode plate and the electrode pillar on both sides of the storage material layer, can form a storage capacitor. One electrode pillar can correspondingly form multiple storage capacitors (i.e., storage cells). Multiple storage capacitors corresponding to one electrode pillar share the electrode pillar and are connected in parallel to form a storage capacitor unit. The electrode pillar can be connected to a selection unit. Thus, the selection unit and the storage capacitor unit together constitute a storage unit. The storage units are horizontally arrayed to form a memory.
[0016] Research has revealed that during the process of removing the exposed portion of the protective material layer 30 using wet chemical etching, grooves are easily formed at the junction of the protective material layer 30 and the insulating dielectric layer 102 (e.g., Figure 3 (As shown in the dashed circle in the middle), the groove affects the morphology and area of the formed storage capacitor, which in turn directly leads to large fluctuations in the electrical performance parameters of the final storage device.
[0017] The fundamental reason why grooves are easily formed at the junction of the protective material layer 30 and the insulating dielectric layer 102 is that, in order to remove the full thickness of the exposed protective material layer 30 and expose the pillar structure 20, an isotropic etching process, usually wet etching, is required. Ordinary isotropic etching processes will additionally remove a portion of the protective material layer 30 in the extension direction of the pillar structure 20. Furthermore, since the protective material layer 30 is relatively thin, after the removal of a portion of its length, the capillary action generated by the narrow space will further introduce the wet etching solution into the junction corner, causing the groove to enlarge further.
[0018] Furthermore, the wet etching time cannot be exactly the same for different wafers, resulting in different sizes of grooves on different wafers; on the same wafer, due to the limited diffusion ability of the etchant in the etching solution, the concentration of wet etching solution that the protective material layer at different distribution locations comes into contact with is different, resulting in different sizes of grooves at different distribution locations on the same wafer.
[0019] In summary, the presence of grooves causes deformation and changes in the size of the subsequently formed storage capacitors. The uneven size of the grooves also leads to inconsistent storage capacitor sizes, resulting in decreased memory performance and yield.
[0020] To address the technical problem, embodiments of the present invention provide a method for forming a memory, comprising: providing a stacked structure, the stacked structure including a dielectric stacked structure, a pillar structure extending longitudinally through the dielectric stacked structure, and a protective material layer located between the dielectric stacked structure and the pillar structure and surrounding and covering the pillar structure, the dielectric stacked structure including a sacrificial layer and an insulating dielectric layer alternately stacked longitudinally, the insulating dielectric layer and the protective material layer comprising the same material; removing the sacrificial layer to form an opening exposing a portion of the sidewall of the protective material layer; performing a chemical vapor deposition (CVD) process through the opening to remove the exposed protective material layer and a portion of the thickness of the insulating dielectric layer, wherein, before the exposed protective material layer is completely removed, byproducts of the CCVD process cover the protective material layer, and the thickness of the byproducts at the junction of the protective material layer and the insulating dielectric layer is greater than the thickness of the byproducts on the surface of the protective material layer.
[0021] The memory formation method provided in this invention uses chemical vapor etching to remove the exposed protective material layer. During the etching process, byproducts generated cover the surface of the protective material layer. Since the thickness of the byproducts at the junction of the protective material layer and the insulating dielectric layer is greater than the thickness of the byproducts on the surface of the protective material layer, this thickness difference plays a key role in the etching process. The thicker byproducts effectively suppress the etching rate at the junction, thereby significantly reducing over-etching of the protective material layer at the junction while removing the exposed protective material layer. This avoids the risk of forming depressions at the junction and improves the consistency of the thickness between the insulating dielectric layer and the remaining protective material layer. As a result, the electrode plates and storage dielectric layers formed subsequently in the space released by the sacrificial layer, the partial thickness of the insulating dielectric layer, and the protective material layer are more regular in shape, and the size of the memory cells is more controllable without being affected by depressions. This improves the performance and product yield of the memory.
[0022] To make the above-mentioned objects, features and advantages of the embodiments of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.
[0023] in, Figures 4 to 8 The diagram shows the structural schematics corresponding to each step of the memory formation method in an embodiment of the present invention.
[0024] refer to Figure 4 A stacked structure 210 is provided, which includes a dielectric stacked structure 208, a column structure 200 extending longitudinally through the dielectric stacked structure 208, and a protective material layer 206 located between the dielectric stacked structure 208 and the column structure 200 and surrounding and covering the column structure 200. The dielectric stacked structure 208 includes a sacrificial layer 202 and an insulating dielectric layer 201 that are alternately stacked longitudinally. The insulating dielectric layer 201 and the protective material layer 206 are made of the same material.
[0025] Specifically, in the subsequent process step of removing the sacrificial layer 202, the protective material layer 206 isolates the etching environment from the pillar structure 200, preventing the surface material of the pillar structure 200 from being damaged by the etching environment, thereby ensuring the electrical performance and structural integrity of the pillar structure 200.
[0026] It should be noted that the insulating dielectric layer 201 and the protective material layer 206 are made of the same material, which can create the same reaction interface for the subsequent chemical vapor etching process. Since the insulating dielectric layer 201 and the protective material layer 206 are made of the same material, the chemical vapor etching process has similar etching rates for the insulating dielectric layer 201 and the protective material layer 206. This helps to form a thicker byproduct at the junction of the protective material layer 206 and the insulating dielectric layer 201 while removing the protective material layer 206, avoiding the formation of depressions, thereby improving the morphological consistency of the subsequently formed memory cells.
[0027] Specifically, the sacrificial layer 202 is used to define the spatial location required for the subsequent formation of the electrode plate. By removing the sacrificial layer 202 to form an opening, the spatial area for forming the electrode plate is released.
[0028] The insulating dielectric layer 201 serves to provide interlayer electrical isolation for the subsequent formation of electrode plates, preventing short circuits between adjacent electrode plates and ensuring the independence of memory cells at different heights (with the column structure extension direction as the vertical direction).
[0029] It should be noted that the column structure 200 is used to provide a vertical electrical connection channel for each memory cell of the memory.
[0030] In this embodiment, the column structure 200 is specifically an electrode column, which is used together with the subsequently formed storage medium layer and electrode plate to form a storage capacitor (i.e., a storage cell).
[0031] However, this is not the only possibility. In some embodiments, the pillar structure includes a channel pillar, and in subsequent processes, other portions of the memory cell can be formed on the exposed surface of the channel pillar, such as a floating gate structure, including a tunneling dielectric layer, a polysilicon floating gate, a gate dielectric layer, and an electrode plate stacked sequentially in a direction away from the surface of the channel pillar, thereby forming a NAND memory. In some embodiments, the pillar structure 200 includes an insulating core, a channel layer, a tunneling dielectric layer (e.g., silicon oxide), an insulating memory layer (e.g., silicon nitride), and a gate dielectric layer (e.g., silicon oxide) stacked sequentially from the inside to the outside along the axis. The opening formed after the sacrificial layer is subsequently removed is filled to form a gate electrode plate, thereby forming a NAND memory. Further examples are not provided here; the pillar structure and memory type can be specifically configured according to actual needs.
[0032] In this embodiment, the method of forming the stacked structure 210 further includes forming a selection unit electrically connected to the electrode post, the selection unit being used to select the electrode post.
[0033] Specifically, a selection unit electrically connected to the electrode post enables addressing and access to specific storage capacitor cells (including multiple parallel storage capacitors corresponding to one electrode post). The selection unit is electrically connected to the selected electrode post. When it is necessary to read or write data to a certain storage capacitor cell, the selection unit corresponding to that storage capacitor cell is activated, thereby establishing an electrical path through the selection unit to the electrode post. This allows the storage capacitor cell to be selected and connected to the peripheral circuit, while other unselected storage capacitor cells remain electrically isolated, thus enabling independent operation of individual storage capacitor cells in a high-density array.
[0034] In this embodiment, the selection unit includes a MOS transistor, the source of which is used to connect to the bit line, the gate of which is used to connect to the word line, and the drain of which is electrically connected to the pillar structure 200.
[0035] It should be noted that the source of the MOS transistor is connected to the bit line, which can transmit the signal current or voltage required for read and write operations to the selected memory capacitor cell through the bit line. The gate of the MOS transistor is connected to the word line, which can control the MOS transistor to turn on and off by applying a voltage signal to the word line, thereby realizing the selection of memory capacitor cells. The drain of the MOS transistor is electrically connected to the pillar structure 200. When the MOS transistor is turned on, a low-resistance path is formed between the bit line and the electrode pillar, enabling read and write operations to be performed.
[0036] In this embodiment, the insulating dielectric layer 201 and the protective material layer 206 comprise silicon oxide.
[0037] refer to Figure 5 Remove the sacrificial layer 202 to form an opening 220 that exposes part of the sidewall of the protective material layer 206.
[0038] Specifically, opening 220 provides a channel for the reaction material (i.e., etching gas) to enter the subsequent chemical vapor etching process, so that the etching gas can contact the protective material layer 206 through opening 220 and undergo an etching reaction.
[0039] In this embodiment, the process for removing the sacrificial layer 202 includes a wet etching process.
[0040] The sacrificial layer 202 is made of a different material than the insulating dielectric layer 201 and the protective material layer 206. As an example, the sacrificial layer 202 comprises silicon nitride. Wet etching typically has a high etch selectivity, enabling rapid removal of the sacrificial layer 202, while the etching rate for the insulating dielectric layer 201 and the protective material layer 206, which are made of silicon oxide, is extremely low, reducing the risk of damage to the insulating dielectric layer 201 and the protective material layer 206 during the etching process.
[0041] refer to Figures 6 to 7A chemical vapor deposition process is performed through opening 220 to remove the exposed protective material layer 206 and a portion of the thickness of the insulating dielectric layer 201. Before the exposed protective material layer 206 is completely removed, byproducts 280 of the chemical vapor deposition process cover the protective material layer 206, and the thickness of the byproducts 280 at the corner where the protective material layer 206 and the insulating dielectric layer 201 meet is greater than the thickness of the byproducts 280 on the surface of the protective material layer 206.
[0042] In wet etching processes, etching byproducts usually dissolve in the solvent in the etching solution and are lost, preventing them from accumulating on the reaction surface and forming self-limiting etching.
[0043] The exposed protective material layer 206 is removed by chemical vapor etching (CVD). CVD is an isotropic vapor etching process. During the etching process, byproducts 280 are generated that can cover the surfaces of the protective material layer 206 and the insulating dielectric layer 201. The byproducts 280 at the corner where the protective material layer 206 and the insulating dielectric layer 201 meet accumulate due to the larger specific surface area at the corner, resulting in a thickness of the byproducts 280 at the corner that is greater than the thickness of the byproducts 280 on the surface of the protective material layer 206.
[0044] Byproduct 280 forms a capping layer at the etching reaction interface (i.e., the surface of the protective material layer 206 exposed by opening 220). The capping layer of byproduct 280 exists on the surface of the protective material layer 206 being etched and has a certain thickness. The capping layer acts as a physical barrier, blocking the diffusion of newly introduced etching gas to the protective material layer 206. The greater the thickness of the capping layer, the stronger the blocking ability, and the less etching gas diffuses to the surface of the protective material layer 206. Thus, the thickness of the capping layer can affect the reaction rate between the protective material layer 206 and the etching gas. In turn, by controlling the distribution of the capping layer thickness at different locations, the proportion of the protective material layer 206 removed at different locations can be controlled.
[0045] Therefore, the thickness difference between the byproduct 280 capping layer at the corner and the surface of the protective material layer 206 plays a crucial role in the etching process. The thicker byproduct 280 effectively suppresses the etching rate at the junction corner, thereby significantly reducing over-etching of the protective material layer 206 at the junction corner while etching away the exposed protective material layer 206. This avoids the risk of forming significant depressions at the junction corner and improves the consistency of the thickness between the insulating dielectric layer 201 and the remaining protective material layer 206. Consequently, the shape of the electrode plate formed in the space released by the partially thick insulating dielectric layer 201, sacrificial layer 202, and protective material layer 206 becomes more regular, and the size and morphology of the memory cells are controllable, thereby improving the performance and product yield of the memory.
[0046] In this embodiment, the steps of removing the exposed protective material layer 206 and removing a portion of the thickness of the insulating dielectric layer 201 using chemical vapor etching include: providing etching gas, the etching gas reacting chemically with the protective material layer 206 and the insulating dielectric layer 201 exposed by the opening 220 to generate byproduct 280, controlling process conditions to maintain byproduct 280 covering the surface of the remaining protective material layer 206, and stopping the supply of etching gas after the protective material layer 206 exposed by the opening 220 has been completely reacted, and removing byproduct 280. The process conditions include process temperature and process gas pressure.
[0047] It should be noted that the removal of byproduct 280 is achieved through precise control of process temperature and process gas pressure. One method is to increase the temperature and / or change the process gas pressure after the protective material layer 206 has completely reacted, causing the byproduct 280 to undergo thermal decomposition and / or sublimation, thus being removed in one go. Another method is to dynamically maintain the formation and removal of byproduct 280 during the etching process. This is achieved by setting the process temperature and process gas pressure to a range that allows the formation rate of byproduct 280 to be within an appropriate range, while maintaining a certain process temperature and process gas pressure in the gas phase environment. This allows the byproduct 280 to be continuously removed while it is being formed, with the removal rate and formation rate forming a dynamic balance, thereby maintaining a controlled thickness of byproduct 280 at the reaction interface.
[0048] In this embodiment, controlling the process conditions to maintain the byproduct 280 covering the surface of the remaining opening 220 includes simultaneously controlling the generation rate and removal rate of the byproduct 280.
[0049] Specifically, by simultaneously controlling the formation and removal rates of byproduct 280, the stable presence and thickness of byproduct 280 at the reaction interface can be precisely maintained. If only the formation rate is controlled without controlling the removal rate, byproduct 280 will accumulate to an excessive thickness, potentially resulting in insufficient etching gas diffusion to the surface of the protective material layer 206, thus hindering the etching process. Conversely, if the removal rate is too fast, byproduct 280 cannot effectively accumulate to form a capping layer of a certain thickness, and the etching will lose its self-limiting property, leading to morphology control failure. By simultaneously controlling the formation and removal rates, byproduct 280 can both inhibit the reaction and not completely terminate the chemical vapor deposition reaction. Furthermore, the thicker byproduct 280 at corners can be utilized to protect the morphology of the protective material layer 206 at the corners.
[0050] In this embodiment, the etching gas includes hydrogen fluoride (HF) and ammonia (NH3).
[0051] Hydrogen fluoride and ammonia can react chemically with silicon oxide to generate solid ammonium fluorosilicate byproduct 280. Furthermore, the generated ammonium fluorosilicate byproduct 280 exhibits high stability within a specific process temperature window, forming an effective coating layer at the reaction interface and being decomposed and removed without significantly increasing the temperature.
[0052] In this embodiment, byproduct 280 includes ammonium fluorosilicate.
[0053] It should be noted that ammonium fluorosilicate has good thermal decomposition characteristics, which is beneficial for removing the byproduct 280 by controlling the process temperature in the subsequent process.
[0054] In this embodiment, a chemical vapor deposition process is performed to remove the exposed protective material layer 206 and a portion of the thickness of the insulating dielectric layer 201. The chemical reaction formula is shown below: ; .
[0055] Specifically, the above chemical reaction formula describes the transformation process from silicon oxide to byproduct 280 ammonium fluorosilicate: First, hydrogen fluoride gas reacts with silicon oxide to generate gaseous silicon fluoride and water; subsequently, silicon fluoride reacts further with more hydrogen fluoride and ammonia to generate solid byproduct 280 ammonium fluorosilicate, which is deposited on the surface of the protective material layer 206.
[0056] In this embodiment, removing byproduct 280 includes causing byproduct 280 to decompose upon heating.
[0057] It should be noted that after ammonium fluorosilicate decomposes upon heating, it regenerates gaseous silicon fluoride, hydrogen fluoride, and ammonia. These gaseous products can be easily removed by a vacuum system, leaving no residue in the reaction chamber or on the surface of the storage device. This avoids process contamination and provides a clean interface for subsequent process steps.
[0058] In this embodiment, the chemical reaction formula for the decomposition reaction is as follows: .
[0059] In this embodiment, the chemical vapor etching process includes plasma-assisted chemical vapor etching. Plasma-assisted chemical vapor etching can provide more reactive reactants by dissociating the etching gas, thereby increasing the etching rate and improving production efficiency.
[0060] It should be noted that the process gas pressure should not be too high or too low. If the process gas pressure is too high, it means that the concentration of etching gas molecules in the reaction chamber is too high, which will lead to an excessively rapid formation rate of byproduct 280. An excessively rapid formation rate may cause the byproduct 280 layer to become excessively thick, or even accumulate prematurely at the entrance of opening 220 and block the channel, hindering the etching gas from entering the deep region, resulting in uneven etching. An excessively thick byproduct 280 layer will in turn prevent the etching gas from diffusing to the surface of the protective material layer 206, thereby blocking etching and making it impossible to completely remove the protective material layer 206 in the deep region. If the process gas pressure is too low, the etching reaction rate will be too slow. At the same time, the low gas pressure will cause the removal rate of byproduct 280 to be relatively too fast, resulting in the inability to form an effective and continuous covering layer on the reaction surface. This weakens the protective effect of byproduct 280 at corners, increases the risk of depressions at corners, and greatly increases the risk of inconsistency in the thickness of the insulating dielectric layer 201 and the remaining protective material layer 206. Therefore, in this embodiment, the process gas pressure of the process conditions is between 2100 mTorr and 3000 mTorr.
[0061] It should also be noted that the process temperature should not be too high or too low. If the process temperature is too high, the thermal decomposition rate of the ammonium fluorosilicate byproduct 280 will be significantly accelerated, possibly even exceeding its formation rate. This can easily lead to an excessively thin byproduct 280 layer or an unstable formation, failing to achieve the purpose of protecting the morphology at the corners. Furthermore, excessively high temperatures can easily cause thermal damage to other film layers in the memory. If the process temperature is too low, the decomposition rate of the byproduct 280 will be too slow, causing it to accumulate excessively and adhere firmly to the surface of the protective material layer 206. This will severely hinder the continuation of the chemical vapor etching reaction, resulting in an abnormally long etching process time or even the cessation of the etching reaction. Therefore, in this embodiment, the process temperature is between 100°C and 110°C.
[0062] That is, the chemical vapor etching process includes plasma-assisted chemical vapor etching. For the materials and etching gas in the above embodiments of this application, the process gas pressure is between 2100 mTorr and 3000 mTorr, and the process temperature is between 100°C and 110°C. This allows the thickness of the by-products at the junction of the protective material layer and the insulating dielectric layer to be greater than the thickness of the by-products on the surface of the protective material layer.
[0063] refer to Figure 8After removing the exposed protective material layer 206, the method further includes: using the space released by the partially thick insulating dielectric layer 201 and protective material layer 206 as a groove 221, the groove 221 communicating with the opening 220 to form a horizontal groove 230, depositing a conformally covering storage dielectric layer 261 covering the insulating dielectric layer 201, protective material layer 206 and electrode post surface in the horizontal groove 230; and forming an electrode plate 260 in the remaining space of the horizontal groove 230.
[0064] It should be noted that the horizontal groove 230 provides space for the subsequent formation of the storage medium layer 261 and the electrode plate 260.
[0065] It should also be noted that the storage medium layer 261 is used as the core functional layer of the memory. The storage medium layer includes a variable resistance layer that stores data by changing resistance under the action of current or voltage, such as one or more of a magnetic tunnel junction material layer, a phase change material layer or a resistive switching material layer. Alternatively, the storage medium layer includes a polarization layer that stores data by changing polarization state under the action of voltage, such as a ferroelectric material layer.
[0066] Specifically, the storage medium layer 261 includes a magnetic tunnel junction material layer, a ferroelectric material layer, a phase change material layer, or a resistive switching material layer, enabling the memory to be implemented as a magnetic random access memory (MRAM), a ferroelectric random access memory (FeRAM), a phase change random access memory (PCRAM), or a resistive random access memory (RRAM). However, it is not limited to these; as mentioned above, the materials filling the pillar structures and horizontal slots can be configured according to actual needs to achieve different memory structures.
[0067] It should be noted that the electrode plate 260 is used to form a storage cell with the electrode post through the storage medium layer 261. During read and write operations, voltage is applied between the electrode plate 260 and the electrode post, thereby generating an electric field or current on the storage medium layer 261 to change its state (write) or sense its state (read).
[0068] In this embodiment, the materials of the electrode posts and electrode plates 260 can be the same or different. Both can be materials with good conductivity and compatible with the storage medium layer 261, such as titanium nitride, tungsten, titanium, tantalum, tantalum nitride or their composite stacks.
[0069] Accordingly, embodiments of the present invention also provide a memory.
[0070] The memory is formed by the memory forming method provided by the present invention.
[0071] For a detailed description of the memory, please refer to the previous description; it will not be repeated here.
[0072] While the present invention has been disclosed above, it is not limited thereto. Any person skilled in the art can make various modifications and alterations without departing from the spirit and scope of the invention; therefore, the scope of protection of the present invention should be determined by the scope defined in the claims.
Claims
1. A method for forming a memory, characterized in that, include: A stacked structure is provided, the stacked structure including a dielectric stacked structure, a column structure extending longitudinally through the dielectric stacked structure, and a protective material layer located between the dielectric stacked structure and the column structure and surrounding and covering the column structure, the dielectric stacked structure including a sacrificial layer and an insulating dielectric layer alternately stacked longitudinally, the insulating dielectric layer and the protective material layer comprising the same material; Remove the sacrificial layer to form an opening that exposes part of the sidewall of the protective material layer; A chemical vapor deposition (CVD) process is performed through the opening to remove the exposed protective material layer and a portion of the thickness of the insulating dielectric layer. Before the exposed protective material layer is completely removed, byproducts of the CVD process cover the protective material layer, and the thickness of the byproducts at the corner where the protective material layer and the insulating dielectric layer meet is greater than the thickness of the byproducts on the surface of the protective material layer.
2. The method for forming a memory as described in claim 1, characterized in that, The column structure includes an electrode column, and the method further includes forming a selection unit electrically connected to the electrode column, the selection unit being used to select the electrode column; After removing the exposed protective material layer, the method further includes: using the space released by the partial thickness of the protective material layer and the insulating dielectric layer as a groove, the groove communicating with the opening to form a horizontal groove, depositing a storage dielectric layer in the horizontal groove to conformally cover the insulating dielectric layer, the protective material layer and the surface of the electrode post; and forming an electrode plate in the remaining space of the horizontal groove.
3. The method for forming a memory as described in claim 1, characterized in that, The steps of removing the exposed protective material layer and removing a portion of the thickness of the insulating dielectric layer using a chemical vapor deposition process include: An etching gas is provided, which chemically reacts with the protective material layer and the insulating dielectric layer exposed by the opening to generate the byproduct. Process conditions are controlled to maintain the byproduct covering the surface of the remaining protective material layer. After the exposed protective material layer has been completely reacted, the etching gas is stopped, and the byproduct is removed. The process conditions include process temperature and process gas pressure.
4. The method for forming a memory as described in claim 3, characterized in that, The control of process conditions to maintain the byproduct covering the surface of the remaining opening includes controlling both the generation rate and the removal rate of the byproduct.
5. The method for forming a memory as described in claim 4, characterized in that, The insulating dielectric layer and the protective material layer comprise silicon oxide, the etching gas comprises hydrogen fluoride and ammonia, the byproduct comprises ammonium fluorosilicate, and the chemical reaction formula for performing a chemical vapor etching process to remove the exposed protective material layer and a portion of the thickness of the insulating dielectric layer is as follows: ; ; Removing the byproducts includes thermally decomposing them, and the chemical reaction formula for the decomposition reaction is as follows: 。 6. The method for forming a memory as described in claim 5, characterized in that, The chemical vapor etching process includes plasma-assisted chemical vapor etching.
7. The method for forming a memory as described in claim 6, characterized in that, The process conditions include: The process gas pressure is between 2100 mTorr and 3000 mTorr; The process temperature is between 100℃ and 110℃.
8. The method for forming a memory as described in claim 2, characterized in that, The storage medium layer includes a variable resistance layer that stores data by changing resistance under the action of current or voltage, or a polarization layer that stores data by changing polarization state under the action of voltage.
9. The method for forming a memory as described in claim 2, characterized in that, The selection unit includes a MOS transistor, the source of which is used to connect to a bit line, the gate of which is used to connect to a word line, and the drain of which is electrically connected to the pillar structure.
10. A memory, characterized in that, Formed using the method described in any one of claims 1 to 9.