Semiconductor structure and its formation method

By constructing a sidewall structure close to the gate structure in the semiconductor structure and optimizing the wet etching process, the problem of the metal silicide layer being too close to the first gate structure is solved, thereby improving the carrier tunneling efficiency and suppressing leakage current, and improving the reliability and performance of the device.

CN123124425APending Publication Date: 2026-11-17SEMICON TECH INNOVATION CENT(BEIJING) CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510639447.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the manufacturing processes of hybrid integrated tunneling field-effect transistors (TFETs) and traditional CMOS devices, existing technologies suffer from the problem of the metal silicide layer being too close to the first gate structure, leading to leakage current and breakdown risks, which affect the stability of device performance.

Method used

A gate structure is formed on a substrate and a sidewall structure is constructed on its sidewall, including a first sidewall and a second sidewall close to the gate structure. The sidewall structure at the source of the second gate structure is removed, and the etching resistance of the first sidewall is improved by wet etching, lateral etching is suppressed, and the band structure and electric field distribution are optimized.

Benefits of technology

It improves carrier tunneling efficiency, reduces leakage current and breakdown risk, and enhances the electrical performance and reliability of semiconductor structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124425A_ABST
    Figure CN123124425A_ABST
Patent Text Reader

Abstract

A semiconductor structure and its formation method are disclosed. During the formation of the semiconductor structure, the first sidewall is more etch-resistant than the self-aligned barrier layer. Therefore, the first sidewall on both sidewalls of the first gate structure and on the drain side of the second gate structure can effectively resist lateral etching by wet etching solution, suppressing the "hollowing-out" phenomenon of the first sidewall. This facilitates control of the source and drain in the first region and the drain leakage current in the second region, reducing the risk of semiconductor structure breakdown and improving the reliability and performance of the semiconductor structure. Furthermore, the source and drain doped layers are located on the top of the substrate on both sides of the gate structure, and no sidewall structure is formed on the sidewall at the source in the source and drain doped layers on the side of the second gate structure. This allows for more effective modulation of the energy band structure and electric field distribution of the source, thereby improving the efficiency of carrier tunneling from the source into the channel and enhancing the electrical performance of the semiconductor structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor manufacturing, and more particularly to a semiconductor structure and a method for forming the same. Background Technology

[0002] In the field of integrated circuit design and manufacturing, as electronic devices continue to develop towards higher performance and higher integration, power consumption control has become a key challenge. Integrated circuits are widely used in various electronic systems, from everyday consumer electronics to complex industrial control devices. Their power consumption directly affects factors such as the device's battery life, heat dissipation design, and operating costs. Therefore, reducing power consumption has always been one of the core technological goals pursued in this field.

[0003] Tunnel field-effect transistors (TFETs), as a novel type of semiconductor device, are attracting increasing attention due to their excellent subthreshold characteristics. Compared to traditional CMOS devices, TFETs exhibit better current control capabilities under low-voltage operation, achieving the same level of current switching at lower voltages, which gives them a potential advantage in low-power circuit design.

[0004] In the field of integrated circuit design and manufacturing, reducing power consumption has always been one of the key technical goals. Tunneling field-effect transistors (TFETs) have attracted widespread attention due to their excellent subthreshold characteristics. Hybrid integration of TFETs with traditional complementary metal-oxide-semiconductor (CMOS) devices, utilizing TFETs to handle the low-frequency components of the circuit while the high-frequency components are handled by traditional CMOS devices, is significant for reducing overall circuit power consumption. However, challenges remain in actual manufacturing processes. Summary of the Invention

[0005] The problem addressed by the embodiments of the present invention is to provide a semiconductor structure and a method for forming the same, thereby improving the electrical performance of the semiconductor structure.

[0006] To address the aforementioned problems, embodiments of the present invention provide a method for forming a semiconductor structure, comprising: providing a substrate, the substrate including a first region and a second region; forming a gate structure on the substrate, wherein the gate structure on the first region serves as a first gate structure and the gate structure on the second region serves as a second gate structure; forming a sidewall structure on the sidewall of the gate structure, the sidewall structure including a first sidewall and a second sidewall, wherein the first sidewall is closer to the gate structure than the second sidewall; after forming the sidewall structure, forming source / drain doped layers on the top of the substrate on both sides of the gate structure; removing the sidewall structure at the source electrode of the second gate structure; forming a self-aligned barrier layer exposing the top of the gate structure and the surfaces of the source / drain doped layers on both sides of the gate structure; performing wet etching on the surfaces of the source / drain doped layers and the self-aligned barrier layer on the top of the gate structure, wherein the first sidewall is more resistant to etching than the self-aligned barrier layer.

[0007] This invention provides a semiconductor structure, comprising: a substrate including a first region and a second region, wherein a high-frequency device is formed in the first region and a low-frequency device is formed in the second region; a gate structure located on the substrate, wherein the gate structure in the first region serves as a first gate structure and the gate structure in the second region serves as a second gate structure; source / drain doped layers located on the top of the substrate on both sides of the gate structure; and sidewall structures located on two sidewalls of the first gate structure and on the sidewall of the drain electrode in the source / drain doped layers of the second gate structure, wherein the sidewall structures include a first sidewall and a second sidewall, wherein the first sidewall is closer to the gate structure than the second sidewall, and the etching resistance of the first sidewall is greater than that of silicon oxide.

[0008] Compared with the prior art, the technical solution of the embodiments of the present invention has the following advantages:

[0009] In the semiconductor structure formation method provided by the embodiments of the present invention, a gate structure is formed on a substrate, the gate structure on the first region serves as a first gate structure, the gate structure on the second region serves as a second gate structure, a sidewall structure is formed on the sidewall of the gate structure, the sidewall structure includes a first sidewall and a second sidewall, the first sidewall being closer to the gate structure than the second sidewall; a source / drain doped layer is formed on the top of the substrate on both sides of the gate structure; then the sidewall structure at the source electrode in the source / drain doped layer on the side of the second gate structure is removed, thereby improving the efficiency of carrier tunneling from the source electrode into the channel when the semiconductor structure is working, effectively modulating the band structure and electric field distribution at the source electrode in the second region, and improving the electrical performance of the semiconductor structure. Furthermore, because the self-aligned barrier layer on the surface of the source and drain doped layer and the top of the gate structure are wet-etched, the first sidewall is more resistant to etching than the self-aligned barrier layer. As a result, the first sidewall on both sidewalls of the first gate structure and the drain side of the second gate structure can effectively resist the lateral etching of the wet etching solution, suppress the "hollowing out" phenomenon of the first sidewall, which is beneficial to control the source and drain in the first region and the drain leakage current in the second region, reduce the risk of semiconductor structure breakdown, and improve the reliability and performance of the semiconductor structure. Attached Figure Description

[0010] Figure 1 This is a schematic diagram of a semiconductor structure.

[0011] Figures 2 to 13 This is a schematic diagram of the structure corresponding to each step in the semiconductor structure formation method. Detailed Implementation

[0012] As the background technology shows, reducing power consumption has always been one of the key technical goals in the field of integrated circuit design and manufacturing. Tunneling field-effect transistors (TFETs) have attracted widespread attention due to their excellent subthreshold characteristics. Hybrid integration of TFETs with traditional CMOS devices, utilizing TFETs to handle the low-frequency components of the circuit while using traditional CMOS devices for the high-frequency components, is significant for reducing overall circuit power consumption. However, challenges remain in the actual manufacturing process.

[0013] In particular, during the fabrication of hybrid integrated circuits, a single-sidewall tunneling field-effect transistor (TST) structure was chosen. Removing the source sidewall of the TST allows the metal silicide layer at the source to extend towards the tunneling channel, effectively increasing impurity segregation and thus enhancing the on-state current of the TST. Before forming the metal silicide layer, the oxide layer on the source surface of the TST needs to be removed. This is typically achieved through over-etching to ensure complete removal of the oxide layer and improve the quality of the metal silicide layer formation. However, this leads to poor performance in CMOS devices. The following section will explain the reason using a semiconductor structure as an example.

[0014] Figure 1 The diagram shows a schematic of a semiconductor structure.

[0015] The semiconductor structure includes: a substrate 1, which includes a first region I and a second region II, wherein a high-frequency device (e.g., CMOS) is formed in the first region I and a low-frequency device (e.g., TFET) is formed in the second region II; a gate structure 2, located on the substrate 1, wherein the gate structure 2 in the first region I serves as a first gate structure 2a and the gate structure 2 in the second region II serves as a second gate structure 2b; a source / drain doped layer 3, located on the top of the substrate 1 on both sides of the gate structure 2; a sidewall structure 4, located on the two sidewalls of the first gate structure 2a and on the sidewall of the drain electrode in the source / drain doped layer 3 on the side of the second gate structure 2b, wherein the sidewall structure 4 includes a first sidewall 4a and a second sidewall 4b, wherein the first sidewall 4a is closer to the gate structure 2 than the second sidewall 4b, and the first sidewall 4a is typically made of silicon oxide, whose resistance to wet etching is generally not as good as that of the second sidewall 4b; and a metal silicide layer 5, located on top of the source / drain doped layer 3 and on top of the gate structure 2.

[0016] It should be noted that the metal silicide layer 5 is formed using a self-aligned silicide process. If, during the self-aligned silicide process, there are unremoved oxide layers or residual oxides on the top of the source / drain doped layer 3 and the gate structure 2, the formation quality of the self-aligned silicide layer will be reduced. Therefore, the top of the source / drain doped layer 3 and the gate structure 2 needs to be cleaned by a wet etching step. However, because the material of the first sidewall 4a is silicon oxide, during wet etching, when using hydrofluoric acid (HF) solution for cleaning, the first sidewall 4a is etched laterally, causing an "inward cut". As a result, the metal silicide layer 5 in the second region II will fill the inward cut region (as shown in Figure A), causing the distance between the metal silicide layer and the first gate structure 2a to be too close. This increases the leakage current between the source and drain of the first region I, increases the risk of breakdown, and seriously affects the performance stability of the CMOS device in the first region.

[0017] To address the aforementioned technical problem, the semiconductor structure formation method provided in this embodiment of the invention involves forming a gate structure on a substrate, wherein the gate structure on the first region serves as a first gate structure, the gate structure on the second region serves as a second gate structure, and a sidewall structure is formed on the sidewall of the gate structure. The sidewall structure includes a first sidewall and a second sidewall, with the first sidewall being closer to the gate structure than the second sidewall. A source / drain doped layer is formed on the top of the substrate on both sides of the gate structure. Then, the sidewall structure at the source electrode in the source / drain doped layer on the side of the second gate structure is removed. This improves the efficiency of carrier tunneling from the source electrode into the channel when the semiconductor structure is in operation, effectively modulates the band structure and electric field distribution at the source electrode in the second region, and improves the electrical performance of the semiconductor structure. Furthermore, because the self-aligned barrier layer on the surface of the source and drain doped layer and the top of the gate structure are wet-etched, the first sidewall is more resistant to etching than the self-aligned barrier layer. As a result, the first sidewall on both sidewalls of the first gate structure and the drain side of the second gate structure can effectively resist the lateral etching of the wet etching solution, suppress the "hollowing out" phenomenon of the first sidewall, which is beneficial to control the source and drain in the first region and the drain leakage current in the second region, reduce the risk of semiconductor structure breakdown, and improve the reliability and performance of the semiconductor structure.

[0018] To make the above-mentioned objects, features and advantages of the embodiments of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. Figures 2 to 13 This is a schematic diagram of the structure corresponding to each step in the semiconductor structure formation method.

[0019] Accordingly, the present invention provides a method for forming a semiconductor structure. (See reference) Figure 2 A substrate (not shown) is provided, the substrate comprising a first region I and a second region II.

[0020] The substrate is the process platform for forming semiconductor structures. In subsequent processes, the first region I is used to form high-frequency devices, and the second region II is used to form low-frequency devices, which can integrate high-frequency devices and low-frequency devices in the same substrate.

[0021] In the step of providing a substrate, the substrate includes: a substrate 100; a shallow trench isolation (STI) structure 101 formed on top of the substrate 100 at the junction of the first region I and the second region II; a well region 102 formed on top of the first region I in the substrate 100; and a gate oxide layer 103 formed on top of the substrate 100, the shallow trench isolation (STI), and the well region 102.

[0022] In this embodiment, the substrate 100 is made of silicon, germanium, silicon carbide or gallium arsenide. The substrate 100 may also be a silicon substrate 100 on an insulator or a germanium substrate 100 on an insulator.

[0023] The isolation structure 101 is used to achieve electrical isolation between the first region I and the second region II, which can effectively prevent leakage current from occurring between devices subsequently formed in the first region I and devices formed in the second region II.

[0024] In this embodiment, the material of the isolation structure 101 includes silicon oxide. Silicon oxide is a commonly used and easily fabricated dielectric material in semiconductor processes.

[0025] In this embodiment, the top of the isolation structure 101 is flush with the top of the substrate 100. As an example, chemical mechanical polishing (CMP) can be used to achieve the flush alignment between the top of the isolation structure 101 and the top of the substrate 100.

[0026] In this embodiment, well region 102 is a P-type well region, which provides the necessary P-type substrate 100 environment for forming NMOS transistors.

[0027] The gate oxide material layer 103 prepares for the subsequent formation of the gate oxide layer 104, which is used to isolate the substrate and the gate structure formed thereafter.

[0028] In this embodiment, the gate oxide layer 103 is made of silicon oxide. In other embodiments, the gate oxide layer may also be made of silicon oxynitride.

[0029] It should be noted that the first region I is used to form a complementary metal-oxide-semiconductor (CMOS) device, and the second region II is used to form a tunnel field-effect transistor (TFET).

[0030] In subsequent processes, by integrating complementary metal-oxide-semiconductor devices and tunneling field-effect transistors on the same substrate 100, the low-power characteristics of tunneling field-effect transistors are used to process low-frequency signals, and the high-performance characteristics of complementary metal-oxide-semiconductor devices are used to process high-frequency signals, thereby achieving efficient operation of the entire circuit at different frequencies and ultimately reducing the overall power consumption of the semiconductor structure.

[0031] refer to Figure 3A gate structure 105 is formed on the substrate, wherein the gate structure 105 on the first region I serves as a first gate structure 105a, and the gate structure 105 on the second region II serves as a second gate structure 105b.

[0032] A gate structure 105 is formed on the substrate 100. During the operation of the subsequently formed semiconductor structure, the gate structure 105 can control the opening and closing of the channel. Specifically, the gate structure 105 on the first region I serves as a first gate structure 105a, which is used to control the opening and closing of the channel in the CMOS. The gate structure 105 on the second region II serves as a second gate structure 105b, which is used to control the opening and closing of the tunneling field-effect transistor.

[0033] In this embodiment, the gate structure 105 is made of polysilicon. The gate oxide layer 104 is used to isolate the substrate 100 and the gate structure 105.

[0034] refer to Figure 4 A first lightly doped region 106 (LDD) is formed in the substrate on both sides of the first gate structure 105a. The first lightly doped region 106 helps to achieve an ultra-shallow junction (USJ), thereby reducing the channel leakage current of the CMOS device subsequently formed in the first region I and reducing the short-channel effect.

[0035] In addition, the first lightly doped region 106 forms a concentration gradient with the subsequently formed heavily doped source and drain doped layers, making it difficult for doped ions in the subsequently formed source and drain doped layers to pass through the first lightly doped region 106 and enter the channel region below the gate structure 105. This helps to control the electric field strength in the channel region from increasing, prevents the generation of hot carriers, and makes the gate structure 105 less likely to be damaged.

[0036] The step of forming the first lightly doped region 106 includes: forming an offset sidewall 117 on the sidewall of the gate structure 105; after forming the offset sidewall 117, forming a second gate structure 105b covering the second region II and exposing the first gate structure 105a of the first region I, a mask layer 114; and performing lightly doped ion implantation on the substrate located on both sides of the first gate structure 105a to form the first lightly doped region 106. The offset sidewall 117 is used to define the position of the first lightly doped region 106.

[0037] The offset sidewall 117 is a single-layer structure or a multi-layer structure. In this embodiment, the material of the offset sidewall 117 includes one or more of silicon nitride, silicon oxycarbide, and silicon carbonitride.

[0038] It should be noted that, in the step of forming the first lightly doped region 106 in the substrate on both sides of the first gate structure 105a, the first lightly doped region 106 on both sides of the first gate structure 105a is doped with N-type ions. In other embodiments, in the step of forming the first lightly doped region in the substrate on both sides of the first gate structure, the first lightly doped region on both sides of the first gate structure is doped with P-type ions.

[0039] It should be noted that after forming the first lightly doped region 106, the first lightly doped region 106 is annealed, and the annealing process is either peak annealing or laser annealing. Peak annealing or laser annealing can activate the dopant ions in the first lightly doped region 106 and repair lattice defects.

[0040] refer to Figure 5 and Figure 6 A sidewall structure 107 is formed on the sidewall of the gate structure 105. The sidewall structure 107 includes a first sidewall 107a and a second sidewall 107b. The first sidewall 107a is closer to the gate structure 105 than the second sidewall 107b.

[0041] The sidewall structure 107 is used to protect the sidewall of the gate structure 105 and to define the formation location of the source and drain doped layers during the subsequent formation of the source and drain doped layers. In addition, the sidewall structure 107 is a stacked structure to optimize the performance of the sidewall structure 107.

[0042] In this embodiment, the dielectric constant of the first sidewall 107a material is in the range of 2.5 to 3.0. That is, the dielectric constant of the first sidewall 107a material is close to the K value of conventional dielectric materials (e.g., silicon oxide, whose dielectric constant (K value is about 3.9)), so as not to significantly change the parasitic capacitance between the gate structure 105 and the subsequently formed source and drain doped layers.

[0043] It should also be noted that the first sidewall 107a has a smaller etch selectivity compared to silicon oxide. In other words, in the subsequent wet etching process of the self-aligned barrier layer on the top of the gate structure 105 and the surface of the source / drain doped layer, the first sidewall 107a is not easily etched. Therefore, even if over-etching is required to ensure that the top of the gate structure 105 and the surface of the source / drain doped layer are thoroughly cleaned, the first sidewall 107a can effectively avoid excessive lateral etching.

[0044] As an example, the material of the first sidewall 107a includes carbon-doped silicon oxide (SiOC). Carbon-doped silicon oxide has a dielectric constant close to that of silicon oxide, and it is less susceptible to damage during subsequent thorough cleaning of the top of the gate structure 105 and the surfaces of the source and drain doped layers.

[0045] As an example, the second sidewall 107b is made of silicon nitride. Silicon nitride has high hardness and chemical stability, which can effectively protect the sidewalls of the gate structure 105 and the first sidewall 107a, ensuring the stability of the overall sidewall structure.

[0046] In the step of forming a sidewall structure 107 on the sidewall of the gate structure 105, the first sidewall 107a includes: a first portion (perpendicular to the surface of the substrate 100), the first portion being formed between the second sidewall 107b and the gate structure 105; and a second portion (parallel to the surface of the substrate 100), formed at the bottom of the first portion and connected to the first portion, the second portion extending in a direction away from the gate structure 105, and the second portion being located between the second sidewall 107b and the substrate (i.e. forming an L-shaped first sidewall 107a).

[0047] When wet etching is subsequently performed on the surface of the source / drain doped layer and the self-aligned barrier layer on top of the gate structure 105 to ensure thorough surface cleaning, the first sidewall 107a of the first region I can effectively resist the etching of the wet solution due to the material itself. Correspondingly, the second part of the sidewall structure 107 can cover and protect the substrate surface area adjacent to the bottom edge of the gate structure 105. Even if the wet etching solution has a certain lateral erosion capability, the etch-resistant second part can effectively prevent the etching solution from penetrating to the interface between the second sidewall 107b and the substrate, avoiding the "undercut" phenomenon. This ensures that the bottom interface of the sidewall structure 107 on the side of the first gate structure 105a remains intact, which is beneficial for accurately controlling the formation range of the subsequent metal silicide layer in the source / drain doped layer.

[0048] Specifically, the step of forming a sidewall structure 107 on the sidewall of the gate structure 105 includes: as follows Figure 5 As shown, a first sidewall material layer 115 is conformally covered on the gate structure 105 and the substrate 100; after conformally covering the first sidewall material layer 115, a second sidewall material layer 116 is conformally covered on the gate structure 105 and the substrate 100; as Figure 6 As shown, a maskless dry etching process is used to remove the first sidewall material layer 115 and the second sidewall material layer 116 on the substrate 100, and the remaining first sidewall material layer 115 and second sidewall material layer 116 located on the sidewall of the gate structure 105 serve as the sidewall structure 107.

[0049] By conformally depositing a first sidewall material layer 115 and a second sidewall material layer 116 and performing anisotropic dry etching, a composite structure consisting of a first sidewall 107a and a second sidewall 107b is formed on the sidewall of the gate structure 105.

[0050] As an example, a first sidewall material layer 115 is formed using chemical vapor deposition (CVD). CVD has excellent conformal coverage capabilities and allows for precise control of film composition and thickness, thereby uniformly depositing a compliant carbon-doped silicon oxide film on the sidewalls of the gate structure 105 with complex morphology.

[0051] Similarly, a second sidewall material layer 116 is formed using chemical vapor deposition (CVD). CVD has good step coverage and thickness uniformity, enabling the uniform deposition of silicon nitride thin films on the first sidewall material layer 115. This results in good morphology and size control for the sidewall structure 107, which is beneficial for accurately defining the formation areas of subsequent source / drain doped layers.

[0052] refer to Figure 7 After forming a sidewall structure 107 on the sidewall of the gate structure 105, a source / drain doped layer 108 is formed on the top of the substrate 100 on both sides of the gate structure 105.

[0053] After the sidewall structure 107 is formed, a source / drain doped layer 108 is formed on the top of the substrate 100 on both sides of the gate structure 105. The sidewall structure 107 is used to define the formation location of the source / drain doped layer 108 and define the effective channel length of the device, so that it can be connected to the external circuit through the source / drain doped layer 108.

[0054] In this embodiment, an ion implantation process is used to form source / drain doped layers 108 on top of the substrate 100 on both sides of the gate structure 105. During the ion implantation process to form the source / drain doped layers 108, the sidewall structure 107 serves as a self-aligned structure to define the formation location of the source / drain doped layers 108.

[0055] Specifically, the source and drain doped layers 108 on the side of the first gate structure 105a and the source on the side of the second gate structure 105b are doped with N-type ions, and the drain on the side of the second gate structure 105b is doped with P-type ions.

[0056] By doping the source and drain doping layers 108 of the first gate structure 105a with N-type ions and the source of the second gate structure 105b with P-type ions, an NMOS transistor of a CMOS device is formed in the first region I, and a tunneling field-effect transistor (P-TFET) with an N-type source and a P-type drain is constructed in the second region II. High-speed switching characteristics are achieved through the high electron mobility of the NMOS transistor, while a steep subthreshold swing and extremely low off-state leakage current are achieved using the interband tunneling mechanism in the source (N-type), channel, and drain (P-type) structure of the P-TFET. Therefore, it is possible to integrate high-frequency logic units (composed of CMOS) and low-power switching units (composed of P-TFETs) on the same chip.

[0057] It should also be noted that the source and drain doped layers 108 on both sides of the first gate structure 105a in the first region I are in contact with the first lightly doped region 106.

[0058] In the first region I, the heavily doped source / drain doped layers 108 on both sides of the first gate structure 105a are in contact with the first lightly doped region 106, thereby achieving gradient doping from the channel edge to the high-concentration source / drain doped layers 108. This effectively reduces the peak electric field intensity in the region near the drain end channel when the CMOS device is working, which is beneficial to improving the reliability of the CMOS device.

[0059] Continue to refer to Figure 7 The method for forming the semiconductor structure further includes annealing the source / drain doped layer 108.

[0060] An annealing process is performed to provide sufficient heat energy for impurity atoms injected into the substrate 100 to replace silicon lattice sites, transforming them into an electrically active state and repairing lattice defects caused by ion bombardment. This results in the source / drain doped layer 108 having good conductivity and low contact resistance, thereby improving the electrical performance of the semiconductor structure.

[0061] In this embodiment, the annealing process is either peak annealing or laser annealing. Peak annealing or laser annealing can activate the doped ions in the source / drain doped layer 108 and repair lattice defects.

[0062] refer to Figure 8 and Figure 9 Remove the sidewall structure 107 at the source of the source-drain doped layer 108 on the side of the second gate structure 105b.

[0063] By selectively removing the sidewall structure 107 on the source side of the second gate structure 105b, the metal silicide layer is subsequently formed on the second gate source. The metal silicide on the source can then extend slightly toward the channel direction below the second gate structure 105b, reducing the distance between the metal silicide layer and the channel. This optimizes the electric field distribution at the source of the tunneling field-effect transistor, making it easier for charge carriers to tunnel from the source into the channel, which is beneficial for improving the on-state current (Ion) of the tunneling field-effect transistor.

[0064] Specifically, the step of removing the sidewall structure 107 at the source electrode in the source / drain doped layer 108 on the side of the second gate structure 105b includes: forming a shielding material layer 110 covering the gate structure 105 and the substrate 100; patterning the shielding material layer 110 to form a shielding layer 109, wherein the shielding layer 109 exposes the sidewall structure 107 at the source electrode on the side of the second gate structure 105b; and using the shielding layer 109 as a mask to remove the sidewall structure 107 exposed by the shielding layer 109.

[0065] By forming a shielding material layer 110 covering the gate structure 105 and the substrate 100, and patterning the shielding material layer 110 to form a shielding layer 109, the removal region is defined, and etching is performed using the shielding layer 109 as a mask. This achieves selective removal of the sidewall structure 107 on the source side of the second gate structure 105b, while protecting the sidewall structure 107 on the drain side of the tunneling field-effect transistor and the sidewall structures 107 on both sides of the CMOS device from being affected, thus meeting the requirements of the single-sided sidewall structure 107 of the tunneling field-effect transistor.

[0066] In this embodiment, the material of the shielding layer 109 includes silicon oxide. Silicon oxide is a commonly used and low-cost dielectric material with high process compatibility. In other embodiments, the material of the shielding layer includes an organic dielectric layer, an anti-reflective coating on the organic dielectric layer, and a photoresist layer on the anti-reflective coating. Specifically, the material of the organic dielectric layer is spin-on carbon (SOC). Spin-on carbon is low-cost, simple to form, and has high process compatibility. The material of the anti-reflective coating includes silicon-containing anti-reflective coating (SiARC) material.

[0067] In this embodiment, the step of removing the sidewall structure 107 at the source electrode in the source / drain doped layer 108 on the side of the second gate structure 105b includes using a wet etching process. The wet etching process is isotropic etching, has a high etching rate, is simple to operate, and has low process cost. Furthermore, the wet etching solution will not come into contact with the sidewall structure 107 on the drain side of the tunneling field-effect transistor covered by the shielding layer 109, nor with the sidewall structures 107 on both sides of the CMOS device, thus avoiding damage to the sidewall structure 107 on the drain side of the tunneling field-effect transistor and the sidewall structures 107 on both sides of the CMOS device.

[0068] refer to Figure 10 The method for forming the semiconductor structure further includes: forming a second lightly doped region 111 on the top of the substrate 100 on the side of the second gate structure 105b, wherein the second lightly doped region 111 is connected to the source / drain doped layer 108 on the side of the second gate structure 105b.

[0069] As an example, the top of the substrate 100 on the side of the second gate structure 105b is lightly doped to form a second lightly doped region 111. This light doping process creates a doping concentration gradient transition region between the channel edge and the subsequently formed high-concentration source / drain doped layer 108. This effectively modulates the electric field distribution in the second region II, particularly controlling the electric field peak and gradient near the tunnel junction of the tunneling field-effect transistor, thereby improving the device's breakdown voltage and reliability.

[0070] Specifically, on the source side of the second gate structure 105b, the second lightly doped region 111 is located on top of the source / drain doped layer 108 and on top of the substrate 100 between the source / drain doped layer 108 and the offset sidewall 117; on the drain side of the second gate structure 105b, the second lightly doped region 111 is located on top of the source / drain doped layer 108.

[0071] It should be noted that the second lightly doped region 111 on the source side of the second gate structure 105b is doped with N-type ions, while the second lightly doped region 111 on the drain side of the second gate structure 105b is doped with P-type ions. In other words, P-type ions are doped on the side where the sidewall structure 107 is retained, and N-type ions are doped on the side where the sidewall structure 107 is removed.

[0072] In this embodiment, the step of lightly doping the top of the substrate 100 on the side of the second gate structure 105b includes ion implantation.

[0073] refer to Figure 11 and Figure 12The method for forming the semiconductor structure further includes: after removing the sidewall structure 107 at the source of the second gate structure 105b, forming a self-aligned barrier layer 113 that exposes the top of the gate structure 105 and the surfaces of the source / drain doped layers 108 on both sides of the gate structure 105. The self-aligned barrier layer 113 exposes the area that needs to be subsequently processed with metal silicide.

[0074] In this embodiment, the step of forming a self-aligned barrier layer 113 that exposes the top of the gate structure 105 and the surfaces of the source / drain doped layers 108 on both sides of the gate structure 105 includes: forming a barrier material layer 112 covering the gate structure 105 and the substrate 100; removing the barrier material layer 112 from the top of the gate structure 105 and the surfaces of the source / drain doped layers 108 on both sides of the gate structure 105, with the remaining barrier material layer 112 serving as the self-aligned barrier layer 113.

[0075] By forming a barrier material layer 112 covering the gate structure 105 and the substrate 100, the patterned barrier material layer 112 forms a self-aligned block (SAB). The self-aligned block 113 defines the effective range of the wet etching solution, thereby ensuring that the wet etching only acts on the areas where the metal silicide layer needs to be formed, namely the surface of the source / drain doped layer 108 and the top of the gate. Other areas, such as the top of the sidewall structure 107 and the isolation structure 101, are protected, achieving precise control of the surface cleaning area and preparing for the subsequent formation of the metal silicide layer.

[0076] In this embodiment, the self-aligned barrier layer 113 is made of silicon oxide. Silicon oxide is a commonly used and low-cost dielectric material with high process compatibility. In other embodiments, the self-aligned barrier layer is made of an organic dielectric layer, an anti-reflective coating on the organic dielectric layer, and a photoresist layer on the anti-reflective coating. Specifically, the organic dielectric layer is made of spin-on carbon (SOC). Spin-on carbon is low-cost, simple to form, and has high process compatibility. The anti-reflective coating is made of silicon-containing anti-reflective coating (SiARC) material.

[0077] In this embodiment, a dry etching process is used to remove the barrier material layer 112 on the top of the gate structure 105 and the surface of the source / drain doped layers 108 on both sides of the gate structure 105, forming a self-aligned barrier layer 113. The dry etching process is an anisotropic etching process with good control over the etching profile, enabling precise opening of the surface of the source / drain doped layers 108 and the top of the gate structure 105. This prepares for subsequent wet etching cleaning of the surface of the source / drain doped layers 108 and the top of the gate structure 105, as well as for the self-aligned formation of the metal silicide layer, simplifying the metal silicide layer formation steps.

[0078] Continue to refer to Figure 12 Wet etching is performed on the surface of the source / drain doped layer 108 and the self-aligned barrier layer 113 on top of the gate structure 105. The first sidewall 107a is more resistant to etching than the self-aligned barrier layer 113.

[0079] In the semiconductor structure formation method provided in this embodiment of the invention, a gate structure 105 is formed on a substrate. The gate structure 105 on the first region I serves as a first gate structure 105a, and the gate structure 105 on the second region II serves as a second gate structure 105b. A sidewall structure 107 is formed on the sidewall of the gate structure 105. The sidewall structure 107 includes a first sidewall 107a and a second sidewall 107b. The first sidewall 107a is closer to the gate structure 105 than the second sidewall 107b. A source / drain doped layer 108 is formed on the top of the substrate on both sides of the gate structure 105. Then, the sidewall structure 107 at the source of the source / drain doped layer 108 on the side of the second gate structure 105b is removed. This improves the efficiency of carrier tunneling from the source into the channel when the semiconductor structure is working, effectively modulates the band structure and electric field distribution at the source in the second region II, and improves the electrical performance of the semiconductor structure. Furthermore, because the surface of the source / drain doped layer 108 and the self-aligned barrier layer 113 on the top of the gate structure 105 are wet-etched, the first sidewall 107a is more resistant to etching than the self-aligned barrier layer 113. As a result, the first sidewall 107a on the two sidewalls of the first gate structure 105a and the drain side of the second gate structure 105b can effectively resist the lateral etching of the wet etching solution, suppress the "hollowing out" phenomenon of the first sidewall 107a, which is beneficial to control the source and drain of the first region I and the drain leakage current of the second region II, reduce the risk of semiconductor structure breakdown, and improve the reliability and performance of the semiconductor structure.

[0080] In this embodiment, the material of the self-aligned barrier layer includes silicon oxide; in the step of wet etching the surface of the source / drain doped layer and the self-aligned barrier layer 113 on the top of the gate structure, the first sidewall is more resistant to etching than silicon oxide.

[0081] It should also be noted that during the wet etching process of the surface of the source / drain doped layer 108 and the self-aligned barrier layer 113 on the top of the gate structure 105, the first sidewall 107a is more resistant to etching than the second sidewall 107b.

[0082] After removing the sidewall structure 107 at the source of the second gate structure 105b, wet etching is performed on the surface of the source / drain doped layer 108 and the self-aligned barrier layer 113 on top of the gate structure 105. Taking advantage of the fact that the first sidewall 107a is more resistant to etching than the second sidewall 107b, the first sidewall 107a can be effectively used as an etching barrier layer when cleaning regions where a metal silicide layer needs to be formed (e.g., the surface of the source of a tunneling field-effect transistor). This prevents the wet etching solution from laterally eroding (i.e., "hollowing out") the first sidewall 107a in the first region I and the second region II, solving the problem of CMOS device performance degradation caused by cleaning regions where a metal silicide layer needs to be formed, improving the reliability of the CMOS device, and increasing the cleaning process window during the formation of the metal silicide layer.

[0083] In this embodiment, the wet etching solution used in the step of wet etching the surface of the source / drain doped layer 108 and the self-aligned barrier layer 113 on top of the gate structure 105 includes hydrofluoric acid. The wet etching solution includes a solution of hydrofluoric acid (HF). Utilizing the high selective etching capability of hydrofluoric acid on oxide layers such as silicon oxide, it can effectively clean exposed surfaces, such as the surface of the source / drain doped layer 108, the top of the gate structure 105, and the source corner region on the second gate side, as well as any possible residual oxides, thus improving the quality of the subsequently formed metal silicide layer.

[0084] refer to Figure 13 The method for forming the semiconductor structure further includes: performing wet etching on the surface of the source / drain doped layer 108 and the self-aligned barrier layer 113 on the top of the gate structure 105, and then forming a metal silicide layer 114 on the top of the gate structure 105 and the top of the source / drain doped layer 108.

[0085] After wet etching and cleaning of the self-aligned barrier layer 113 on the surface of the source / drain doped layer 108 and the top of the gate structure 105, a metal silicide layer 114 is formed on the exposed top of the gate structure 105 and the source / drain doped layer 108. The cleaned surfaces are utilized to promote the metal-silicide reaction between the metal and silicon, forming metal silicide compounds. This reduces the contact resistance on the top of the gate structure 105 and the top of the source / drain doped layer 108, which is beneficial for improving the high-frequency performance of CMOS devices and the conduction performance of tunneling field-effect transistors.

[0086] In this embodiment, a metal silicide layer 114 is formed on top of the gate structure 105 and on top of the source / drain doped layer 108 using a self-aligned silicide process.

[0087] The self-aligned silicide process utilizes the characteristic that metal reacts only with the exposed silicon (or polysilicon) surface under annealing conditions, and does not react with dielectric materials such as silicon dioxide or silicon nitride. This allows metal silicides to be automatically and without additional mask alignment formed on the exposed source / drain doped layer 108 and the top of the gate structure 105, simplifying the process flow for forming low-resistance contacts and providing high alignment accuracy.

[0088] It should be noted that in the step of forming the self-aligned silicide layer, since the sidewall at the source of the second gate structure 105b has been removed, the second lightly doped region 111 at that location is exposed, and the corresponding metal silicide layer 114 is also formed on the second lightly doped region 111 at the source of the second gate structure 105b. In other words, the distance between the metal silicide layer 114 at the source of the second gate structure 105b and the channel in the tunneling field-effect transistor is small, which can effectively optimize the electric field distribution in the tunneling junction region or enhance the impurity segregation effect, increase the on-state current of the tunneling field-effect transistor, and improve the electrical performance of the tunneling field-effect transistor.

[0089] In this embodiment, the metal silicide layer 114 is nickel silicide (NiSi). Nickel silicide has advantages such as low silicon consumption, low formation temperature, low stress, and no size effect at narrow linewidths, thus enabling the formation of high-quality, low-resistance contacts at advanced process nodes. In other embodiments, the material of the metal silicide layer also includes titanium silicide (TiSi2) or cobalt silicide (CoSi2).

[0090] refer to Figure 13This invention also provides a semiconductor structure. The semiconductor structure includes: a substrate comprising a first region I and a second region II, wherein a high-frequency device is formed in the first region I and a low-frequency device is formed in the second region II; a gate structure 105 located on the substrate, wherein the gate structure 105 in the first region I serves as a first gate structure 105a and the gate structure 105 in the second region II serves as a second gate structure 105b; source / drain doped layers 108 located on the top of the substrate on both sides of the gate structure 105; and sidewall structures 107 located on the two sidewalls of the first gate structure 105a and on the sidewall of the drain electrode in the source / drain doped layers 108 on the side of the second gate structure 105b. The sidewall structures 107 include a first sidewall 107a and a second sidewall 107b, wherein the first sidewall 107a is closer to the gate structure 105 than the second sidewall 107b, and the etching resistance of the first sidewall 107a is greater than that of silicon oxide.

[0091] In the semiconductor structure provided in this embodiment of the invention, a gate structure 105 is located on a substrate. The gate structure 105 in the first region I serves as a first gate structure 105a, and the gate structure 105 in the second region II serves as a second gate structure 105b. Sidewall structures 107 are located on the two sidewalls of the first gate structure 105a and the drain sidewall of the second gate structure 105b. The sidewall structure 107 includes a first sidewall 107a and a second sidewall 107b. The first sidewall 107a is closer to the gate structure 105 than the second sidewall 107b, and the etching resistance of the first sidewall 107a is greater than that of silicon oxide. Thus, during the formation of the semiconductor structure, the more etch-resistant first sidewall 107a can act as an effective etching barrier layer, which can define the etching range and prevent the first sidewall 107a from being excessively etched laterally on both sides of the first gate structure 105a in the first region I, thus preventing the "hollowing out" phenomenon. This ensures that the sidewall structures 107a on both sides of the first gate structure 105a in the first region I are intact, which helps to avoid leakage current caused by the intrusion of metal silicides and optimizes the electrical performance of the semiconductor structure.

[0092] Furthermore, since high-frequency devices are formed in the first region I and low-frequency devices are formed in the second region II, the source-drain doped layer 108 is located on the top of the substrate on both sides of the gate structure 105, and no sidewall structure 107 is formed on the sidewall of the source-drain doped layer 108 on the side of the second gate structure 105b. This allows for more effective modulation of the energy band structure and electric field distribution of the source, thereby improving the efficiency of carrier tunneling from the source into the channel and improving the electrical performance of the semiconductor structure.

[0093] The substrate includes a first region I and a second region II, wherein a high-frequency device is formed in the first region I and a low-frequency device is formed in the second region II.

[0094] The first region I contains high-frequency devices, and the second region II contains low-frequency devices. This allows for the hybrid integration of transistors with different operating characteristics on the substrate 100, thereby meeting the differentiated requirements of different functional modules for switching speed and static power consumption. The high drive capability and high operating frequency characteristics of the devices in the first region I are selectively utilized, along with the excellent subthreshold swing and low cutoff current characteristics of the devices in the second region II. High-speed logic or RF circuits can be placed in the first region I, while power-sensitive low-frequency, standby, or memory circuits can be placed in the second region II, improving the electrical performance of the semiconductor structure.

[0095] In this embodiment, the substrate includes: a substrate 100; a shallow trench isolation (STI) structure 101 located on top of the substrate 100 at the junction of the first region I and the second region II; a well region 102 located on top of the first region I in the substrate 100; and a gate oxide layer 104 located on top of the substrate 100, the shallow trench isolation (STI), and the well region 102.

[0096] In this embodiment, the substrate 100 is made of silicon, germanium, silicon carbide or gallium arsenide. The substrate 100 may also be a silicon substrate 100 on an insulator or a germanium substrate 100 on an insulator.

[0097] The isolation structure 101 is used to achieve electrical isolation between the first region I and the second region II, which can effectively prevent leakage current between devices subsequently formed in the first region I and devices formed in the second region II.

[0098] In this embodiment, the material of the isolation structure 101 includes silicon oxide. Silicon oxide is a commonly used and easily fabricated dielectric material in semiconductor processes.

[0099] In this embodiment, the top of the isolation structure 101 is flush with the top of the substrate 100. As an example, chemical mechanical polishing (CMP) can be used to achieve the flush alignment between the top of the isolation structure 101 and the top of the substrate 100.

[0100] In this embodiment, well region 102 is a P-type well region, which provides the necessary P-type substrate 100 environment for forming NMOS transistors.

[0101] The gate oxide layer 104 is used to isolate the substrate 100 and the gate structure 105.

[0102] In this embodiment, the gate oxide layer 104 is made of silicon oxide. In other embodiments, the gate oxide layer may also be made of silicon oxynitride.

[0103] It should be noted that the first region I is used to form a complementary metal-oxide-semiconductor (CMOS) device, and the second region II is used to form a tunnel field-effect transistor (TFET).

[0104] By integrating complementary metal-oxide-semiconductor devices and tunneling field-effect transistors on the same substrate 100, the low-power characteristics of tunneling field-effect transistors are used to process low-frequency signals, and the high-performance characteristics of complementary metal-oxide-semiconductor devices are used to process high-frequency signals, thereby achieving efficient operation of the entire circuit at different frequencies and ultimately reducing the overall power consumption of the semiconductor structure.

[0105] A gate structure 105 is located on the substrate, wherein the gate structure 105 in the first region I serves as a first gate structure 105a, and the gate structure 105 in the second region II serves as a second gate structure 105b.

[0106] When the semiconductor structure is operating, the gate structure 105 can control the opening and closing of the channel. Specifically, the gate structure 105 on the first region I serves as the first gate structure 105a, which is used to control the opening and closing of the channel in the CMOS. The gate structure 105 on the second region II serves as the second gate structure 105b, which is used to control the opening and closing of the tunneling field-effect transistor.

[0107] In this embodiment, the material of the gate structure 105 includes polysilicon.

[0108] The semiconductor structure includes an offset sidewall 117 located on the sidewall of the gate structure 105 and between the gate structure and the first sidewall 107a.

[0109] The offset sidewall 117 is a single-layer structure or a multi-layer structure. In this embodiment, the material of the offset sidewall 117 includes one or more of silicon nitride, silicon oxycarbide, and silicon carbonitride.

[0110] The semiconductor structure further includes a first lightly doped region 106 (LDD), located on top of the substrate 100 on the side of the first gate structure 105a.

[0111] The first lightly doped region 106 helps achieve an ultra-shallow junction (USJ), thereby reducing the channel leakage current of the CMOS device subsequently formed in the first region I and minimizing the short-channel effect. The first lightly doped region 106 forms a concentration gradient with the subsequently formed source / drain doped layers 108, making it difficult for dopant ions in the subsequently formed source / drain doped layers 108 to penetrate the first lightly doped region 106 and enter the channel region below the gate structure 105. This helps control the electric field strength in the channel region, easily preventing the generation of hot carriers and making the gate structure 105 less susceptible to damage.

[0112] In this embodiment, the first lightly doped regions 106 on both sides of the first gate structure 105a are doped with N-type ions. In other embodiments, the first lightly doped regions on both sides of the first gate structure may also be doped with P-type ions.

[0113] The semiconductor structure further includes a source / drain doped layer 108, located on the top of the substrate on both sides of the gate structure 105.

[0114] Specifically, the source and drain doped layers 108 on the side of the first gate structure 105a and the source on the side of the second gate structure 105b are doped with N-type ions, and the drain on the side of the second gate structure 105b is doped with P-type ions.

[0115] By doping the source and drain doping layers 108 of the first gate structure 105a with N-type ions and the source of the second gate structure 105b with P-type ions, an NMOS transistor of a CMOS device is formed in the first region I, and a tunneling field-effect transistor (P-TFET) with an N-type source and a P-type drain is constructed in the second region II. High-speed switching characteristics are achieved through the high electron mobility of the NMOS transistor, while a steep subthreshold swing and extremely low off-state leakage current are achieved using the interband tunneling mechanism in the source (N-type), channel, and drain (P-type) structure of the P-TFET. Therefore, it is possible to integrate high-frequency logic units and low-power switching units on the same chip.

[0116] It should also be noted that the source and drain doped layers 108 on both sides of the first gate structure 105a in the first region I are in contact with the first lightly doped region 106.

[0117] In the first region I, the heavily doped source / drain doped layers 108 on both sides of the first gate structure 105a are in contact with the first lightly doped region 106, thereby achieving gradient doping from the channel edge to the high-concentration source / drain doped layers 108. This effectively reduces the peak electric field intensity in the region near the drain end channel when the CMOS device is working, which is beneficial to improving the reliability of the CMOS device.

[0118] Sidewall structures 107 are located on the two sidewalls of the first gate structure 105a and on the drain sidewall of the source / drain doped layer 108 of the second gate structure 105b. The sidewall structures 107 include a first sidewall 107a and a second sidewall 107b. The first sidewall 107a is closer to the gate structure 105 than the second sidewall 107b, and the first sidewall 107a is more resistant to etching than the second sidewall 107b. The sidewall structures 107 protect the sidewalls of the gate structure 105. Furthermore, the sidewall structures 107 are multilayered to optimize their performance.

[0119] In this embodiment, the first sidewall 107a is more etch-resistant than the second sidewall 107b. Therefore, during the formation of the semiconductor structure, the more etch-resistant first sidewall 107a can act as an effective etching barrier layer, defining the etching range and preventing excessive lateral etching of the first sidewall 107a on both sides of the first gate structure 105a in the first region I, thus preventing a "hollowing-out" phenomenon. This ensures the integrity of the sidewall structures 107a on both sides of the first gate structure 105a in the first region I, which helps avoid leakage current caused by metal silicide intrusion and optimizes the electrical performance of the semiconductor structure.

[0120] In this embodiment, the dielectric constant of the first sidewall 107a material is in the range of 2.5 to 3.0. That is, the dielectric constant of the first sidewall 107a material is close to the K value of conventional dielectric materials (e.g., silicon oxide, whose dielectric constant (K value is about 3.9)), so as not to significantly change the parasitic capacitance between the gate structure 105 and the source / drain doped layer 108.

[0121] As an example, the first sidewall 107a is carbon-doped silicon oxide (SiOC). Carbon-doped silicon oxide has a dielectric constant close to that of silicon oxide and is not easily damaged when the top of the gate structure 105 and the surface of the source / drain doped layer 108 are thoroughly cleaned.

[0122] As an example, the second sidewall 107b is made of silicon nitride. Silicon nitride has high hardness and chemical stability, which can effectively protect the sidewalls of the gate structure 105 and the first sidewall 107a, ensuring the stability of the overall sidewall structure.

[0123] In this embodiment, the first sidewall 107a includes: a first portion (perpendicular to the surface of the substrate 100), the first portion being located between the second sidewall 107b and the gate structure 105; and a second portion (parallel to the surface of the substrate 100), located at the bottom of the first portion and connected to the first portion, the second portion extending in a direction away from the gate structure 105, and the second portion being located between the second sidewall 107b and the substrate.

[0124] The semiconductor structure further includes a second lightly doped region 111, located on top of the substrate 100 on the side of the second gate structure 105b, and the second lightly doped region 111 is connected to the source / drain doped layer 108 on the side of the second gate structure 105b.

[0125] The second lightly doped region 111 is located on the top of the substrate 100 on the side of the second gate structure 105b. In other words, a doping concentration gradient transition region is established between the channel edge and the high-concentration source / drain doped layer 108, which can effectively modulate the electric field distribution of the second region II. In particular, the peak value and gradient of the electric field are controlled near the tunnel junction of the tunneling field-effect transistor, which can improve the breakdown voltage and reliability of the device.

[0126] Specifically, on the source side of the second gate structure 105b, the second lightly doped region 111 is located on top of the source / drain doped layer 108 and on top of the substrate 100 between the source / drain doped layer 108 and the offset sidewall 117; on the drain side of the second gate structure 105b, the second lightly doped region 111 is located on top of the source / drain doped layer 108.

[0127] It should be noted that the second lightly doped region 111 on the source side of the second gate structure 105b is doped with N-type ions, while the second lightly doped region 111 on the drain side of the second gate structure 105b is doped with P-type ions. In other words, P-type ions are doped on the side where the sidewall structure 107 is retained, and N-type ions are doped on the side where the sidewall structure 107 is removed.

[0128] The semiconductor structure further includes a metal silicide layer 114, located on top of the source / drain doped layer 108 and on top of the gate structure 105.

[0129] Metal silicide compounds are used to reduce the contact resistance at the top of the gate structure 105 and the top of the source / drain doped layer 108, which is beneficial to improving the high-frequency performance of CMOS devices and the conduction performance of tunneling field-effect transistors.

[0130] It should be noted that the metal silicide layer 114 is also formed on the second lightly doped region 111 of the source side of the second gate structure 105b. That is, the distance between the metal silicide layer 114 of the source side of the second gate structure 105b and the channel in the tunneling field-effect transistor is small, which can effectively optimize the electric field distribution of the tunneling junction region or enhance the impurity segregation effect, increase the on-state current of the tunneling field-effect transistor, and improve the electrical performance of the tunneling field-effect transistor.

[0131] In this embodiment, the metal silicide layer 114 is nickel silicide (NiSi). Nickel silicide has advantages such as low silicon consumption, low formation temperature, low stress, and no size effect at narrow linewidths, thus enabling the formation of high-quality, low-resistance contacts at advanced process nodes. In other embodiments, the material of the metal silicide layer also includes titanium silicide (TiSi2) or cobalt silicide (CoSi2).

[0132] The semiconductor structure described in this embodiment can be formed using the formation method described in the foregoing embodiments, or it can be formed using other formation methods. For a detailed description of the semiconductor structure described in this embodiment, please refer to the corresponding descriptions in the foregoing embodiments; these descriptions will not be repeated here.

[0133] While the present invention has been disclosed above, it is not limited thereto. Any person skilled in the art can make various modifications and alterations without departing from the spirit and scope of the invention; therefore, the scope of protection of the present invention should be determined by the scope defined in the claims.

Claims

1. A method for forming a semiconductor structure, characterized in that, include: A substrate is provided, the substrate comprising a first region and a second region; A gate structure is formed on the substrate, wherein the gate structure in the first region serves as a first gate structure, and the gate structure in the second region serves as a second gate structure; A sidewall structure is formed on the sidewall of the gate structure, the sidewall structure including a first sidewall and a second sidewall, wherein the first sidewall is closer to the gate structure than the second sidewall; After the sidewall structure is formed, source and drain doped layers are formed on the top of the substrates on both sides of the gate structure; Remove the sidewall structure at the source of the second gate structure; A self-aligned barrier layer is formed that exposes the top of the gate structure and the surfaces of the source and drain doped layers on both sides of the gate structure. The surface of the source / drain doped layer and the self-aligned barrier layer on top of the gate structure are subjected to wet etching, and the first sidewall is more resistant to etching than the self-aligned barrier layer.

2. The method for forming a semiconductor structure as described in claim 1, characterized in that, The material of the first sidewall includes carbon-doped silicon oxide.

3. The method for forming a semiconductor structure as described in claim 1, characterized in that, The dielectric constant of the first sidewall material is in the range of 2.5 to 3.

0.

4. The method for forming a semiconductor structure as described in claim 1, characterized in that, The step of forming a self-aligned barrier layer that exposes the top of the gate structure and the surfaces of the source / drain doped layers on both sides of the gate structure includes: A barrier material layer is formed covering the gate structure and the substrate; The barrier material layers on the top of the gate structure and on both sides of the source / drain doped layer are removed, and the remaining barrier material layers serve as the self-aligned barrier layer.

5. The method for forming a semiconductor structure as described in claim 1, characterized in that, The material of the self-aligned barrier layer includes silicon oxide; In the step of wet etching the surface of the source / drain doped layer and the self-aligned barrier layer on top of the gate structure, the first sidewall is more resistant to etching than silicon oxide.

6. The method for forming a semiconductor structure as described in claim 1, characterized in that, In the step of forming a sidewall structure on the sidewall of the gate structure, the first sidewall includes: A first portion is formed between the second sidewall and the gate structure; The second portion is formed at the bottom of the first portion and connected to the first portion, the second portion extends in a direction away from the gate structure, and the second portion is formed between the second sidewall and the substrate.

7. The method for forming a semiconductor structure as described in claim 1, characterized in that, The step of removing the sidewall structure at the source of the source / drain doped layer on the side of the second gate structure includes: A shielding material layer is formed covering the gate structure and the substrate; The shielding material layer is graphically represented to form a shielding layer, which exposes the sidewall structure at the source of the second gate structure. Using the shielding layer as a mask, the sidewall structure exposed by the shielding layer is removed.

8. The method for forming a semiconductor structure as described in claim 1, characterized in that, The step of removing the sidewall structure at the source of the source-drain doped layer on the side of the second gate structure includes using a wet etching process.

9. The method for forming a semiconductor structure as described in claim 1, characterized in that, The step of forming a sidewall structure on the sidewall of the gate structure includes: A first sidewall material layer is conformally covered on the gate structure and the substrate; After conformally covering the first sidewall material layer, a second sidewall material layer is conformally covered on the gate structure and the substrate. The first and second sidewall material layers on the substrate are removed using a maskless dry etching process, and the remaining first and second sidewall material layers located on the sidewall of the gate structure serve as the sidewall structure.

10. The method for forming a semiconductor structure as described in claim 1, characterized in that, The first region is used to form a complementary metal-oxide-semiconductor device, and the second region is used to form a tunneling field-effect transistor.

11. The method for forming a semiconductor structure as described in claim 1, characterized in that, In the step of performing wet etching on the surface of the source / drain doped layer and the self-aligned barrier layer on top of the gate structure, the wet etching solution includes hydrofluoric acid.

12. The method for forming a semiconductor structure as described in claim 1, characterized in that, The method for forming the semiconductor structure further includes: After wet etching of the surface of the source / drain doped layer and the self-aligned barrier layer on top of the gate structure, a metal silicide layer is formed on top of the gate structure and on top of the source / drain doped layer.

13. A semiconductor structure, characterized in that, include: The substrate includes a first region and a second region, wherein a high-frequency device is formed in the first region and a low-frequency device is formed in the second region; A gate structure is located on the substrate, wherein the gate structure in the first region serves as a first gate structure, and the gate structure in the second region serves as a second gate structure; The source and drain doped layers are located on top of the substrate on both sides of the gate structure; The sidewall structure is located on the two sidewalls of the first gate structure and on the sidewall of the drain electrode in the source-drain doped layer of the second gate structure. The sidewall structure includes a first sidewall and a second sidewall. The first sidewall is closer to the gate structure than the second sidewall. The etching resistance of the first sidewall is greater than that of silicon oxide.

14. The semiconductor structure as described in claim 13, characterized in that, The material of the first sidewall includes carbon-doped silicon oxide.

15. The semiconductor structure as described in claim 13, characterized in that, The dielectric constant of the material of the first sidewall is in the range of 2.5 to 3.

0.

16. The semiconductor structure as described in claim 13, characterized in that, The first sidewall includes: The first part is located between the second sidewall and the gate structure; The second part is located at the bottom of the first part and connected to the first part, the second part extends in a direction away from the gate structure, and the second part is located between the second sidewall and the substrate.

17. The semiconductor structure as claimed in claim 13, characterized in that, The first region includes a complementary metal-oxide-semiconductor device, and the second region includes a tunneling field-effect transistor.

18. The semiconductor structure as claimed in claim 13, characterized in that, The semiconductor structure further includes a metal silicide layer located on top of the source / drain doped layer and on top of the gate structure.