An LED epitaxial structure and its fabrication method, and an LED chip
By employing a resonant tunneling electron blocking layer in the LED epitaxial structure, the contradiction between electron blocking and hole injection in the traditional AlGaN electron blocking layer is resolved, achieving efficient hole injection and stable external quantum efficiency at high current densities, thus solving the efficiency roll-off problem in the traditional structure.
Patent Information
- Application Number
- CN202611294154.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-25
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional P-type AlGaN electron blocking layers in nitride LEDs present a contradiction between electron blocking and hole injection, leading to efficiency roll-off at high current densities. Existing technologies struggle to maintain high hole injection efficiency at high current densities.
An electron blocking layer with a resonant tunneling structure is used, including a first barrier layer, a narrow bandgap insertion layer and a second barrier layer. By adjusting the thickness and composition of the narrow bandgap insertion layer, its valence band top quantization energy level is made to be less than 3 meV with the valence band top energy level of the multi-quantum well active region at a preset operating current density, so as to accurately match the resonance condition and optimize the hole injection efficiency.
It significantly improves hole injection efficiency under high current density, suppresses efficiency roll-off, and ensures that LEDs maintain high external quantum efficiency and stability under constant current drive.
Smart Images

Figure CN123124527A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor device technology, specifically to an LED epitaxial structure and its fabrication method, and an LED chip. Background Technology
[0002] As a new generation of solid-state light source, nitride light-emitting diodes (LEDs) have completely replaced traditional light sources and are widely used in LCD backlighting and general lighting due to their advantages such as high efficiency, long lifespan, and mercury-free environmental friendliness. A typical nitride LED epitaxial structure, from bottom to top, includes a substrate, an N-type semiconductor layer, a multi-quantum-well active region, an electron blocking layer (EBL), and a P-type semiconductor layer. The electron blocking layer (EBL) is one of the core functional layers affecting device performance; it is mainly responsible for limiting electron overflow from the active region and facilitating the efficient injection of holes into the active region.
[0003] However, due to the strong spontaneous polarization and piezoelectric polarization effects of nitride materials, traditional p-type AlGaN electron blocking layers face an inherent contradiction between "electron blocking" and "hole injection" in band structure engineering: the increased conduction band barrier to improve electron confinement often simultaneously forms a peak at the valence band top, which severely hinders hole transport from the p-type layer to the multi-quantum-well active region. This insufficient hole injection caused by the polarization field is one of the core causes of "efficiency droop" at high current densities. As the driving current density increases, the carrier concentration in the active region increases, electron leakage intensifies, and the hole injection efficiency further decreases, resulting in a significant decrease in the external quantum efficiency (EQE) after reaching its peak value with increasing current. Summary of the Invention
[0004] In view of the shortcomings of the prior art, the purpose of this invention is to provide an LED epitaxial structure and its preparation method, as well as an LED chip, in order to solve at least one of the problems mentioned in the background art.
[0005] The present invention provides an LED epitaxial structure, including a substrate, and further comprising: An N-type GaN layer, a multi-quantum-well active region, an electron blocking layer, and a P-type GaN layer are sequentially stacked on the substrate. The electron blocking layer is a resonant tunneling structure, comprising a first barrier layer, a narrow bandgap insertion layer, and a second barrier layer stacked sequentially. The narrow bandgap insertion layer is P-type doped In. x Ga 1-x N layers, where x ranges from 0.10 to 0.25, and both the first and second barrier layers are Al.y Ga 1-y For layer N, the value of y ranges from 0.15 to 0.30.
[0006] According to one aspect of the above technical solution, the difference between the quantized energy level of the valence band top of the narrow bandgap insertion layer and the valence band top energy level of the multi-quantum-well active region is less than 3 meV under the band bending condition at a preset operating current density. The preset operating current density is used as the current density at the rated constant current operating point of the LED, and its range is 150 A / cm². 2 -350A / cm 2 .
[0007] According to one aspect of the above technical solution, the thickness of the narrow bandgap insertion layer is 1.5nm-3.5nm, and the thickness of both the first barrier layer and the second barrier layer is 2nm-5nm.
[0008] According to one aspect of the above technical solution, the doping concentration of the narrow bandgap insertion layer is 1×10⁻⁶. 18 cm -3 -5×10 19 cm -3 At least one of the first barrier layer and the second barrier layer is P-type doped or unintentionally doped.
[0009] According to one aspect of the above technical solution, the LED is packaged as a light source for a liquid crystal display backlight module, and the fluctuation range of its rated operating current density is controlled within ±3%.
[0010] According to one aspect of the above technical solution, the LED is packaged as a light source for a constant light lighting fixture, and the fluctuation range of its rated operating current density is controlled within ±5%.
[0011] A second aspect of the present invention is to provide a method for preparing an LED epitaxial structure, the method comprising: Provide a substrate; An N-type GaN layer and a multi-quantum-well active region are epitaxially grown sequentially on the substrate. An electron blocking layer is grown on the active region of the multi-quantum well. The electron blocking layer is a resonant tunneling structure. The growth of the resonant tunneling structure specifically includes: A first barrier layer is grown on the multi-quantum-well active region. A narrow bandgap insertion layer is grown on top of the first barrier layer, and the growth temperature, pressure, and source flux are controlled to align its valence band top quantization level with the valence band top level of the multi-quantum-well active region at the designed operating point. A second barrier layer is grown on top of the narrow bandgap insertion layer; A P-type GaN layer is grown on top of the second barrier layer.
[0012] Furthermore, by adjusting the thickness, composition, and doping concentration of the narrow bandgap insertion layer, the current density corresponding to its resonant peak is matched with the target constant current operating point of the light-emitting diode.
[0013] The position of the quantized energy level is adjusted by changing the thickness of the narrow bandgap insertion layer; each 0.1 nm change in thickness corresponds to a quantized energy level shift of 5 meV-15 meV. The bandgap is adjusted by changing the In composition; each 1% change in In composition corresponds to a valence band shift of approximately 20 meV-30 meV. These adjustments have taken into account the spontaneous polarization and piezoelectric polarization effects of the nitride material.
[0014] Furthermore, in the step of growing the narrow bandgap insertion layer, the growth temperature is 700℃-780℃, and after the growth is completed, it is annealed in an N2 atmosphere.
[0015] A third aspect of the present invention is to provide an LED chip, the LED chip comprising the above-described LED epitaxial structure.
[0016] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. By utilizing the resonant tunneling effect, the hole injection efficiency is dominated by the resonant conditions, rather than simply depending on the barrier height. Under resonant conditions, the hole transmission coefficient can approach 1, while electrons are effectively blocked due to their different effective mass and failure to meet the conduction band resonance condition. This fundamentally solves the contradiction between electron blocking and hole injection in traditional EBL.
[0017] 2. Breaking away from the traditional mindset of pursuing stability over a wide current range, this design is optimized for the specific application scenario of constant current drive, locking the resonance peak at a stable rated operating point. This allows for maintaining extremely high hole injection efficiency even under high current density, significantly suppressing efficiency roll-off. Attached Figure Description
[0018] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which: Figure 1 This is a schematic diagram of the LED epitaxial structure of the present invention; Figure 2 This is a schematic diagram of the electron blocking layer of the present invention; In the figure: 1. Substrate; 2. Low-temperature GaN nucleation layer; 3. Undoped GaN layer; 4. N-type GaN layer; 5. Multiple quantum well active region; 6. Electron blocking layer; 7. P-type GaN layer; 8. P-type contact layer; 60. First barrier layer; 61. Narrow bandgap insertion layer; 62. Second barrier layer. Detailed Implementation
[0019] To make the objectives, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings. Several embodiments of the present invention are shown in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0020] Example 1 like Figures 1-2 As shown, Embodiment 1 of the present invention provides an LED epitaxial structure, comprising: Substrate 1: Sapphire substrate (0001 side).
[0021] Low-temperature GaN nucleation layer 2 (thickness 25nm).
[0022] Undoped GaN layer 3 (1.5 μm thick).
[0023] N-type GaN layer 4: 2 μm thick, Si doping concentration 5 × 10⁻⁶ 18 cm -3 .
[0024] The active region of the multi-quantum well is composed of 5 alternating stacked In-type quantum wells. 0.15 Ga 0.85 N-well layer and GaN barrier layer, In 0.15 Ga 0.85 The thickness of the N-well layer is 2.5 nm, and the thickness of the GaN barrier layer is 10 nm.
[0025] Resonant tunneling electron blocking layer 6, specifically: First Barrier Layer 60: Al 0.22 Ga 0.78 N, thickness 3.5nm, unintentionally doped; Narrow bandgap insertion layer 61: In 0.18 Ga 0.82 N, thickness 2.2 nm, P-type doped (Mg doping concentration 8 × 10⁻⁶) 18 cm -3 ); Second barrier layer 62: Al 0.22 Ga 0.78 N, thickness 3.5 nm, P-type doped (Mg doping concentration 2 × 10⁻⁶) 19 cm -3 ).
[0026] By adjusting the In composition (x=0.18) and thickness (2.2 nm) of the narrow bandgap insertion layer, the energy difference between the first hole quantization level at the top of its valence band and the valence band top of the last quantum well in the active region is made to be 350 A / cm. 2 Less than 3 meV at current density.
[0027] P-type GaN layer 7: 150 nm thick, Mg doping concentration 3 × 10⁻⁶ 19 cm -3 .
[0028] P-type contact layer 8: 5 nm thick, Mg doping concentration > 1 × 10⁸ 20 cm -3 .
[0029] Accordingly, the method for fabricating LED epitaxial structures includes: The aforementioned structures were sequentially epitaxially grown on a sapphire substrate using an MOCVD (Multi-Layer Chemical Vapor Deposition) system. During growth, high-purity H2 and / or N2 were used as carrier gases, and trimethylgallium (TMGa), trimethylindium (TMIn), trimethylaluminum (TMAl), and NH3 were used as Ga, In, Al, and N sources, respectively. SiH4 and Cp2Mg were used as N-type and P-type doping sources, respectively. The growth temperatures for each layer were controlled as follows: quantum well active region 750℃, AlGaN barrier layer 980℃, and InGaN narrow bandgap insertion layer 720℃. After growth, the layers were annealed at 700℃ for 5 min in an N2 atmosphere to activate Mg doping. After annealing, the epitaxial structure is fabricated into an LED chip using standard LED chip manufacturing processes. Specifically, this includes: etching down to the N-type GaN layer to form a mesa structure using inductively coupled plasma (ICP) etching technology with a Cl2 / BCl3 mixed gas as the etchant; depositing Ni / Au metal layers sequentially on the surface of the P-type GaN layer as P-type electrodes using electron beam evaporation, and depositing Ti / Al / Ti / Au metal layers sequentially on the exposed N-type GaN layer as N-type electrodes, followed by rapid thermal annealing in an N2 atmosphere to achieve ohmic contact; finally, covering the front side of the chip with a SiO2 insulating passivation layer, and exposing the bonding areas of the P-type and N-type electrodes using a windowing process. The specific parameters of the above process steps are all conventionally chosen and are well-known to those skilled in the art, and will not be elaborated further here.
[0030] Example 2 The difference between Embodiment 2 and Embodiment 1 of the present invention is as follows: Target constant current operating point: 150A / cm 2 (Corresponds to approximately 100mA drive current, suitable for low-power bulb lamps). First barrier layer: Al 0.2 Ga 0.8 N, thickness 4nm, unintentionally doped; Narrow bandgap insertion layer: In 0.12 Ga 0.88 N, thickness 3nm, P-type doped (Mg doping concentration 5×10⁻⁶) 18 cm -3 ); Second barrier layer: Al 0.2 Ga 0.8 N, thickness 4nm, P-type doped (Mg doping concentration 1.5×10⁻⁶) 19 cm -3 ); A lower current density means a different electric field distribution in the active region, requiring adjustments to the In composition and thickness to match the band bending at that operating point.
[0031] Comparative Example 1 The difference between Comparative Example 1 and Example 1 of the present invention is as follows: At 150A / cm 2 Tests were conducted at current densities to verify the sensitivity of the resonant tunneling structure to the operating current density.
[0032] Comparative Example 2 The difference between Comparative Example 2 and Example 1 of the present invention is as follows: The electron blocking layer adopts a conventional single-layer structure: Al 0.22 Ga 0.78 N, with a thickness of 20 nm, P-type doped (Mg doping concentration of 2 × 10⁻⁶). 19 cm -3 It does not include resonant tunneling structures.
[0033] Comparative Example 3 The difference between Comparative Example 3 and Example 1 of the present invention is as follows: First barrier layer: Al 0.25 Ga 0.75 N, thickness 2.5nm; Narrow bandgap insertion layer: In 0.25 Ga 0.75 N, thickness 1.5nm (high In content, thin trap, corresponding to high current density resonance peak); Second barrier layer: Al 0.25 Ga 0.75 N, thickness 2.5nm; The resonance peak of this structure is designed to be around 600 A / cm². 2 At 350A / cm 2 It is in a detuned state at the constant current operating point.
[0034] Comparative Example 4 The difference between Comparative Example 4 and Example 1 of this invention is as follows: First barrier layer: Al0.2 Ga 0.8 N, thickness 3nm, P-type doped (Mg doping concentration 1×10⁻⁶) 18 cm -3 ); Narrow bandgap insertion layer: Al 0.1 Ga 0.9 N, thickness 5nm, unintentionally doped; Second barrier layer: Al 0.2 Ga 0.8 N, thickness 3nm, unintentionally doped.
[0035] Comparative Example 5 The difference between Comparative Example 5 and Example 1 of this invention is as follows: Narrow bandgap insertion layer using In 0.08 Ga 0.92 N, thickness 2.2 nm, P-type doped (Mg doping concentration 8 × 10⁻⁶) 18 cm -3 The first and second barrier layers are the same as in Example 1 (A1). 0.22 Ga 0.78 N, thickness 3.5nm).
[0036] Comparative Example 6 The difference between Comparative Example 6 and Example 1 of the present invention is as follows: Narrow bandgap insertion layer using In 0.28 Ga 0.72 N, thickness 2.2 nm, P-type doped (Mg doping concentration 8 × 10⁻⁶) 18 cm -3 ).
[0037] Comparative Example 7 The difference between Comparative Example 7 and Example 1 of this invention is that: The first and second barrier layers use Al 0.12 Ga 0.88 N, thickness 3.5nm, unintentionally doped.
[0038] Comparative Example 8 The difference between Comparative Example 8 and Example 1 of this invention is that: The first and second barrier layers use Al 0.32 Ga 0.68 N, thickness 3.5 nm, P-type doped (Mg doping concentration 2 × 10⁻⁶) 19 cm -3 ) Please refer to Table 1 below, which shows the parameters corresponding to the above embodiments and comparative examples of the present invention. The epitaxial wafers prepared in the above embodiments and comparative examples were packaged into 3528 surface-mount LEDs using the same process. Test conditions: room temperature (25℃), driven by a programmable constant current source, stabilization time of 100ms for each test point, and optical power collected using an integrating sphere, as shown in Table 1.
[0039] Table 1:
[0040] Note: The hole injection efficiency and electron leakage current density in the table are data extracted from TCAD simulation (simulation software: Silvaco Atlas, using polarization model and ABC composite model). The simulated physical model has been calibrated with the measured EQE curves, and the error is within an acceptable range.
[0041] As shown in Table 1, both Examples 1 and 2 exhibited superior external quantum efficiency and hole injection efficiency compared to their respective comparative examples at their designed rated constant current operating points. Electron leakage was significantly suppressed, and efficiency roll-off was controlled at a low level, fully verifying the effectiveness of the technical approach of aligning the energy levels of the resonant tunneling electron blocking layer with the constant current operating point.
[0042] Comparative Example 1 uses the same resonant tunneling structure as Example 1, but operates at a current density that deviates from the design value. Its external quantum efficiency and hole injection efficiency are significantly lower than those of the conventional EBL structure, indicating that the performance of the resonant tunneling structure is highly dependent on the matching of the operating current. Deviating from the design point will lead to detuning of the resonant condition and degradation of device performance.
[0043] Comparative Example 2 uses a traditional AlGaN single-layer electron blocking layer, which exhibits typical defects such as insufficient hole injection and severe electron leakage under high current density, resulting in a significant efficiency roll-off. It constitutes the most direct technical comparison benchmark of this invention.
[0044] Comparative Example 3 uses a resonant tunneling structure, but its resonant peak is designed at a current density that deviates from the target operating point. At the target constant current operating point, its external quantum efficiency is even lower than that of the traditional EBL structure. This shows that the resonant structure, which is arbitrarily designed without precise matching of the operating point, not only fails to exert its due technical advantages, but may also be inferior to the conventional structure due to tunneling obstruction in the detuned state.
[0045] While Comparative Example 4 shows slightly better external quantum efficiency and hole injection efficiency at the rated constant current operating point than the traditional EBL structure, it still lags significantly behind the embodiments of this invention. The difference in mechanism lies in the fact that this invention uses P-type doped InGaN as a narrow bandgap insertion layer. The activation energy of its Mg dopant is much lower than that of the AlGaN material system, allowing for a higher concentration of effective holes at the same doping concentration. Simultaneously, this narrow bandgap insertion layer itself is a direct carrier of the resonant tunneling quantized energy level, directly providing a high concentration of holes at this energy level without requiring additional hole tunneling through a wide-bandgap P-type barrier. This physically alleviates the contradiction between electron blocking capability and hole injection efficiency more effectively.
[0046] As can be seen from Table 1 and Comparative Examples 5-8 above, when the In composition x of the narrow bandgap insertion layer or the Al composition y of the barrier layer exceeds the critical range defined by this invention (x=0.10~0.25, y=0.15-0.30), the external quantum efficiency and hole injection efficiency of the device at the rated constant current operating point are significantly lower than those of Examples 1 and 2. Electron leakage increases and efficiency roll-off intensifies: Comparative Example 5 (x=0.08) cannot establish resonant tunneling due to excessive energy level difference; Comparative Example 6 (x=0.28) suffers simultaneous degradation of efficiency and reliability due to phase separation and defects; Comparative Example 7 (y=0.12) suffers increased electron leakage due to insufficient barrier; and Comparative Example 8 (y=0.32) suffers from alignment damage due to polarization field detuning and growth stress. The above results fully demonstrate from both experimental and simulation perspectives that x=0.10-0.25 and y=0.15-0.30 is the intersection range that simultaneously satisfies the three constraints of "resonance alignment with an energy level difference of less than 3 meV", "effective electron blocking", and "high P-type hole supply". Any component exceeding the boundary will cause at least one core constraint to fail, which confirms the aforementioned discussion of the component boundary mechanism and also shows that the limitation of the component range in this invention is not arbitrarily selected, but is supported by both physical mechanisms and experimental data.
[0047] Furthermore, this invention employs a combination of low-temperature photoluminescence spectroscopy (LT-PL, 10K) measurements and TCAD band structure simulation to quantitatively verify the energy difference between the valence band top quantized level of the narrow bandgap insert layer and the valence band top energy level of the last well in the multi-quantum-well active region (see the row for valence band top energy level difference (meV) in the table above): In Examples 1 and 2, the energy level differences measured at their respective rated constant current operating points were approximately 2.5 meV and 2.8 meV, respectively, both less than 3 meV, verifying the feasibility of the alignment condition; the energy level differences in Comparative Examples 5 to 8 were approximately 12 meV, 18 meV, 15 meV, and 22 meV, respectively, all significantly greater than 3 meV, thus indirectly confirming the correlation between the alignment condition and the critical range of the composition.
[0048] Based on the above comparative analysis, it can be seen that the present invention achieves synergistic optimization of hole injection efficiency and electron blocking capability at the rated constant current operating point by precisely matching the quantized energy level of the resonant tunneling structure with the electric field conditions of the constant current operating point, and by using P-type InGaN as a narrow bandgap insertion layer to improve hole supply efficiency.
[0049] In the description of this specification, references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0050] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this patent should be determined by the appended claims.
Claims
1. An LED epitaxial structure, characterized in that, Including the substrate, it also includes: An N-type GaN layer, a multi-quantum-well active region, an electron blocking layer, and a P-type GaN layer are sequentially stacked on the substrate. The electron blocking layer is a resonant tunneling structure, comprising a first barrier layer, a narrow bandgap insertion layer, and a second barrier layer stacked sequentially. The narrow bandgap insertion layer is P-type doped In. x Ga 1-x N layers, where x ranges from 0.10 to 0.25, and both the first and second barrier layers are Al. y Ga 1-y For layer N, the value of y ranges from 0.15 to 0.
30.
2. The LED epitaxial structure according to claim 1, characterized in that, The difference between the quantized energy level of the valence band top of the narrow bandgap insertion layer and the valence band top energy level of the multi-quantum-well active region is less than 3 meV under band bending conditions at a preset operating current density. The preset operating current density is used as the current density at the rated constant current operating point of the LED, and its range is 150 A / cm². 2 -350A / cm 2 .
3. The LED epitaxial structure according to claim 2, characterized in that, The thickness of the narrow bandgap insertion layer is 1.5nm-3.5nm, and the thickness of both the first barrier layer and the second barrier layer is 2nm-5nm.
4. The LED epitaxial structure according to claim 1, characterized in that, The doping concentration of the narrow bandgap insertion layer is 1×10⁻⁶. 18 cm -3 -5×10 19 cm -3 At least one of the first barrier layer and the second barrier layer is P-type doped or unintentionally doped.
5. The LED epitaxial structure according to claim 2, characterized in that, The LED is packaged as a light source for a liquid crystal display backlight module, and the fluctuation range of its rated operating current density is controlled within ±3%.
6. The LED epitaxial structure according to claim 2, characterized in that, The LED is packaged as a light source for a constant light lighting fixture, and the fluctuation range of its rated operating current density is controlled within ±5%.
7. A method for fabricating an LED epitaxial structure, characterized in that, The preparation method is used to prepare the LED epitaxial structure according to any one of claims 1-6, and the preparation method includes: Provide a substrate; An N-type GaN layer and a multi-quantum-well active region are epitaxially grown sequentially on the substrate. An electron blocking layer is grown on the active region of the multi-quantum well. The electron blocking layer is a resonant tunneling structure. The growth of the resonant tunneling structure specifically includes: A first barrier layer is grown on the multi-quantum-well active region. A narrow bandgap insertion layer is grown on top of the first barrier layer, and the growth temperature, pressure, and source flux are controlled to align its valence band top quantization level with the valence band top level of the multi-quantum-well active region at the designed operating point. A second barrier layer is grown on top of the narrow bandgap insertion layer; A P-type GaN layer is grown on top of the second barrier layer.
8. The method for preparing an LED epitaxial structure according to claim 7, characterized in that, By adjusting the thickness, composition, and doping concentration of the narrow bandgap insertion layer, the current density corresponding to its resonance peak is matched with the target constant current operating point of the light-emitting diode.
9. The method for preparing an LED epitaxial structure according to claim 7, characterized in that, In the step of growing the narrow bandgap insertion layer, the growth temperature is 700℃-780℃, and after the growth is completed, it is annealed in a N2 atmosphere.
10. An LED chip, characterized in that, The LED chip includes the LED epitaxial structure as described in any one of claims 1-6.