High-efficiency LED packaging structure and its fabrication method based on light field reconstruction and interface anchoring coupling
By employing an embedded interlocking design using equal-height white glue, gradient fluorescent glue, and high-convexity lenses, the problem of limited luminous efficacy improvement in LED packaging was solved, achieving an LED packaging structure with high luminous efficacy, high color consistency, and high reliability.
Patent Information
- Application Number
- CN202611427714.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-17
AI Technical Summary
In existing LED packaging technologies, there are inherent contradictions between the bottom reflective structure, phosphor system, and lens design, which limits the improvement of luminous efficacy and makes it impossible to break through the 3% industry bottleneck. Furthermore, it is difficult to achieve high luminous efficacy, high reliability, and high color consistency.
The light field is reconstructed by using a uniform height white glue structure, combined with an embedded interlocking anchoring design of large-particle phosphor and high-convexity lens, forming an LED packaging structure that couples light field reconstruction and interface anchoring, thereby improving luminous efficiency through optical chain synergy.
It achieved a luminous efficacy improvement of over 4%, color consistency superior to 3SDCM, and the device showed no peeling failure in 1000 thermal shock tests with a yield of ≥91%, breaking through the luminous efficacy limit of existing technologies.
Smart Images

Figure CN123124536A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of LED light source technology, and particularly relates to a high-efficiency LED packaging structure and its preparation method that features light field reconstruction and interface anchoring coupling. Background Technology
[0002] White LEDs, with their advantages of energy saving, long lifespan, and environmental friendliness, have become the core light source in the current lighting and backlight display fields. High luminous efficacy, high reliability, and high color consistency are the core goals of continuous iteration of LED packaging technology. Currently, the industry's methods to improve LED luminous efficacy mainly focus on three independent technical directions: bottom reflection optimization, phosphor system optimization, and self-forming lens structure optimization. However, due to deep-rooted industry technical biases and inherent process contradictions, the luminous efficacy improvement of a single generation of technology has always been unable to break through the industry bottleneck of 3%.
[0003] Regarding the design of the bottom reflective structure, the industry generally adopts a low-height white glue filling scheme, leading to a bias in curing technology: those skilled in the art generally believe that if the white glue height is increased to be flush with the top surface of the wafer, it will encroach on the phosphor filling space inside the support cup, resulting in insufficient phosphor filling and excessive light color shift. At the same time, the micro gap between the white glue and the wafer sidewall is prone to stray light and glue creep defects, which degrade optical performance. Therefore, the conventional white glue height is only 1 / 3 to 1 / 2 of the wafer thickness. Large-angle lateral light radiated from the wafer sidewall cannot be effectively reflected, and most of the light is absorbed by the support cup wall and bottom. The bottom light loss has long been maintained at 8% to 12%, becoming the primary bottleneck for improving light efficiency.
[0004] In fluorescence conversion processes, the industry generally uses small- to medium-sized phosphors, leading to a bias in curing technology: those skilled in the art generally believe that large-sized phosphors have too fast a settling rate, easily causing localized uneven concentration and excessive color tolerance, failing to meet the color consistency requirements for mass production; furthermore, large-sized phosphors have a large scattering cross-section under conventional large-angle chaotic light fields, increasing scattering loss. Therefore, the intrinsic material advantages of large-sized phosphors—low scattering and high effective light radiation—have always been untapped, forcing the industry to sacrifice luminous efficiency for color consistency, resulting in persistently high backscattering loss in the phosphor layer.
[0005] In the design of self-forming lenses, the industry generally restricts lens height, leading to a bias in the technology: those skilled in the art generally believe that excessively high self-forming lenses are prone to problems such as adhesive collapse, poor molding consistency, and low yield. They also believe that a flat interface where the fluorescent adhesive surface is flush with the cup rim provides optimal lens adhesion; if the fluorescent adhesive surface is lower than the cup rim, the bonding area between the lens and the support is reduced, significantly increasing the risk of lens peeling failure under thermal cycling conditions. Therefore, the height of conventional self-forming lenses is only 0.2 to 0.4 times the cup rim diameter, resulting in a small light-emitting interface curvature, severe total internal reflection loss, and an inability to further improve light extraction efficiency.
[0006] More importantly, existing technologies are all isolated optimizations of single modules. Those skilled in the art are unaware of the strong optical coupling relationship between the three optimization directions and the inherent process contradictions: increasing the height of the white adhesive to improve reflection will encroach on the space of the phosphor adhesive and cause color shift; large-particle phosphor reduces scattering but worsens color consistency; increasing the height of the lens to improve light extraction efficiency will exacerbate the risk of peeling. Existing technologies can only compromise among these contradictions. The gains from optimizing a single technology are offset by the losses of other modules, making it impossible to achieve a simultaneous optimal configuration of the three, and thus unable to break through the 3% luminous efficacy improvement limit, let alone achieve a leapfrog improvement of more than 4%. Therefore, there is an urgent need to develop an LED packaging solution that can break through industry technical biases, resolve inherent process contradictions, and achieve synergistic gains across multiple modules, in order to overcome the current luminous efficacy bottleneck while ensuring device reliability and color consistency. Summary of the Invention
[0007] The purpose of this invention is to provide a high-efficiency LED packaging structure and its preparation method that features light field reconstruction and interface anchoring coupling. This aims to resolve the inherent contradictions in existing technologies, such as "white glue increasing reflectivity and phosphor space encroachment, leading to excessive color deviation," "low scattering of large-particle phosphors and uneven sedimentation, resulting in poor color consistency," and "high light output from high-convexity lenses and weak interface bonding, leading to easy peeling and failure." This invention breaks through the limitations of single-module optimization, constructs a multi-module optical collaborative system, achieves a super-superimposed luminous efficiency gain far exceeding that of a single technology, achieves a stable luminous efficiency improvement of over 4%, and realizes a unity of high luminous efficiency, high color stability, and high reliability.
[0008] To achieve the above objectives, this invention provides a high-efficiency LED packaging structure with light field reconstruction and interface anchoring coupling, comprising a support, a blue LED chip, a white reflective adhesive layer, a fluorescent adhesive layer, and a lens. The support is provided with a cup-shaped cavity, and the blue LED chip is fixed at the center of the bottom of the cup-shaped cavity.
[0009] The white reflective adhesive layer is disposed in the annular functional area of the cup-shaped cavity, and the height difference between the top surface of the cured white reflective adhesive layer and the top surface of the blue LED chip is ≤15μm;
[0010] The fluorescent adhesive layer is coated on top of the white reflective adhesive layer, and the top surface of the fluorescent adhesive layer is lower than the cup-shaped cavity end face, forming an annular anchoring and receiving step;
[0011] The fluorescent adhesive layer has a gradient concentration distribution structure inside, and the concentration of phosphor in the fluorescent adhesive is higher on the side closer to the blue LED chip than on the side farther away from the blue LED chip;
[0012] The lens is a spherical convex lens formed by the self-forming of liquid surface tension. The bottom of the lens is embedded in the interior of the annular anchoring accommodating step and forms an embedded interlocking anchoring structure. The apex of the lens protrudes from the cup-shaped cavity end face. The convexity of the lens is >0.5D.
[0013] The lens is made of high-transmittance silicone, and the difference between the refractive index of the lens and the refractive index of the fluorescent adhesive is ≤0.03.
[0014] Optionally, the bracket is a PCT3030 bracket, a PCT2835 bracket, or a metal SMD bracket, and the cup diameter of the cup-shaped cavity is 1.8~3.0mm and the cup depth is 0.35~0.45mm.
[0015] Optionally, the blue LED chip is a standard blue LED chip, a flip-chip blue LED chip, or a vertical blue LED chip in the 450~455nm wavelength band.
[0016] Optionally, the white reflective adhesive layer is doped. The white silicone has a diffuse reflectance of ≥92% in the 450nm band and a viscosity of 8k~12kcps; the distance between the white reflective adhesive layer and the sidewall of the bracket is 20~35μm.
[0017] Optionally, the fluorescent adhesive layer contains yellow powder, which is YAG yellow powder, GaYAG green powder, or LuAG green powder, and the particle size of the yellow powder is in the range of 15~35μm.
[0018] Optionally, the fluorescent adhesive layer contains 1113 system red powder or KSF red powder.
[0019] Optionally, the depth of the annular anchor receiving step is 0.05-0.10 mm.
[0020] Optionally, the depth of the annular anchoring accommodating step accounts for 15% to 35% of the total depth of the cup-shaped cavity.
[0021] This invention also provides a method for fabricating a high-efficiency LED packaging structure with light field reconstruction and interface anchoring coupling, which includes the following steps:
[0022] S1: Die Bonding Wire Bonding: The blue LED chip is fixed to the bottom center of the cup-shaped cavity of the bracket using die bond adhesive. After curing, the gold wire bonding leads are completed; ensuring that the chip is centered and firmly fixed.
[0023] S2: Precise application and curing of high-reflectivity white adhesive: Using a high-precision closed-loop metering dispensing valve, high-reflectivity silicone white adhesive is precisely applied to the annular functional area of the cup-shaped cavity surrounding the blue LED chip. After curing, the height difference between the top surface of the white reflective adhesive layer and the top surface of the blue LED chip is ≤15μm. Pre-curing is carried out at 120~160℃ for 20~40min to form a flat and continuous high-reflectivity substrate and light field reconstruction interface.
[0024] S3: Low-position large-particle-size fluorescent adhesive sedimentation molding: Prepare fluorescent adhesive containing large-particle-size yellow powder with D50=15~35μm; apply fluorescent adhesive to the cup-shaped cavity of the support at fixed points, and control the amount of adhesive so that the adhesive surface after curing is 0.05~0.10mm lower than the end face of the cup mouth; use a centrifugal electrostatic device to uniformly settle the large-particle-size yellow powder on the flat white adhesive substrate by gravity to form a gradient concentration distribution; then cure at 120~160℃ for 20~40min to form a fluorescent adhesive layer with annular anchoring accommodating steps;
[0025] S4: Preparation of high-convexity anchored lens: High-transparency lens silicone is applied to the top surface of the fluorescent adhesive layer and the annular step area of the cup-shaped cavity. It is formed into a spherical crown convex structure by relying on the surface tension of the liquid. The amount of adhesive is controlled so that the height of the lens vertex is greater than 0.5 times the diameter of the cup opening. The lens adhesive is embedded in the step to form an embedded interlocking anchored structure. The finished LED packaging structure is obtained by curing at 70~100℃ for 50~70min and at 140-160℃ for 220~270min.
[0026] Optionally, the prepared LED package structure showed no peeling failure after 1000 thermal shock tests at -40℃ to +125℃, with an interfacial shear force ≥20N, color tolerance <3SDCM, and a yield ≥91%. The luminous efficacy is improved by ≥4.8% compared to the conventional benchmark.
[0027] The high-efficiency LED packaging structure and its fabrication method based on light field reconstruction and interface anchoring coupling provided in this invention have at least one of the following technical effects:
[0028] 1. Breaking through the bias of bottom reflection technology and completely solving the contradiction between light loss and color shift: For the first time, a white glue structure with the same height as the wafer is adopted to completely recover the lateral stray light from the sidewall of the wafer, reducing the bottom light loss from 8%~12% to less than 2%; at the same time, the optical path of the phosphor layer is shortened by light field reconstruction, and complete light conversion can be achieved without thick phosphor glue, completely solving the problem of "white glue with the same height occupying the phosphor space and causing color shift", and achieving the unity of high reflectivity and high color consistency.
[0029] 2. Overcoming technical biases in phosphor application and unleashing the low scattering advantages of large-particle-size phosphors: By utilizing a uniformly flat white glue substrate, the pain points of uneven sedimentation and excessive color tolerance of large-particle-size phosphors are solved, reducing backscattering loss of the phosphor layer by more than 40%, significantly increasing the effective light radiation ratio, and significantly improving luminous efficiency while ensuring mass production-grade color consistency (≤3SDCM).
[0030] 3. Overcoming the biases in lens forming technology to achieve dual gains of high light output and high reliability: The mechanical anchoring structure is formed by using low-position fluorescent adhesive steps, which inversely improves the bonding strength of the high-convexity lens interface (shear force is increased by more than 30%), completely eliminating the risk of thermal cycling peeling failure; the high-convexity lens significantly expands the emission angle, reduces total internal reflection loss by more than 30%, and significantly improves light extraction efficiency.
[0031] 4. Three-layer optical chain collaboration produces unexpected super-superposition effects: it is not a simple superposition of single features, but a hierarchical optical closed-loop collaborative system. Verification by multiple comparative examples shows that single-technology optimization only improves performance by 1%~2%, and simple superposition of the three only by 2.3%. This invention's collaborative architecture achieves a stable improvement of over 4%, breaking the industry's 3% limit, and its effect far exceeds conventional expectations.
[0032] 5. Strong process compatibility, suitable for large-scale mass production: All processes are based on conventional dispensing, settling, and curing processes with no need for additional equipment. The process is highly stable and the yield is controllable (99% yield in the example), and it can be directly adapted to existing production lines. Attached Figure Description
[0033] To more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0034] Figure 1 This is a cross-sectional view of a high-efficiency LED packaging structure with light field reconstruction and interface anchoring coupling provided in an embodiment of the present invention.
[0035] The following are the labeling elements in the figure:
[0036] 1—Bracket; 2—Blue LED chip; 3—White adhesive reflective layer
[0037] 4—Fluorescent adhesive layer; 5—Lens; 6—Annular positioning anchoring step
[0038] 7—Lens height; 8—Cup mouth diameter Detailed Implementation
[0039] Embodiments of the present invention are described in detail below, examples of which are illustrated in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain embodiments of the present invention, and should not be construed as limiting the present invention.
[0040] This invention abandons the traditional industry approach of compromise and optimization, and pioneers a core design concept of "reverse utilization of technical bias + three-layer optical chain synergy." It transforms three originally mutually restrictive and contradictory technical shortcomings into mutually adaptable and mutually beneficial technical advantages, forming a closed-loop optical gain system, including:
[0041] 1. Reverse the contradiction of white glue process: The cavity light field is reconstructed by using white glue of equal height, which converts the large-angle lateral light of the chip into near-axial small-angle light, greatly shortening the light propagation path in the phosphor layer. Sufficient light conversion can be completed without thick phosphor layer, thus eliminating the color shift problem caused by the white glue increasing in height and squeezing the phosphor space in principle.
[0042] 2. Reverse the contradictions in phosphor manufacturing process: By using uniform white glue to form a flat, uneven substrate, a uniform sedimentation carrier is provided for large-particle phosphors, which completely solves the industry problems of uneven sedimentation and excessive color tolerance of large-particle phosphors, and fully releases the advantages of low scattering and high effective radiation of large-particle phosphors.
[0043] 3. Reverse the contradiction of lens reliability: By using the low-position fluorescent adhesive surface to form an annular anchoring step at the cup mouth, the bottom of the high-convexity lens is embedded in the step to form a mechanical interlocking structure, which greatly improves the bonding area and bonding strength, and completely solves the reliability problem of easy peeling of high-convection lenses;
[0044] 4. Constructing a three-layer chain-like synergistic gain: The small-angle light field output by the equal-height white glue is precisely adapted to the low-scattering working range of the large-particle phosphor, and the parallel light after low-loss conversion is precisely adapted to the anti-total internal reflection light output range of the high-convexity lens. The three-layer structure gains gains step by step and empowers each other, producing a super superposition effect of 1+1+1>3, achieving an unexpected improvement in light efficiency.
[0045] Specifically, such as Figure 1 As shown, this invention provides a high-efficiency LED packaging structure with light field reconstruction and interface anchoring coupling, including a support 1, a blue LED chip 2, a white reflective adhesive layer 3, a fluorescent adhesive layer 4, and a lens 5, the lens 5 having a lens height 7. The support 1 is provided with a cup-shaped cavity, and the blue LED chip 2 is fixed at the center of the bottom of the cup-shaped cavity.
[0046] The white reflective adhesive layer 3 is disposed in the annular functional area of the cup-shaped cavity. The height difference between the top surface of the cured white reflective adhesive layer 3 and the top surface of the blue LED chip 2 is ≤15μm, achieving a flush or nearly flush configuration. The top surface of the white adhesive reflective layer is precisely flush with the top surface of the blue LED chip 2, forming a continuous and flat overall high-reflectivity plane. This plane is used to reflect all the large-angle lateral light emitted from the sidewall of the blue LED chip 2 upwards, reconstructing the chaotic light field within the cup-shaped cavity into a near-axial small-angle ordered light field. The distance between the sidewall of the white adhesive reflective layer and the sidewall of the blue LED chip 2 is controlled at 20~50μm, and the diffuse reflectivity in the 450nm band is ≥92%.
[0047] The fluorescent adhesive layer 4 is coated on top of the white reflective adhesive layer 3, and the top surface of the fluorescent adhesive layer 4 is lower than the cup-shaped cavity end face, forming an annular anchoring and receiving step 6.
[0048] The fluorescent adhesive layer 4 has a gradient concentration distribution structure, and the concentration of phosphor in the fluorescent adhesive is higher on the side closer to the blue LED chip 2 than on the side farther away from the blue LED chip 2.
[0049] The lens 5 is a spherical convex lens 5 formed by liquid surface tension. The bottom of the lens 5 is embedded in the interior of the annular anchoring accommodating step 6 and forms an embedded interlocking anchoring structure. The apex of the lens 5 protrudes from the cup-shaped cavity end face. The convexity of the lens 5 is >0.5D.
[0050] The lens 5 is made of high-transmittance silicone, and the difference between the refractive index of the lens 5 and the refractive index of the fluorescent adhesive is ≤0.03, resulting in extremely low interfacial Fresnel loss.
[0051] Furthermore, the bracket 1 is a PCT3030 bracket 1, a PCT2835 bracket 1, or a metal SMD bracket 1, and the cup diameter of the cup-shaped cavity is 1.8~3.0mm, and the cup depth is 0.35~0.45mm.
[0052] Furthermore, the blue LED chip 2 is a standard blue LED chip 2, a flip-chip blue LED chip 2, or a vertical blue LED chip 2 in the 450~455nm wavelength band.
[0053] Furthermore, the white reflective adhesive layer 3 is doped. The white reflective silicone has a diffuse reflectance of ≥92% in the 450nm band and a viscosity of 8k~12kcps; the distance between the white reflective adhesive layer 3 and the sidewall of the support 1 is 20~35μm. The distance can be 20μm, 25μm, 30μm, or 35μm, etc.
[0054] Furthermore, the fluorescent adhesive layer 4 contains yellow powder, which is YAG yellow powder, GaYAG green powder, or LuAG green powder, and the particle size of the yellow powder ranges from 15 to 35 μm. The fluorescent adhesive layer 4 contains large-particle-size yellow powder with a median particle size D50 of 15 to 35 μm, and a gradient distribution structure with high concentration near the wafer side and low concentration far from the wafer side is formed by centrifugal sedimentation process. Fluoride red phosphor can be selectively added to adapt to high color rendering scenarios.
[0055] Furthermore, the fluorescent adhesive layer 4 contains 1113 system red powder or KSF red powder.
[0056] Furthermore, the depth of the annular anchoring accommodating step 6 is 0.05-0.10 mm. The depth can be 0.05 mm, 0.07 mm, 0.09 mm or 0.10 mm.
[0057] Furthermore, the depth of the annular anchoring accommodating step 6 accounts for 15% to 35% of the total depth of the cup-shaped cavity, and the depth of the annular anchoring accommodating step 6 can account for 15%, 20%, 25%, 30%, or 35% of the total depth of the cup-shaped cavity.
[0058] This invention also provides a method for fabricating a high-efficiency LED packaging structure with light field reconstruction and interface anchoring coupling, which includes the following steps:
[0059] S1: Die bonding and wire bonding: The blue LED chip 2 is fixed to the bottom center of the cup-shaped cavity of the bracket 1 with die bonding adhesive. After curing, the gold wire bonding leads are completed; ensuring that the chip is centered and firmly fixed.
[0060] S2: Precise application and curing of high-reflectivity white adhesive: Using a high-precision closed-loop metering dispensing valve, high-reflectivity silicone white adhesive is precisely applied to the annular functional area of the cup-shaped cavity surrounding the blue LED chip 2. After curing, the height difference between the top surface of the white reflective adhesive layer 3 and the top surface of the blue LED chip 2 is ≤15μm. Pre-curing is carried out at 120~160℃ for 20~40min to form a flat and continuous high-reflectivity substrate and light field reconstruction interface.
[0061] S3: Low-position large-particle-size fluorescent adhesive sedimentation molding: Prepare fluorescent adhesive containing large-particle-size yellow powder with D50=15~35μm; apply fluorescent adhesive to the cup-shaped cavity of the support 1 at fixed points, and control the amount of adhesive so that the adhesive surface after curing is 0.05~0.10mm lower than the end face of the cup mouth; use a centrifugal electrostatic device to uniformly settle the large-particle-size yellow powder on the flat white adhesive substrate by gravity to form a gradient concentration distribution; then cure at 120~160℃ for 20~40min to form a fluorescent adhesive layer 4 with annular anchoring accommodating step 6;
[0062] S4: Preparation of high-convexity anchored lens 5: High-transparency silicone for lens 5 is applied to the top surface of fluorescent adhesive layer 4 and the annular step area of the cup-shaped cavity. It is formed into a spherical crown convex structure by relying on the surface tension of the liquid. The amount of adhesive is controlled so that the height of the vertex of lens 5 is greater than 0.5 times the diameter of the cup 8. The adhesive of lens 5 is embedded in the step to form an embedded interlocking anchored structure. It is cured at 70~100℃ for 50~70min and at 140-160℃ for 220~270min to obtain the finished LED packaging structure.
[0063] The prepared LED package structure showed no peeling failure after 1000 thermal shock tests at -40℃ to +125℃, with an interfacial shear force ≥20N, color tolerance <3SDCM, and a yield ≥91%. The luminous efficacy is improved by ≥4.8% compared to the conventional benchmark.
[0064] The high-efficiency LED packaging structure and its fabrication method based on light field reconstruction and interface anchoring coupling provided in this invention have the following advantages:
[0065] 1. Breaking through the bias of bottom reflection technology and completely solving the contradiction between light loss and color shift: For the first time, a white glue structure with the same height as the wafer is adopted to completely recover the lateral stray light from the sidewall of the wafer, reducing the bottom light loss from 8%~12% to less than 2%; at the same time, the optical path of the phosphor layer is shortened by light field reconstruction, and complete light conversion can be achieved without thick phosphor glue, completely solving the problem of "white glue with the same height occupying the phosphor space and causing color shift", and achieving the unity of high reflectivity and high color consistency.
[0066] 2. Overcoming technical biases in phosphor application and unleashing the low scattering advantages of large-particle-size phosphors: By utilizing a uniformly flat white glue substrate, the pain points of uneven sedimentation and excessive color tolerance of large-particle-size phosphors are solved, reducing backscattering loss of the phosphor layer by more than 40%, significantly increasing the effective light radiation ratio, and significantly improving luminous efficiency while ensuring mass production-grade color consistency (≤3SDCM).
[0067] 3. Overcoming the biases in lens 5 molding technology to achieve dual gains of high light output and high reliability: The mechanical anchoring structure is formed by using low-position fluorescent adhesive steps, which inversely improves the interface bonding strength of the high-convexity lens 5 (shear force is increased by more than 30%), completely eliminating the risk of thermal cycling peeling failure; the high-convexity lens 5 significantly expands the emission angle, reduces total internal reflection loss by more than 30%, and significantly improves light extraction efficiency.
[0068] 4. Three-layer optical chain collaboration produces unexpected super-superposition effects: it is not a simple superposition of single features, but a hierarchical optical closed-loop collaborative system. Verification by multiple comparative examples shows that single-technology optimization only improves performance by 1%~2%, and simple superposition of the three only by 2.3%. This invention's collaborative architecture achieves a stable improvement of over 4%, breaking the industry's 3% limit, and its effect far exceeds conventional expectations.
[0069] 5. Strong process compatibility, suitable for large-scale mass production: All processes are based on conventional dispensing, settling, and curing processes with no need for additional equipment. The process is highly stable and the yield is controllable (99% yield in the example), and it can be directly adapted to existing production lines.
[0070] The prior art is further illustrated below with comparative examples.
[0071] Comparative Example 1 (Standard): 0.08mm low-white glue + D50=12μm yellow powder + 1113 system red powder + glue surface flush. Color temperature 4000K, Ra>80, average luminous efficacy 100% (242Lm / W), peel defect rate 6.8% (500C), shear force ≈18N, and yield rate of color tolerance <3SDCM is 91.23%.
[0072] Comparative Example 2 (white glue of equal height only): White glue 0.15mm flush, otherwise the same as 1. Average luminous efficacy 101.2% (244.9Lm / W, +1.2%), yield rate of color tolerance <3SDCM is 81.23% (color deviation).
[0073] Comparative Example 3 (large particle size only): Yellow powder D50=30μm, otherwise the same as 1. Average luminous efficacy 100.8% (243.9Lm / W, +0.8%), yield of color tolerance <3SDCM is 80.23% (uneven sedimentation).
[0074] Comparative Example 4 (High Lens 5 only): Lens 51.1mm (0.55D), otherwise the same as 1. Average luminous efficacy 101.5% (245.65Lm / W, +1.5%), peel failure rate 8.3%, shear force ≈15N, and yield rate of color tolerance <3SDCM is 85%.
[0075] Comparative Example 5 (simple superposition without steps): equal-height white glue + 30μm yellow powder + 0.55D lens 5, glue surface flush. Average luminous efficacy 102.3% (247.58Lm / W, +2.3%), peel failure rate 7.5%, shear force ≈15N, yield rate of color tolerance <3SDCM is 82%.
[0076] Comparative Example 6 (with steps but no settling): Same structure as Example 1, except centrifugal settling is omitted in S3. Average luminous efficacy is 103.0% (249.26Lm / W, +3.0%), and the yield rate of color tolerance <3SDCM is 88% (gradient not formed), proving that the "settling process" is a necessary synergistic step.
[0077] Comparative Example 7 (with a step but lens 5 not embedded): The step is 0.08mm, and the amount of adhesive applied to lens 5 is insufficient, resulting in incomplete embedding. The average luminous efficacy is 103.4% (250.23Lm / W, +3.4%), and the peeling failure rate is 5.0% (insufficient anchoring), proving that "embedded interlocking" is a necessary step. The yield rate for color tolerance <3SDCM is 88%.
[0078] Comparative Example 8 (white adhesive too low, out of range): White adhesive 0.05mm (far lower than wafer 0.15mm). Average luminous efficacy 101.8% (246.36Lm / W, +1.8%), bottom side light not recovered, bottom loss still 7%+, proving that "equal height and level" is not arbitrary.
[0079] Comparative Example 9 (white adhesive too high, exceeding the range): White adhesive 0.22mm (0.06mm higher than the top surface of the wafer). Average luminous efficacy 102.0% (246.84Lm / W, +2.0%), blocking light emission from the top surface of the wafer and causing adhesive creep, yield of 75% with color tolerance <3SDCM, proving the necessity of flush height.
[0080] Comparative Example 10 (step too deep, exceeding the range): Step 0.18mm (occupies 51% of cup depth, exceeding 15%~35%). Average luminous efficacy 103.4% (250.23Lm / W, +3.4%). The fluorescent adhesive was too thin and the lens 5 was embedded too deeply, resulting in weak bonding. The peeling failure rate was 4.5%, and the yield rate for color tolerance <3SDCM was 55%, confirming the upper limit of step depth.
[0081] Comparative Example 11 (Lens 5 is too low, out of range): Lens 5 0.3D (<0.5D). Average luminous efficacy 103.5% (250.47Lm / W, +3.5%), high total internal reflection loss, 89% yield with color tolerance <3SDCM, confirming the height threshold of Lens 5.
[0082] Comparative Example 12 (Yellow powder too large, exceeding the range): Yellow powder D50 = 38μm (>35μm). Average luminous efficacy 104.0% (251.68Lm / W, +4.0%), severely uneven sedimentation, color tolerance <3SDCM, yield rate 63%, confirming the upper limit of particle size.
[0083] The technical solution of the present invention will be described below through embodiments.
[0084] Example 1 (Basic collaborative solution, complete process).
[0085] S1: Die bonding: 3030 PCT, blue LED chip 2-core, gold wire bonding, chip top surface 0.15mm from cup bottom;
[0086] S2: High-reflectivity white glue: Apply high-reflectivity white glue to the closed-loop metering valve, and after curing, it should be flush with the surface at 0.15mm (height difference ≤15μm), with a sidewall spacing of 20-35μm, at 130℃ for 30min; diffuse reflectance ≥92%;
[0087] S3: Low-position fluorescent adhesive: D50=30μm yellow powder (+ optional KSF), applied at fixed points, after curing the adhesive surface is 0.10mm lower than the cup mouth (occupying about 29% of the cup depth, falling into 15%~35%), settling at room temperature for 30min to form a gradient, 130℃ / 30min;
[0088] S4: High convexity lens 5: Lens 5 adhesive refractive index 1.54 (difference from fluorescent adhesive ≤0.03), self-forming spherical cap, vertex 1.3mm (0.545D), bottom embedded step, cured at 80℃ for 60min, cured at 150℃ for 240min.
[0089] The average luminous efficacy is 104.8% (253.62Lm / W, +4.8%), the yield rate with color tolerance <3SDCM is 91.85%, the peel rate is 0% after 1000 cold and hot shocks, the shear force is ≈20N, the light emission half angle is 120°, and the yield rate with color tolerance <5SDCM is 99.12%.
[0090] Example 2 (Ra80, 4000K).
[0091] Example 1 + 12wt% KSF. Average luminous efficacy 106.5% (257.73Lm / W, +6.5%), Ra=80, yield of color tolerance <3SDCM is 78.13%, 0% peeling after 1000 thermal shocks, shear force ≈20N, light emission half-angle 120°, yield of color tolerance <5SDCM is 95.25%.
[0092] Through 12 sets of comparative examples, the necessity of each core technical feature of the present invention and the rationality of the parameter value range are verified, the defects of the prior art and the technical barriers of the present invention are clarified, and the specific conclusions are as follows:
[0093] 1. The standard benchmark comparison example 1 uses a standard process with low white glue, small particle size yellow powder, and flush glue surface. The light efficacy benchmark value is 242Lm / W, the peeling failure rate is 6.8% after 500 cycles of hot and cold cycling, the shear force is about 18N, the color tolerance is <3SDCM, and the yield is 91.23%. It has problems such as limited light efficacy and poor interface bonding stability.
[0094] 2. Single parameter optimization Comparative Examples 2, 3, and 4, which individually adopted the structures of equal-height white glue, large-particle-size yellow powder, and high-convex lens, only slightly improved the light efficiency, but also showed defects such as color deviation, uneven powder sedimentation, aggravated poor interface peeling, and decreased shear strength. This proves that a single improvement cannot take into account light efficiency, color consistency, and structural reliability.
[0095] 3. Simple Technique Superposition Comparative Example 5 integrates the aforementioned single optimization parameters without setting anchoring steps and gradient fluorescence structures. The luminous efficiency is slightly improved, but the chromaticity yield and structural reliability are not effectively improved, proving that the simple superposition of technical features has no synergistic gain effect.
[0096] 4. Verification of the necessity of the process: Comparative examples 6 and 7 demonstrate that the centrifugal sedimentation process is a necessary step to form a gradient concentration distribution of phosphor and ensure color consistency, and the interlocking anchoring structure with the step embedded at the bottom of lens 5 is a core necessary structure to improve the device's anti-peeling performance and structural stability.
[0097] 5. Parameter range verification Comparative examples 8 to 12 demonstrate that the white glue height, anchoring step depth, lens 5 convexity, and phosphor particle size all have reasonable value ranges. Exceeding the limited range will result in defects such as large bottom light loss, chip light emission obstruction, extremely poor color consistency, insufficient interface bonding strength, and increased total internal reflection loss, thus proving the inventiveness and necessity of the parameter limitation of this invention.
[0098] The embodiments of this invention cover the entire technical scope defined by the claims, and through the synergistic combination of multiple technical features, they take into account the device's luminous efficiency, colorimetric consistency, and long-term reliability, as detailed below:
[0099] In Example 1, a 3030PCT support 1 is used. After die bonding, the top surface of the blue LED chip 2 is 0.15mm from the bottom of the cup. High-reflectivity white glue is applied through a closed-loop metering valve. After curing, it is flush with the top surface of the blue LED chip 2 (height difference ≤15μm), the sidewall spacing is 20~35μm, and the diffuse reflectivity is ≥92%. Phosphor glue is prepared using yellow powder with D50=30μm. After point coating, it settles at room temperature for 30min to form a gradient concentration distribution. After curing, the top surface of the phosphor glue is 0.10mm lower than the end face of the cup mouth. The anchoring step depth accounts for 29% of the cup depth, falling into the optimal range of 15%~35%. A high-transmittance lens 5 with a refractive index of 1.54 (the refractive index difference with the phosphor glue is ≤0.03) is selected to form a 0.545D spherical convex lens 5. The bottom is embedded with the anchoring step and cured in sections.
[0100] The test results of this solution are as follows: luminous efficacy reaches 253.62Lm / W (4.8% improvement over the baseline), yield is 91.85% for color tolerance <3SDCM and 99.12% for color tolerance <5SDCM, and the light emission half-angle is 120°; it has no peeling failure after 1000 thermal shock tests, and the interface shear force is about 20N, combining high luminous efficacy, high color consistency and ultra-high structural reliability.
[0101] Example 2 is based on Example 1, with the addition of 12wt% KSF red powder, adapted to a color temperature of 4000K and a color rendering index of Ra≥80. Test results: Luminous efficacy reached 257.73Lm / W (6.5% improvement relative to the baseline), color rendering index Ra=80, color tolerance <5SDCM, yield 95.25%, zero peeling failure in 1000 cycles of thermal shock testing, and shear force stable at 20N, ensuring high reliability and high luminous efficacy.
[0102] The comparison between the embodiments of the present invention and the comparative examples can be seen in Table 1 below:
[0103]
[0104] Table 1
[0105] Compared to existing conventional processes and simple, superimposed improvement schemes, this invention, through the synergistic combination of equal-height reflective white glue, gradient-settling fluorescent glue, defined-range anchoring steps, and embedded spherical convex lens 5, breaks through the technical bottleneck of existing technologies that cannot simultaneously achieve luminous efficacy, color consistency, and structural reliability. By reasonably limiting various structural parameters, powder parameters, and preparation processes, it significantly improves the photoelectric performance and long-term stability of LED devices, demonstrating significant technological advancement and practicality.
[0106] In other words, existing industry improvements often focus on localized optimizations of single materials, structures, or processes, resulting in inherent technical contradictions such as "increasing light inevitably leads to color deviation, stabilizing color inevitably leads to reduced efficiency, and improving efficiency inevitably leads to deteriorated reliability." Simple technological superposition cannot eliminate the interference between parameters, making it difficult to achieve a comprehensive performance leap. This invention differs from existing piecemeal improvement solutions by pioneering a multi-dimensional coupled and collaborative system: It eliminates bottom light loss and top surface shading drawbacks through a wafer-level uniform-height white adhesive structure, accurately recovering lateral stray light; it constructs a controllable phosphor gradient concentration distribution based on a natural sedimentation process, physically addressing the pain points of uneven sedimentation and color gamut shift in large-particle-size powder; and it uses an optimal 15%~35% proportion anchoring step structure, matched with the embedded assembly of the spherical convex lens 5, forming a mechanically interlocked anchoring structure, completely solving the reliability problems of lens 5 peeling and interface delamination. Simultaneously, it matches the refractive index difference limit and optimal convexity parameter of the lens 5, maximizing the optimization of the light output angle and reducing total internal reflection loss. This invention is not a mere superposition of conventional technical features, but rather an integrated innovation that fundamentally breaks through the industry's technical bottleneck of the incompatibility between high luminous efficacy, high color consistency, and high structural stability in LED devices through precise matching of parameter ranges, structural complementarity, and process empowerment. It can still achieve zero peeling failure under the stringent test of 1000 thermal shocks, while significantly improving luminous efficacy and color yield. Compared with existing technologies, it has outstanding substantive features and significant progress, and has extremely high industrial application value.
[0107] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A high-efficiency LED packaging structure with light field reconstruction and interface anchoring coupling, comprising a support, a blue LED chip, a white reflective adhesive layer, a phosphoric adhesive layer, and a lens, wherein the support is provided with a cup-shaped cavity, and the blue LED chip is fixed at the center of the bottom of the cup-shaped cavity; characterized in that, The white reflective adhesive layer is disposed in the annular functional area of the cup-shaped cavity, and the height difference between the top surface of the cured white reflective adhesive layer and the top surface of the blue LED chip is ≤15μm; The fluorescent adhesive layer is coated on top of the white reflective adhesive layer, and the top surface of the fluorescent adhesive layer is lower than the cup-shaped cavity end face, forming an annular anchoring and receiving step; The fluorescent adhesive layer has a gradient concentration distribution structure inside, and the concentration of phosphor in the fluorescent adhesive is higher on the side closer to the blue LED chip than on the side farther away from the blue LED chip; The lens is a spherical convex lens formed by the self-forming of liquid surface tension. The bottom of the lens is embedded in the interior of the annular anchoring accommodating step and forms an embedded interlocking anchoring structure. The apex of the lens protrudes from the cup-shaped cavity end face. The convexity of the lens is >0.5D. The lens is made of high-transmittance silicone, and the difference between the refractive index of the lens and the refractive index of the fluorescent adhesive is ≤0.
03. 2.The high-LE LED package structure of light field reconstruction and interface anchor coupling according to claim 1, wherein, The support is a PCT3030 support, a PCT2835 support, or a metal SMD support, and the cup diameter of the cup-shaped cavity is 1.8~3.0mm, and the cup depth is 0.35~0.45mm. 3.The high-LE LED package structure of light field reconstruction and interface anchor coupling according to claim 1, wherein, The blue LED chip is a standard blue LED chip, a flip-chip blue LED chip, or a vertical blue LED chip in the 450~455nm wavelength band.
4. The high-efficiency LED packaging structure with light field reconstruction and interface anchoring coupling according to claim 1, characterized in that, The white reflective adhesive layer is a white silica gel doped with The white reflective adhesive layer has a 450 nm wave band diffuse reflectivity of ≥92% and a viscosity of 8 kcps~12 kcps. The distance between the white reflective adhesive layer and the support side wall is 20~35 μm.
5. The high-efficiency LED packaging structure with light field reconstruction and interface anchoring coupling according to claim 1, characterized in that, The fluorescent adhesive layer contains yellow powder, which is YAG yellow powder, GaYAG green powder or LuAG green powder, and the particle size of the yellow powder is in the range of 15~35μm.
6. The high-efficiency LED packaging structure with light field reconstruction and interface anchoring coupling according to claim 4, characterized in that, The fluorescent adhesive layer contains either 1113 system red powder or KSF red powder.
7. The high-efficiency LED packaging structure with light field reconstruction and interface anchoring coupling according to claim 1, characterized in that, The depth of the annular anchorage step is 0.05-0.10 mm.
8. The high-efficiency LED packaging structure with light field reconstruction and interface anchoring coupling according to claim 1, characterized in that, The depth of the annular anchoring accommodating step accounts for 15% to 35% of the total depth of the cup-shaped cavity.
9. A method for fabricating a high-efficiency LED packaging structure with light field reconstruction and interface anchoring coupling, used to fabricate the high-efficiency LED packaging structure with light field reconstruction and interface anchoring coupling as described in any one of claims 1-8, characterized in that, Includes the following steps: S1: Die Bonding Wire Bonding: The blue LED chip is fixed to the bottom center of the cup-shaped cavity of the bracket using die bond adhesive. After curing, the gold wire bonding leads are completed. S2: Precise application and curing of high-reflectivity white adhesive: Using a high-precision closed-loop metering dispensing valve, high-reflectivity silicone white adhesive is precisely applied to the annular functional area of the cup-shaped cavity surrounding the blue LED chip. After curing, the height difference between the top surface of the white reflective adhesive layer and the top surface of the blue LED chip is ≤15μm. Pre-curing is carried out at 120~160℃ for 20~40min to form a flat and continuous high-reflectivity substrate and light field reconstruction interface. S3: Low-position large-particle-size fluorescent adhesive sedimentation molding: Prepare fluorescent adhesive containing large-particle-size yellow powder with D50=15~35μm; apply fluorescent adhesive to the cup-shaped cavity of the support at fixed points, and control the amount of adhesive so that the adhesive surface after curing is 0.05~0.10mm lower than the end face of the cup mouth; use a centrifugal electrostatic device to uniformly settle the large-particle-size yellow powder on the flat white adhesive substrate by gravity to form a gradient concentration distribution; then cure at 120~160℃ for 20~40min to form a fluorescent adhesive layer with annular anchoring accommodating steps; S4: Preparation of high-convexity anchored lens: High-transparency lens silicone is applied to the top surface of the fluorescent adhesive layer and the annular step area of the cup-shaped cavity. It is formed into a spherical crown convex structure by relying on the surface tension of the liquid. The amount of adhesive is controlled so that the height of the lens vertex is greater than 0.5 times the diameter of the cup opening. The lens adhesive is embedded in the step to form an embedded interlocking anchored structure. The finished LED packaging structure is obtained by curing at 70~100℃ for 50~70min and at 140-160℃ for 220~270min.
10. The method for fabricating a high-efficiency LED packaging structure with light field reconstruction and interface anchoring coupling according to claim 8, characterized in that, The prepared LED packaging structure showed no peeling failure after 1000 thermal shock tests at -40℃ to +125℃, with an interface shear force ≥20N, color tolerance <3SDCM, and yield ≥91%.