A carbon nanotube thin-film transistor, its fabrication method and application

By combining a low work function metal gate electrode with a high-k gate dielectric in situ and a carbon nanotube channel layer in a carbon nanotube thin-film transistor, the interface quality is optimized, which solves the problem of insufficient radiation resistance in existing carbon nanotube transistors and improves the stability of the device under high-energy irradiation environment.

CN123124561APending Publication Date: 2026-11-17XIAN JIAOTONG LIVERPOOL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611319165.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing carbon nanotube transistors suffer from issues related to radiation resistance, such as high gate dielectric-gate electrode interface quality, high internal defect density, and high interface state density. These limitations make it difficult to meet the comprehensive performance and reliability requirements in high-frequency, low-power, high-stability, and integrable application scenarios.

Method used

An ultrathin, dense high-k oxide gate dielectric is formed by in-situ oxidation of the surface of a low work function metal gate electrode. This is combined with a carbon nanotube channel layer to reduce native defects and radiation-induced traps in the gate dielectric. The interface quality is optimized through an interface passivation layer, resulting in a thin-film transistor structure with strong resistance to total dose irradiation.

Benefits of technology

It significantly improves the stability of devices under gamma-ray or X-ray irradiation, making them suitable for low-power and integrable radiation-resistant electronic devices, and reduces threshold voltage drift and gate drain current degradation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124561A_ABST
    Figure CN123124561A_ABST
Patent Text Reader

Abstract

This invention provides a carbon nanotube thin-film transistor, its fabrication method, and its applications. The thin-film transistor includes: a substrate; a metal gate electrode disposed on the substrate; an oxide gate dielectric layer formed by in-situ oxidation of at least a portion of the surface layer of the metal gate electrode away from the substrate; a semiconducting carbon nanotube channel layer disposed on the oxide gate dielectric layer; and source and drain electrodes respectively disposed at both ends of the semiconducting carbon nanotube channel layer. The oxide gate dielectric layer and the unoxidized metal gate electrode portion are continuously formed from the same metal layer, which reduces defects introduced by additional deposition interfaces and precursor residues, and helps to reduce gate dielectric native traps and radiation-induced charge accumulation. This structure is suitable for low-power, flexible, or integrable carbon nanotube electronic devices under total ionizing dose environments of gamma rays or X-rays.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of nanoelectronic devices and radiation-resistant semiconductor technology, specifically relating to a carbon nanotube thin-film transistor, its preparation method, and its application. Background Technology

[0002] Radiation-resistant thin-film transistors and integrated circuits typically employ device systems such as silicon-based CMOS (complementary metal-oxide-semiconductor), oxide thin-film transistors, carbon nanotube thin-film transistors, or organic thin-film transistors. Among these, carbon nanotubes are considered a channel material with high radiation resistance potential due to their intrinsic advantages, including low atomic number, strong C / C bonds, nanoscale channel cross-section, and high carrier mobility.

[0003] In existing research on the total dose irradiation resistance of carbon nanotube transistors, commonly used gate dielectric materials include SiO2, HfO2, ZrO2, ion gels, solid electrolytes, and organic-inorganic composite dielectrics. Common approaches to improve irradiation resistance include reducing the thickness of the gate dielectric, using high-capacitance gate dielectrics, optimizing device structure, selecting flexible or low-scattering-section substrates, introducing encapsulation layers, and analyzing the sources of device degradation through layered irradiation.

[0004] However, the above-mentioned technical solutions still have many shortcomings. On the one hand, high-k gate dielectrics prepared by mainstream atomic layer deposition (ALD) processes are prone to problems such as discontinuous nucleation, precursor residues, and interface defects on low-dimensional semiconductor surfaces, resulting in numerous native defects inside the dielectric and at the interface. After irradiation, oxide traps, boundary traps, and interface traps further accumulate, causing device performance degradation phenomena such as threshold voltage drift, subthreshold swing degradation, decreased mobility, and increased gate leakage current. On the other hand, the selection of gate dielectric thickness also faces a dilemma: excessively thick gate dielectrics are prone to accumulating irradiation-induced charges, exacerbating the total dose effect; excessively thin gate dielectrics are prone to tunneling leakage and breakdown risks, restricting the reliability and durability of the device.

[0005] Furthermore, while ion-gel or solid-state electrolyte gate dielectrics can provide larger equivalent gate capacitance and improve the device's ability to operate at low voltages, they still have significant limitations in terms of operating frequency, thermal stability, environmental stability, integration compatibility, and long-term reliability. For radiation-resistant carbon nanotube thin-film transistors requiring high frequency, low power consumption, high stability, and integrability in application scenarios, the above-mentioned gate dielectric solutions cannot simultaneously meet the comprehensive requirements of performance and reliability.

[0006] In summary, in existing carbon nanotube radiation-resistant devices, the interface quality between the gate dielectric and the gate electrode, the internal defect density of the dielectric, and the interface state density between the dielectric and the channel still need improvement; the synergistic design between the functional layers of the device is not yet sufficient, and the intrinsic radiation resistance advantage of the carbon nanotube channel cannot be effectively utilized at the device level. Summary of the Invention

[0007] To address the shortcomings of existing technologies, the present invention aims to provide a carbon nanotube thin-film transistor, its fabrication method, and its applications. The present invention forms an ultrathin, dense, and interface-controllable high-k oxide gate dielectric by directly in-situ oxidizing the surface of a metal gate electrode, and then bonding it with a carbon nanotube channel layer. This reduces native defects and irradiation-induced traps in the gate dielectric, thereby improving the device's stability under total γ-ray or X-ray irradiation.

[0008] To achieve this objective, the present invention adopts the following technical solution: In a first aspect, the present invention provides a carbon nanotube thin-film transistor, the carbon nanotube thin-film transistor comprising: Substrate; Metal gate electrode disposed on the substrate; An oxide gate dielectric layer formed by in-situ oxidation of at least a portion of the surface layer of the metal gate electrode away from the substrate; Semiconducting carbon nanotube channel layer disposed on the oxide gate dielectric layer; And, respectively, source electrode and drain electrode disposed at both ends of the semiconductor carbon nanotube channel layer.

[0009] In this invention, the in-situ oxidized high-k gate dielectric is directly formed from a portion of the surface layer of the metal gate, thus continuously connecting with the unoxidized metal gate. There is no intermediate layer formed through an independent deposition process between them, fundamentally avoiding the defects introduced by precursor residue, non-uniform nucleation, and additional interface layers in the ALD process. This significantly reduces the density of intrinsic defects within the gate dielectric and at the interface. Furthermore, the dense in-situ oxide layer and the controllable gate electrode / gate dielectric interface suppress the formation of oxide traps and interface traps, thereby reducing threshold voltage drift and gate leakage current degradation after total dose irradiation. The carbon nanotube channel itself has a low atomic number and strong C / C bond structure, resulting in a small intrinsic irradiation absorption cross section, further enhancing the device's resistance to total dose irradiation. The synergistic effect of these three aspects—eliminating the source of precursor defects, the intrinsic material advantages of the high-k dielectric and carbon nanotube channel, and the interface optimization of the process and structure—jointly constitutes the overall advantage of the device in terms of total dose irradiation resistance.

[0010] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. The technical objectives and beneficial effects of the present invention can be better achieved and realized through the following preferred technical solutions.

[0011] Preferably, the substrate is a flexible substrate or a rigid insulating substrate. The flexible substrate includes any one of polyimide (PI), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), or paper-based substrate. The rigid insulating substrate includes any one of glass, quartz, or silicon wafers (Si / SiO2) with a silicon dioxide layer on the surface.

[0012] Preferably, the gate electrode comprises any one of Y, Al, Sc, Hf, Zr, Ti or Ta, or an alloy formed from at least two of the above metals.

[0013] Preferably, the gate electrode is any one of Y, Al, or Sc, or an alloy formed from at least two of Y, Al, or Sc.

[0014] In this invention, a low work function metal (such as Y, Al, Sc) gate electrode can regulate the threshold voltage of a carbon nanotube thin film transistor, enabling the device to achieve enhancement-mode or near-enhancement-mode operation at low operating voltages.

[0015] Preferably, the thickness of the metal gate electrode is 5nm to 200nm, such as 5nm, 16nm, 24nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 100nm, 120nm, 150nm or 200nm, and more preferably 20nm to 80nm.

[0016] Preferably, the oxide gate dielectric layer comprises any one of Y2O3, Al2O3, Sc2O3, HfO2, ZrO2, TiO2 or Ta2O5 or an oxide formed from the alloy.

[0017] Preferably, the thickness of the oxide gate dielectric layer is 2nm to 20nm, such as 2nm, 4nm, 5nm, 6nm, 7nm, 8nm, 10nm, 12nm, 15nm or 20nm, and more preferably 4nm to 8nm.

[0018] Understandably, the thickness of the oxide gate dielectric layer is less than the thickness of the gate electrode. In this invention, the oxide gate dielectric layer is generated in situ on the metal gate electrode and is extremely thin. This significantly reduces the effective volume available for irradiation-induced charges to occupy, thus limiting the total accumulation of oxide-induced charges at the source. Simultaneously, this ultra-thin structure, combined with its high dielectric constant, significantly increases the gate capacitance per unit area, enabling the device to possess strong gate control capabilities even at low voltages. This effectively suppresses the interference of irradiation-induced charges on the channel potential.

[0019] Preferably, an interface passivation layer is provided between the oxide gate dielectric layer and the semiconducting carbon nanotube channel layer; the interface passivation layer includes any one of a phosphonic acid self-assembled molecular layer, an organosilane layer, or an Al2O3 layer.

[0020] In this invention, the phosphonic acid self-assembled molecular layer can be formed by immersing the oxide gate dielectric layer in an organophosphonic acid solution, allowing the phosphonic acid groups to combine with the surface of the metal oxide, followed by solvent cleaning, drying, and heat treatment; the organosilane layer can be formed by hydroxylating the oxide surface followed by gas-phase or solution-based silanization; and the Al2O3 layer can be formed by atomic layer deposition.

[0021] Preferably, the thickness of the interface passivation layer is 0.5nm to 5nm, such as 0.5nm, 1nm, 2nm, 3nm, 4nm or 5nm, and more preferably 1nm to 3nm.

[0022] Preferably, the semiconducting carbon nanotube channel layer is a semiconducting single-walled carbon nanotube network.

[0023] Preferably, the channel length of the carbon nanotube channel layer is 0.5μm to 100μm, such as 0.5μm, 1μm, 2μm, 5μm, 8μm, 10μm, 15μm, 20μm, 50μm, 70μm or 100μm, and more preferably 2μm to 20μm.

[0024] Preferably, the materials of the source electrode and the drain electrode each independently include any one of Au, Pd, Pt, Ag, Cu, Ni, Ti / Au, Cr / Au or Pd / Au.

[0025] It is understandable that Ti / Au, Cr / Au, and Pd / Au are all stacked structures, with the Ti, Cr, or Pd layer located at the bottom for direct contact with the carbon nanotube channel layer, and the Au layer located at the top.

[0026] Preferably, the carbon nanotube thin-film transistor further includes an encapsulation layer covering the source electrode, the drain electrode, and the semiconducting carbon nanotube channel layer; the encapsulation layer includes any one or a combination of at least two of Al2O3, HfO2, parylene, perfluorinated resin (CYTOP), polymethyl methacrylate, polystyrene, styrene-ethylene-butene-styrene block copolymer, or polyimide.

[0027] Understandably, the encapsulation layer can effectively inhibit the erosion of carbon nanotube channel layers and gate dielectric layers by water and oxygen, reducing performance degradation caused by environmental factors.

[0028] Preferably, the encapsulation layer is a single layer or a stacked structure.

[0029] In a second aspect, the present invention provides a method for fabricating a carbon nanotube thin-film transistor as described in the first aspect, the method comprising: S1, forming a metal gate electrode on the substrate; S2, At least a portion of the surface layer of the metal gate electrode away from the substrate is oxidized in situ to form an oxide gate dielectric layer; S3, a semiconductor carbon nanotube channel layer is formed on the oxide gate dielectric layer; S4, a source electrode and a drain electrode are formed at both ends of the semiconducting carbon nanotube channel layer, respectively.

[0030] Preferably, before step S1, the substrate is sequentially cleaned and dried.

[0031] Preferably, the cleaning agent includes any one or a combination of at least two of acetone, isopropanol, or deionized water.

[0032] Preferably, the method of forming the gate electrode in step S1 includes any one of electron beam evaporation, thermal evaporation, magnetron sputtering, printing, or transfer printing.

[0033] Preferably, the in-situ oxidation in step S2 includes any one of oxygen plasma oxidation, thermal oxidation, or ozone oxidation.

[0034] This invention does not limit specific oxidation parameters, which can be adjusted according to the type of metal, the thickness of the target oxide layer, and the equipment conditions.

[0035] Preferably, before step S3, the oxide gate dielectric layer is passivated. The passivation process includes any one of annealing, oxygen plasma oxygenation, phosphonic acid self-assembly modification, organosilanes modification, or Al2O3 modification.

[0036] In this invention, by introducing an interface passivation layer on the surface of the gate dielectric layer, the oxygen vacancy defects inside the gate dielectric and the interface trap state density at the interface between the gate dielectric and the carbon nanotube channel can be effectively reduced, thereby reducing the accumulation of irradiation-induced trap charges and improving the device's resistance to total dose irradiation stability.

[0037] Preferably, the method of forming the carbon nanotube channel layer in step S3 includes: depositing carbon nanotube ink into a preset channel region of the in-situ oxide gate dielectric layer, and then removing the dispersant by annealing to form a carbon nanotube channel layer; or, transferring a pre-formed carbon nanotube film to the preset channel region of the in-situ oxide gate dielectric layer by transfer printing to form a carbon nanotube channel layer.

[0038] Preferably, the deposition method includes any one of immersion, spin coating, aerosol printing, inkjet printing, or spraying.

[0039] Preferably, the annealing process includes thermal annealing or vacuum annealing.

[0040] Understandably, after the channel layer is formed, the channel area can be patterned as needed, and then annealed, encapsulated, and wired together sequentially.

[0041] Thirdly, the present invention also provides an application of the carbon nanotube thin-film transistor as described in the first aspect in electronic devices or integrated circuits.

[0042] The numerical range described in this invention includes not only the point values ​​listed above, but also any point values ​​within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific point values ​​included in the range.

[0043] Compared with the prior art, the present invention has the following beneficial effects: This invention synergistically integrates a low work function metal gate, an in-situ oxidized high-k gate dielectric, a carbon nanotube channel, an interface passivation layer, and an encapsulation layer to form a total dose-resistant thin-film transistor structure. This structure can reduce native defects in the gate dielectric and radiation-induced traps from the source, significantly improving the stability of the device under high-energy irradiation environments such as gamma rays and X-rays. It is suitable for low-power, flexible, or integrable radiation-resistant electronic devices. Attached Figure Description

[0044] Figure 1 This is a schematic diagram of the structure of the carbon nanotube thin film transistor provided in Example 1.

[0045] Figure 2 The graph shows the transfer characteristic curves and gate leakage current diagrams of the carbon nanotube thin film transistor provided in Example 1 before and after irradiation.

[0046] Figure 3 The graphs show the transfer characteristics and gate leakage current of the carbon nanotube thin-film transistor before and after irradiation, as provided in Comparative Example 1.

[0047] In the figure: 1-substrate; 2-gate electrode; 3-oxide gate dielectric layer; 4-carbon nanotube channel layer; 5-source electrode; 6-drain electrode; 7-encapsulation layer. Detailed Implementation

[0048] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.

[0049] "The scope of this invention can be defined by a lower limit and an upper limit. The selected lower limit and upper limit define the boundary of a specific range. The range defined in this way can be defined by the inclusion or exclusion of endpoints. Any endpoint can be independently selected for inclusion or exclusion, and all lower limit and upper limit values ​​can be arbitrarily combined to form a new range. That is, any lower limit value can be combined with any upper limit value to form an effective range. For example, if the ranges of 60~120 and 80~110 are listed for specific parameters, it should be understood that the ranges of 60~110 and 80~120 also fall within the scope of this invention. In addition, if the minimum range values ​​1 and 2 are listed, and the maximum range values ​​3, 4 and 5 are also listed, then 1~3, 1~4, and 2~3, 1~4, 2~5 ... All ranges from 1 to 5, 2 to 3, 2 to 4, and 2 to 5 fall within the scope of this invention. In this invention, the numerical range "a to b" represents a shortened representation of any combination of real numbers between a and b, where both a and b are real numbers. For example, the numerical range "0 to 5" indicates that all real numbers between 0 and 5 have been fully listed in this document; "0 to 5" is merely a shortened representation of this numerical combination. When a parameter is expressed as an integer ≥ 2, it is equivalent to listing positive integers that meet the requirements, such as 2, 3, 4, 5, 6, 7, 8, 9, and 10. When a parameter is expressed as an integer selected from "2 to 10", it is equivalent to listing any integer among 2, 3, 4, 5, 6, 7, 8, 9, and 10.

[0050] In this invention, "a combination of at least two" refers to a quantity greater than or equal to 2 unless otherwise specified. For example, "any one or a combination of at least two" means that any one of the listed items can be selected, or a combination of at least two of the listed items formed in a manner that does not conflict and enables the implementation of this invention. In this invention, unless otherwise specified, the features or solutions corresponding to "and / or" cover any one of two or more related listed items, as well as any and all combinations of the related listed items. The arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. For example, "A and / or B" means a set consisting of A, B, and combinations of A and B, where "containing A and / or B" can be understood, depending on the context of the statement, as containing A, containing B, or simultaneously containing both A and B. In this invention, "optional" means that the corresponding feature, component, step or solution is not necessary, that is, it is selected from either "with" or "without". If there are multiple "optional" limitations in a technical solution, unless otherwise specified and there is no technical conflict or mutual constraint, each "optional" limitation is independent and does not affect the others.

[0051] In this invention, technical features or solutions described using open-ended terms such as "comprising" or "including" do not exclude additional non-conflicting elements beyond the listed elements unless otherwise specified. They are considered to disclose both closed-ended features or solutions consisting solely of the listed elements and open-ended features or solutions that may include additional non-conflicting elements beyond the listed elements. For example, if A includes a1, a2, and a3, unless otherwise specified, this means that A can consist only of a1, a2, and a3, or it can include other non-conflicting elements based on a1, a2, and a3. This corresponds to the disclosure of technical solutions such as "A consists of a1, a2, and a3," "A is selected from a1, a2, and a3," and "A not only includes a1, a2, and a3, but may also include other non-conflicting elements." All embodiments and optional embodiments of this invention, unless otherwise specified and without technical conflict, can be combined to form new technical solutions, and such combinations fall within the scope of this invention. The term "embodiment" as used in this invention means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment or implementation of the invention. The appearance of this phrase in various locations throughout the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment mutually exclusive with other embodiments. Those skilled in the art will understand, explicitly and implicitly, that the embodiments described in this invention can be combined with other embodiments that do not conflict with the technology. The ordinal numbers "first," "second," "third," and "fourth," etc., used in the expressions "first aspect," "second aspect," "third aspect," and "fourth aspect" in this invention are for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly specifying the importance or quantity of the indicated technical features. They serve only as a non-exhaustive enumeration and do not constitute a closed limitation on quantity.

[0052] In this invention, the order in which the steps are written in the methods described in each embodiment does not imply a strict execution order. The actual execution order of each step should be determined based on its function and possible internal logic. Unless otherwise specified, all steps of this invention can be executed in the order they are written, or in any order without technical conflict. For example, if the method includes steps (a) and (b), it means that the method may include steps (a) and (b) executed sequentially, or it may include steps (b) and (a) executed sequentially. If the method also includes step (c), then step (c) can be added to the method in any order without conflict, including but not limited to the execution order of steps (a), (b), and (c), steps (a), (c), and (b), steps (c), (a), and (b), etc.

[0053] The term "embodiment" as used in this invention means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment or implementation of the invention. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a mutually exclusive, independent, or alternative embodiment. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described in this invention can be combined with other embodiments.

[0054] In this invention, "room temperature" generally refers to 4℃~35℃, and can refer to 20℃±5℃. In some embodiments of this invention, room temperature refers to 20℃~30℃.

[0055] Example 1 This embodiment provides an in-situ oxidized Y / Y₂O₃ gate dielectric carbon nanotube thin-film transistor: employing a bottom-gate top-contact structure. For example... Figure 1 As shown, the device includes a 70 μm thick polyimide substrate 1, a Y-gate electrode 2, a Y₂O₃ gate dielectric layer 3 with a thickness of approximately 6 nm formed by in-situ oxidation of the surface of the Y-gate electrode 2, a semiconducting single-walled carbon nanotube network 4, Au source and drain electrodes 5 and 6 with a thickness of 40 nm, and a 500 nm thick CYTOP encapsulation layer 7. The carbon nanotube channel length is 10 μm and the channel width is 100 μm. The fabrication method is as follows: S1. The polyimide substrate is cleaned sequentially with acetone, isopropanol and deionized water, and dried at 80°C for 30 min; a Y metal layer with an initial thickness of 30 nm is deposited by electron beam evaporation.

[0056] S2. The sample was placed in an oxygen plasma device and the Y metal surface was oxidized in situ under the conditions of oxygen flow rate of 30 sccm, power of 100W and processing time of 120s to form a Y2O3 gate dielectric layer with a thickness of about 6nm; then it was annealed in a nitrogen environment at 150℃ for 30min.

[0057] S3. Semiconductor single-walled carbon nanotube ink is deposited in a predetermined channel region of the Y2O3 gate dielectric layer, and dried according to the ink system to form a semiconductor carbon nanotube network.

[0058] S4. Au source and drain electrodes are formed by thermal evaporation, followed by the formation of a CYTOP encapsulation layer.

[0059] Example 2 This embodiment provides an in-situ oxidized Al / Al2O3 gate dielectric carbon nanotube thin-film transistor: employing a bottom-gate top-contact structure. The device includes a 70 μm thick polyethylene terephthalate (PET) substrate, an Al gate electrode, an approximately 4 nm thick Al2O3 gate dielectric layer formed by in-situ oxidation of the Al gate electrode surface, a semiconducting single-walled carbon nanotube network, a 40 nm thick Au source / drain electrode, and a 100 nm thick parylene encapsulation layer. The carbon nanotube channel length is 0.5 μm, and the channel width is 100 μm. The fabrication method is as follows: S1. The PET substrate was sequentially cleaned with acetone, isopropanol and deionized water, and dried at 80°C for 30 min; an Al metal layer with an initial thickness of 20 nm was deposited by electron beam evaporation. S2. The sample was placed in an oxygen plasma device and the Al metal surface was oxidized in situ under the conditions of oxygen flow rate of 10 sccm, power of 20W and processing time of 20s to form an Al2O3 gate dielectric layer with a thickness of about 4nm; then it was annealed in a nitrogen environment at 150℃ for 30min. S3. Semiconductor single-walled carbon nanotube ink is deposited in the preset channel region of the Al2O3 gate dielectric layer, and dried according to the ink system to form a semiconductor carbon nanotube network. S4. Au source electrode and drain electrode are formed by thermal evaporation, followed by the formation of a parylene encapsulation layer.

[0060] Example 3 This embodiment provides an in-situ oxidized Sc / Sc2O3 gate dielectric carbon nanotube thin-film transistor: employing a bottom-gate top-contact structure. The device includes a 70 μm thick polyimide (PI) substrate, an 80 nm thick Sc gate electrode, an approximately 8 nm thick Sc2O3 gate dielectric layer formed by in-situ oxidation of the Sc gate electrode surface, a semiconducting single-walled carbon nanotube network, a 40 nm thick Au source / drain electrode, and a 1 μm thick CYTOP encapsulation layer. The carbon nanotube channel length is 100 μm, and the channel width is 100 μm. The fabrication method is as follows: S1. The PI substrate is cleaned sequentially with acetone, isopropanol and deionized water, and dried at 80°C for 30 min; an Sc metal layer with an initial thickness of 80 nm is deposited by magnetron sputtering. S2. Place the sample in a thermal oxidation device and oxidize it in an oxygen atmosphere at 400°C for 180 min to perform in-situ oxidation on the Sc metal surface, forming a Sc2O3 gate dielectric layer with a thickness of about 8 nm; then anneal it in a nitrogen environment at 300°C for 60 min. S3. Semiconductor single-walled carbon nanotube ink is deposited in the preset channel region of the Sc2O3 gate dielectric layer, and dried according to the ink system to form a semiconductor carbon nanotube network. S4. Au source and drain electrodes are formed by thermal evaporation, followed by the formation of a CYTOP encapsulation layer.

[0061] Example 4 The difference between this embodiment and Embodiment 1 is that a 2 nm thick phosphonic acid self-assembled molecular layer is provided between the Y2O3 gate dielectric layer and the semiconducting single-walled carbon nanotube network as an interface passivation layer; after step S2, a phosphonic acid self-assembled molecular layer is formed on the Y2O3 surface: the sample is immersed in an octadecylphosphonic acid anhydrous ethanol solution with a concentration of 1 mmol / L and left to stand at 25°C for 12 h; after removal, it is washed 3 times with anhydrous ethanol, dried with nitrogen, and heat-treated at 100°C for 30 min to form a phosphonic acid self-assembled molecular layer with a thickness of about 2 nm.

[0062] The remaining structures and preparation methods are consistent with those in Example 1.

[0063] Comparative Example 1 The difference between this comparative example and Example 1 is that a Y metal gate electrode is first formed on the substrate, and then a Y2O3 gate dielectric layer with a thickness of about 6nm is formed on the Y metal gate electrode by an independent deposition process. That is, the Y2O3 layer is not formed by in-situ oxidation of the surface layer of the Y metal gate electrode. The remaining structures and preparation methods are consistent with those in Example 1.

[0064] Performance evaluation methods and representativeness verification The technical effects of this invention can be evaluated by the changes in transfer characteristic curves, threshold voltage, subthreshold swing, hysteresis, and gate-drain current before and after irradiation. During testing, Co-60 gamma rays or X-rays can be used, with the device port grounded or subjected to a preset bias for total ionizing dose irradiation. Transfer characteristic curves and gate-drain current are tested before and after irradiation under the same electrical conditions, where the gate voltage VGS scans from -2V to 1V, and the drain voltage VDS is -0.25V.

[0065] In representative verification of the devices in Example 1 and Comparative Example 1, irradiation with a total dose of 5 Mrad (Si) and a dose rate of 60 rad (Si) / s was performed using Co-60 γ-rays. Figure 2 and Figure 3 As shown, the transfer characteristic curves and gate leakage current measured before and after irradiation in Example 1 did not show a significant degradation trend, indicating that the in-situ oxidized Y / Y2O3 gate dielectric structure provided in Example 1 maintains good electrical stability under this total dose condition, while Comparative Example 1 shows a significant degradation trend. This representative result demonstrates the feasibility of the core structure of this invention.

[0066] The above embodiments are for illustrative purposes only. Any conventional substitutions or adjustments made by those skilled in the art to materials, dimensions, oxidation methods, interface modifications, and encapsulation methods without altering the core concept of "in-situ oxidation of the metal gate electrode surface to form a continuous oxide gate dielectric layer, and construction of carbon nanotube channels thereon" are within the scope of this invention.

Claims

1. A carbon nanotube thin-film transistor, characterized in that, include: Substrate; Metal gate electrode disposed on the substrate; An oxide gate dielectric layer formed by in-situ oxidation of at least a portion of the surface layer of the metal gate electrode away from the substrate; Semiconducting carbon nanotube channel layer disposed on the oxide gate dielectric layer; And, respectively, source electrode and drain electrode disposed at both ends of the semiconductor carbon nanotube channel layer.

2. The carbon nanotube thin-film transistor according to claim 1, characterized in that, The metal gate electrode includes any one of Y, Al, Sc, Hf, Zr, Ti or Ta, or an alloy formed from at least two of the above metals; Preferably, the metal gate electrode is any one of Y, Al or Sc, or an alloy formed from at least two of Y, Al or Sc; Preferably, the thickness of the metal gate electrode is 5nm to 200nm, and more preferably 20nm to 80nm.

3. The carbon nanotube thin-film transistor according to claim 2, characterized in that, The oxide gate dielectric layer includes any one of Y2O3, Al2O3, Sc2O3, HfO2, ZrO2, TiO2 or Ta2O5 or an oxide formed from the alloy; Preferably, the thickness of the oxide gate dielectric layer is 2nm~20nm, and more preferably 4nm~8nm.

4. The carbon nanotube thin-film transistor according to any one of claims 1-3, characterized in that, An interface passivation layer is disposed between the oxide gate dielectric layer and the semiconducting carbon nanotube channel layer; the interface passivation layer includes any one of a phosphonic acid self-assembled molecular layer, an organosilane layer, or an Al2O3 layer. Preferably, the thickness of the interface passivation layer is 0.5nm to 5nm, and more preferably 1nm to 3nm.

5. The carbon nanotube thin-film transistor according to any one of claims 1-4, characterized in that, The semiconducting carbon nanotube channel layer is a semiconducting single-walled carbon nanotube network; Preferably, the channel length of the carbon nanotube channel layer is 0.5 μm to 100 μm, and more preferably 2 μm to 20 μm.

6. The carbon nanotube thin-film transistor according to any one of claims 1-5, characterized in that, The carbon nanotube thin-film transistor further includes an encapsulation layer covering the source electrode, the drain electrode, and the semiconducting carbon nanotube channel layer; the encapsulation layer includes any one or a combination of at least two of Al2O3, HfO2, parylene, perfluorinated resin, polymethyl methacrylate, polystyrene, styrene-ethylene-butene-styrene block copolymer, or polyimide.

7. A method for fabricating a carbon nanotube thin-film transistor as described in any one of claims 1-6, characterized in that, The preparation method includes: S1, forming a metal gate electrode on the substrate; S2, At least a portion of the surface layer of the metal gate electrode away from the substrate is oxidized in situ to form an oxide gate dielectric layer; S3, a semiconductor carbon nanotube channel layer is formed on the oxide gate dielectric layer; S4, a source electrode and a drain electrode are formed at both ends of the semiconducting carbon nanotube channel layer, respectively.

8. The preparation method according to claim 7, characterized in that, The in-situ oxidation described in step S2 includes any one of oxygen plasma oxidation, thermal oxidation, or ozone oxidation.

9. The preparation method according to claim 7 or 8, characterized in that, Before step S3, the oxide gate dielectric layer is passivated. The passivation process includes any one of annealing, oxygen plasma oxygenation, phosphonic acid self-assembly modification, organosilicon modification, or Al2O3 modification.

10. The application of the carbon nanotube thin-film transistor according to any one of claims 1-6 in a total ionization dose resistant electronic device or integrated circuit.