Thin films and their preparation methods, optoelectronic devices and their preparation methods, display devices

By treating the pre-fabricated film with a first protic acid and a second protic acid, the problem of high surface roughness of inorganic nanoparticle films was solved, resulting in lower surface roughness and higher optoelectronic device performance.

CN123124641APending Publication Date: 2026-11-17GUANGDONG JUHUA RES INST OF ADVANCED DISPLAY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510630930.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-15
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Thin films prepared from inorganic nanoparticles currently have high surface roughness, which affects the performance of optoelectronic devices.

Method used

The pre-fabricated film is treated sequentially with a first protic acid and a second protic acid. The first protic acid is stronger and is used to increase the surface energy and passivate quantum dot defects, while the second protic acid is weaker and is used to stabilize the coordination environment and mitigate the damage of strong acid to quantum dots.

Benefits of technology

This reduces the surface roughness of the thin film, thereby improving the luminescence performance and lifespan of optoelectronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124641A_ABST
    Figure CN123124641A_ABST
Patent Text Reader

Abstract

This application discloses a thin film and its preparation method, an optoelectronic device and its preparation method, and a display device, relating to the field of display technology. The thin film preparation method provided in this application employs protic acid treatment, resulting in a thin film with low surface roughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of display technology, and in particular to a thin film and its preparation method, an optoelectronic device and its preparation method, and a display device. Background Technology

[0002] Nanoparticles refer to microscopic particles with sizes on the nanometer scale, at least less than 100 nanometers in one dimension. Inorganic nanoparticles possess characteristics such as small size effect, surface and interface effect, quantum size effect, macroscopic quantum tunneling effect, strong adsorption capacity and chemical activity, and strong permeability, and are widely used in optoelectronic fields, biomedicine, and other fields.

[0003] In related technologies, films prepared using inorganic nanoparticles have relatively high surface roughness, which needs further improvement. Summary of the Invention

[0004] In view of the above, this application provides a thin film and a method for preparing the same, an optoelectronic device and a method for preparing the same, and a display device.

[0005] The embodiments of this application are implemented as follows: a method for preparing a thin film includes the following steps:

[0006] A preform is provided, wherein the material of the preform includes quantum dots;

[0007] The pre-prepared membrane is treated sequentially with a first protic acid and a second protic acid to form a thin film;

[0008] Wherein, the pKa of the second protic acid is greater than that of the first protic acid.

[0009] Accordingly, this application also provides a thin film, wherein the optoelectronic device is prepared by the above-described preparation method.

[0010] Accordingly, embodiments of this application also provide a method for fabricating an optoelectronic device, comprising the following steps:

[0011] A device preform is provided, the device preform comprising a first electrode and a preform film stacked together, the material of the preform film comprising quantum dots;

[0012] The pre-formed film is treated sequentially with a first protic acid and a second protic acid on the side away from the first electrode to form a thin film, wherein the pKa of the second protic acid is greater than that of the first protic acid;

[0013] A second electrode is formed on the thin film to obtain a photoelectric device.

[0014] Accordingly, this application also provides an optoelectronic device, which is prepared by the above-described preparation method.

[0015] Accordingly, this application also provides a display device, which includes an optoelectronic device prepared by the above-described preparation method, or includes the above-described optoelectronic device.

[0016] The thin film preparation method provided in this application has a low surface roughness. Attached Figure Description

[0017] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0018] Figure 1 This is a flowchart of a thin film preparation method provided in an embodiment of this application;

[0019] Figure 2 This is a flowchart illustrating a method for fabricating an optoelectronic device according to an embodiment of this application;

[0020] Figure 3 This is a schematic diagram of the structure of an optoelectronic device provided in an embodiment of this application.

[0021] Explanation of reference numerals in the attached figures:

[0022] 100 - Optoelectronic device; 10 - First electrode; 20 - First carrier functional layer; 30 - Light-emitting layer; 40 - Second carrier functional layer; 50 - Second electrode. Detailed Implementation

[0023] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application. Furthermore, it should be understood that the specific embodiments described herein are only for illustration and explanation of this application and are not intended to limit this application.

[0024] In this application, unless otherwise stated, directional terms such as "upper" and "lower" generally refer to the upper and lower positions of the device in its actual use or operating state, specifically the orientation shown in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. Furthermore, in the description of this application, the term "comprising" means "including but not limited to". The terms first, second, third, etc., are used merely as illustrative purposes and do not impose numerical requirements or establish a numerical order.

[0025] In this application, "and / or" describes the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. A and B can be singular or plural.

[0026] In this application, "at least one" means one or more, and "more than one" means two or more. "One or more", "at least one of the following", or similar expressions refer to any combination of these items, including any combination of single or multiple items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.

[0027] Various embodiments of this application may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a hard limitation on the scope of this application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Furthermore, whenever a numerical range is referred to herein, it means including any referenced number (fraction or integer) within the referred range.

[0028] In the fabrication of optoelectronic devices, the quantum dot surface in the light-emitting layer usually contains ligands, making the light-emitting layer nonpolar. In contrast, the inorganic nanoparticles in the charge carrier functional layer are usually polar. When prepared by solution methods such as inkjet printing, the inorganic nanoparticles need to be dissolved in polar solvents, resulting in poor spreadability on the nonpolar light-emitting layer. This affects the film-forming properties of the charge carrier functional layer and, consequently, the light-emitting performance of the optoelectronic device.

[0029] The technical solution of this application is as follows:

[0030] Firstly, please refer to Figure 1 This application provides a method for preparing a thin film, comprising the following steps:

[0031] S11. A preform is provided, wherein the material of the preform includes quantum dots;

[0032] S12. The pre-prepared membrane is treated sequentially with a first protic acid and a second protic acid to form a thin film;

[0033] Wherein, the pKa of the second protic acid is greater than that of the first protic acid.

[0034] It should be noted that pKa refers to the acidity coefficient, which represents the ability of an acid to dissociate hydrogen ions. pKa can characterize the strength of a protic acid; the larger the pKa, the weaker the acid.

[0035] The thin film preparation method provided in this application involves sequentially treating a pre-formed film with a first protic acid and a second protic acid. The first protic acid is more acidic, which can increase the surface energy of the film and is beneficial to the subsequent film preparation. Furthermore, the anion of the first protic acid can coordinate to the quantum dot surface, reducing surface defects of the quantum dots. The second protic acid is less acidic, and its buffering effect can stabilize the coordination environment and alleviate phenomena such as etching, oxidation, and aggregation on the quantum dot surface that may be caused by strong acid. This effectively stabilizes the surface structure of the quantum dots, improves the film formation quality, and reduces the surface roughness of the film.

[0036] In some embodiments, the average particle size of the quantum dots is 2nm to 10nm, for example, it can be 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm, 10nm or any range between two of the above values.

[0037] In some embodiments, the quantum dots may be selected from, but are not limited to, one or more of single-structure quantum dots, core-shell structure quantum dots, and perovskite quantum dots.

[0038] The materials for the single-structure quantum dots, the core material of the core-shell quantum dots, and the shell material of the core-shell quantum dots can be selected from, but are not limited to, one or more compounds from group II-VI, group IV-VI, group III-V, and group I-III-VI. The shell of the core-shell quantum dots may consist of one or more layers. The group II-VI compounds may be selected from, but are not limited to, one or more of CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe, and HgZnSTe. The IV-VI group compounds may be selected from, but are not limited to, one or more of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe, and SnPbSTe. The group III-V compounds may be selected from, but are not limited to, one or more of GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs, and InAlPSb. The group I-III-VI compounds may be selected from, but are not limited to, one or more of CuInS2, CuInSe2, and AgInS2. It should be noted that for the aforementioned materials consisting of single-structure quantum dots, or core-shell structure quantum dots, or shell-structure quantum dots, the provided chemical formulas only indicate the elemental composition, not the content of each element. For example, CdZnSe only indicates that it is composed of three elements: Cd, Zn, and Se. If the content of each element were specified, it would correspond to Cd... x Zn1-x Se, 0 <x<1。

[0039] As an example, the core-shell structured quantum dots can be selected from, but are not limited to, one or more of CdSe / CdSeS / CdS, InP / ZnSeS / ZnS, CdZnSe / ZnSe / ZnS, CdSeS / ZnSeS / ZnS, CdSe / ZnS, CdSe / ZnSe / ZnS, ZnSe / ZnS, ZnSeTe / ZnS, CdSe / CdZnSeS / ZnS, and InP / ZnSe / ZnS. In the above descriptions of CdSe / ZnS, etc., the " / " indicates that the material after the " / " (as the shell) covers the material before the " / " (as the core).

[0040] The materials used for the perovskite quantum dots can be selected from, but are not limited to, doped or undoped inorganic perovskite semiconductors or organic-inorganic hybrid perovskite semiconductors. The general structural formula of the inorganic perovskite semiconductor is AMX3, where A is Cs. + Ion, M is a divalent metal cation selected from Pb 2+ Sn 2+ Cu 2+ Ni 2+ Cd 2+ Cr 2+ Mn 2+ Co 2+ Fe 2+ 、Ge 2 + Yb 2+ Eu 2+ One or more of the following, where X is a halide anion selected from Cl... - ,Br - I - One or more of the following. The general structural formula of the organic-inorganic hybrid perovskite semiconductor is BMX3, where B is an organic amine cation selected from CH3(CH2). n-2 NH3 + Or [NH3(CH2)] n NH3] 2+ Where n≥2, M is a divalent metal cation selected from Pb 2+ Sn 2+ Cu 2+ Ni 2+ Cd 2+ Cr 2+ Mn 2+ Co 2+ Fe 2+ 、Ge 2+ Yb 2+ Eu 2+One or more of the following, where X is a halide anion selected from Cl... - ,Br - I - One or more of them.

[0041] In some embodiments, in the preform, a first ligand is coordinated to the quantum dot.

[0042] The first ligand includes one or more of the following: aliphatic amine ligands having 1 to 24 carbon atoms, fatty acid ligands having 1 to 24 carbon atoms, carboxyl ligands, phosphate ligands, halide ion ligands, thiol ligands having 1 to 24 carbon atoms, trialiphatic phosphine having 9 to 30 carbon atoms, aryl phosphine having 12 to 30 carbon atoms, trialiphatic phosphine oxide having 9 to 30 carbon atoms, and triaryl phosphine oxide having 18 to 30 carbon atoms.

[0043] The aliphatic amine ligands having 1 to 24 carbon atoms include one or more of oleylamine, n-decylamine, octylamine, dioctylamine, trioctylamine, dodecylamine, myristicamine, palmitamine, and stearylamine.

[0044] The fatty acid ligands having 1 to 24 carbon atoms include one or more of oleic acid, decanoic acid, caprylic acid, dicaprylic acid, tricaprylic acid, dodecanoic acid, myristic acid, palmitic acid, stearic acid, thioglycolic acid, and thiopropionic acid.

[0045] The carboxylate ligand is selected from one or more of magnesium carboxylate ligands, calcium carboxylate ligands, aluminum carboxylate ligands, zirconium carboxylate ligands, lithium carboxylate ligands, sodium carboxylate ligands, and barium carboxylate ligands. The carboxyl group in the carboxylate ligand is a fatty acid ion with 1 to 20 carbon atoms.

[0046] The phosphate ligand is selected from one or more of magnesium phosphate ligand, calcium phosphate ligand, aluminum phosphate ligand, zirconium phosphate ligand, lithium phosphate ligand, sodium phosphate ligand, and barium phosphate ligand.

[0047] The halide ion ligand is selected from one or more of fluoride ions, chloride ions, bromide ions, and iodide ions.

[0048] The thiol ligand having 1 to 24 carbon atoms is selected from one or more of 1,2-ethanedithiol, propanethiol, butanethiol, octylthiol, dodecanethiol, octadecylthiol, benzylthiol, 1,2-benzenethiol, 1,3-benzenethiol, and 1,4-benzenethiol.

[0049] The trialiphatic phosphine having 9 to 30 carbon atoms is selected from one or more of tripropylphosphine, tributylphosphine, tripentylphosphine, trihexylphosphine, triheptylphosphine, trioctylphosphine, trinonylphosphine, and tridecylphosphine.

[0050] The arylphosphine having 12 to 30 carbon atoms is selected from one or more of diphenylphosphine, triphenylphosphine, tris(m-toluene)phosphine, tris(2-toluyl)phosphine, and tris(p-methylphenyl)phosphine.

[0051] The trialiphatic phosphine oxide with 9 to 30 carbon atoms is selected from one or more of tripropylphosphine oxide, tributylphosphine oxide, tripentylphosphine oxide, trihexylphosphine oxide, triheptylphosphine oxide, trioctylphosphine oxide, trinonylphosphine oxide, and tridecylphosphine oxide.

[0052] The triarylphosphine oxide having 18 to 30 carbon atoms is selected from one or more of triphenylphosphine oxide, tri(m-toluene)phosphine oxide, tri(2-toluene)phosphine oxide, and tri(p-methylphenyl)phosphine oxide.

[0053] It should be noted that the first ligand on the quantum dot can be derived from the raw materials, solvents, and other substances used in the synthesis process of the quantum dot.

[0054] In some embodiments, the thickness of the preform is 20nm to 60nm, for example, it can be 20nm, 30nm, 40nm, 50nm, 60nm or any range between two of the above values.

[0055] In some embodiments, the pKa of the first protic acid is ≤1, for example, it can be ≤0, ≤-1, ≤-2, ≤-3, ≤-4, etc. Within this pKa range, the first protic acid is more acidic, which can effectively improve the surface energy of the preform and passivate defects in the quantum dots.

[0056] In some embodiments, the pKa of the second protic acid is greater than 1, for example, it can be greater than 2, greater than 4, greater than 6, greater than 8, etc. Within this pKa range, the acidity of the second protic acid is relatively weak, which can effectively stabilize the coordination environment and improve the structural stability of the quantum dot.

[0057] In some embodiments, the first protic acid is selected from one or more of a first inorganic acid and a first organic acid, wherein the first organic acid includes C1-C5 organic acids. The long-chain first ligands on the quantum dots, particularly fatty acid and aliphatic amine ligands, which are substitutes for the inorganic acid anions or short-chain organic acid anions in the first protic acid, further passivate the surface defects of the quantum dots, reduce the carrier transport distance, and enhance the carrier recombination efficiency.

[0058] For example, when the first ligand is a fatty acid or carboxylate containing a carboxyl group, the first protic acid can form hydrogen bonds with the carboxyl group (-COOH) on the surface of the quantum dot through its solvent molecules, thereby lowering the activation energy of the protonation reaction and making the ligand exchange process more gentle and controllable. Then, the H in the first protic acid... + Protonated carboxyl group (-COOH→-COO) - H +This causes the ligands to detach, and then the inorganic acid anion in the first protic acid or the organic acid anion with a shorter chain length coordinates with the metal ion located at the quantum dot to form a stable short-chain ligand.

[0059] Further, the first inorganic acid includes one or more of hydrochloric acid (HCl, pKa≈-8), halogen acid, hydrohalogen acid, perhalogen acid, nitric acid (HNO3, pKa≈-1.34), and sulfuric acid (H2SO4, pKa≈-3.0).

[0060] The halogen acid includes one or more of chloric acid (HClO3, pKa≈-1.0), bromic acid (HBrO3, pKa≈-1), and iodic acid (HIO3, pKa≈0.8).

[0061] The hydrohalic acid includes one or more of hydrobromic acid (HBr, pKa≈-9) and hydroiodic acid (HI, pKa≈-10).

[0062] The perhalic acid includes one or more of perchloric acid (HClO4, pKa≈-8.0) and perbromic acid (HBrO4, pKa≈-2).

[0063] The C1-C5 organic acids include C1-C5 polyhalogenated organic acids. These C1-C5 polyhalogenated organic acids include one or more of trifluoroacetic acid (F3CCOOH, pKa≈0.23) and trichloroacetic acid (Cl3CCOOH, pKa≈0.64). It should be noted that polyhalogenated organic acids refer to organic acids in which at least two hydrogen atoms are replaced by halogens. The number of halogen substitutions in polyhalogenated organic acids can be two, three, four, etc. Multiple halogen substitutions can utilize the strong electron-withdrawing effect of halogens to enhance the acidity of polyhalogenated organic acids and facilitate protonation.

[0064] In some embodiments, the second protic acid is selected from one or more of a second inorganic acid and a second organic acid, wherein the second organic acid comprises C1-C12-C23-C4 ... 10 Organic acids. The anions in the second protic acid are inorganic acid anions or short-chain organic acid anions, which can act as buffers and regulate the coordination environment. Moreover, their acidity is smaller than that of the first protic acid, so they will not significantly affect the coordination of the inorganic acid anions in the first protic acid.

[0065] Further, the second inorganic acid includes one or more of phosphoric acid (H3PO4, pKa≈2.12), boric acid (H3BO3, pKa≈9.24), hydrocyanic acid (HCN, pKa≈9.21), metasilicic acid (H2SiO3, pKa≈9.77), and hypohalous acids. The hypohalous acid includes one or more of hypoiodic acid (HOI, pKa≈10.5), hypochlorous acid (HOCl, pKa≈7.54), and hypobromic acid (HOBr, pKa≈8.55).

[0066] The C1-C 10 Organic acids include C1-C 10 Aliphatic hydrocarbons, C1-C 10 Aromatic acids, C1-C 10 Hydroxy acids, C1-C 10 One or more of the monohalogenated organic acids.

[0067] Wherein, C1-C 10 Aliphatic hydrocarbon acids include one or more of the following: formic acid (HCOOH, pKa≈3.74), acetic acid (CH3COOH, pKa≈4.76), propionic acid (CH3CH2COOH, pKa≈4.87), acrylic acid (CH2=CHCOOH, pKa≈4.26), and butyric acid (CH3CH2CH2COOH, pKa≈4.82).

[0068] The C1-C 10 Aromatic acids include benzoic acid (C6H5COOH, pKa≈4.20).

[0069] The C1-C 10 Hydroxy acids include one or more of citric acid (HOOCC(OH)(CH2COOH)2, pKa≈3.13) and malic acid (HOOCCH2C(OH)(COOH), pKa≈3.46).

[0070] The C1-C 10 Monohalogenated organic acids include one or more of α-chlorobutyric acid (CH3CH2CHClCOOH, pKa≈2.84), β-chlorobutyric acid (CH3CHClCH2COOH, pKa≈4.06), and γ-chlorobutyric acid (Cl(CH2)3CHCOOH, pKa≈2.84). It should be noted that monohalogenated organic acids refer to organic acids in which only one hydrogen atom is replaced by a halogen. Monohalogenated organic acids contain less halogen, which can effectively buffer the pH of the system and prevent quantum dots from being etched.

[0071] It should be noted that the first protic acid is used to treat one side of the pre-formed film. The first protic acid is mainly used to exchange with the first ligand on the quantum dot surface and will not form a separate film layer with a clear boundary. Correspondingly, the second protic acid is mainly used to buffer the coordination environment after the first protic acid treatment and will not form a separate film layer with a clear boundary.

[0072] In some embodiments, treatment with the first protic acid includes the following steps:

[0073] S121. A first protic acid solution is provided, wherein the first protic acid solution comprises the first protic acid and a first solvent;

[0074] S122. The first protic acid solution is placed on the preform.

[0075] In some embodiments, the mass concentration of the first protic acid in the first protic acid solution is 2‰ to 5‰, for example, it can be 2‰, 2.5‰, 3‰, 3.5‰, 4‰, 4.5‰, 5‰, or any range between two of the above values. Within the range of the mass concentration of the first protic acid, protonation treatment of the preform surface can be promoted and ligand replacement can be promoted, while corrosion of the preform can be avoided.

[0076] In some embodiments, the first solvent comprises a polar solvent. Further, the polar solvent comprises one or more of water, trimethoxybutanol, diethylene glycol dimethyl ether, methanol, ethanol, propanol, butanol, ethylene glycol, isopropanol, glycerol, dimethyl sulfoxide, acetone, tetrahydrofuran, N,N-dimethylformamide, pyrrole, and butyric acid.

[0077] In some embodiments, the ratio of the molar number of the first protic acid to the surface area of ​​one side of the preform treated with the first protic acid is (0.1–0.5) mmol / nm. 2 For example, it can be 0.1 mmol / nm 2 0.2 mmol / nm 2 0.3 mmol / nm 2 0.4 mmol / nm 2 0.5 mmol / nm 2 Or the range between any two of the above values, etc. It can be understood that the first protic acid solution can be placed on the preform by spin coating, so that the first protic acid covers one side of the preform, thereby allowing the first protic acid to fully treat that side of the preform, effectively replacing the first ligand, and avoiding a large amount of first protic acid residue.

[0078] In some embodiments, the treatment time of the first proton acid is 5 min to 15 min, for example, it can be 5 min, 8 min, 10 min, 12 min, 15 min, or any range between two of the above values. Within this time range, it is beneficial for the first proton acid to protonate the preformed film, and it is also beneficial to avoid corrosion of the preformed film.

[0079] In some embodiments, after the first protic acid solution is placed on the preform, the process further includes performing a first annealing. Further, the temperature of the first annealing is 80°C to 100°C, for example, 80°C, 85°C, 90°C, 95°C, 100°C, or any range between two of the above values. The time of the first annealing is 10 min to 20 min, for example, 10 min, 12 min, 14 min, 16 min, 18 min, 20 min, or any range between two of the above values. Thus, under the conditions of the first annealing, it is beneficial to remove the first solvent and to avoid structural damage to the preform caused by the strongly acidic first protic acid due to excessively high temperature.

[0080] In some embodiments, treatment with the second protic acid includes the following steps:

[0081] S123. Provide a second protic acid solution, wherein the second protic acid solution includes the second protic acid and a second solvent;

[0082] S124. The second protic acid solution is placed on the preform.

[0083] In some embodiments, the mass concentration of the second protic acid in the second protic acid solution is 5‰ to 8‰, for example, it can be 5‰, 5.5‰, 6‰, 6.5‰, 7‰, 7.5‰, 8‰, or any range between two of the above values. Within the range of the mass concentration of the second protic acid, buffering treatment of the pre-formed film surface can be promoted, reducing the damage to the quantum dot structure caused by the instantaneous high acid concentration region that may be formed by the first protic acid, and also promoting the stable coordination of the anion of the first protic acid with the metal ions in the quantum dots.

[0084] In some embodiments, the second solvent comprises a polar solvent. Further, the polar solvent comprises one or more of water, trimethoxybutanol, diethylene glycol dimethyl ether, methanol, ethanol, propanol, butanol, ethylene glycol, isopropanol, glycerol, dimethyl sulfoxide, acetone, tetrahydrofuran, N,N-dimethylformamide, pyrrole, and butyric acid.

[0085] In some embodiments, the ratio of the molar number of the second protic acid to the surface area of ​​one side of the preform treated with the second protic acid is (0.1–0.5) mmol / nm. 2 For example, it can be 0.1 mmol / nm 2 0.2 mmol / nm 2 0.3 mmol / nm 2 0.4 mmol / nm 2 0.5 mmol / nm 2 Or the range between any two of the above values, etc. It can be understood that the second protic acid solution can be placed on the preform by spin coating, so that the second protic acid covers one side of the preform, thereby allowing the second protic acid to fully treat that side of the preform and effectively stabilize the structure and coordination environment of the quantum dots.

[0086] In some embodiments, the treatment time of the second protic acid is 20 min to 40 min, for example, it can be 20 min, 25 min, 30 min, 35 min, 40 min, or any range between two of the above values. Within the range of said time, it is beneficial for the second protic acid to play a buffering role and stabilize the coordination environment of the metal ions.

[0087] In some embodiments, after placing the second protic acid solution on the side of the pre-formed film away from the first electrode 10, the process further includes performing a second annealing. Further, the temperature of the second annealing is 120°C to 150°C, for example, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, or any range between two of the above values. The time of the second annealing is 20 min to 30 min, for example, 20 min, 22 min, 24 min, 26 min, 28 min, 30 min, or any range between two of the above values. Thus, under the conditions of the second annealing, it is beneficial to remove the second solvent and stabilize the coordination environment.

[0088] It should be noted that after the first protic acid and the second protic acid are treated respectively, the displaced first ligand, as well as the residual first and second protic acids, can be removed by washing.

[0089] It should also be noted that during the second protic acid treatment, when there are still coordinable sites on the surface of the quantum dot, the anion of the second protic acid may be coordinated and connected to the quantum dot.

[0090] In this scheme, both the first and second protic acid treatments are performed in solution form. The polar solvent in the solution can change the polarity of the film, making it easier for the subsequent carrier dispersion to spread evenly. Compared with gaseous acid treatment, solution treatment is gentler and the treatment effect is more uniform. In contrast, the molecular diffusion rate in gaseous acid treatment is faster, which makes it easier to form instantaneous high acid concentration regions, leading to corrosion of quantum dots.

[0091] In some embodiments, the process further includes performing a first plasma treatment before the first protic acid treatment.

[0092] Further, the first plasma treatment includes: providing a first gas and exciting the first gas to generate plasma to treat the preformed membrane.

[0093] In some embodiments, the first gas includes one or more of argon, hydrogen, oxygen, chlorine, ammonia, nitrogen, CF4, and SF6.

[0094] In some embodiments, the gas flow rate of the first gas is 20 sccm to 50 sccm, for example, it can be 20 sccm, 30 sccm, 40 sccm, 50 sccm or any range between the above two values.

[0095] It should be noted that the generation of plasma by exciting the first gas can be achieved by conventional techniques in the field, such as electric fields, radio frequency, microwaves, lasers, electron beams, etc.

[0096] In some embodiments, the method for exciting the first gas to generate plasma is a first radio frequency discharge method. Further, the power of the first radio frequency discharge is 50W to 200W, for example, it can be 50W, 80W, 100W, 120W, 150W, 180W, 200W, or any range between two of the above values; the frequency of the first radio frequency discharge is 10MHz to 30MHz, for example, it can be 10MHz, 15MHz, 20MHz, 25MHz, 30MHz, or any range between two of the above values.

[0097] In some embodiments, the treatment with the second protic acid further includes: performing a second plasma treatment.

[0098] Furthermore, the second plasma treatment includes: providing a second gas and exciting the second gas to generate plasma to treat the preformed membrane.

[0099] In some embodiments, the second gas includes one or more of argon, hydrogen, oxygen, chlorine, ammonia, nitrogen, CF4, and SF6.

[0100] In some embodiments, the gas flow rate of the second gas is 10 sccm to 20 sccm, for example, it can be 10 sccm, 12 sccm, 14 sccm, 16 sccm, 18 sccm, 20 sccm or any range between two of the above values.

[0101] It should be noted that the generation of plasma by exciting the second gas can be achieved using conventional techniques in the field, such as electric fields, radio frequency, microwaves, lasers, electron beams, etc.

[0102] In some embodiments, the method for exciting the second gas to generate plasma is a second radio frequency discharge method. Further, the power of the second radio frequency discharge is 100W to 300W, for example, it can be 100W, 150W, 200W, 250W, 300W, or any range between two of the above values; the frequency of the second radio frequency discharge is 10MHz to 30MHz, for example, it can be 10MHz, 15MHz, 20MHz, 25MHz, 30MHz, or any range between two of the above values.

[0103] This method involves performing a first plasma treatment before the first protic acid treatment, which helps clean the surface of the pre-formed film, remove organic contaminants and oxides, and improve the uniformity of the first and second protic acid treatments. Performing a second plasma treatment after the second protic acid treatment helps remove residual organic ligand fragments, promotes the bonding of anions from the first protic acid to the quantum dot surface, reduces localized quantum dot aggregation caused by the first and second protic acid treatments, and improves the uniformity of the film.

[0104] In some embodiments, the quantum dots in the thin film are coordinated with a second ligand, the second ligand comprising one or more of inorganic acid radicals and C1-C5 organic acid radicals.

[0105] Furthermore, the inorganic acid radical ions include one or more of the following: halide ions, halide ions, hydrohalate ions, perhalate ions, nitrate ions, and sulfate ions.

[0106] The C1-C5 organic acid anions include one or more of trifluoroacetate ions and trichloroacetate ions.

[0107] The shorter chain length of the second ligand in the quantum dots of the thin film is beneficial for promoting carrier transport and for ensuring uniform spreading of the subsequent carrier functional layer when prepared by solution method.

[0108] In some embodiments, the surface roughness of the film is 0.7 nm to 1.5 nm, for example, it can be 0.7 nm, or any range between the two values ​​mentioned above. It should be noted that the surface roughness of the film here refers to the surface roughness of one side of the film treated with the first protic acid and the second protic acid.

[0109] Secondly, embodiments of this application also provide a thin film prepared by the above-described preparation method.

[0110] It is understood that the material of the thin film includes quantum dots, which can be used as the light-emitting layer 30 in the optoelectronic device 100.

[0111] Thirdly, please refer to Figure 2 This application provides a method for fabricating an optoelectronic device 100, comprising the following steps:

[0112] S21. Provide a device preform, the device preform including a first electrode 10 and a pre-embedded light-emitting layer stacked together, the material of the pre-embedded light-emitting layer including quantum dots;

[0113] S22. The side of the pre-fabricated light-emitting layer away from the first electrode 10 is treated sequentially with a first protic acid and a second protic acid to form a light-emitting layer 30, wherein the pKa of the second protic acid is greater than that of the first protic acid.

[0114] S23. A second electrode 50 is formed on the light-emitting layer 30 to obtain an optoelectronic device 100.

[0115] The method for fabricating the optoelectronic device 100 provided in this application involves sequentially treating a pre-fabricated light-emitting layer with a first protic acid and a second protic acid. The first protic acid is more acidic, which can increase the surface energy of the light-emitting layer 30, which is beneficial for the fabrication of subsequent film layers. Furthermore, the anions of the first protic acid can coordinate to the surface of quantum dots, reducing surface defects and shortening the carrier transport path, thus improving the carrier injection and recombination efficiency. The second protic acid is less acidic, and its buffering effect can stabilize the coordination environment, mitigating phenomena such as etching, oxidation, and aggregation on the quantum dot surface that may be caused by strong acids, thereby effectively stabilizing the surface structure of the quantum dots. The combined treatment of the first and second protic acids reduces defects in the quantum dots, improves the uniformity of subsequent film layer fabrication, promotes carrier transport, stabilizes the quantum dot structure, improves the luminous efficiency of the optoelectronic device 100, and extends the service life of the optoelectronic device 100.

[0116] In S21 and S23:

[0117] In some embodiments, the first electrode 10 and the second electrode 50 each independently include one or more of a metal electrode, a carbon electrode, a metal oxide electrode, and a composite electrode; the material of the metal electrode includes one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb, and Mg; the material of the carbon electrode includes one or more of graphite, carbon nanotubes, graphene, and carbon fibers; the material of the metal oxide electrode includes one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO, MoO3, and AMO; the composite electrode includes one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2, and TiO2 / Al / TiO2. In this context, " / " indicates a stacked structure. For example, AZO / Ag / AZO represents a composite electrode consisting of sequentially stacked AZO, Ag, and AZO layers.

[0118] In some embodiments, the device preform further includes a first carrier functional layer 20, which is located between the first electrode 10 and the preformed light-emitting layer.

[0119] In some embodiments, the provision of the second electrode 50 on the light-emitting layer 30 includes: providing a second carrier functional layer 40 on the light-emitting layer 30, and providing the second electrode 50 on the second carrier functional layer 40.

[0120] In some embodiments, the first carrier functional layer 20 is a first hole functional layer, and the second carrier functional layer 40 is a first electron functional layer. It can be understood that the first electrode 10 is the anode, and the second electrode 50 is the cathode. The resulting optoelectronic device 100 is a positively positioned optoelectronic device 100.

[0121] In some embodiments, the first carrier functional layer 20 is a second electron functional layer, and the second carrier functional layer 40 is a second hole functional layer. It can be understood that in this case, the first electrode 10 is a cathode, and the second electrode 50 is an anode. The resulting optoelectronic device 100 is an inverted optoelectronic device 100.

[0122] The first hole functional layer and the second hole functional layer each independently include one or more of the following: hole injection layer and hole transport layer.

[0123] The first electronic functional layer and the second electronic functional layer each independently include one or more of the following: an electron injection layer and an electron transport layer.

[0124] In some embodiments, the material of the second electronic functional layer includes one or more of a first doped metal oxide particle, a first undoped metal oxide particle, a group IIB-VIA semiconductor material, a group IIIA-VA semiconductor material, and a group IB-IIIA-VIA semiconductor material. The material of the first undoped metal oxide particle includes one or more of ZnO, TiO2, SnO2, ZrO2, and Ta2O5. The metal oxide in the first doped metal oxide particle includes one or more of ZnO, TiO2, SnO2, ZrO2, Ta2O5, and Al2O3. The doping element in the first doped metal oxide particle includes one or more of Al, Mg, Li, Mn, Y, La, Cu, Ni, Zr, Ce, In, and Ga. The IB-VIA group semiconductor materials include one or more of ZnS, ZnSe, and CdS; the IIIA-VA group semiconductor materials include one or more of InP and GaP; and the IB-IIIA-VIA group semiconductor materials include one or more of CuInS and CuGaS. The doping amount of the dopant element in the first doped metal oxide particle is 0.1wt% to 20wt%, for example, it can be 0.1wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%, or any range between two values.

[0125] In some embodiments, the material of the first hole functional layer comprises an organic p-type semiconductor material or an inorganic p-type semiconductor material, wherein the organic p-type semiconductor material comprises 4,4'-N,N'-dicarbazolyl-biphenyl, N,N'-diphenyl-N,N'-bis(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine, N,N'-bis(3-methylphenyl)-N,N'-bis(phenyl)- Spiro, N,N'-bis(4-(N,N'-diphenyl-amino)phenyl)-N,N'-diphenylbenzidine, 4,4',4'-tris(N-carbazolyl)-triphenylamine, 4,4',4'-tris(carbazol-9-yl)triphenylamine, trichloroisocyanuric acid, 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazabenzphenanthrene, 4,4',4'-tris(N-3-methylphenyl-N-phenylamino)triphenylamine, poly[(9,9'-dioctylfluorene-2,7-diyl)-co-(4, 4'-(N-(4-sec-butylphenyl)diphenylamine), poly(4-butylphenyl-diphenylamine), poly[bis(4-phenyl)(4-butylphenyl)amine], polyaniline, polypyrrole, poly(p-)phenylenevinylene, poly(phenylenevinylene), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylenevinylene], poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylenevinylene], copper phthalocyanine, aromatic tertiary amines, polynuclear aromatic tertiary amines, 4,4'-bis(p-)phenylenevinylene The following are included in the list of N,N,N',N'-tetraarylbenzidine, PEDOT, PEDOT:PSS and its derivatives, PEDOT:PSS derivatives doped with s-MoO3, poly(N-vinylcarbazole) and its derivatives, polymethacrylate and its derivatives, poly(9,9-octylfluorene) and its derivatives, poly(spirofluorene) and its derivatives, N,N'-bis(naphthyl-1-yl)-N,N'-diphenylbenzidine, spironolactone (NPB), microcrystalline cellulose, and tetracyanoquinone dimethyl ether.The inorganic P-type semiconductor material comprises one or more of the following: nanocrystalline diamond, doped graphene, undoped graphene, second-doped metal oxide particles, second-undoped metal oxide particles, metal sulfides, metal selenides, and metal nitrides. The metal oxides in the second-doped and second-undoped metal oxide particles each independently comprise one or more of MoO3, WO3, NiO, CrO3, CuO, and V2O5. The doping element in the second-doped metal oxide particles comprises one or more of Mo, W, Ni, Cr, Cu, and V. The metal sulfides include CuS and MoS. 3. One or more of WS3, wherein the metal selenide includes one or more of MoSe3 and WSe3, and the metal nitride includes p-type gallium nitride, wherein the doping amount of the dopant element in the second doped metal oxide particle is 0.1wt% to 20wt%, for example, it can be 0.1wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%, or any range between two values.

[0126] In some embodiments, the material of the second carrier functional layer 40 comprises inorganic nanoparticles, which include N-type inorganic nanoparticles or P-type inorganic nanoparticles. It is understood that the material of the first electron functional layer comprises N-type inorganic nanoparticles, and the material of the second hole functional layer comprises P-type inorganic nanoparticles.

[0127] It should be noted that treating the pre-fabricated light-emitting layer with the first and second protic acids can significantly enhance the surface energy of the light-emitting layer 30, thereby enhancing the wettability and uniform spreading of the solution of N-type inorganic nanoparticles or P-type inorganic nanoparticles on the light-emitting layer 30, improving the film quality of the second charge carrier functional layer 40, reducing the surface roughness of the second charge carrier functional layer 40, and optimizing the interfacial contact between the light-emitting layer 30 and the second charge carrier functional layer 40, further improving the light-emitting performance and stability of the optoelectronic device 100.

[0128] In some embodiments, the average particle size of the N-type inorganic nanoparticles is 2 nm to 10 nm, for example, it can be 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, or any range between two of the above values. It should be noted that in this application, the particle size is obtained by transmission electron microscopy (TEM).

[0129] In some embodiments, the N-type inorganic nanoparticles include one or more of a first doped metal oxide particle, a first undoped metal oxide particle, a group IIB-VIA semiconductor material, a group IIIA-VA semiconductor material, and a group IB-IIIA-VIA semiconductor material. The first undoped metal oxide particle is composed of one or more of ZnO, TiO2, SnO2, ZrO2, and Ta2O5. The metal oxide in the first doped metal oxide particle is composed of one or more of ZnO, TiO2, SnO2, ZrO2, Ta2O5, and Al2O3. The doping element in the first doped metal oxide particle is composed of one or more of Al, Mg, Li, Mn, Y, La, Cu, Ni, Zr, Ce, In, and Ga. B-VIA group semiconductor materials include one or more of ZnS, ZnSe, and CdS; IIIA-VA group semiconductor materials include one or more of InP and GaP; and IB-IIIA-VIA group semiconductor materials include one or more of CuInS and CuGaS. The doping amount of the dopant element in the first doped metal oxide particle is 0.1wt% to 20wt%, for example, it can be 0.1wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%, or any range between two values.

[0130] In some embodiments, the average particle size of the P-type inorganic nanoparticles is 2nm to 10nm, for example, it can be 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm, 10nm or any range between two of the above values.

[0131] In some embodiments, the p-type inorganic nanoparticles include one or more of a second doped metal oxide particle, a second undoped metal oxide particle, a metal sulfide, a metal selenide, and a metal nitride. The metal oxides in the second doped metal oxide particle and the second undoped metal oxide particle each independently include one or more of MoO3, WO3, NiO, CrO3, CuO, and V2O5. The doping element in the second doped metal oxide particle includes one or more of Mo, W, Ni, Cr, Cu, and V. The metal sulfide includes CuS, MoS3, and WS3. One or more, wherein the metal selenide includes one or more of MoSe3 and WSe3, and the metal nitride includes p-type gallium nitride, wherein the doping amount of the dopant element in the second doped metal oxide particle is 0.1wt% to 20wt%, for example, it can be 0.1wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%, or any range between two values.

[0132] In some embodiments, the thickness of the first carrier functional layer 20 is 20 nm to 60 nm, for example, it can be 20 nm, 30 nm, 40 nm, 50 nm, 60 nm or any range between two of the above values. It should be noted that in this application, the thickness of the thin film is obtained by a profilometer.

[0133] In some embodiments, the thickness of the second carrier functional layer 40 is 20nm to 60nm, for example, it can be 20nm, 30nm, 40nm, 50nm, 60nm or any range between two of the above values.

[0134] In some embodiments, the surface roughness of the second charge carrier functional layer 40 is 0.5 nm to 1.5 nm, for example, it can be 0.5 nm, 0.6 nm, 0.7 nm, 0.8 nm, 0.9 nm, 1.0 nm, 1.1 nm, 1.2 nm, 1.3 nm, 1.4 nm, 1.5 nm, or any range between two of the above values. It should be noted that in this application, the surface roughness of the thin film is obtained by atomic force microscopy (AFM). During the preparation of the second charge carrier functional layer 40, uniform solvent deposition is beneficial to improving its film formation uniformity, thereby reducing its surface roughness.

[0135] It should be noted that the first electrode 10, the first charge carrier functional layer 20, the pre-fabricated light-emitting layer, the second charge carrier functional layer 40, and the second electrode 50 can be implemented using conventional techniques in the art, such as chemical or physical methods. Chemical methods include chemical vapor deposition, continuous ion layer adsorption and reaction, anodic oxidation, electrolytic deposition, and co-precipitation. Physical methods include physical deposition and solution methods. Physical deposition methods include thermal evaporation deposition, electron beam evaporation deposition, magnetron sputtering, multi-arc ion deposition, physical vapor deposition, atomic layer deposition, pulsed laser deposition, etc.; solution methods can include spin coating, printing, inkjet printing, blade coating, dip coating, immersion coating, spraying, roller coating, casting, slot coating, and strip coating, etc.

[0136] Specifically, in some embodiments, the method for preparing the second carrier functional layer 40 includes the following steps:

[0137] S231. Provide an inorganic nanoparticle dispersion, wherein the inorganic nanoparticle dispersion includes inorganic nanoparticles and a third solvent;

[0138] S232. The inorganic nanoparticle dispersion is disposed on the light-emitting layer 30 to form a second carrier functional layer 40.

[0139] In some embodiments, the inorganic nanoparticles include N-type inorganic nanoparticles or P-type inorganic nanoparticles.

[0140] In some embodiments, the inorganic nanoparticle dispersion has a mass concentration of 10 mg / mL to 50 mg / mL, for example, 10 mg / mL, 20 mg / mL, 30 mg / mL, 40 mg / mL, 50 mg / mL, or any range between two of the above values. Within this mass concentration range, uniform dissolution and dispersion of the inorganic nanoparticles is beneficial.

[0141] In some embodiments, the third solvent comprises a polar solvent. Further, the polar solvent comprises one or more of trimethoxybutanol, diethylene glycol dimethyl ether, methanol, ethanol, propanol, butanol, ethylene glycol, isopropanol, glycerol, dimethyl sulfoxide, acetone, tetrahydrofuran, N,N-dimethylformamide, pyrrole, and butyric acid. It is understood that after treatment with the first and second protic acids, the pre-fabricated luminescent layer exhibits better compatibility with polar solvents, which is more conducive to the uniform spreading of the inorganic nanoparticle dispersion.

[0142] In some embodiments, after the inorganic nanoparticle dispersion is applied to the light-emitting layer 30, a third annealing process is further included. The third annealing temperature is 80°C to 150°C, for example, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, or any range between two of the above values. The third annealing time is 5 min to 30 min, for example, 5 min, 10 min, 15 min, 20 min, 25 min, 30 min, or any range between two of the above values. Thus, under the conditions of the third annealing, it is beneficial to remove the third solvent and promote the film formation of the inorganic nanoparticle dispersion.

[0143] In S22:

[0144] It should be noted that the quantum dots, the first protic acid, the second protic acid, and the processing method of the pre-fabricated light-emitting layer are as described above and will not be repeated here; the pre-fabricated light-emitting layer and the light-emitting layer 30 can refer to the pre-fabricated film and thin film described above and will not be repeated here.

[0145] Fourthly, please refer to Figure 3 This application also provides an optoelectronic device 100, which is prepared by the above-described preparation method.

[0146] Specifically, the optoelectronic device 100 includes a first electrode 10, a light-emitting layer 30, and a second electrode 50 stacked together. The material of the light-emitting layer 30 includes quantum dots. A second ligand is coordinated and connected to the quantum dots on the side of the light-emitting layer 30 near the second electrode 50. The second ligand includes one or more of inorganic acid radical ions and C1-C5 organic acid radical anions.

[0147] Furthermore, the inorganic acid radical ions include one or more of the following: halide ions, halide ions, hydrohalate ions, perhalate ions, nitrate ions, and sulfate ions.

[0148] The C1-C5 organic acid anions include one or more of trifluoroacetate ions and trichloroacetate ions.

[0149] The optoelectronic device 100 may further include one or more of a first carrier functional layer 20 and a second carrier functional layer 40. The first carrier functional layer 20 and the second carrier functional layer 40 are described above and will not be repeated here.

[0150] Fifthly, embodiments of this application also provide a display device, the display device comprising the optoelectronic device 100 prepared by the above-described preparation method, or comprising the above-described optoelectronic device 100.

[0151] The display device can be any electronic product with display function, including but not limited to smartphones, tablets, laptops, digital cameras, digital camcorders, smart wearable devices, smart weighing scales, in-vehicle displays, televisions, or e-book readers. Among them, smart wearable devices can be, for example, smart bracelets, smartwatches, virtual reality (VR) headsets, etc.

[0152] The present application will be specifically described below through specific embodiments. The following embodiments are only some embodiments of the present application and are not intended to limit the present application.

[0153] Thin Film Example 1

[0154] This embodiment provides a thin film and a method for preparing the same. The method for preparing the thin film includes the following steps:

[0155] In step S31, a 30 mg / mL n-octane dispersion of blue CdSeS / ZnS quantum dots (average particle size of 7 nm) was placed on a substrate. Oleic acid and oleylamine ligands were attached to the surface of the CdSeS / ZnS quantum dots. The spin coating speed was 3000 rpm and the time was 30 s. Then, the mixture was annealed at 100 °C for 10 min to form a pre-film with a thickness of 50 nm.

[0156] Step S32: Introduce a mixed gas of Ar and O2 (Ar:O2 = 4:1) at a total flow rate of 20 sccm, and use radio frequency discharge (power 100W, frequency 15MHz) to excite and generate plasma to process the preformed film for 8 minutes.

[0157] Step S33, according to 0.2 mmol / nm 2 A 3‰ hydrochloric acid (first protic acid) ethanol solution was spin-coated onto one side of the pre-formed film at 3000 rpm. After standing for 10 min, it was annealed at 80℃ for 10 min, and the displaced oleic acid and oleylamine ligands were removed by washing. The solution was then prepared at 0.2 mmol / nm. 2 A 7‰ ethanol solution of acetic acid (a second protic acid) was spin-coated onto the same side of the hydrochloric acid-treated pre-film at a spin speed of 3000 rpm. After standing for 20 minutes, the film was annealed at 120°C for 20 minutes and then cleaned to remove residual substances, thus obtaining the film.

[0158] Step S34: Introduce a mixed gas of Ar and Cl2 (Ar:Cl2 = 14:1) at a total flow rate of 15 sccm, and excite the thin film in step S33 by radio frequency discharge (power 200W, frequency 20MHz) to generate plasma for treatment. The treatment time is 5 min.

[0159] Thin Film Example 2

[0160] This thin film embodiment is basically the same as thin film embodiment 1, except that the first protic acid in step S33 is replaced with sulfuric acid in this thin film embodiment.

[0161] Thin Film Example 3

[0162] This thin film embodiment is basically the same as thin film embodiment 1, except that the first protic acid in step S33 is replaced with nitric acid in this thin film embodiment.

[0163] Thin Film Example 4

[0164] This thin film embodiment is basically the same as thin film embodiment 1, except that the first protic acid in step S33 is replaced with trifluoroacetic acid in this thin film embodiment.

[0165] Thin Film Example 5

[0166] This thin film embodiment is basically the same as thin film embodiment 1, except that the first protic acid in step S33 is replaced with trichloroacetic acid in this thin film embodiment.

[0167] Thin Film Example 6

[0168] This thin film embodiment is basically the same as thin film embodiment 1, except that the second protic acid in step S33 is replaced with citric acid in this thin film embodiment.

[0169] Thin Film Example 7

[0170] This thin film embodiment is basically the same as thin film embodiment 1, except that the second protic acid in step S33 is replaced with boric acid in this thin film embodiment.

[0171] Thin Film Example 8

[0172] This thin film embodiment is basically the same as thin film embodiment 1, except that the second protic acid in step S33 is replaced with metasilicic acid in this thin film embodiment.

[0173] Thin Film Example 9

[0174] This thin film embodiment is basically the same as thin film embodiment 1, except that the second protic acid in step S33 is replaced with malic acid in this thin film embodiment.

[0175] Thin Film Example 10

[0176] This thin film embodiment is basically the same as thin film embodiment 1, except that the second protic acid in step S33 is replaced with phosphoric acid in this thin film embodiment.

[0177] Thin Film Example 11

[0178] This thin film embodiment is basically the same as thin film embodiment 1, except that the second protic acid in step S33 is replaced with hydrogen cyanide in this thin film embodiment.

[0179] Thin Film Example 12

[0180] This film embodiment is basically the same as film embodiment 1, except that step S34 is not performed in this film embodiment.

[0181] Thin Film Example 13

[0182] This film embodiment is basically the same as film embodiment 1, except that step S32 is not performed in this film embodiment.

[0183] Thin Film Example 14

[0184] This film embodiment is basically the same as film embodiment 1, except that steps S32 and S34 are not performed in this film embodiment.

[0185] Thin Film Comparative Example 1

[0186] This comparative example of a thin film is basically the same as that of thin film example 14, except that step S33 was not performed in this comparative example of a thin film.

[0187] Thin Film Comparative Example 2

[0188] This comparative film is basically the same as that of film example 14, except that the second protic acid treatment in step S33 was not performed in this comparative film, only the first protic acid treatment was performed.

[0189] The surface roughness Ra of the acid-treated side of the films of thin film Examples 1-14 and Comparative Examples 1-2 was tested, and the results are shown in Table 1.

[0190] Table 1

[0191]

[0192]

[0193] From Table 1, we can obtain:

[0194] By treating the pre-formed film with a first protic acid and a second protic acid, the first protic acid is more acidic and the anion is an inorganic anion or a short-chain anion, which can replace the original long-chain ligands in the quantum dots and passivate the surface defects of the quantum dots. The introduction of the second protic acid can stabilize the interface after the first protic acid treatment, avoid the acidity being too strong and destroying the structure of the quantum dots in the film, protect the quantum dots from damage, and reduce the surface roughness of the film.

[0195] Device Example 1

[0196] This embodiment of the device provides an optoelectronic device and its fabrication method. The fabrication method of the optoelectronic device includes the following steps:

[0197] Step S40: Provide ITO glass, use a cotton swab dipped in a small amount of soapy water to wipe the ITO surface to remove visible impurities, then use deionized water, acetone, ethanol and isopropanol for ultrasonic cleaning for 15 minutes, then blow dry with nitrogen gas and irradiate with UV for 15 minutes to form an ITO anode with a thickness of 120nm.

[0198] Step S41: Spin-coat PEDOT:PSS onto the ITO anode and anneal at 80°C for 30 min to form a hole injection layer;

[0199] Step S42: Spin-coat TFB onto the hole injection layer and anneal at 80°C for 30 minutes to form a hole transport layer;

[0200] Step S43: An octane dispersion of 30 mg / mL blue CdSeS / ZnS quantum dots (average particle size 7 nm) is placed on the hole transport layer. Oleic acid and oleylamine ligands are attached to the surface of the CdSeS / ZnS quantum dots. The spin coating speed is 3000 rpm and the time is 30 s. Then, it is annealed at 100 °C for 10 min to form a pre-fabricated light-emitting layer with a thickness of 50 nm.

[0201] Step S44: Introduce a mixed gas of Ar and O2 (Ar:O2 = 4:1) at a total flow rate of 20 sccm, and excite the pre-fabricated light-emitting layer by radio frequency discharge (power 100W, frequency 15MHz) for 8 minutes to generate plasma.

[0202] Step S45, according to 0.2 mmol / nm 2 A 3‰ hydrochloric acid (first protic acid) ethanol solution was spin-coated onto the side of the pre-fabricated light-emitting layer away from the hole transport layer at a spin speed of 3000 rpm. After standing for 10 min, it was annealed at 80℃ for 10 min, and the displaced oleic acid and oleylamine ligands were removed by washing. The solution was then applied at a concentration of 0.2 mmol / nm. 2 A 7‰ ethanol solution of acetic acid (second protic acid) was spin-coated onto the side of the pre-fabricated light-emitting layer away from the hole transport layer at a spin speed of 3000 rpm. After standing for 20 minutes, the mixture was annealed at 120°C for 20 minutes, and the residual substances were removed by cleaning to form the light-emitting layer.

[0203] Step S46: Introduce a mixed gas of Ar and Cl2 (Ar:Cl2 = 14:1), with a total flow rate of 15 sccm, and excite the luminescent layer by radio frequency discharge (power 200W, frequency 20MHz) to generate plasma for processing. Processing time is 5 min.

[0204] Step S47: Spin-coat a 20 mg / mL ethanol dispersion of ZnO (average particle size of 4 nm) onto the luminescent layer at a spin speed of 3000 rpm for 30 s, and then anneal at 80 °C for 30 min to form an electron transport layer with a thickness of 60 nm.

[0205] Step S48: After placing the target in a vacuum coating machine, Ag target material is vapor-deposited on the electron transport layer to form a cathode with a thickness of 100 nm.

[0206] Step S49: Encapsulate the device in an environment where both oxygen and water content are below 0.1 ppm to obtain the optoelectronic device.

[0207] Device Example 2

[0208] This device embodiment is basically the same as device embodiment 1, except that the first protic acid in step S45 is replaced with sulfuric acid in this device embodiment.

[0209] Device Example 3

[0210] This device embodiment is basically the same as device embodiment 1, except that the first protic acid in step S45 is replaced with trifluoroacetic acid in this device embodiment.

[0211] Device Example 4

[0212] This device embodiment is basically the same as device embodiment 1, except that the first protic acid in step S45 is replaced with trichloroacetic acid in this device embodiment.

[0213] Device Example 5

[0214] This device embodiment is basically the same as device embodiment 1, except that the second protic acid in step S45 is replaced with citric acid in this device embodiment.

[0215] Device Example 6

[0216] This device embodiment is basically the same as device embodiment 1, except that the second protic acid in step S45 is replaced with boric acid in this device embodiment.

[0217] Device Example 7

[0218] This device embodiment is basically the same as device embodiment 1, except that the second protic acid in step S45 is replaced with metasilicic acid in this device embodiment.

[0219] Device Example 8

[0220] This device embodiment is basically the same as device embodiment 1, except that step S46 is not performed in this device embodiment.

[0221] Device Example 9

[0222] This device embodiment is basically the same as device embodiment 1, except that step S44 is not performed in this device embodiment.

[0223] Device Example 10

[0224] This device embodiment is basically the same as device embodiment 1, except that steps S44 and S46 are not performed in this device embodiment.

[0225] Device Example 11

[0226] This embodiment of the device provides an optoelectronic device and its fabrication method. The fabrication method of the optoelectronic device includes the following steps:

[0227] Step S50: Evaporate Ag target material to form a cathode with a thickness of 100 nm;

[0228] Step S51: Spin-coat an ethanol dispersion of 20 mg / mL ZnO (average particle size of 4 nm) onto the anion layer at a spin speed of 3000 rpm for 30 s, and then anneal at 80 °C for 30 min to form an electron transport layer with a thickness of 60 nm.

[0229] Step S52: An octane dispersion of 30 mg / mL blue CdSeS / ZnS quantum dots (average particle size 7 nm) was placed on the electron transport layer. Oleic acid and oleylamine ligands were attached to the surface of the CdSeS / ZnS quantum dots. The spin coating speed was 3000 rpm and the time was 30 s. Then, it was annealed at 100 °C for 10 min to form a pre-fabricated light-emitting layer with a thickness of 50 nm.

[0230] Step S53: Introduce a mixed gas of Ar and O2 (Ar:O2 = 4:1) at a total flow rate of 20 sccm, and excite the pre-fabricated light-emitting layer by radio frequency discharge (power 100W, frequency 15MHz) for 8 minutes to generate plasma.

[0231] Step S54, according to 0.2 mmol / nm 2 A 3‰ solution of hydrochloric acid (first protic acid) in ethanol was spin-coated onto the side of the pre-fabricated luminescent layer furthest from the electron transport layer at a spin speed of 3000 rpm. After standing for 10 min, the mixture was annealed at 80 °C for 10 min, and then washed to remove the displaced oleic acid and oleylamine ligands. The solution was then applied at a concentration of 0.2 mmol / nm. 2 A 7‰ ethanol solution of acetic acid (second protic acid) was spin-coated onto the side of the pre-prepared luminescent layer away from the electron transport layer at a spin speed of 3000 rpm. After standing for 20 minutes, the mixture was annealed at 120°C for 20 minutes, and the residual substances were removed by cleaning to form the luminescent layer.

[0232] Step S55: Introduce a mixed gas of Ar and Cl2 (Ar:Cl2 = 14:1), with a total flow rate of 15 sccm, and excite the luminescent layer by radio frequency discharge (power 200W, frequency 20MHz) to generate plasma for processing. Processing time is 5 min.

[0233] Step S56: Spin-coat a 20 mg / mL NiO (average particle size of 4 nm) ethanol dispersion onto the light-emitting layer at a spin speed of 3000 rpm for 30 s, and then anneal at 80 °C for 30 min to form a hole transport layer with a thickness of 60 nm.

[0234] Step S57: ITO is deposited on the hole transport layer to form an anode with a thickness of 120 nm;

[0235] Step S58: Encapsulate in an environment where both oxygen and water content are below 0.1 ppm to obtain the optoelectronic device.

[0236] Device Example 12

[0237] This device embodiment is basically the same as device embodiment 11, except that the first protic acid in step S54 is replaced with nitric acid in this device embodiment.

[0238] Device Example 13

[0239] This device embodiment is basically the same as device embodiment 11, except that the first protic acid in step S54 is replaced with trifluoroacetic acid in this device embodiment.

[0240] Device Example 14

[0241] This device embodiment is basically the same as device embodiment 11, except that the first protic acid in step S54 is replaced with trichloroacetic acid in this device embodiment.

[0242] Device Example 15

[0243] This device embodiment is basically the same as device embodiment 11, except that the second protic acid in step S54 is replaced with malic acid in this device embodiment.

[0244] Device Example 16

[0245] This device embodiment is basically the same as device embodiment 11, except that the second protic acid in step S54 is replaced with phosphoric acid in this device embodiment.

[0246] Device Example 17

[0247] This device embodiment is basically the same as device embodiment 11, except that the second protic acid in step S54 is replaced with hydrogen cyanide in this device embodiment.

[0248] Device Example 18

[0249] This device embodiment is basically the same as device embodiment 11, except that step S55 is not performed in this device embodiment.

[0250] Device Example 19

[0251] This device embodiment is basically the same as device embodiment 11, except that step S53 is not performed in this device embodiment.

[0252] Device Example 20

[0253] This device embodiment is basically the same as device embodiment 11, except that steps S53 and S55 are not performed in this device embodiment.

[0254] Device Comparison Example 1

[0255] The comparative example of this device is basically the same as that of device embodiment 10, except that step S25 is not performed in this device embodiment.

[0256] Device Comparison Example 2

[0257] The comparative example of this device is basically the same as that of device embodiment 10, except that the second proton acid treatment in step S25 was not performed in this comparative example, only the first proton acid treatment was performed.

[0258] Device Comparison Example 3

[0259] The comparative example of this device is basically the same as that of device embodiment 20, except that step S54 is not performed in this comparative example.

[0260] The uniformity of electron transport layer formation and surface roughness Ra, current efficiency CE and lifespan T95@1000nit of the optoelectronic devices in Examples 1-10 and Comparative Examples 1-2 were tested, and the results are shown in Table 2.

[0261] The uniformity of hole transport layer formation and surface roughness Ra, current efficiency CE and lifespan T95@1000nit of the optoelectronic devices in Examples 11-20 and Comparative Example 3 were tested, and the results are shown in Table 3.

[0262] The surface roughness was obtained using atomic force microscopy (AFM).

[0263] Film uniformity was tested using a white light interferometer and calculated using the following formula: Film uniformity = (average film thickness ± 10 nm) / total film surface area of ​​the entire film × 100%.

[0264] Current efficiency was measured using a Keithley 2400 high-precision digital source meter, an Ocean Optic USB2000+ spectrometer, and an LS-160 luminance meter.

[0265] The test method for lifetime T95@1000nit is as follows: Under a constant current drive of 2mA, the time required for the brightness of the device to decrease to a certain percentage of its maximum brightness is defined as T95. This lifetime is the measured lifetime. To shorten the testing cycle, device lifetime testing is usually performed at high brightness by accelerating device aging, and the lifetime at high brightness is obtained by fitting the extended exponential decay brightness decay formula. For example, the lifetime at 1000nit is measured as T95@1000nit. The specific calculation formula is as follows:

[0266]

[0267] Among them, T95 L For longer lifespan at low brightness, T95 H For the measured lifetime under high brightness, L H To accelerate the device to its maximum brightness, L L The value is 1000 nits, and A is the acceleration factor. In this experiment, the lifetime of several groups of QLED devices under rated brightness was measured, and the value of A was found to be 1.7.

[0268] Table 2

[0269]

[0270] From Table 2, we can obtain:

[0271] As shown in Device Examples 1-10 and Comparative Examples 1-2, by treating the pre-fabricated light-emitting layer with a first protic acid and a second protic acid, the first protic acid, with its strong acidity and inorganic or short-chain anions, can replace the original long-chain ligands in the quantum dots, passivate the surface defects of the quantum dots, reduce the surface roughness of the light-emitting layer, and effectively shorten the electron transport path, thereby improving the current efficiency of the optoelectronic device. The first protic acid protonates the surface of the light-emitting layer, while the second protic acid stabilizes the structure of the quantum dots and causes the surface of the light-emitting layer to tend towards a change in polarity, which is beneficial for the deposition of N-type inorganic nanoparticles and improves the uniformity of its dispersion. This, in turn, helps to reduce the surface roughness of the electron transport layer and significantly improves the film uniformity. Through the combined treatment of the first and second protic acids, and further plasma treatment, the light-emitting layer can be cleaned, residual substances removed, and the tight bonding between the anions of the first protic acid and the quantum dots promoted, thus significantly improving the current efficiency of the optoelectronic device and extending its service life.

[0272] Table 3

[0273]

[0274] From Table 3, we can obtain:

[0275] As can be seen from Device Examples 11-20 and Device Comparative Example 3, by treating the pre-fabricated light-emitting layer with a first protic acid and a second protic acid, and then further preparing a hole transport layer formed by P-type inorganic nanoparticles, it is beneficial to reduce the surface roughness of the hole transport layer and significantly improve its film uniformity, thus promoting hole transport. The introduction of the second protic acid can stabilize the interface after the first protic acid treatment, preventing excessive acidity from damaging the structure of quantum dots in the light-emitting layer and protecting the quantum dots from damage. The optoelectronic devices provided in this application have high current efficiency and long service life.

[0276] The technical solutions provided by the embodiments of this application have been described in detail above. Specific examples have been used to illustrate the principles and implementation methods of this application. The description of the above embodiments is only for the purpose of helping to understand the method and core ideas of this application. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this application. Therefore, the content of this specification should not be construed as a limitation of this application.

Claims

1. A method for preparing a thin film, characterized in that, Includes the following steps: A preform is provided, wherein the material of the preform includes quantum dots; The pre-prepared membrane is treated sequentially with a first protic acid and a second protic acid to form a thin film; Wherein, the pKa of the second protic acid is greater than that of the first protic acid.

2. The preparation method according to claim 1, characterized in that, The pKa of the first protic acid is ≤1; The second protic acid has a pKa > 1; and / or The first protic acid is selected from one or more of the first inorganic acid and the first organic acid, and the first organic acid includes C1-C5 organic acids; The second protic acid is selected from one or more of a second inorganic acid and a second organic acid, wherein the second organic acid includes C1-C... 10 Organic acids.

3. The preparation method according to claim 2, characterized in that, The first inorganic acid includes one or more of hydrochloric acid, halogen acid, hydrohalogen acid, perhalogen acid, nitric acid, and sulfuric acid; the halogen acid includes one or more of chloric acid, bromic acid, and iodic acid; the hydrohalogen acid includes one or more of hydrobromic acid and hydroiodic acid; and the perhalogen acid includes one or more of perchloric acid and perbromic acid. The C1-C5 organic acids include C1-C5 polyhalogenated organic acids, and the C1-C5 polyhalogenated organic acids include one or more of trifluoroacetic acid and trichloroacetic acid; The second inorganic acid includes one or more of phosphoric acid, boric acid, hydrocyanic acid, metasilicic acid, and hypohalic acid; the hypohalic acid includes one or more of hypoiodic acid, hypochlorous acid, and hypobromic acid. The C1-C 10 Organic acids include C1-C 10 Aliphatic hydrocarbons, C1-C 10 Aromatic acids, C1-C 10 Hydroxy acids, C1-C 10 One or more of monohalogenated organic acids; the C1-C 10 Aliphatic hydrocarbon acids include one or more of formic acid, acetic acid, propionic acid, acrylic acid, and butyric acid, wherein the C1-C 10 Aromatic acids include benzoic acid, the C1-C 10 Hydroxy acids include one or more of citric acid and malic acid, wherein the C1-C 10 Monohalogenated organic acids include one or more of α-chlorobutyric acid, β-chlorobutyric acid, and γ-chlorobutyric acid.

4. The preparation method according to claim 1, characterized in that, The treatment using the first protic acid includes the following steps: providing a first protic acid solution, the first protic acid solution comprising the first protic acid and a first solvent; placing the first protic acid solution on the preformed membrane; and / or The treatment using the second protic acid includes the following steps: providing a second protic acid solution, the second protic acid solution comprising the second protic acid and a second solvent; and placing the second protic acid solution on the preform.

5. The preparation method according to claim 4, characterized in that, In the first protic acid solution, the mass concentration of the first protic acid is 2‰ to 5‰; In the second protic acid solution, the mass concentration of the second protic acid is 5‰ to 8‰; The first solvent and the second solvent each independently include a polar solvent; the polar solvent includes one or more of the following: water, trimethoxybutanol, diethylene glycol dimethyl ether, methanol, ethanol, propanol, butanol, ethylene glycol, isopropanol, glycerol, dimethyl sulfoxide, acetone, tetrahydrofuran, N,N-dimethylformamide, pyrrole, and butyric acid; The ratio of the molar number of the first protic acid to the surface area of ​​one side of the preform treated with the first protic acid is (0.1–0.5) mmol / nm. 2 ; The ratio of the molar number of the second protic acid to the surface area of ​​one side of the preform treated with the second protic acid is (0.1–0.5) mmol / nm. 2 ; The treatment time for the first protic acid is 5 min to 15 min; The treatment time for the second protic acid is 20 min to 40 min; After the first protic acid solution is placed on the preform, the process further includes: performing a first annealing; the temperature of the first annealing is 80℃~100℃; and the time of the first annealing is 10min~20min. After the second protic acid solution is placed on the preform, the process further includes: performing a second annealing; the temperature of the second annealing is 120℃~150℃; and the time of the second annealing is 20min~30min.

6. The preparation method according to claim 5, characterized in that, The process prior to the first protic acid treatment further includes: performing a first plasma treatment; the first plasma treatment includes: providing a first gas, exciting the first gas to generate plasma to treat the preformed membrane; and / or The process of treating with the second protic acid further includes: performing a second plasma treatment; the second plasma treatment includes: providing a second gas and exciting the second gas to generate plasma to treat the preform.

7. The preparation method according to claim 6, characterized in that, The first gas and the second gas each independently include one or more of argon, hydrogen, oxygen, chlorine, ammonia, nitrogen, CF4, and SF6; The flow rate of the first gas is 20 sccm to 50 sccm; The flow rate of the second gas is 10 sccm to 20 sccm; The method for exciting the first gas to generate plasma is a first radio frequency discharge method; the power of the first radio frequency discharge is 50W to 200W; the frequency of the first radio frequency discharge is 10MHz to 30MHz. The method for exciting the second gas to generate plasma is a second radio frequency discharge method; the power of the second radio frequency discharge is 100W to 300W; the frequency of the first radio frequency discharge is 10MHz to 30MHz.

8. The preparation method according to claim 1, characterized in that, The average particle size of the quantum dots is 2 nm to 10 nm. The quantum dots are selected from one or more of single-structure quantum dots, core-shell quantum dots, and perovskite quantum dots; the materials of the single-structure quantum dots, the core materials of the core-shell quantum dots, and the shell materials of the core-shell quantum dots are respectively selected from one or more of group II-VI compounds, group IV-VI compounds, group III-V compounds, and group I-III-VI compounds; the shell of the core-shell quantum dots includes one or more layers; the group II-VI compounds are selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, C One or more of dSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe, and HgZnSTe; the IV-VI group compounds are selected from SnS, SnSe, S The compounds are selected from one or more of the following: nTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe, and SnPbSTe; the III-V compounds are selected from GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, and AlNAs. One or more of AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs, and InAlPSb; wherein the group I-III-VI compounds are selected from one or more of CuInS2, CuInSe2, and AgInS2;The core-shell quantum dots are selected from one or more of CdSe / CdSeS / CdS, InP / ZnSeS / ZnS, CdZnSe / ZnSe / ZnS, CdSeS / ZnSeS / ZnS, CdSe / ZnS, CdSe / ZnSe / ZnS, ZnSe / ZnS, ZnSeTe / ZnS, CdSe / CdZnSeS / ZnS, and InP / ZnSe / ZnS; the perovskite quantum dots are made of doped or undoped inorganic perovskite semiconductors or organic-inorganic hybrid perovskite semiconductors; the inorganic perovskite semiconductor has the general structural formula AMX3, where A is Cs; + Ion, M is a divalent metal cation selected from Pb 2+ Sn 2+ Cu 2+ Ni 2+ Cd 2+ Cr 2+ Mn 2+ Co 2+ Fe 2+ 、Ge 2+ Yb 2+ Eu 2+ One or more of the following, where X is a halide anion selected from Cl... - ,Br - I - One or more of the following; the general structural formula of the organic-inorganic hybrid perovskite semiconductor is BMX3, where B is an organic amine cation selected from CH3(CH2). n-2 NH3 + Or [NH3(CH2)] n NH3] 2+ Where n≥2, M is a divalent metal cation selected from Pb 2+ Sn 2+ Cu 2+ Ni 2+ Cd 2+ Cr 2+ Mn 2+ Co 2+ Fe 2+ 、Ge 2+ Yb 2+ Eu 2+ One or more of the following, where X is a halide anion selected from Cl... - ,Br - I - One or more of the following; and / or In the pre-formed film, a first ligand is coordinated to the quantum dot; the first ligand includes one or more of the following: aliphatic amine ligands with 1 to 24 carbon atoms, fatty acid ligands with 1 to 24 carbon atoms, carboxylate ligands, phosphate ligands, halide ion ligands, thiol ligands with 1 to 24 carbon atoms, trialiphatic phosphine with 9 to 30 carbon atoms, arylphosphine with 12 to 30 carbon atoms, trialiphatic phosphine oxide with 9 to 30 carbon atoms, and triarylphosphine oxide with 18 to 30 carbon atoms; the aliphatic amine ligands with 1 to 24 carbon atoms include oleylamine, n-decylamine, octylamine, and dioctylamine. The ligand is selected from one or more of the following: amine, trioctylamine, dodecylamine, myristicamine, palmitamine, and stearylamine; the fatty acid ligand having 1 to 24 carbon atoms includes one or more of the following: oleic acid, decanoic acid, octanoic acid, dioctanoic acid, trioctanoic acid, dodecanoic acid, myristic acid, palmitic acid, stearic acid, thioglycolic acid, and mercaptopropionic acid; the carboxylate ligand is selected from one or more of the following: magnesium carboxylate ligand, calcium carboxylate ligand, aluminum carboxylate ligand, zirconium carboxylate ligand, lithium carboxylate ligand, sodium carboxylate ligand, and barium carboxylate ligand; the phosphate ligand is selected from the following: magnesium phosphate ligand, calcium phosphate ligand, aluminum phosphate ligand, zirconium phosphate ligand, lithium phosphate ligand, and phosphate. One or more of sodium ligands and barium phosphate ligands; the halide ion ligand is selected from one or more of fluoride ions, chloride ions, bromide ions, and iodide ions; the thiol ligand having 1 to 24 carbon atoms is selected from one or more of 1,2-ethanedithiol, propanethiol, butanethiol, octylthiol, dodecanethiol, octadecylthiol, benzenethiol, 1,2-benzenethiol, 1,3-benzenethiol, and 1,4-benzenethiol; the trialiphatic phosphine having 9 to 30 carbon atoms is selected from one or more of tripropylphosphine, tributylphosphine, tripentylphosphine, trihexylphosphine, triheptylphosphine, trioctylphosphine, trinonylphosphine, and tridecylphosphine. The arylphosphine with 12 to 30 carbon atoms is selected from one or more of diphenylphosphine, triphenylphosphine, tri(m-toluene)phosphine, tri(2-toluyl)phosphine, and tri(p-methylphenyl)phosphine; the trialilophosphine oxide with 9 to 30 carbon atoms is selected from one or more of tripropylphosphine oxide, tributylphosphine oxide, tripentylphosphine oxide, trihexylphosphine oxide, triheptylphosphine oxide, trioctylphosphine oxide, trinonylphosphine oxide, and tridecylphosphine oxide; the triarylphosphine oxide with 18 to 30 carbon atoms is selected from one or more of triphenylphosphine oxide, tri(m-toluene)phosphine oxide, tri(2-toluyl)phosphine oxide, and tri(p-methylphenyl)phosphine oxide. In the thin film, the quantum dots are coordinated with a second ligand, which includes one or more of inorganic acid radicals and C1-C5 organic acid radicals; the inorganic acid radicals include one or more of halide ions, halide ions, hydrohalide ions, perhalate ions, nitrate ions, and sulfate ions; the C1-C5 organic acid radicals include one or more of trifluoroacetate ions and trichloroacetate ions. The thickness of the pre-formed film is 20nm to 60nm; The surface roughness of the film is 0.7 nm to 1.5 nm.

9. A thin film, characterized in that, It is prepared by the preparation method according to any one of claims 1 to 8.

10. A method for fabricating an optoelectronic device, characterized in that, Includes the following steps: A device preform is provided, the device preform comprising a first electrode and a preformed light-emitting layer stacked together, the material of the preformed light-emitting layer comprising quantum dots; The pre-fabricated light-emitting layer is treated sequentially with a first protic acid and a second protic acid on the side away from the first electrode to form a light-emitting layer, wherein the pKa of the second protic acid is greater than that of the first protic acid; A second electrode is formed on the light-emitting layer to obtain a photoelectric device.

11. The preparation method according to claim 10, characterized in that, The pKa of the first protic acid is ≤1; The second protic acid has a pKa > 1; and / or The first protic acid is selected from one or more of a first inorganic acid and a first organic acid, wherein the first organic acid includes C1-C5 organic acids; optionally, the first inorganic acid includes one or more of hydrochloric acid, halogen acid, hydrohalogen acid, perhalogen acid, nitric acid, and sulfuric acid; the halogen acid includes one or more of chloric acid, bromic acid, and iodic acid; the hydrohalogen acid includes one or more of hydrobromic acid and hydroiodic acid; the perhalogen acid includes one or more of perchloric acid and perbromic acid; optionally, the C1-C5 organic acid includes C1-C5 polyhalogenated organic acids, wherein the C1-C5 polyhalogenated organic acids include one or more of trifluoroacetic acid and trichloroacetic acid; The second protic acid is selected from one or more of a second inorganic acid and a second organic acid, wherein the second organic acid includes C1-C... 10 Organic acids; optionally, the second inorganic acid includes one or more of phosphoric acid, boric acid, hydrocyanic acid, metasilicic acid, and hypohalic acid; the hypohalic acid includes one or more of hypoiodic acid, hypochlorous acid, and hypobromic acid; optionally, the C1-C 10 Organic acids include C1-C 10 Aliphatic hydrocarbons, C1-C 10 Aromatic acids, C1-C 10 Hydroxy acids, C1-C 10 One or more of monohalogenated organic acids; the C1-C 10 Aliphatic hydrocarbon acids include one or more of formic acid, acetic acid, propionic acid, acrylic acid, and butyric acid, wherein the C1-C 10 Aromatic acids include benzoic acid, the C1-C 10 Hydroxy acids include one or more of citric acid and malic acid, wherein the C1-C 10 Monohalogenated organic acids include one or more of α-chlorobutyric acid, β-chlorobutyric acid, and γ-chlorobutyric acid.

12. The preparation method according to claim 10, characterized in that, The first electrode and the second electrode each independently comprise one or more of the following: a metal electrode, a carbon electrode, a metal oxide electrode, and a composite electrode; the material of the metal electrode comprises one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb, and Mg; the material of the carbon electrode comprises one or more of graphite, carbon nanotubes, graphene, and carbon fibers; the material of the metal oxide electrode comprises one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO, MoO3, and AMO; the composite electrode comprises one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2, and TiO2 / Al / TiO2; and / or The device preform also includes a first charge carrier functional layer, which is located between the first electrode and the preformed light-emitting layer; and / or The step of setting a second electrode on the light-emitting layer includes: setting a second carrier functional layer on the light-emitting layer, and setting the second electrode on the second carrier functional layer.

13. The preparation method according to claim 12, characterized in that, The first carrier functional layer is a first hole functional layer, the second carrier functional layer is a first electron functional layer, the first electrode is an anode, and the second electrode is a cathode; or, the first carrier functional layer is a second electron functional layer, the second carrier functional layer is a second hole functional layer, the first electrode is a cathode, and the second electrode is an anode; wherein... The material of the second electronic functional layer includes one or more of the following: first doped metal oxide particles, first undoped metal oxide particles, IIB-VIA group semiconductor materials, IIIA-VA group semiconductor materials, and IB-IIIA-VIA group semiconductor materials. The material of the first undoped metal oxide particles includes one or more of ZnO, TiO2, SnO2, ZrO2, and Ta2O5. The metal oxide in the first doped metal oxide particles includes one or more of ZnO, TiO2, SnO2, ZrO2, Ta2O5, and Al2O3. The doping element in the first doped metal oxide particle includes one or more of Al, Mg, Li, Mn, Y, La, Cu, Ni, Zr, Ce, In, and Ga; the IIB-VIA group semiconductor material includes one or more of ZnS, ZnSe, and CdS; the IIIA-VA group semiconductor material includes one or more of InP and GaP; and the IB-IIIA-VIA group semiconductor material includes one or more of CuInS and CuGaS. The doping amount of the doping element in the first doped metal oxide particle is 0.1wt% to 20wt%. The material of the first hole functional layer includes organic p-type semiconductor materials or inorganic p-type semiconductor materials, wherein the organic p-type semiconductor material includes 4,4'-N,N'-dicarbazolyl-biphenyl, N,N'-diphenyl-N,N'-bis(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine, N,N'-bis(3-methylphenyl)-N,N'-bis(phenyl)-spiro, N,N' -Di(4-(N,N'-diphenyl-amino)phenyl)-N,N'-diphenylbenzidine, 4,4',4'-tris(N-carbazolyl)-triphenylamine, 4,4',4'-tris(carbazo-9-yl)triphenylamine, trichloroisocyanuric acid, 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazabenzophenanthrene, 4,4',4'-tris(N-3-methylphenyl-N-phenylamino)triphenylamine, poly[(9,9'-dioctylfluorene-2,7-diyl)-co-(4,4'-( N-(4-sec-butylphenyl)diphenylamine), poly(4-butylphenyl-diphenylamine), poly[bis(4-phenyl)(4-butylphenyl)amine], polyaniline, polypyrrole, poly(p-)phenylenevinylene, poly(phenylenevinylene), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylenevinylene], poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylenevinylene], copper phthalocyanine, aromatic tertiary amines, polynuclear aromatic tertiary amines, 4,4'-bis(p-carbazole) The following compounds are included: N,N,N',N'-tetraarylbenzidine, PEDOT, PEDOT:PSS and its derivatives, PEDOT:PSS derivatives doped with s-MoO3, poly(N-vinylcarbazole) and its derivatives, polymethacrylate and its derivatives, poly(9,9-octylfluorene) and its derivatives, poly(spirofluorene) and its derivatives, N,N'-bis(naphthyl-1-yl)-N,N'-diphenylbenzidine, spironolactone (NPB), microcrystalline cellulose, and tetracyanoquinone dimethyl ether.The inorganic P-type semiconductor material includes one or more of the following: nanocrystalline diamond, doped graphene, undoped graphene, second-doped metal oxide particles, second-undoped metal oxide particles, metal sulfides, metal selenides, and metal nitrides. The metal oxides in the second-doped and second-undoped metal oxide particles each independently include one or more of MoO3, WO3, NiO, CrO3, CuO, and V2O5. The doping element in the second-doped metal oxide particles includes one or more of Mo, W, Ni, Cr, Cu, and V. The metal sulfide includes one or more of CuS, MoS3, and WS3. The metal selenide includes one or more of MoSe3 and WSe3. The metal nitride includes P-type gallium nitride. The doping amount of the doping element in the second-doped metal oxide particles is 0.1 wt% to 20 wt%.

14. The preparation method according to claim 13, characterized in that, The material of the second carrier functional layer comprises inorganic nanoparticles, which include N-type inorganic nanoparticles or P-type inorganic nanoparticles; the material of the first electron functional layer comprises the N-type inorganic nanoparticles, or the material of the second hole functional layer comprises P-type inorganic nanoparticles; wherein... The average particle size of the N-type inorganic nanoparticles is 2 nm to 10 nm. The N-type inorganic nanoparticles include one or more of the following: first doped metal oxide particles, first undoped metal oxide particles, IIB-VIA group semiconductor materials, IIIA-VA group semiconductor materials, and IB-IIIA-VIA group semiconductor materials. The first undoped metal oxide particles are made of one or more of ZnO, TiO2, SnO2, ZrO2, and Ta2O5. The metal oxide in the first doped metal oxide particles is made of one or more of ZnO, TiO2, SnO2, ZrO2, Ta2O5, and Al2O3. The doping elements in the doped metal oxide particles include one or more of Al, Mg, Li, Mn, Y, La, Cu, Ni, Zr, Ce, In, and Ga; the IIB-VIA group semiconductor materials include one or more of ZnS, ZnSe, and CdS; the IIIA-VA group semiconductor materials include one or more of InP and GaP; and the IB-IIIA-VIA group semiconductor materials include one or more of CuInS and CuGaS. The doping amount of the doping elements in the first doped metal oxide particles is 0.1 wt% to 20 wt%. The average particle size of the P-type inorganic nanoparticles is 2 nm to 10 nm. The P-type inorganic nanoparticles include one or more of the following: second doped metal oxide particles, second undoped metal oxide particles, metal sulfides, metal selenides, and metal nitrides. The metal oxides in the second doped metal oxide particles and the second undoped metal oxide particles each independently include one or more of MoO3, WO3, NiO, CrO3, CuO, and V2O5. The doping element in the second doped metal oxide particles includes one or more of Mo, W, Ni, Cr, Cu, and V. The metal sulfide includes one or more of CuS, MoS3, and WS3. The metal selenide includes one or more of MoSe3 and WSe3. The metal nitride includes P-type gallium nitride. The doping amount of the doping element in the second doped metal oxide particles is 0.1 wt% to 20 wt%. The thickness of the first carrier functional layer is 20nm to 60nm; The thickness of the second carrier functional layer is 20 nm to 60 nm; The surface roughness of the second carrier functional layer is 0.5 nm to 1.5 nm.

15. The preparation method according to claim 12, characterized in that, The method for preparing the second carrier functional layer includes the following steps: providing an inorganic nanoparticle dispersion, wherein the inorganic nanoparticle dispersion includes inorganic nanoparticles and a third solvent; depositing the inorganic nanoparticle dispersion on the light-emitting layer to form the second carrier functional layer; wherein, In the inorganic nanoparticle dispersion, the mass concentration of the inorganic nanoparticles is 10 mg / mL to 50 mg / mL; The third solvent includes a polar solvent; the polar solvent includes one or more of the following: trimethoxybutanol, diethylene glycol dimethyl ether, methanol, ethanol, propanol, butanol, ethylene glycol, isopropanol, glycerol, dimethyl sulfoxide, acetone, tetrahydrofuran, N,N-dimethylformamide, pyrrole, and butyric acid. After the inorganic nanoparticle dispersion is placed on the luminescent layer, the process further includes: performing a third annealing; the temperature of the third annealing is 80℃~150℃, and the time of the third annealing is 5min~30min.

16. An optoelectronic device, characterized in that, It is prepared by the preparation method according to any one of claims 10 to 15.

17. The optoelectronic device as described in claim 16, characterized in that, The optoelectronic device includes a first electrode, a light-emitting layer, and a second electrode stacked together. The material of the light-emitting layer includes quantum dots. A second ligand is coordinated and connected to the quantum dots on the side of the light-emitting layer closest to the second electrode. The second ligand includes one or more of inorganic acid radical ions and C1-C5 organic acid radical anions. The inorganic acid radicals include one or more of the following: halide ions, halide ions, hydrohalide ions, perhalide ions, nitrate ions, and sulfate ions. The C1-C5 organic acid anions include one or more of trifluoroacetate ions and trichloroacetate ions.

18. A display device, characterized in that, It includes optoelectronic devices prepared by the preparation method according to any one of claims 10 to 15, or optoelectronic devices according to any one of claims 16 to 17.