Methods for fabricating hole transport layers and solar cells

By forming a transition metal oxide layer on the nickel oxide surface and then doping it with hydrogen, the intrinsic defects of the nickel oxide hole transport layer and the problem of uneven deposition of the self-assembled molecular layer were solved, thus improving the performance and stability of perovskite solar cells.

CN123124650APending Publication Date: 2026-11-17THREE GORGES (BEIJING) RENEWABLE ENERGY RES INST CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611622237.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, nickel oxide hole transport layers suffer from numerous intrinsic defects and uneven deposition of self-assembled molecular layers, which affect the open-circuit voltage and long-term stability of perovskite solar cells.

Method used

A transition metal oxide layer is formed on the surface of nickel oxide using an electron beam evaporation process, and hydrogen doping is performed in a gas atmosphere containing hydrogen and oxygen. Subsequently, a self-assembled molecular layer is formed, and the surface chemical state is controlled to achieve uniform deposition.

Benefits of technology

Effective passivation of nickel oxide defects improves hole transport efficiency, enhances the coverage and interface matching of self-assembled molecular layers, improves the open-circuit voltage, fill factor and photoelectric conversion efficiency of solar cells, and improves the long-term stability of the cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124650A_ABST
    Figure CN123124650A_ABST
Patent Text Reader

Abstract

This application provides a method for fabricating a hole transport layer and a method for fabricating a solar cell. The method for fabricating the hole transport layer includes: depositing a transition metal oxide layer using an electron beam evaporation process in a gaseous atmosphere containing a mixed gas and oxygen, wherein the mixed gas contains hydrogen and an inert gas, and the transition metal includes nickel; and forming a self-assembled molecular layer on the transition metal oxide layer to obtain the hole transport layer. This application introduces hydrogen doping into the electron beam evaporation process to fill oxygen vacancies and adjust the Fermi level, thereby reducing the defect state density. Furthermore, the self-assembled molecular layer enhances the hydroxyl binding sites on the substrate surface, promoting ordered molecular spreading and uniform film formation. This solves the problems of high intrinsic defect density and uneven deposition of the self-assembled molecular layer in the hole transport layer in the prior art. Simultaneously, it optimizes interface matching, reduces contact resistance, improves the open-circuit voltage, fill factor, and photoelectric conversion efficiency of the solar cell, and enhances the excellent long-term stability of the device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of photovoltaic technology, and more specifically, to a method for preparing a hole transport layer and a method for preparing a solar cell. Background Technology

[0002] Nickel oxide, due to its suitable band structure, exhibits excellent energy level matching between its conduction band bottom and valence band top and perovskite materials. It also possesses advantages such as good chemical stability, non-toxicity, and low cost, making it a promising hole transport material. However, direct contact between nickel oxide and perovskite leads to problems such as easy redox reactions, energy level mismatch, and high defect state density, affecting device performance. Crucially, nickel oxide itself contains numerous intrinsic defects, such as oxygen vacancies and nickel interstitial atoms, resulting in an extremely high defect state density on its thin film surface. These defects not only act as carrier recombination centers, reducing hole extraction efficiency, but also affect the deposition of subsequent functional layers.

[0003] In recent years, self-assembled molecular materials have become a research hotspot in hole transport layers due to their high hole mobility, tunable energy levels, and molecular-level interface modification capabilities. To achieve both the stability of nickel oxide and the excellent interfacial properties of self-assembled molecules, existing technologies have proposed constructing composite hole transport layers of nickel oxide / self-assembled molecules, namely, depositing a self-assembled monolayer (SAM) on the surface of nickel oxide, aiming to achieve synergistic effects.

[0004] However, in practical applications, nickel oxide films exhibit numerous intrinsic defects, with low density and highly uneven spatial distribution of surface chemically active sites. This directly hinders the formation of uniform chemical adsorption and ordered self-assembly of molecules on the nickel oxide surface. The result is significant agglomeration, voids, or disordered stacking of the self-assembled molecular film, with severely insufficient coverage and continuity, falling far short of the ideal monolayer coverage. This uneven deposition of self-assembled molecules weakens the intended interface passivation and energy level modulation effects, becoming a key bottleneck restricting the improvement of open-circuit voltage and long-term stability of perovskite solar cells.

[0005] Therefore, there is an urgent need in this field for a technique that can effectively passivate the intrinsic defects of nickel oxide and simultaneously increase and regulate its surface active binding sites, thereby guiding self-assembled molecules to achieve uniform, orderly, and high-coverage deposition.

[0006] The information disclosed above in the background section is only intended to enhance the understanding of the background art of the art described herein. Therefore, the background art may contain certain information that does not constitute prior art known to those skilled in the art in this country. Summary of the Invention

[0007] The main objective of this application is to provide a method for preparing a hole transport layer and a method for preparing a solar cell, so as to solve the problems of high intrinsic defect density and uneven deposition of self-assembled molecular layers in the prior art.

[0008] To achieve the above objectives, according to one aspect of this application, a method for preparing a hole transport layer is provided, comprising the following steps: oxidizing a transition metal to obtain a transition metal oxide layer by electron beam evaporation in a gaseous atmosphere including a mixed gas and oxygen, wherein the mixed gas includes hydrogen and an inert gas, and the transition metal includes nickel; forming a self-assembled molecular layer on the transition metal oxide layer to obtain the hole transport layer.

[0009] Optionally, the electron beam evaporation process includes the following steps: introducing the mixed gas and the oxygen into a chamber containing a substrate; using the transition metal as an evaporation source in the chamber, bombarding the transition metal with an electron beam to cause the transition metal to evaporate and react with the oxygen to form the transition metal oxide layer located on the substrate.

[0010] Optionally, prior to the step of introducing the mixed gas and the oxygen, the electron beam evaporation process further includes the step of: evacuating the chamber to reduce the vacuum level inside the chamber to below 5 × 10⁻⁶. -4 Pa.

[0011] Optionally, in the step of introducing the mixed gas and the oxygen, the hydrogen component in the mixed gas is 1%-5%, the flow rate of the mixed gas is 1-10 sccm, the flow rate of the oxygen is 5-20 sccm, and the pressure in the chamber is adjusted to not exceed 9 × 10⁻⁶. -3 Pa.

[0012] Optionally, the hydrogen component in the mixture is 2%-3%.

[0013] Optionally, the flow ratio of the oxygen to the mixed gas is between 3:1 and 5:1.

[0014] Optionally, during the bombardment of the transition metal by the electron beam, the accelerating voltage of the electron beam is 10-20kV, and the beam current of the electron beam is 50-100mA.

[0015] Optionally, during the process of bombarding the transition metal with the electron beam, the temperature of the substrate is 20-100°C, the evaporation rate is 0.1-1 nm / s, and the thickness of the transition metal oxide layer is 10-50 nm.

[0016] Optionally, the temperature of the substrate is 50-80°C.

[0017] According to another aspect of this application, a method for fabricating a solar cell is provided, comprising the following steps: providing a substrate, forming the hole transport layer on the substrate using the method for fabricating the hole transport layer described above; and sequentially forming a perovskite layer and an electron transport layer on the hole transport layer.

[0018] The hole transport layer preparation method provided by this application involves oxidizing a transition metal including nickel into a transition metal oxide using an electron beam evaporation process in a gaseous atmosphere containing hydrogen and oxygen. This allows for hydrogen doping of the transition metal oxide using hydrogen in the gaseous atmosphere during the evaporation process. In existing processes for preparing solar cells, when transition metal oxides containing nickel oxide are used as hole transport materials, these oxides generally possess a large number of intrinsic defects (such as oxygen vacancies), resulting in a high defect state density. These defects act as non-radiative recombination centers, reducing hole transport efficiency and severely limiting device performance. Furthermore, existing technologies introduce a self-assembled molecular layer (SAM) between the hole transport layer and the perovskite layer; however, the surface chemically active sites of the hole transport material are insufficient and unevenly distributed, leading to uneven SAM layer coverage. This application, by introducing hydrogen doping into transition metal oxides as described above, not only passivates defects in transition metal oxides such as nickel oxide and reduces defect state density, but also allows for the regulation of the chemical state of the thin film surface of transition metal oxides such as nickel oxide. This increases the density and uniformity of active hydroxyl binding sites on the substrate surface, thereby increasing the number of effective anchoring sites with SAM materials. The high density and uniformity of these sites promote the orderly spreading and uniform film formation of SAM molecules, resulting in a dense, continuous, and pinhole-free capping layer, significantly improving film uniformity and coverage. Furthermore, the capped SAM layer effectively optimizes interface energy level matching, reduces contact resistance, and suppresses non-radiative recombination. Therefore, applying the hole transport layer obtained by the above preparation method to perovskite and tandem solar cells can effectively improve the open-circuit voltage, fill factor, and photoelectric conversion efficiency of the cells, while simultaneously achieving excellent long-term stability under aging conditions such as damp heat and light exposure. Attached Figure Description

[0019] The accompanying drawings, which form part of this application, are used to provide a further understanding of this application. The illustrative embodiments and descriptions of this application are used to explain this application and do not constitute an undue limitation of this application. In the drawings: Figure 1 A schematic flowchart of a method for preparing a hole transport layer according to an embodiment of this application is shown; Figure 2 A flowchart illustrating another method for preparing a hole transport layer according to an embodiment of this application is shown. Figure 3A schematic flowchart of a method for fabricating a solar cell according to an embodiment of this application is shown; Figure 4 A schematic diagram of a single-junction solar cell according to an embodiment of this application is shown; and Figure 5 A schematic diagram of a tandem solar cell provided according to an embodiment of this application is shown.

[0020] The above figures include the following reference numerals: 10. Substrate; 20. Hole transport layer; 210. Transition metal oxide layer; 220. Self-assembled molecular layer; 30. Perovskite layer; 40. Passivation layer; 50. Electron transport layer; 60. Metal electrode; 70. Composite layer; 80. Buffer layer; 90. Transparent conductive layer; 100. Antireflection layer. Detailed Implementation

[0021] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of this application. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains.

[0022] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the exemplary embodiments according to this application. As used herein, the singular form is intended to include the plural form as well, unless the context clearly indicates otherwise. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.

[0023] It should be noted that the terms "first," "second," etc., in the specification, claims, and accompanying drawings of this application are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate for the embodiments of this application described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion; for example, a process, method, system, product, or apparatus that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to such processes, methods, products, or apparatus.

[0024] It should be understood that when an element (such as a layer, film, region, or substrate) is described as being "on" another element, the element may be directly on the other element, or there may be an intermediate element present. Furthermore, in the specification and claims, when an element is described as being "connected" to another element, the element may be "directly connected" to the other element, or "connected" to the other element via a third element.

[0025] As described in the background section, in the prior art, NiO x In the composite hole transport layer of / SAM, NiO x The surface defects and chemically active sites are few and unevenly distributed, making it difficult for SAM molecules to form uniform and ordered chemical adsorption, resulting in agglomeration and voids, insufficient coverage and integrity, weakening the interface passivation and energy level modulation effects, and introducing leakage current paths, which restricts the open-circuit voltage and stability of the device. In order to solve the problems of high intrinsic defect density and uneven deposition of self-assembled molecular layers (SAM) in the hole transport layer in the prior art, the embodiments of this application provide a method for preparing a hole transport layer and a method for preparing a solar cell.

[0026] The technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings.

[0027] Figure 1 This is a flowchart of a method for preparing a hole transport layer according to an embodiment of this application. Figure 1 As shown, the method includes: Step S11: In a gas atmosphere including a mixed gas and oxygen, the transition metal is oxidized by an electron beam evaporation process to obtain a transition metal oxide layer. The mixed gas includes hydrogen and an inert gas, and the transition metal includes nickel. Step S12: A self-assembled molecular layer is formed on the transition metal oxide layer to obtain a hole transport layer.

[0028] In existing technologies, transition metal oxides containing nickel oxide can be used as hole transport materials. However, transition metal oxides such as nickel oxide generally contain a large number of intrinsic defects (such as oxygen vacancies), resulting in a high defect state density. These defects act as non-radiative recombination centers, reducing hole transport efficiency and severely limiting device performance. In this embodiment, a transition metal containing nickel is oxidized into a transition metal oxide using an electron beam evaporation process in a gaseous atmosphere containing an argon-hydrogen mixture and oxygen. Hydrogen doping of the transition metal oxide is achieved using hydrogen in the evaporation process, thereby filling defects such as oxygen vacancies in transition metal oxides such as nickel oxide.

[0029] On the other hand, existing technologies introduce a self-assembled molecular layer (SAM) between the hole transport layer and the perovskite layer. However, the surface chemically active sites of the hole transport material are insufficient and unevenly distributed, leading to disordered adsorption of SAM molecules, easy aggregation or vacancies. Uneven coverage of the SAM layer causes the subsequently formed perovskite layer to directly contact the hole transport layer, and the anions (such as I) in the perovskite material... - Organic cations readily react with high oxidation state nickel species (such as Ni) in hole transport materials. 3+ Ni 4+ Unfavorable redox reactions can occur, thereby destroying the crystal structure of perovskite, leading to interface degradation, generating new defects, and causing device performance degradation. In this embodiment, after forming a transition metal oxide layer, a SAM layer is superimposed to obtain a hole transport layer. The introduction of hydrogen can regulate the chemical state of the thin film surface of transition metal oxides such as nickel oxide. By increasing the density and uniformity of active hydroxyl binding sites on the substrate surface, the effective anchoring quantity with the SAM material is increased. The high density and uniformity of sites promote uniform nucleation and orderly spreading of SAM molecules, forming a dense, continuous, and pinhole-free superimposed layer, significantly improving film uniformity and coverage. Furthermore, the superimposed SAM layer can effectively optimize interface energy level matching, reduce contact resistance, and suppress non-radiative recombination. Therefore, applying the hole transport layer obtained by the above preparation method to perovskite and tandem solar cells can effectively improve the open-circuit voltage, fill factor, and photoelectric conversion efficiency of the cells, while achieving excellent long-term stability of the cells under aging conditions such as damp heat and light exposure.

[0030] Exemplary embodiments of the method for preparing a hole transport layer according to the embodiments of this application will now be described in more detail. However, these exemplary embodiments may be implemented in many different forms and should be construed as being limited to the embodiments set forth herein. It should be understood that these embodiments are provided so that the disclosure of this application is thorough and complete, and that the concept of these exemplary embodiments is fully conveyed to those skilled in the art.

[0031] First, step S11 is performed: In a gaseous atmosphere including a mixed gas and oxygen, an electron beam evaporation process is used to oxidize the transition metal to obtain a transition metal oxide layer. The mixed gas contains hydrogen and an inert gas, and the transition metal includes nickel. The hydrogen in the above gaseous atmosphere forms a mixed gas with inert gases such as argon to reduce the concentration of hydrogen and oxygen in the gaseous atmosphere and prevent an explosive reaction after the hydrogen and oxygen are mixed.

[0032] In some alternative embodiments, the electron beam evaporation process described above includes the following steps: introducing a mixed gas and oxygen into a chamber containing a substrate, the mixed gas containing hydrogen and an inert gas (such as argon); using a transition metal as an evaporation source in the chamber, bombarding the transition metal with an electron beam to cause the transition metal to evaporate and react with oxygen to form a transition metal oxide layer on the substrate.

[0033] In the above optional embodiments, the substrate can be a transparent conductive substrate or a crystalline silicon substrate. Before placing the substrate in the chamber, it can be pretreated to obtain a clean substrate with controllable surface chemical state. The above transparent conductive substrate can include not only rigid oxide conductive glass (such as FTO, ITO), but also flexible polymer substrates (such as PET / ITO) coated with a transparent conductive layer to meet the requirements of flexible batteries.

[0034] Specifically, the aforementioned substrate can be a crystalline silicon solar cell. Even after texturing and diffusion processes have been completed, trace amounts of organic adsorbates or process volatiles may remain on the surface of the crystalline silicon solar cell (such as those used in perovskite / silicon stacks). Pretreatment of the substrate can include a UV ozone treatment step. UV light excites oxygen to generate ozone and active oxygen atoms, which can oxidize and decompose organic residues into volatile products such as CO2 and H2O at room temperature, thereby removing surface organic contaminants and obtaining a silicon surface with high cleanliness. Crystalline silicon solar cells are directly treated with UV ozone for 15-30 minutes.

[0035] The aforementioned substrate can also be a transparent conductive substrate, such as fluorine-doped tin oxide (FTO) or tin-doped indium oxide (ITO) glass. Both FTO and ITO are metal oxide surfaces, which readily adsorb low surface energy substances (organic adsorbates such as grease and hydrocarbons) from the environment to reduce their surface free energy. Pretreatment of the substrate can include multi-stage cleaning, which may include the following steps: First, the substrate is ultrasonically treated with acetone to remove non-polar oil stains. Acetone has a strong dissolving power for non-polar organic substances such as grease and wax, and the cavitation effect of ultrasound promotes the peeling and dispersion of contaminants from the surface. Next, the substrate is ultrasonically treated with ethanol to remove acetone residue and clean polar impurities. Ethanol can dissolve some polar organic substances and is miscible with acetone and water, effectively replacing residual acetone on the surface and introducing polar groups. Finally, the substrate is ultrasonically treated with deionized water to remove inorganic salts, particles, and water-soluble impurities. Ultrasonic treatment with deionized water can remove tiny particles and ionic contaminants (such as sodium) that adhered during glass cutting and storage. + Cl - (etc.), and remove residual ethanol from the previous stage, thereby further reducing surface contamination. For example, the transparent conductive substrate is ultrasonically cleaned sequentially with acetone, ethanol, and deionized water, with each cleaning session lasting 10-20 minutes.

[0036] After treating the substrate with ultraviolet ozone or performing multi-stage cleaning, the substrate can be first dried with nitrogen to prevent natural evaporation and leave solute residue, while maintaining the dryness of the cleaned surface. Then, the substrate is cleaned with ultraviolet ozone. Ultraviolet ozone forms oxygen-containing polar groups (such as hydroxyl and peroxy groups) on the substrate surface, which not only improves surface wettability, making it easier for subsequent vapor-deposited materials to cover the substrate evenly, but also initially increases the surface chemical adsorption sites, enhancing the adhesion between the vapor-deposited film and the substrate, making it less prone to detachment. For example, after drying the substrate with nitrogen, it is cleaned with ultraviolet ozone for 15-30 minutes. Finally, the substrate is transferred to the sample holder in the vacuum chamber of the electron beam evaporation equipment. The pretreated substrate surface is smooth and free of contamination.

[0037] In the above optional embodiments, prior to the step of introducing the mixed gas and oxygen, the electron beam evaporation process further includes the following step: evacuating the chamber to reduce the vacuum level inside the chamber to below 5 × 10⁻⁶. -4 Pa.

[0038] Specifically, the pressure inside the chamber is reduced to 5 × 10 before the reaction gas is introduced. -4 Vacuuming below Pa effectively eliminates interference from air, water vapor, and trace impurities in the environment, thereby improving the initial purity of the transition metal oxide layer and avoiding increased surface roughness or compositional deviation caused by background gas phase contamination.

[0039] In the above-mentioned optional embodiments, an argon-hydrogen mixture and oxygen can be simultaneously introduced into the vacuum chamber to form a gaseous atmosphere containing hydrogen and oxygen within the chamber. The hydrogen in the argon-hydrogen mixture is used to fill oxygen vacancies in the subsequently formed transition metal oxides such as nickel oxide and reduce the defect state density. In addition, the introduction of hydrogen is also used to regulate the chemical state of the transition metal oxide layer surface and increase the number and uniformity of effective hydroxyl binding sites.

[0040] In the above-mentioned optional embodiments, by introducing inert gases such as argon as buffer media and coordinating with electron beam bombardment, the direct bombardment of the substrate surface by high-energy electrons is effectively shielded, thereby ensuring the stability of the transition metal evaporation source and improving the compactness, high purity and uniform deposition characteristics of the final transition metal oxide layer.

[0041] In the step of introducing a mixed gas and oxygen into the chamber containing the substrate, this embodiment can further optimize the above-mentioned effect by adjusting the following specific parameters: the hydrogen gas fraction in the mixed gas can be 1%-5%, such as 1%, 2%, 3%, 4%, and 5%; the flow rate of the mixed gas can be 1-10 sccm, such as 1 sccm, 3 sccm, 5 sccm, 8 sccm, and 10 sccm; the oxygen flow rate can be 5-20 sccm, such as 5 sccm, 8 sccm, 10 sccm, 12 sccm, 15 sccm, 18 sccm, and 20 sccm; and the pressure in the chamber is adjusted not to exceed 9 × 10⁻⁶. -3 Pa.

[0042] Specifically, by setting the mixed gas flow rate (1-10 sccm), the oxygen flow rate (5-20 sccm), and controlling the pressure inside the chamber to not exceed 1×10 -3 Pa can precisely control the rate of oxidation reaction and the oxygen partial pressure balance, effectively improving the growth quality of the thin film. In addition, the specific hydrogen content also promotes the optimization of the electronic state density on the substrate surface, enhances the interfacial bonding between the transition metal oxide layer and the substrate, and is conducive to the reliable stacking of subsequent functional layers on it.

[0043] Specifically, in the step of introducing the mixed gas and oxygen, by setting the hydrogen gas integral in the mixed gas to 1%-5%, the defect state density of the thin film is effectively reduced, and the electronic state density and chemical bonding characteristics of the substrate surface are adjusted. Thus, the specific gas environment not only improves the formation quality of the thin film, making the film layer more uniform and dense, but also enhances the interfacial bonding force between the transition metal oxide and the substrate, thereby improving the reliability of the thin film in the device stacking process.

[0044] This application employs electron beam evaporation technology, combined with a specific hydrogen content (1%-5%) mixed gas to oxygen flow rate ratio and chamber pressure control (not exceeding 9×10). -3 This process (Pa) allows for precise control of the oxidation reaction rate and oxygen partial pressure balance, effectively reducing the defect state density of the thin film and significantly improving film uniformity and coverage. Furthermore, it eliminates the need for complex subsequent surface modification steps and exhibits excellent stability, making it highly suitable for industrial mass production and large-scale manufacturing applications.

[0045] For example, the hydrogen component in the aforementioned mixed gas is 2%-3%. This specific range achieves synergistic optimization while improving hydrogen doping efficiency. Specifically, on the one hand, this specific range effectively fills oxygen vacancies in transition metal oxides and modulates the Fermi level, effectively reducing defect state density; on the other hand, this specific range effectively avoids the degradation of film conductivity caused by excessive hydrogen. More importantly, the aforementioned concentration range can regulate the chemical state distribution on the surface of transition metal oxides such as nickel oxide, maximizing the density and uniformity of binding sites for active hydroxyl groups on the substrate surface. This provides ideal surface conditions for the orderly arrangement of subsequent SAM layers, not only promoting uniform nucleation and dense spreading of molecules on the substrate but also ensuring the final formation of a dense, continuous, and pinhole-free capping layer. Through the above synergistic optimization, the film formation quality is significantly improved, and the interface energy level matching is further optimized, effectively reducing contact resistance and suppressing non-radiative recombination.

[0046] Furthermore, in the step of introducing the mixed gas and oxygen, the flow ratio of oxygen to the mixed gas is between 3:1 and 5:1, such as 3:1, 16:5, 7:2, 18:5, 4:1, 22:5, 9:2, 24:5, and 5:1. By setting the flow ratio of oxygen to the mixed gas to meet the above range, not only is the stoichiometry of transition metal oxides such as nickel oxide regulated and the balance between hydrogen doping and conductivity optimized, but the density and uniformity of binding sites of active hydroxyl groups on the substrate surface are also maximized, thereby promoting the uniform nucleation, dense spreading, and dense continuous coverage of self-assembled molecules on the substrate.

[0047] In the embodiments of this application, during the formation of transition metal oxides such as nickel oxide, trace amounts of other metal elements (such as Al) are introduced in addition to the H2 / O2 atmosphere. 3+ Zr 4+ or Mg 2+ Co-doping of transition metal oxides (such as NiO) is achieved by utilizing the competitive binding of metal ions with different valence states to oxygen vacancies, thereby further stabilizing transition metal oxides (such as NiO). x ) lattice structure. For example, Al doping may help improve NiO. x Thermal stability is crucial to prevent phase transitions or oxidation state increases (such as Ni) during subsequent high-temperature annealing of SAM film formation. 3+ / Ni 4+ (Generation).

[0048] After introducing a mixture of gas and oxygen into the chamber, during the bombardment of the transition metal with an electron beam, the accelerating voltage of the electron beam can be 10-20 kV, such as 10 kV, 12 kV, 15 kV, 18 kV, and 20 kV; the beam current can be 50-100 mA, such as 50 mA, 60 mA, 70 mA, 80 mA, 90 mA, and 100 mA. By setting the accelerating voltage and beam current of the electron beam to meet the above ranges, the evaporation rate is controlled within the optimal controllable range.

[0049] Meanwhile, during the electron beam bombardment of the transition metal, the substrate temperature can range from 20 to 100°C, such as 20°C, 35°C, 50°C, 65°C, 80°C, and 100°C; the deposition rate can range from 0.1 to 1 nm / s, such as 0.1 nm / s, 0.3 nm / s, 0.5 nm / s, 0.8 nm / s, and 1 nm / s; and the thickness of the transition metal oxide layer can range from 10 to 50 nm, such as 10 nm, 20 nm, 30 nm, 40 nm, and 50 nm. By setting specific deposition rates in conjunction with temperature ranges, the film formation conditions are further refined, ensuring uniform oxide layer growth and a dense structure, and directly improving the long-term reliability and lifespan of the device under high-temperature operation.

[0050] Preferably, the substrate temperature is 50-80°C. Compared to a wider temperature range, this preferred range further promotes the formation of an ordered and dense film of the transition metal oxide layer on the substrate surface. This specific temperature range can promote the adsorption and chemical bonding of hydrogen atoms on the transition metal oxide surface. More importantly, it guides the directional aggregation of hydrogen elements to the film surface, making hydrogen atoms rich in defects and surface active sites. This not only improves the overall film density and effectively reduces defects in the bulk phase, but also enhances the binding capacity of hydroxyl groups on the substrate surface. This provides ideal anchoring conditions for the subsequent ordered arrangement of self-assembled molecular layers (SAMs), enabling them to cover the oxide surface more tightly and uniformly.

[0051] This application employs an electron beam evaporation process. During evaporation, the substrate temperature is low, and an argon-hydrogen mixture and oxygen are simultaneously introduced into the vacuum chamber. This process eliminates the need for high-temperature annealing and is compatible with flexible substrates and various solar cell structures (such as perovskite single-junction and silicon tandem layers). Furthermore, this method is suitable for fabricating hole transport layers in optoelectronic devices such as organic light-emitting diodes (OLEDs), demonstrating broad application prospects.

[0052] After obtaining the transition metal oxide layer using the electron beam evaporation process in step S11, step S12 is performed: a self-assembled molecular layer (SAM) is formed on the transition metal oxide layer to obtain a hole transport layer including the transition metal oxide layer and the SAM.

[0053] In step S12 above, a SAM precursor solution can be coated onto the surface of the transition metal oxide layer using spin coating and then annealed. Taking a nickel oxide thin film as the transition metal oxide layer as an example, after preparing a hydrogen-doped nickel oxide thin film on a glass substrate or a crystalline silicon substrate, the film is allowed to cool naturally to room temperature. Nitrogen gas is then slowly introduced into the chamber to atmospheric pressure, and the chamber is opened to remove the sample. SAM is dissolved in ethanol, and a SAM layer is prepared using spin coating at a concentration of 0.5-1.0 mg / ml and a spin coating speed of 3000-5000 rpm. After spin coating, the layer is annealed at 100°C for 10 min.

[0054] It should be noted that the transition metal is bombarded with an electron beam to cause it to evaporate and react with oxygen, forming a transition metal oxide layer on the substrate. The transition metal can be nickel, or it can include other types of transition metals besides nickel, such as cobalt and manganese.

[0055] In some alternative embodiments, multiple transition metals are sequentially bombarded with an electron beam in a gaseous atmosphere containing a mixture of gases and oxygen, causing the transition metals to evaporate and react with oxygen sequentially, forming a heterojunction structure of transition metal oxide stacks on a substrate. Specifically, in a gaseous atmosphere containing an argon-hydrogen mixture and oxygen, nickel and cobalt (or manganese) can be bombarded with an electron beam separately, causing the transition metals to evaporate and react with oxygen, forming NiO on a substrate. x / CoO x or NiO x / MnO x The heterojunction structure.

[0056] For example, the aforementioned transition metal comprises metallic nickel and metallic cobalt, and the transition metal is sequentially oxidized onto NiO using an electron beam evaporation process. x CoO grown on the surface of the layer x Layer, to obtain a transition metal oxide stack, NiO x The thickness of the layer is equal to or greater than CoO x Twice the thickness of the layer, utilizing its specific electron transport properties to assist hole extraction, while CoO x It has different surface defect chemical properties and can form a more stable interface with SAM.

[0057] This embodiment relates to a specific method for preparing a hole transport layer, such as... Figure 2 As shown, it includes the following steps: Step S1: Select a transparent conductive substrate or a crystalline silicon battery. Treat the crystalline silicon battery with ultraviolet ozone for 15-30 minutes, or perform multi-stage cleaning on the transparent conductive substrate, including ultrasonic cleaning with acetone, ultrasonic cleaning with ethanol, and ultrasonic cleaning with deionized water, with each cleaning session lasting 10-20 minutes. Step S2: Evacuate the chamber to reduce the vacuum level inside the chamber to below 5 × 10⁻⁶. -4 Pa; Step S3: Introduce a mixed gas containing hydrogen and argon into the chamber containing the substrate. The hydrogen component in the mixed gas can be 1%-5%, the flow rate of the mixed gas can be 1-10 sccm, and the flow rate of the oxygen can be 5-20 sccm. Adjust the pressure in the chamber to not exceed 9 × 10⁻⁶ ppm. -3 Pa; Step S4: In the chamber, the transition metal is used as the evaporation source. The transition metal is bombarded by an electron beam to evaporate and react with oxygen to form a transition metal oxide layer on the substrate. The accelerating voltage of the electron beam is 10-20kV, the beam current of the electron beam is 50-100mA, the temperature of the substrate is 20-100℃, the evaporation rate is 0.1-1nm / s, and the thickness of the transition metal oxide layer is 10-50nm. Step S5: Prepare a self-assembled molecular layer by spin coating at a concentration of 0.5-1.0 mg / ml and a spin coating speed of 3000-5000 rpm. After spin coating, anneal at 100℃ for 10 min.

[0058] According to embodiments of this application, a method for preparing a solar cell is also provided. Figure 3 This is a flowchart of a method for fabricating a solar cell according to an embodiment of this application. Figure 3 As shown, the method includes: Step S21: Provide a substrate and form a hole transport layer on the substrate using the hole transport layer preparation method described in the above embodiments; Step S22: A perovskite layer and an electron transport layer are sequentially formed on the hole transport layer.

[0059] In this embodiment, under a gaseous atmosphere including hydrogen and oxygen, an electron beam evaporation process is used to oxidize a transition metal, including nickel, into a transition metal oxide. The hydrogen in the gaseous atmosphere is used during the evaporation process to achieve hydrogen doping of the transition metal oxide. By introducing this hydrogen doping, not only can oxygen vacancies in transition metal oxides such as nickel oxide be filled, but energy levels can also be adjusted, and the defect state density can be reduced. Ultimately, when this fabrication process is applied to solar cells, it can effectively improve the open-circuit voltage, fill factor, and photoelectric conversion efficiency of the cell, while also endowing the device with excellent long-term stability under aging conditions such as humidity, heat, and light.

[0060] First, step S21 is performed: a substrate is provided, and a transition metal oxide layer is obtained by electron beam evaporation in a gas atmosphere including hydrogen and oxygen. The transition metal includes nickel, and a self-assembled molecular layer is formed on the transition metal oxide layer to form a hole transport layer on the substrate.

[0061] Specifically, the substrate can be a transparent conductive substrate or a crystalline silicon substrate. Before placing the substrate in the chamber, it can be pretreated to obtain a clean substrate with controllable surface chemical state. The transparent conductive substrate includes not only rigid oxide conductive glass (such as FTO, ITO), but also flexible polymer substrates (such as PET / ITO) coated with a transparent conductive layer to meet the requirements of flexible batteries.

[0062] In step S21 above, the electron beam evaporation process may include the following steps: introducing a mixed gas and oxygen into a chamber in which a substrate is placed, the mixed gas containing hydrogen and argon; using a transition metal as an evaporation source in the chamber, bombarding the transition metal with an electron beam to cause the transition metal to evaporate and react with oxygen to form a transition metal oxide layer on the substrate.

[0063] Specifically, an argon-hydrogen mixture and oxygen can be simultaneously introduced into the vacuum chamber to create a gaseous atmosphere containing hydrogen and oxygen. Hydrogen, as a key dopant, can fill oxygen vacancies in transition metal oxides and regulate carrier concentration, effectively reducing defect state density; at the same time, it can regulate surface chemical states, maximizing the increase of substrate hydroxyl binding sites, providing ideal anchoring conditions for the subsequent orderly spread of SAM layers.

[0064] In step S21 above, a SAM precursor solution can be coated onto the surface of the transition metal oxide layer using spin coating and then annealed. Taking a nickel oxide thin film as the transition metal oxide layer as an example, after preparing a hydrogen-doped nickel oxide thin film on a glass substrate or a crystalline silicon substrate, the film is allowed to cool naturally to room temperature. Nitrogen gas is then slowly introduced into the chamber to atmospheric pressure, and the chamber is opened to remove the sample. SAM is dissolved in ethanol, and a SAM layer is prepared using spin coating.

[0065] After the hole transport layer in step S21 is prepared, step S22 is performed: a perovskite layer and an electron transport layer are sequentially formed on the hole transport layer.

[0066] The preparation method in this embodiment can be used to prepare a single-junction perovskite solar cell. In some optional embodiments, step S22 includes: the substrate 10 is a transparent conductive substrate; a transition metal oxide layer 210 and a self-assembled molecular layer 220 are sequentially formed on the transparent conductive substrate; after the hole transport layer 20 is prepared, a perovskite layer 30 and a passivation layer 40 are prepared by spin coating; subsequently, an electron transport layer 50 is prepared on the passivation layer 40; finally, a metal electrode 60 is directly thermally vapor-deposited to obtain the desired result. Figure 4 The single-junction perovskite solar cell device shown.

[0067] For example, after preparing a hydrogen-doped nickel oxide thin film on a glass substrate, a SAM layer is prepared by spin coating to complete the hole transport layer; then, a perovskite layer with a thickness of 600-1000 nm is prepared on the SAM layer by spin coating, and the film composition is MA. z FA x Cs 1-x-z Pb(I y Br 1-y )3, where x is 0.5-0.8, y is 0.1-0.3, z is 0.05-0.25, the band gap is 1.66-1.68 eV, the solution concentration is 1.6-1.8 M, and heating is performed after spin coating to obtain a perovskite film; a passivation layer is prepared on the perovskite layer by spin coating using EDAI2 or PDAI2 at a concentration of 0.5 mg / ml, and annealing is performed after spin coating; subsequently, C is prepared by thermal evaporation. 60 The layer serves as an electron transport layer with a thickness of 10-30 nm. Finally, based on a glass substrate, a single-junction perovskite solar cell is fabricated by directly thermally evaporating metal electrodes, thus completing the fabrication of the single-junction perovskite solar cell device.

[0068] In the above example, the process conditions for fabricating a single-junction perovskite solar cell may include: preparing a C60 layer by vacuum evaporation with a vacuum degree of 5 × 10⁻⁶. -4 Below Pa, the evaporation rate is 0.2-0.5 Å / s; the BCP layer is prepared by vacuum evaporation deposition at a vacuum degree of 5 × 10⁻⁶. -4 Below Pa, the evaporation rate is 0.2-0.5 Å / s; Ag electrodes are prepared by vacuum deposition at a vacuum level of 5 × 10⁻⁶. -4 Below Pa, the evaporation rate is 0.5-5 Å / s.

[0069] The preparation method in this embodiment can also be used to prepare tandem solar cells. In some optional embodiments, step S22 includes: using a crystalline silicon bottom cell as a substrate 10, sequentially forming a transition metal oxide layer 210 and a self-assembled molecular layer 220 on the crystalline silicon bottom cell; after completing the preparation of the hole transport layer 20, sequentially preparing a perovskite layer 30 and a passivation layer 40 by spin coating; subsequently preparing an electron transport layer 50 by thermal evaporation on the passivation layer 40; depositing a buffer layer 80 on the electron transport layer and preparing a transparent conductive layer 90 by magnetron sputtering; and sequentially preparing a metal grid line (metal electrode 60) and an antireflection layer 100 by thermal evaporation, to obtain the desired result. Figure 5 The stacked battery device shown is an example. Figure 5 As shown, the above-mentioned stacked battery device may further include a composite layer 70 located between the substrate 10 and the hole transport layer 20. The composite layer 70 is made of a conductive metal oxide, such as ITO, IZO, ICO, etc., and can be prepared by magnetron sputtering.

[0070] For example, after preparing a hydrogen-doped nickel oxide thin film on a glass substrate, a SAM layer is prepared by spin coating to complete the hole transport layer; then, a perovskite layer with a thickness of 600-1000 nm is prepared on the SAM layer by spin coating, and the film composition is MA. z FA x Cs 1-x-z Pb(I y Br 1-y )3, where x is 0.5-0.8, y is 0.1-0.3, z is 0.05-0.25, the band gap is 1.66-1.68 eV, the solution concentration is 1.6-1.8 M, and heating is performed after spin coating to obtain a perovskite film; a passivation layer is prepared on the perovskite layer by spin coating using EDAI2 or PDAI2 at a concentration of 0.5 mg / ml, and annealing is performed after spin coating; subsequently, C is prepared by thermal evaporation. 60 A layer of SnO2 with a thickness of 15-30 nm was prepared using atomic layer deposition. 60 The layer and the SnO2 layer together serve as the electron transport layer; then, the IZO layer with a thickness of 40-100 nm is prepared by magnetron sputtering; finally, the metal grid electrode and the MgF2 antireflection layer are prepared by thermal evaporation to complete the fabrication of the tandem battery device.

[0071] In the above example, the process conditions for fabricating the tandem battery may include: preparing the C60 layer by vacuum evaporation, with a vacuum degree of 5 × 10⁻⁶. -4 Below Pa, the evaporation rate is 0.2-0.5 Å / s; SnO2 is deposited at atomic layer deposition temperature of 80℃; IZO layers are prepared by magnetron sputtering at a sputtering power of 50 W and a sputtering rate of 0.3-0.5 Å / s; Ag gate lines are prepared by vacuum evaporation at a vacuum degree of 5 × 10⁻⁶. -4Below Pa, the evaporation rate is 0.5-5 Å / s; MgF2 is prepared by vacuum deposition at a vacuum degree of 5 × 10⁻⁶. -4 Below Pa, the evaporation rate is 0.5-1 Å / s.

[0072] The preparation method of the hole transport layer and the preparation method of the solar cell described above in this application will be further explained below with reference to specific embodiments and comparative examples.

[0073] Example 1 This embodiment provides a method for preparing a hole transport layer, including the following steps: Select a 2.5×2.5cm ITO glass substrate, and clean it sequentially with acetone, ethanol and deionized water by ultrasonic cleaning for 15min each. After drying with nitrogen, clean it with ultraviolet ozone for 30min. Transfer the substrate to the sample holder in the vacuum chamber of the electron beam evaporation equipment. Nickel particles with a purity of 99.99% were loaded into a graphite crucible, the vacuum chamber was closed, and the vacuum was evacuated to a degree of 2 × 10⁻⁶. -4 Pa; An argon-hydrogen mixture and oxygen are introduced into the chamber. The hydrogen component of the argon-hydrogen mixture is 3%, the flow rate of the argon-hydrogen mixture is 3 sccm, and the flow rate of the oxygen is 12 sccm. The chamber pressure is then adjusted to 5 × 10⁻⁶. -3 Pa; The electron beam generator was started with an accelerating voltage of 15kV, a beam current of 100mA, a substrate temperature of 60℃, and a evaporation rate of 0.1nm / s. When the thickness of the nickel oxide film reached 20nm, the evaporation was stopped to obtain a hydrogen-doped nickel oxide film. The film was then vacuum cooled for 10min, and nitrogen gas was introduced to bring it to atmospheric pressure before it was removed. SAM was dissolved in ethanol to obtain a SAM precursor solution with a concentration of 0.5 mg / ml. A SAM layer was prepared on a hydrogen-doped nickel oxide film by spin coating at a speed of 4000 rpm. After spin coating, the film was annealed at 100 °C for 10 min.

[0074] Example 2 This embodiment provides a method for preparing a hole transport layer, including the following steps: Select a 2.5×2.5cm ITO glass substrate, and clean it sequentially with acetone, ethanol and deionized water by ultrasonic cleaning for 15min each. After drying with nitrogen, clean it with ultraviolet ozone for 30min. Transfer the substrate to the sample holder in the vacuum chamber of the electron beam evaporation equipment. Nickel particles with a purity of 99.99% were loaded into a graphite crucible, the vacuum chamber was closed, and the vacuum was evacuated to a degree of 2 × 10⁻⁶. -4 Pa; An argon-hydrogen mixture and oxygen are introduced into the chamber. The hydrogen component of the argon-hydrogen mixture is 3%, the flow rate of the argon-hydrogen mixture is 6 sccm, and the flow rate of the oxygen is 12 sccm. The chamber pressure is adjusted to 5 × 10⁻⁶. -3 Pa; The electron beam generator was started with an accelerating voltage of 15kV, a beam current of 100mA, a substrate temperature of 60℃, and a evaporation rate of 0.1nm / s. When the thickness of the nickel oxide film reached 20nm, the evaporation was stopped to obtain a hydrogen-doped nickel oxide film. The film was then vacuum cooled for 10min, and nitrogen gas was introduced to bring it to atmospheric pressure before it was removed. SAM was dissolved in ethanol to obtain a SAM precursor solution with a concentration of 0.5 mg / ml. A SAM layer was prepared on a hydrogen-doped nickel oxide film by spin coating at a speed of 4000 rpm. After spin coating, the film was annealed at 100 °C for 10 min.

[0075] Example 3 This embodiment provides a method for preparing a hole transport layer, including the following steps: Select a 2.5×2.5cm ITO glass substrate, and clean it sequentially with acetone, ethanol and deionized water by ultrasonic cleaning for 15min each. After drying with nitrogen, clean it with ultraviolet ozone for 30min. Transfer the substrate to the sample holder in the vacuum chamber of the electron beam evaporation equipment. Nickel particles with a purity of 99.99% were loaded into a graphite crucible, the vacuum chamber was closed, and the vacuum was evacuated to a degree of 4 × 10⁻⁶. -4 Pa; An argon-hydrogen mixture and oxygen are introduced into the chamber. The hydrogen component of the argon-hydrogen mixture is 3%, the flow rate of the argon-hydrogen mixture is 2 sccm, and the flow rate of the oxygen is 20 sccm. The chamber pressure is adjusted to 5 × 10⁻⁶. -3 Pa; The electron beam generator was started with an accelerating voltage of 15kV, a beam current of 100mA, a substrate temperature of 60℃, and a evaporation rate of 0.1nm / s. When the thickness of the nickel oxide film reached 20nm, the evaporation was stopped to obtain a hydrogen-doped nickel oxide film. The film was then vacuum cooled for 10min, and nitrogen gas was introduced to bring it to atmospheric pressure before it was removed. SAM was dissolved in ethanol to obtain a SAM precursor solution with a concentration of 0.5 mg / ml. A SAM layer was prepared on a hydrogen-doped nickel oxide film by spin coating at a speed of 4000 rpm. After spin coating, the film was annealed at 100 °C for 10 min.

[0076] Example 4 This embodiment provides a method for preparing a hole transport layer, which differs from Embodiment 1 in that: An argon-hydrogen mixture and oxygen are introduced into the chamber. The hydrogen component in the argon-hydrogen mixture is 1%, the flow rate of the argon-hydrogen mixture is 1 sccm, and the flow rate of the oxygen is 5 sccm.

[0077] Example 5 This embodiment provides a method for preparing a hole transport layer, which differs from Embodiment 1 in that: An argon-hydrogen mixture and oxygen are introduced into the chamber. The hydrogen component of the argon-hydrogen mixture is 5%, the flow rate of the argon-hydrogen mixture is 10 sccm, and the flow rate of the oxygen is 20 sccm.

[0078] Example 6 This embodiment provides a method for preparing a hole transport layer, which differs from Embodiment 1 in that the hydrogen gas component in the argon-hydrogen mixture is 2%.

[0079] Example 7 This embodiment provides a method for preparing a hole transport layer, which differs from Embodiment 1 in that: An argon-hydrogen mixture and oxygen are introduced into the chamber. The hydrogen component in the argon-hydrogen mixture is 0.5%, the flow rate of the argon-hydrogen mixture is 1 sccm, and the flow rate of the oxygen is 3 sccm.

[0080] Example 8 This embodiment provides a method for preparing a hole transport layer, which differs from Embodiment 1 in that: The flow rate of the argon-hydrogen mixture is 3 sccm, and the flow rate of the oxygen mixture is 9 sccm.

[0081] Example 9 This embodiment provides a method for preparing a hole transport layer, which differs from Embodiment 1 in that: During electron beam bombardment, the substrate temperature is 20℃, the evaporation rate is 0.6nm / s, and the thickness of the transition metal oxide layer is 10nm.

[0082] Example 10 This embodiment provides a method for preparing a hole transport layer, which differs from Embodiment 1 in that: During electron beam bombardment, the substrate temperature is 100℃, the evaporation rate is 1nm / s, and the thickness of the transition metal oxide layer is 50nm.

[0083] Example 11 This embodiment provides a method for preparing a hole transport layer. The difference from Embodiment 1 is that the temperature of the substrate is 50°C during electron beam bombardment.

[0084] Example 12 This embodiment provides a method for preparing a hole transport layer. The difference from Embodiment 1 is that the temperature of the substrate is 80°C during electron beam bombardment.

[0085] Example 13 This embodiment provides a method for preparing a hole transport layer, including the following steps: A 2.5×2.5cm heterogeneous crystalline silicon substrate was selected, cleaned with ultraviolet ozone for 15 minutes, and then transferred to the sample holder in the vacuum chamber of the electron beam evaporation equipment. Nickel particles with a purity of 99.99% were loaded into a graphite crucible, the vacuum chamber was closed, and the vacuum was evacuated to a degree of 4 × 10⁻⁶. -4 Pa; An argon-hydrogen mixture and oxygen are introduced into the chamber. The hydrogen component of the argon-hydrogen mixture is 3%, the flow rate of the argon-hydrogen mixture is 3 sccm, and the flow rate of the oxygen is 12 sccm. The chamber pressure is then adjusted to 5 × 10⁻⁶. -3 Pa; The electron beam generator was started with an accelerating voltage of 15kV, a beam current of 100mA, a substrate temperature of 60℃, and a evaporation rate of 0.1nm / s. When the film thickness reached 15nm, the evaporation was stopped to obtain a hydrogen-doped nickel oxide film. The film was then vacuum cooled for 10min, and nitrogen gas was introduced to bring it to atmospheric pressure before it was removed. SAM was dissolved in ethanol to obtain a SAM precursor solution with a concentration of 0.5 mg / ml. A SAM layer was prepared on a hydrogen-doped nickel oxide film by spin coating at a speed of 4000 rpm. After spin coating, the film was annealed at 100 °C for 10 min.

[0086] Comparative Example 1 This comparative example provides a method for preparing a hole transport layer. The difference from Example 1 is that the nickel oxide layer is prepared using a solution method, including the following steps: The nickel oxide layer was prepared by solution method: 10 mg of nickel oxide powder was dissolved in pure water and ultrasonically vibrated for 20 min; The nickel oxide aqueous solution was spin-coated onto the ITO glass substrate at a speed of 3000 rpm, and then annealed at 120°C for 10 min after spin-coating.

[0087] Comparative Example 2 This comparative example provides a method for preparing a hole transport layer, which differs from Example 1 in that the flow rate of the argon-hydrogen mixture is adjusted to 0.

[0088] Comparative Example 3 This comparative example provides a method for preparing a hole transport layer, which differs from Example 13 in that the flow rate of the argon-hydrogen mixture is adjusted to 0.

[0089] Based on the hole transport layers in Examples 1-12 and Comparative Examples 1-2, single-junction perovskite solar cells are further fabricated, including the following steps: A perovskite layer with a thickness of 800 nm was prepared on the hole transport layer by spin coating. The film composition was MA. 0.15 FA 0.8Cs 0.05 Pb(I 0.75 Br 0.25 3) The band gap was approximately 1.68 eV, the solution concentration was 1.6 M, and the spin-coating steps were: spin-coating at 1000 rpm for 10 s, spin-coating at 5000 rpm for 40 s, and adding 200 μL of chlorobenzene solution to the sample in the last 10 s. After spin-coating, the sample was heated at 120 °C for 15 min to obtain a perovskite film. A passivation layer was prepared by spin-coating using EDAI2 at a concentration of 0.5 mg / mL at a spin-coating speed of 5000 rpm. After spin-coating, the sample was annealed at 100 °C for 10 min. C was prepared by vacuum thermal evaporation. 60 The layer, serving as an electron transport layer, is 30 nm thick and is evacuated to a vacuum level of 4 × 10⁻⁶. -4 Pa, evaporation rate 0.3 Å / s, evaporation rate 0.2-0.5 Å / s; BCP layer as hole blocking layer with a thickness of 10 nm was prepared by vacuum thermal evaporation, and the vacuum degree was evacuated to 4 × 10⁻⁶. -4 Pa, evaporation rate 0.3 Å / s; 200 nm metallic Ag electrode prepared by vacuum thermal evaporation method, vacuum level reached 4 × 10⁻⁶ Pa. -4 Pa, evaporation rate 0.3 Å / s, complete the fabrication of single-junction perovskite solar cell device.

[0090] Based on the hole transport layer in Example 13 and Comparative Example 3, perovskite / heterojunction tandem solar cells are further fabricated, including the following steps: A perovskite layer with a thickness of 800 nm was prepared on the hole transport layer by spin coating. The film composition was MA. 0.15 FA 0.8 Cs 0.05 Pb(I 0.75 Br 0.25 3. The band gap was approximately 1.68 eV, the solution concentration was 1.8 M, and the spin-coating steps were: spin-coating at 1000 rpm for 10 s, spin-coating at 4000 rpm for 40 s, and adding 200 μL of chlorobenzene solution to the sample in the last 10 s. After spin-coating, the sample was heated at 120 °C for 15 min to obtain a perovskite film. A passivation layer was prepared by spin-coating using PDAI2 at a concentration of 0.5 mg / ml at a spin-coating speed of 5000 rpm. After spin-coating, the sample was annealed at 100 °C for 10 min. A 15 nm thick C film was prepared by vacuum thermal evaporation. 60 Layer, evacuate to a vacuum level of 4×10 -4Pa, evaporation rate 0.3 Å / s, evaporation rate 0.2-0.5 Å / s; Atomic layer deposition method was used to prepare a 20 nm thick SnO2 layer at 80 °C; Magnetron sputtering method was used to prepare a 50 nm thick IZO layer at 50 W sputtering power and a sputtering rate of 0.4 Å / s; Vacuum thermal evaporation method was used to prepare a 500 nm thick Ag metal gate electrode, with the vacuum level evacuated to 4 × 10⁻⁶. -4 Pa, evaporation rate 2 Å / s; a 120 nm thick MgF2 antireflection layer was prepared by vacuum thermal evaporation, with the vacuum level evaporated to 4 × 10⁻⁶ Pa. -4 Pa, evaporation rate 0.5 Å / s, complete the fabrication of tandem battery device.

[0091] The performance of the solar cells prepared based on the hole transport layers of Examples 1-13 and Comparative Examples 1-3 were tested respectively, and the test results are shown in the table below.

[0092] The test results from the examples and comparative examples show that the photoelectric conversion efficiency of batteries based on hydrogen-doped nickel oxide and SAM composite hole transport layers is significantly improved, whether in single-junction or stacked configurations. Moreover, the ratio of oxygen to argon-hydrogen mixture affects the doping effect and thus the battery performance.

[0093] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0094] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A method for preparing a hole transport layer, characterized in that, Includes the following steps: In a gaseous atmosphere containing a mixture of gas and oxygen, a transition metal oxide layer is obtained by electron beam evaporation. The mixture of gas contains hydrogen and an inert gas, and the transition metal includes nickel. A self-assembled molecular layer is formed on the transition metal oxide layer to obtain the hole transport layer.

2. The preparation method according to claim 1, characterized in that, The electron beam evaporation process includes the following steps: The mixed gas and the oxygen are introduced into a chamber containing the substrate; Within the chamber, the transition metal is used as an evaporation source. The transition metal is bombarded with an electron beam to cause it to evaporate and react with the oxygen, forming the transition metal oxide layer on the substrate.

3. The preparation method according to claim 2, characterized in that, Prior to the step of introducing the mixed gas and the oxygen, the electron beam evaporation process further includes the following steps: The chamber is evacuated to a vacuum level below 5 × 10⁻⁶. -4 Pa.

4. The preparation method according to claim 2, characterized in that, In the step of introducing the mixed gas and the oxygen, the hydrogen component in the mixed gas is 1%-5%, the flow rate of the mixed gas is 1-10 sccm, the flow rate of the oxygen is 5-20 sccm, and the pressure in the chamber is adjusted to not exceed 9 × 10⁻⁶. -3 Pa.

5. The preparation method according to claim 4, characterized in that, The hydrogen component in the mixture is 2%-3%.

6. The preparation method according to claim 4, characterized in that, The flow rate ratio of oxygen to the mixed gas is between 3:1 and 5:

1.

7. The preparation method according to claim 2, characterized in that, During the bombardment of the transition metal by the electron beam, the accelerating voltage of the electron beam is 10-20kV and the beam current is 50-100mA.

8. The preparation method according to claim 2, characterized in that, During the process of bombarding the transition metal with the electron beam, the temperature of the substrate is 20-100°C, the evaporation rate is 0.1-1 nm / s, and the thickness of the transition metal oxide layer is 10-50 nm.

9. The preparation method according to claim 8, characterized in that, The temperature of the substrate is 50-80℃.

10. A method for preparing a solar cell, characterized in that, Includes the following steps: A substrate is provided, and the hole transport layer is formed on the substrate using the method for preparing a hole transport layer according to any one of claims 1 to 9; A perovskite layer and an electron transport layer are sequentially formed on the hole transport layer.