Ti1-xNiSb thermoelectric materials were prepared by suspension melting, ball milling and spark plasma sintering, which solved the problems of low preparation efficiency and performance optimization in the existing technology, and achieved a highly efficient and simplified preparation process and excellent thermoelectric performance.
Patent Information
- Application Number
- CN202510625609.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-15
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies are difficult to efficiently prepare high-quality Ti1-xNiSb thermoelectric materials, and require long-term annealing to improve the uniformity of sample composition and performance stability, resulting in low preparation efficiency and difficulty in optimizing thermoelectric performance.
Ti1-xNiSb alloy ingots were synthesized using a suspension melting method. Single-phase cation-deficient semi-Hessler Ti1-xNiSb thermoelectric materials were prepared by suspension melting, ball milling, and spark plasma sintering, avoiding the annealing process and achieving uniformity of alloy composition and optimization of thermoelectric properties.
This study achieved efficient preparation of single-phase Ti1-xNiSb thermoelectric materials, simplified the operation process, shortened the production cycle, reduced stoichiometric losses, and optimized the thermoelectric performance by changing the carrier concentration within the pure phase range, thereby improving the thermoelectric figure of merit of the materials.
Smart Images

Figure CN123124654A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of thermoelectric materials, and more particularly to a cation-deficient semi-Hessler Ti. 1-x NiSb thermoelectric materials, their preparation methods, and applications. Background Technology
[0002] Thermoelectric materials hold great promise for applications in high-temperature power generation, particularly in industrial waste heat recovery and energy conversion under high-temperature conditions. Thermoelectric systems in this field typically utilize thermoelectric materials to directly convert heat energy into electrical energy through temperature differences, achieving highly efficient energy utilization. Under high-temperature conditions, thermoelectric materials can operate stably without the generation of mechanical parts, avoiding the wear and failure problems that may occur in traditional mechanical power generation systems. The main advantage of thermoelectric power generation systems is that they require no external power source, providing a continuous and stable power supply to the equipment solely through temperature difference, exhibiting high reliability and low maintenance requirements. In high-temperature environments, thermoelectric materials can effectively convert waste heat into usable electrical energy through the voltage difference generated by the thermal gradient, significantly improving energy utilization efficiency. For example, in the automotive industry, thermoelectric materials can be used to recover waste heat from engine emissions, converting it into electricity to charge vehicle batteries, reducing energy consumption and improving fuel efficiency. Furthermore, in high-temperature industrial processes such as steel and chemicals, the application of thermoelectric power generation technology helps reduce energy consumption and promotes the development of green manufacturing. With the continuous improvement of the performance of thermoelectric materials, thermoelectric power generation has shown great application potential in the field of high-temperature waste heat recovery, becoming one of the important technologies for achieving industrial energy conservation and reducing carbon emissions.
[0003] Thermoelectric materials, as special functional materials, can directly convert thermal energy into electrical energy through the movement of charge carriers within a solid. The dimensionless thermoelectric figure of merit (ZT) is the main indicator for evaluating thermoelectric performance, and its calculation formula is zT = (S... 2σ / κ)T. In the formula, S represents the Seebeck coefficient, σ is the electrical conductivity, κ is the thermal conductivity, and T refers to the absolute temperature. From the definition of zT, it can be seen that a good thermoelectric material should possess both a small κ and large S and σ, thereby maintaining a large temperature difference under a temperature field, generating a strong thermoelectric effect, and reducing energy loss in the form of Joule heating. However, these parameters are mutually coupled and inversely related, increasing the difficulty of optimizing the performance of thermoelectric materials. In recent years, theoretical and technological developments have driven a wave of thermoelectric research worldwide, and various new high-performance thermoelectric materials have emerged. Among them, Half-Heusler (HH) compounds, with their good mechanical and thermoelectric properties and relatively inexpensive and environmentally friendly constituent elements, have received widespread attention from academia and industry as highly promising high-temperature thermoelectric materials. HH compounds have a cubic MgAgAs structure, space group F4_3m, and chemical formula XYZ. In this system, X is typically the least electronegative element, composed of Group I and II elements, transition metals, or rare earth elements, such as Ti, Zr, Hf, V, Nb, and Ta; Y is a highly disruptive transition metal, such as Fe, Co, and Ni; and Z is the most electronegative element, usually a Group IVA or VA element, commonly Sn, Sb, and Bi. Due to the diversity of constituent elements, different combinations of X, Y, and Z elements can result in a wide range of valence electron counts in a half-Hessler compound, exhibiting drastically different physical properties. When the number of valence electrons per unit cell is 18, the valence electrons just completely occupy the bonding orbitals, and the Fermi level is located within the band gap. Therefore, 18-electron half-Hesslers are generally narrow-band semiconductor materials and have received extensive research and attention over the past two decades as high-performance thermoelectric materials. HH compounds with 17 and 19 electrons, due to incomplete bond filling or partial antibonding, allow the Fermi level to enter the conduction or valence band, transforming the system into a metal, and are theoretically unsuitable as thermoelectric materials. However, TiNiSb with a nominal 19 electrons defies this conventional wisdom. Research shows that pure-phase Ti 1-x NiSb contains a large number of cation vacancies, giving it an electron count close to 18, thus exhibiting semiconductor-like transport properties. This means that Ti... 1-x NiSb holds promise as a high-performance thermoelectric semiconductor material. However, current research focuses on Ti... 1-x Research on NiSb as a thermoelectric material is still relatively limited, and there is still much room for future exploration.
[0004] To date, similar to the processes used to synthesize other semi-Hersler (HH) compounds, arc melting remains the primary method for preparing Ti. 1-xThis is a common method for preparing NiSb materials. However, this method has many drawbacks, making it difficult to obtain high-quality samples directly. Moreover, it usually requires a long annealing period (7 days) to improve the homogeneity of the sample composition and the stability of its properties, resulting in low preparation efficiency and often failing to obtain ideal single-phase samples. Summary of the Invention
[0005] The main objective of this application is to provide a cation-deficient semi-Hersler Ti. 1-x NiSb thermoelectric materials, their preparation methods and applications, and the ability to obtain single-phase cation-deficient half-Hessler Ti without annealing. 1-x NiSb thermoelectric materials aim to change Ti 1-x The composition of NiSb in the pure phase region can be optimized by changing the carrier concentration within the pure phase region.
[0006] To achieve the above objectives, this application provides a cation-deficient semi-Hessler Ti 1-x The preparation method of NiSb thermoelectric material includes: placing Ti elemental rods, Ni elemental rods, and Sb elemental rods in a suspension melting device and performing suspension melting under an argon atmosphere to obtain Ti 1-x The NiSb alloy ingot casting process takes approximately 1.5–2 hours. The resulting ingot is then manually crushed and ground using an agate mortar. The ground powder is then further refined in a vibrating ball mill to obtain micron-sized Ti alloy. 1-x NiSb precursor powder; wherein the ball milling time of the vibrating ball mill is 1-3 hours; the obtained micron-sized Ti 1- x NiSb compound precursor powder was loaded into a graphite mold and sintered in a spark plasma sintering furnace at a temperature of 800–1173 K for 10–15 min to obtain defective semi-Hessler Ti. 1-x NiSb thermoelectric materials.
[0007] Optionally, during suspension melting, each sample was melted 3 to 5 times to ensure compositional uniformity.
[0008] Optionally, in the vibrating ball mill, the grinding balls have a diameter of 5–10 mm, a ball-to-material ratio of 1.5–3:1, and a power of 32–40 Hz. Larger diameter grinding balls primarily provide energy, which is beneficial for crushing large-particle-size samples; smaller diameter grinding balls are beneficial for grinding and refining small-particle-size samples; the higher the ball-to-material ratio, the better the ball milling effect.
[0009] Optionally, ball-milled micron-sized Ti 1-x The particle size of the NiSb compound precursor powder is 5–10 μm.
[0010] Optionally, the molar ratio of Ti elemental rods, Ni elemental rods, and Sb elemental rods is 0.7 to 1:1:1.
[0011] Optionally, the purity of the Ti elemental rods, Ni elemental rods, and Sb elemental rods is 99.99%.
[0012] Optionally, the vacuum degree of the spark plasma sintering furnace is less than 10. -5 The pressure is 65-80 MPa; the heating rate is 10-100 K / min; the cooling rate is 10-100 K / min; and the diameter of the graphite mold is 12-40 mm.
[0013] This application also provides a cation-deficient semi-Hersler Ti 1-x NiSb thermoelectric materials, employing the aforementioned cation-deficient half-Hessler Ti 1-x A method for preparing NiSb thermoelectric materials has been obtained.
[0014] This application also provides a cation-deficient semi-Hersler Ti 1-x Application of NiSb thermoelectric materials in thermoelectric conversion systems.
[0015] Compared with the prior art, the beneficial effects of this application are as follows: The cation-deficient semi-Hessler Ti of the present invention 1-x The preparation method of NiSb thermoelectric materials involves suspension melting of Ti, Ni, and Sb elemental rods to achieve alloying. Thorough melting ensures uniform alloy composition. Compared to traditional arc melting, this method is relatively simple to operate, has a short production cycle, minimal stoichiometric loss during melting, and allows for precise control of alloy composition to obtain single-phase products. It can also modify the Ti... 1-x The composition of NiSb in the pure phase region can be optimized by changing the carrier concentration within the pure phase region. Attached Figure Description
[0016] Figure 1 This application relates to a cation-deficient semi-Hessler Ti 1-x Preparation method of NiSb thermoelectric material Ti 1-x XRD patterns of NiSb (x = 0.10-0.18) samples; Figure 2 This application relates to a cation-deficient semi-Hessler Ti 1-x Preparation method of NiSb thermoelectric material Ti 0.90 BSE images of NiSb polished surfaces and Ti 0.90 Compositional analysis diagram of NiSb sample; Figure 3 This application relates to a cation-deficient semi-Hessler Ti1-x Conductivity diagram of NiSb thermoelectric material preparation method; Figure 4 This application relates to a cation-deficient semi-Hessler Ti 1-x Seebeck coefficient diagram of NiSb thermoelectric material preparation method; Figure 5 This application relates to a cation-deficient semi-Hessler Ti 1-x Power factor diagram of NiSb thermoelectric material preparation method; Figure 6 This application relates to a cation-deficient semi-Hessler Ti 1-x Thermal conductivity diagram of NiSb thermoelectric material preparation method; Figure 7 This application relates to a cation-deficient semi-Hessler Ti 1-x Thermoelectric figure of merit diagram of NiSb thermoelectric material preparation method.
[0017] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation
[0018] To make the objectives, technical solutions, and advantages of this application clearer, the technical solutions of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0019] In the examples, the four Ti values with x = 0.10, 0.14, 0.16, and 0.18 showed better results. 1-x NiSb, where: Ti 0.9 The thermal conductivity, Seebeck coefficient, and electrical conductivity of NiSb at 1019 K are κ = 6.12 W·m. -1 K -1 S = 56.36 μV·K -1 σ = 2.98 × 10 5 S·m -1 The zT value is approximately 0.15 at 10¹⁹ K; Ti 0.86 The thermal conductivity, Seebeck coefficient, and electrical conductivity of NiSb at 1019 K are κ = 5.45 W·m. -1 K -1 S = 60.47 μV·K -1 σ = 2.75 × 10 5 S·m -1 The zT value is approximately 0.18 at 10¹⁹ K; Ti0.84 The thermal conductivity, Seebeck coefficient, and electrical conductivity of NiSb at 1019 K are κ = 4.64 W·m. -1 K -1 S = 74.26 μV·K -1 σ = 2.21 × 10 5 S·m -1 The zT value is approximately 0.25 at 10¹⁹ K; Ti 0.82 The thermal conductivity, Seebeck coefficient, and electrical conductivity of NiSb at 1019 K are κ = 4.51 W·m. -1 K -1 S = 78.96 μV·K -1 σ = 2.14 × 10 5 S·m -1 The zT value is approximately 0.31 at 1019K.
[0020] The first embodiment of the present invention provides a cation-deficient semi-Hessler Ti 1-x The preparation method of NiSb thermoelectric materials specifically includes the following steps: Step S1: Ti elemental rods, Ni elemental rods, and Sb elemental rods are placed in a suspension melting apparatus at a molar ratio of 0.7 to 1:1:1 and subjected to suspension melting under an argon atmosphere to obtain Ti. 1-x NiSb alloy ingots; each sample underwent 3-5 melting cycles to ensure compositional uniformity. The purity of the Ti, Ni, and Sb elemental rods was 99.99%.
[0021] Suspension melting of elemental Ti, Ni, and Sb rods was used to alloy the three pure metals. During melting, the sample did not come into contact with the crucible, effectively preventing the crucible material from affecting the Ti. 1-x Contamination of NiSb alloys is mitigated to ensure their purity and performance. Rapid solidification of the molten alloy in a suspension state after melting helps form a fine and uniform grain structure, thereby improving the alloy's strength, toughness, and other mechanical properties. During suspension melting, electromagnetic stirring ensures thorough mixing of the molten alloy, resulting in a more homogeneous composition.
[0022] Step S2, Ti 1-x NiSb alloy ingots were manually crushed and ground in an agate mortar for 30–60 minutes. The ground sample powder was then placed in a vibrating ball mill for further ball milling to obtain micron-sized Ti. 1-xNiSb precursor powder; wherein the ball milling time of the vibrating ball mill is 1-3 hours; in the vibrating ball mill, the diameter of the grinding balls is 5-10 mm, the ball-to-material ratio is 1.5-3:1, and the power is 32-40 Hz; the grinding balls with larger diameters mainly provide energy and are beneficial for crushing samples with large particle sizes; the grinding balls with smaller diameters are beneficial for grinding and refining samples with small particle sizes; the larger the ball-to-material ratio, the better the ball milling effect; after ball milling, powder with a uniform particle size distribution of 5-10 μm is obtained.
[0023] Step S3, the obtained micron-sized Ti 1-x NiSb compound precursor powder is loaded into a graphite mold with a diameter of 12–40 mm and placed in a spark plasma sintering furnace for sintering. Unlike hot pressing sintering, which relies on indirect heating from an external heat source, spark plasma sintering utilizes a large pulse of direct current to directly act on the raw material powder. During this process, a large amount of Joule heat is generated instantaneously inside the powder, resulting in an extremely high heating rate, reaching up to 1000 K·min. -1 This characteristic allows for rapid heating and cooling processes, significantly reducing the preparation time and effectively minimizing the temperature gradient. Thanks to these advantages, spark plasma sintering can retain Ti to the greatest extent possible. 1-x The microstructure of the NiSb precursor powder not only helps reduce lattice thermal conductivity but also yields a more uniform microstructure. This leads to the formation of Ti... 1-x NiSb thermoelectric material; during sintering, the temperature is increased to 1173K at a heating rate of 10–100K / min, held for 10–15 min, and then decreased to room temperature at a cooling rate of 10–100K / min; the vacuum degree of the spark plasma sintering furnace is less than 10. -5 The pressure is 65-80 MPa.
[0024] In step 2, the sample powder after manual grinding is loaded into the ball mill jar, and in step 3, the ball-milled powder is loaded into the graphite mold. Both operations are carried out in a glove box with water content ≤0.01ppm, oxygen content ≤0.40ppm, and argon protection.
[0025] Example 1 Step S1: Weigh 3.854g of Ti elemental rod, 5.252g of Ni elemental rod, and 10.894g of Sb elemental rod and place them in a suspension melting apparatus. Perform suspension melting four times under an argon atmosphere to obtain Ti. 0.9 NiSb alloy ingots; Step S2, Ti 0.9NiSb alloy ingots were manually crushed and ground in an agate mortar for 30 minutes. The ground sample powder and grinding balls with diameters of 5 mm and 10 mm were loaded into a stainless steel ball mill jar at a ball-to-powder ratio of 3:1, sealed, and then placed in a vibrating ball mill at a power of 32 Hz for 3 hours to obtain micron-sized Ti. 0.9 NiSb precursor powder; Step S3, the obtained micron-sized Ti 0.9 NiSb compound precursor powder was loaded into a 12 mm diameter graphite mold and sintered in a spark plasma sintering furnace at a temperature of 1173 K, a pressure of 65 MPa, and a holding time of 10 min. The vacuum degree of the spark plasma sintering furnace was less than 10. -5 Ti 0.9 NiSb thermoelectric materials.
[0026] The Ti obtained in this embodiment 0.9 The performance of NiSb thermoelectric material was tested, and the results showed that the thermal conductivity, Seebeck coefficient, and electrical conductivity at 1019 K were κ = 6.12 W·m. -1 K -1 S = 56.36 μV·K -1 σ = 2.98 × 10 5 S·m -1 According to zT=(S 2 The zT value of the product prepared in this embodiment is calculated to be approximately 0.15 at 1019 K.
[0027] Example 2 Step S1: Weigh 3.716g of Ti elemental rod, 5.296g of Ni elemental rod, and 10.988g of Sb elemental rod and place them in a suspension melting apparatus. Perform suspension melting four times under an argon atmosphere to obtain Ti. 0.86 NiSb alloy ingots; Step S2, Ti 0.86 NiSb alloy ingots were manually crushed and ground in an agate mortar for 30 minutes. The ground sample powder and grinding balls with diameters of 5 mm and 10 mm were loaded into a stainless steel ball mill jar at a ball-to-powder ratio of 3:1, sealed, and then placed in a vibrating ball mill at a power of 32 Hz for 3 hours to obtain micron-sized Ti. 0.86 NiSb precursor powder; Step S3, the obtained micron-sized Ti 0.9 NiSb compound precursor powder was loaded into a 12 mm diameter graphite mold and sintered in a spark plasma sintering furnace at a temperature of 1173 K, a pressure of 65 MPa, and a holding time of 10 min. The vacuum degree of the spark plasma sintering furnace was less than 10. -5Ti 0.86 NiSb thermoelectric materials.
[0028] The Ti obtained in this embodiment 0.86 The performance of NiSb thermoelectric material was tested, and the results showed that the thermal conductivity, Seebeck coefficient, and electrical conductivity at 1019 K were κ = 5.45 W·m. -1 K -1 S = 60.47 μV·K -1 σ = 2.75 × 10 5 S·m -1 According to zT=(S 2 The zT value of the product prepared in this embodiment is calculated to be approximately 0.18 at 1019 K.
[0029] Example 3 Step S1: Weigh 3.644g of Ti elemental rod, 5.320g of Ni elemental rod, and 11.036g of Sb elemental rod and place them in a suspension melting apparatus. Perform suspension melting four times under an argon atmosphere to obtain Ti. 0.84 NiSb alloy ingots; Step S2, Ti 0.84 NiSb alloy ingots were manually crushed and ground in an agate mortar for 30 minutes. The ground sample powder and grinding balls with diameters of 5 mm and 10 mm were loaded into a stainless steel ball mill jar at a ball-to-powder ratio of 3:1, sealed, and then placed in a vibrating ball mill at a power of 32 Hz for 3 hours to obtain micron-sized Ti. 0.84 NiSb precursor powder; Step S3, the obtained micron-sized Ti 0.84 NiSb compound precursor powder was loaded into a 12 mm diameter graphite mold and sintered in a spark plasma sintering furnace at a temperature of 1173 K, a pressure of 65 MPa, and a holding time of 10 min. The vacuum degree of the spark plasma sintering furnace was less than 10. -5 Ti 0.84 NiSb thermoelectric materials.
[0030] The Ti obtained in this embodiment 0.84 The performance of NiSb thermoelectric material was tested, and the results showed that the thermal conductivity, Seebeck coefficient, and electrical conductivity at 1019 K were κ = 4.64 W·m. -1 K -1 S = 74.26 μV·K -1 σ = 2.21 × 10 5 S·m -1 According to zT=(S 2The zT value of the product prepared in this embodiment is calculated to be approximately 0.25 at 1019 K.
[0031] Example 4 Step S1: Weigh 3.574g of Ti elemental rod, 5.342g of Ni elemental rod, and 11.084g of Sb elemental rod and place them in a suspension melting apparatus. Perform suspension melting four times under an argon atmosphere to obtain Ti. 0.82 NiSb alloy ingots; Step S2, Ti 0.82 NiSb alloy ingots were manually crushed and ground in an agate mortar for 30 minutes. The ground sample powder and grinding balls with diameters of 5 mm and 10 mm were loaded into a stainless steel ball mill jar at a ball-to-powder ratio of 3:1, sealed, and then placed in a vibrating ball mill at a power of 32 Hz for 3 hours to obtain micron-sized Ti. 0.82 NiSb precursor powder; Step S3, the obtained micron-sized Ti 0.82 NiSb compound precursor powder was loaded into a 12 mm diameter graphite mold and sintered in a spark plasma sintering furnace at a temperature of 1173 K, a pressure of 65 MPa, and a holding time of 10 min. The vacuum degree of the spark plasma sintering furnace was less than 10. -5 Ti 0.82 NiSb thermoelectric materials.
[0032] The Ti obtained in this embodiment 0.82 The performance of NiSb thermoelectric material was tested, and the results showed that the thermal conductivity, Seebeck coefficient, and electrical conductivity at 1019 K were κ = 4.51 W·m. -1 K -1 S = 78.96 μV·K -1 σ = 2.14 × 10 5 S·m -1 According to zT=(S 2 The zT value of the product prepared in this embodiment is calculated to be approximately 0.31 at 1019 K.
[0033] The Ti obtained from the above embodiments 1-x A comparative analysis of NiSb thermoelectric materials was conducted, and the results are as follows: Figures 1 to 7 . Figure 1 To utilize unannealed Ti obtained by suspension melting 1-x The XRD patterns of NiSb (x = 0.10-0.18) samples were obtained from... Figure 1 It can be seen that the main phase of the sample is the HH phase, which has a cubic MgAgAs type crystal structure and belongs to the F-43m space group. The obtained pure phase Ti 1-xThe NiSb samples range from x = 0.10 to 0.18, which is significantly different from the pure phase composition of the arc-melted samples (x = 0.15 to 0.25), and no annealing is required during the preparation process. Figure 2 This indicates that Ti was obtained in Example 3. 0.90 The Ti, Ni, and Sb elements are uniformly distributed in the NiSb thermoelectric material. The thermoelectric properties were further characterized using an unannealed sample. Figures 3 to 7 Therefore, as the Ti vacancy content increases, Ti 1- x The σ values of NiSb samples generally decreased; at the same temperature, Ti... 1-x The |S| of the NiSb samples (x = 0.10–0.18) increased with increasing Ti vacancy content; the PF also increased with increasing Ti vacancy content, and at 1073 K, Ti... 0.82 The maximum power factor (PF) of NiSb is 13.9 × 10⁻⁶. -4 W m -1 K -2 Within the range of x = 0.10–0.18, the κ value at the same temperature decreases with increasing Ti vacancy content; at 1073 K, Ti… 0.82 The minimum κ value of NiSb is approximately 4.51 W·m⁻¹K⁻¹; at 10⁷³ K, Ti 0.82 NiSb has the highest zT value, approximately 0.31, which is four times that of nominal TiNiSb (~0.08) at the same temperature.
[0034] The fourth embodiment of the present invention provides a cation-deficient semi-Hessler Ti 0.82 NiSb thermoelectric materials, through the aforementioned cation-deficient half-Hessler Ti 0.82 A method for preparing NiSb thermoelectric materials has been obtained.
[0035] The fourth embodiment of the present invention provides a cation-deficient semi-Hessler Ti 0.82 Application of NiSb thermoelectric materials in thermoelectric conversion systems.
[0036] The above are merely preferred embodiments of this application and do not limit the patent scope of this application. Any equivalent structural or procedural transformations made using the content of this application's specification and drawings, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of this application.
Claims
1. A cation-deficient semi-Hessler Ti 1-x The method for preparing NiSb thermoelectric materials is characterized by... include: Ti monomer rod, Ni monomer rod, Sb monomer rod are placed in a suspension smelting equipment, and suspension smelting is carried out under an argon atmosphere to obtain Ti 1-x NiSb alloy ingot; The obtained ingot is manually crushed by agate mortar, and the crushed sample powder is placed in a vibration ball mill for ball milling to obtain micron-sized Ti 1-x NiSb precursor powder; wherein the ball milling time of the vibration ball mill is 1-3 h, so that the sample powder is sufficiently refined; The obtained micron-scale Ti 1-x NiSb compound precursor powder was loaded into a graphite mold and sintered in a spark plasma sintering furnace to obtain defective semi-Hessler Ti. 1-x NiSb thermoelectric materials are sintered at temperatures of 800–1173 K and for sintering times of 10–15 min.
2. The cation-deficient semi-Hessler Ti according to claim 1 1-x The method for preparing NiSb thermoelectric materials is characterized by... During the suspension melting process, each sample was melted 3 to 5 times to ensure uniformity of composition.
3. The cation-deficient semi-Hessler Ti according to claim 1 1-x The method for preparing NiSb thermoelectric materials is characterized by... In the aforementioned vibrating ball mill, the grinding balls have a diameter of 5–10 mm, a ball-to-material ratio of 1.5–3:1, and a power of 32–40 Hz. Larger diameter grinding balls provide energy, which is beneficial for crushing large-particle-size samples; smaller diameter grinding balls are beneficial for grinding and refining small-particle-size samples; the higher the ball-to-material ratio, the better the ball milling effect.
4. The cation-deficient semi-Hessler Ti according to claim 1 1-x The method for preparing NiSb thermoelectric materials is characterized by... The ball-milled micron-sized Ti 1-x The particle size of the NiSb compound precursor powder is 5–10 μm.
5. The cation-deficient semi-Hessler Ti according to claim 1 1-x The method for preparing NiSb thermoelectric materials is characterized by... The molar ratio of the Ti elemental rod, the Ni elemental rod, and the Sb elemental rod is 0.7 to 1:1:
1.
6. The cation-deficient semi-Hessler Ti according to claim 1 1-x The method for preparing NiSb thermoelectric materials is characterized by... The purity of the Ti elemental rod, the Ni elemental rod, and the Sb elemental rod is all 99.99%.
7. The cation-deficient semi-Hessler Ti according to claim 1 1-x The method for preparing NiSb thermoelectric materials is characterized by... The vacuum degree of the discharge plasma sintering furnace is less than 10. -5 The pressure is 65-80 MPa; the heating rate is 10-100 K / min; the cooling rate is 10-100 K / min; and the diameter of the graphite mold is 13-40 mm.
8. A cation-deficient semi-Hessler Ti 1-x NiSb thermoelectric material, characterized in that... The cation-deficient semi-Hessler Ti according to any one of claims 1-7 1-x A method for preparing NiSb thermoelectric materials has been obtained.
9. A cation-deficient semi-Hessler Ti 1-x Application of NiSb thermoelectric materials in thermoelectric conversion systems.