Spin orbital moment structure, magnetic memory device including the spin orbital moment structure, and method for manufacturing the same.

By combining the spin orbital moment structure with the interface effect, the write current density of SOT-MRAM devices is reduced, solving the problem of high switching current density in traditional SOT-MRAM and realizing low-power spintronic applications.

CN123124663APending Publication Date: 2026-11-17CITY UNIVERSITY OF HONG KONG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610581331.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2026-04-29
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional SOT-MRAM devices have high write current density, which limits the density of memory cell arrays, and existing technologies have difficulty effectively reducing switching current density.

Method used

By employing a spin-orbit moment structure, combining the interface-induced orbital Lashba-Edelstein effect with the synergistic effect of spin current in the two-dimensional spin-orbit coupling layer, ultra-low switching current density is achieved through out-of-plane counterdamping torque, and the spin current enhancement effect at the interface between the two-dimensional spin-orbit coupling layer and the oxide layer is utilized.

Benefits of technology

This achievement realizes ultra-low switching current density, reduces write current density, and improves the energy efficiency of memory devices, demonstrating the potential of van der Waals heterostructures in CMOS electronic applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124663A_ABST
    Figure CN123124663A_ABST
Patent Text Reader

Abstract

This invention provides a spin-orbit moment structure, comprising: an oxide layer; a two-dimensional spin-orbit coupling (2D-SOC) layer deposited on the oxide layer; and a free magnetic layer deposited on the 2D-SOC layer. When a switching current is applied to the spin-orbit moment structure: the 2D-SOC layer is configured to provide a master spin current that induces an out-of-plane anti-damped spin-orbit moment perpendicular to the magnetic moment; and an auxiliary spin current is generated at the interface between the 2D-SOC layer and the oxide layer. The thickness of the 2D-SOC layer is less than the spin diffusion length of the 2D-SOC layer, such that the auxiliary spin current has a stacking enhancement effect on the master spin current. The structure exhibits an ultra-low switching current density, representing a significant advancement in low-power spintronics applications.
Need to check novelty before this filing date? Find Prior Art

Description

Cross-referencing of patent applications

[0001] This application claims priority to U.S. Provisional Patent Application No. 63 / 805,334, filed May 14, 2025, the disclosure of which is incorporated herein by reference in its entirety. Technical Field

[0002] This invention relates generally to spintronic devices and magnetic memory technology, and more specifically, to spin-orbit moment structures capable of achieving ultra-low switching current densities. Background Technology

[0003] The rapid development of artificial intelligence (AI), the Internet of Things (IoT), and autonomous systems has led to a surge in demand for high-speed computing and high-density data storage, accompanied by a sharp increase in energy consumption and excessive heat generation. Traditional silicon-based electronic devices, which rely on electron charge for computing and data storage, are facing physical and economic bottlenecks. The miniaturization trend of transistors, predicted by Moore's Law and continuing for decades, is gradually slowing down due to quantum effects and heat dissipation problems, while energy losses caused by charge leakage and resistive heating further reduce device efficiency. These challenges have driven in-depth research into next-generation technologies, such as spintronic devices that utilize electron spin rather than electron charge for low-power data storage and computing, including magnetic random access memory (MRAM) and spin field-effect transistors (Spin-FETs). Regardless of the specific application, effective control of magnetization in ferromagnetic materials with perpendicular magnetic anisotropy (PMA) is of great significance.

[0004] The emerging third-generation spin-orbit moment MRAM (SOT-MRAM) represents a significant advancement in spintronics research over the past few decades. Unlike traditional MRAM, SOT-MRAM devices utilize spin current generated by charge current, rather than magnetic field generated by current, and torque induced by spin accumulation at the interface, to switch the relative orientation of free layer magnetization, thereby enabling data writing operations.

[0005] However, conventional SOT-MRAMs have high write current densities or switching current densities, which limit the density of the memory cell array due to thermal management requirements. Conventional SOT-MRAMs typically use heavy metals, such as Pt and Ta, or two-dimensional materials, such as Bi₂Te₂Se and WTe₂, as the spin-orbit coupling (SOC) layer, and their switching current densities are typically in the range of 10⁻⁶. 6 Up to 10 7 The current density is in the range of A / cm². Such a high current density poses a significant challenge to the widespread application of SOT-MRAM. Summary of the Invention

[0006] To address the aforementioned technical challenges, this invention provides a spin-orbit moment (SOT) structure that utilizes the synergistic effect of the interface-induced orbital Rashba–Edelstein effect and the spin current driven by intrinsic spin–orbit-coupling in the two-dimensional spin-orbit coupling layer, combined with the out-of-plane counterdamping torque generated at the spin-orbit coupling / oxide interface induced by symmetry, thereby achieving ultra-low switching current density.

[0007] According to a first aspect of the invention, a spin-orbit moment structure is provided. The spin-orbit moment structure includes: an oxide layer; a two-dimensional spin-orbit coupling (2D-SOC) layer deposited on the oxide layer; and a free magnetic layer deposited on the two-dimensional spin-orbit coupling layer. When a switching current is applied to the spin-orbit moment structure: the two-dimensional spin-orbit coupling layer is configured to provide a master spin current that induces an out-of-plane anti-damped spin-orbit moment perpendicular to the magnetic moment; and an auxiliary spin current is generated at the interface between the two-dimensional spin-orbit coupling layer and the oxide layer. The thickness of the two-dimensional spin-orbit coupling layer is less than the spin diffusion length of the two-dimensional spin-orbit coupling layer, such that the auxiliary spin current has a stacking enhancement effect on the master spin current.

[0008] According to a second aspect of the present invention, a memory device is provided. The memory device includes: a spin-orbit moment structure of the first aspect; a fixed magnetic layer; a tunneling barrier disposed between the free magnetic layer and the fixed magnetic layer; a bit line electrode electrically connected to the fixed magnetic layer; and a write line electrode electrically connected to the free magnetic layer and the oxide layer. The tunneling barrier exhibits a tunneling magnetoresistance dependent on the magnetization state of the free magnetic layer and is switchable between a low value and a high value, the low value and the high value representing a first logic state and a second logic state, respectively.

[0009] According to a third aspect of the present invention, a method for manufacturing a spin-orbit moment structure of the first aspect is provided. The method includes: preparing a two-dimensional spin-orbit coupling film using a dry transfer technique or a thin-film deposition technique; depositing a metal layer on a substrate by magnetron sputtering and exposing the metal layer to an ambient environment for a predetermined time period to allow the formation of an oxide layer; sputtering a conductive material onto the oxide layer to obtain an electrode layer, and performing a photolithography process to pattern the electrode layer, thereby obtaining a patterned electrode; sequentially picking up a free magnetic single-crystal film and the two-dimensional spin-orbit coupling film using a selected hexagonal boron nitride (hBN) sheet in a controlled atmosphere; and sequentially transferring the two-dimensional spin-orbit coupling film and the free magnetic single-crystal film onto the oxide layer and the electrode on the substrate to form a spin-orbit moment heterostructure.

[0010] By optimizing the thickness of the two-dimensional spin-orbit coupling layer, the two-dimensional spin-orbit coupling layer, together with the spin-orbit coupling / oxide interface, can serve as a bifunctional spin current source to enhance spin-charge current interconversion. Deterministic field-free control of the magnetization of the free magnetic layer is achieved through ultra-low switching current density. Based on FGaT / WTe2 / CuO x The SOT structure fabricated from heterostructures exhibits an average 3.6 × 10⁻⁶ Ω·cm. 5 Ultra-low switching current density of A cm⁻² (minimum current density of 1.4 × 10⁻¹⁰) 5 This ultra-low switching current density (A cm⁻²) is an order of magnitude lower than the previously reported WTe² value and approximately two orders of magnitude lower than the current density in conventional heavy metal systems. This ultra-low switching current density represents a significant advancement in this low-power spintronic application, demonstrating the potential of van der Waals heterostructure interface engineering beyond CMOS electronics applications. Attached Figure Description

[0011] Embodiments of the present invention will now be described in more detail with reference to the accompanying drawings, wherein...

[0012] Figure 1 This is a schematic diagram of an SOT structure according to an embodiment of the present invention;

[0013] Figure 2 This is a schematic diagram of a magnetic memory device including the SOT structure according to an embodiment of the present invention;

[0014] Figure 3 This is a flowchart of a method for manufacturing the SOT structure according to an embodiment of the present invention;

[0015] Figure 4A and Figure 4BEach of the following embodiments of the present invention is illustrated using FGaT / WTe2 / CuO. x Three-dimensional isometric views and cross-sectional views of a heterogeneous SOT structure, which maintains mirror symmetry about the bc plane but breaks mirror symmetry about the ac plane, where c represents the out-of-plane axis;

[0016] Figure 5 FGaT / WTe2 / CuO is shown x Crystal structure of Td-WTe2 in heterostructure;

[0017] Figure 6 It is hBN / FGaT (approximately 15 nm) / WTe2 (approximately 8 uc) / CuO x Optical micrograph of a heterostructure sample (approximately 3 nm), in which current is applied along the a-axis of WTe2 and transverse voltage along the b-axis is measured;

[0018] Figure 7 The following diagram shows FGT / WTe2(2uc) / CuO under no magnetic field. x Current density-Hall resistance curve of heterostructure sample;

[0019] Figure 8 It is along hBN / FGaT (approximately 15 nm) / WTe2 (approximately 8 uc) / CuO at room temperature. x (Approximately 3 nm) Anomalous Hall effect (AHE) lap measured when a magnetic field is applied to the out-of-plane direction of the sample;

[0020] Figure 9 It is along hBN / FGaT (approximately 15 nm) / WTe2 (approximately 8 uc) / CuO at room temperature. x (Approximately 3 nm) Abnormal Hall effect lap measured when a current is applied along the a-axis of the sample;

[0021] Figure 10 The field-free switching of FGaT magnetization induced by current under different WTe2 thicknesses is shown;

[0022] Figure 11 The critical switching current density (J) is shown. c The dependence of the y-axis coordinate on the thickness of WTe2 is shown in logarithmic form.

[0023] Figure 12 J is shown c Compared with various reported FGaT / WTe2 / CuO x Comparison of data for heterogeneous devices, where the x-axis coordinates are displayed logarithmically;

[0024] Figure 13 The study showed hBN / FGaT (approximately 15 nm) / WTe2 (2 uc) / CuO. x Current-induced field-free magnetization switching of FGaT in the device at different temperatures;

[0025] Figure 14 The study showed hBN / FGaT (approximately 15 nm) / WTe2 (2 uc) / CuO. x Critical current density J of the device c With temperature change;

[0026] Figure 15 This illustrates hBN / FGaT (approximately 15 nm) / WTe2 (2 uc) / CuO achieved at 300 K by a series of current pulses applied along the a-axis of WTe2 (write pulse: ±300 μA, 1 ms; read current: 1 μA; pulse interval: 10 s). x Deterministic switching of devices;

[0027] Figure 16 The following diagrams show hBN / FGaT (approximately 15 nm) / WTe2 (2 uc) / CuO. x Current-induced Rxy curves of hBN / FGaT (approximately 15 nm) / WTe2(2 uc) / SiO2, hBN / FGaT (approximately 15 nm) / WTe2(2 uc) / Al2O3, and hBN / WTe2(2 uc) / SiO2; and

[0028] Figure 17 FGaT (approximately 15 nm) / CuO was shown. x A magnetic field of 3 nm is used for switching, where the magnetic field Hx is along the direction of the current. Detailed Implementation

[0029] In the following description, details of the invention are set forth as preferred embodiments. It will be apparent to those skilled in the art that modifications, including additions and / or substitutions, can be made without departing from the scope and spirit of the invention. Certain specific details may be omitted to avoid obscuring the invention; however, the manner in which this disclosure is written is sufficient to enable those skilled in the art to implement the teachings herein without excessive experimentation.

[0030] Figure 1 This is a schematic diagram of a spin orbit moment (SOT) structure 100 according to an embodiment of the present invention.

[0031] The structure comprises three layers: a free magnetic layer 110, a two-dimensional (2D) spin-orbit coupling (SOC) layer 120, and an oxide layer 130. The 2D SOC layer 120 provides a spin current through the spin Hall effect (SHE) to generate an unconventional out-of-plane counterdamped SOT in the vertical magnetic moment. The free magnetic layer is switched by the SOT generated by the spin current, thereby achieving field-free current switching.

[0032] When a switching current is applied to the spin-orbit moment structure, the two-dimensional spin-orbit coupling layer 120 is configured to provide a master spin current that induces an out-of-plane anti-damped spin-orbit moment perpendicular to the magnetic moment.

[0033] The thickness of the two-dimensional spin-orbit coupling layer 120 is less than the spin diffusion length of the spin-orbit coupling material in the layer, causing an auxiliary spin current to be generated at the interface between the two-dimensional spin-orbit coupling layer 120 and the oxide layer 130. This auxiliary spin current is generated due to the spin Rashba-Edelstein effect (SREE) or the orbital Rashba-Edelstein effect (OREE). Therefore, by combining the main spin current of the two-dimensional spin-orbit coupling layer 120 with the auxiliary spin current from the interface, the total spin current can be enhanced. Preferably, the thickness of the two-dimensional spin-orbit coupling layer 120 is approximately 2 nm.

[0034] The free magnetic layer 110 is made of a perpendicular magnetic anisotropy (PMA) material, which is selected from: Fe3GeTe2 (FGT), Fe3GaTe2 (FGaT), Cr2Ge2Te6 (CGT), Cr2Si2Te6 (CST), Co, CoFeB, CoTb, and Tm3Fe5O. 12 (TIG), analogues or combinations thereof.

[0035] The two-dimensional spin-orbit coupling layer 120 is made of a thin conductive material with strong spin-orbit coupling. The thin conductive material is selected from: two-dimensional van der Waals materials, such as WTe2, MoTe2, TaIrTe4, the like, or combinations thereof; heavy metals, such as Pt, W, the like, or combinations thereof; conductive oxides, such as SrIrO3, SrRuO3, the like, or combinations thereof; and topological materials, such as Bi2Se3, Bi2Te3, the like, or combinations thereof.

[0036] The oxide layer 130 is made of a metal oxide material, which is selected from CuO. x SiO2, Al2O3, SrTiO3, analogues or combinations thereof.

[0037] Figure 2 A schematic diagram of a magnetic memory device 200 including an SOT structure according to an embodiment of the present invention is shown. As shown, the magnetic memory device 200 includes an SOT structure comprising a free magnetic layer (FM2), a two-dimensional spin-orbit coupling layer 210, and an oxide layer 220. The magnetic memory device further includes a pinned magnetic layer (FM1) and a tunneling barrier (TB) sandwiched between the free magnetic layer FM2 and the pinned magnetic layer FM1 and configured to provide (or present) tunneling magnetic resistance (TMR). The memory device 200 further includes bit line electrodes 230 electrically connected to the pinned magnetic layer; and word line electrodes (not shown) electrically connected to the free magnetic layer and the oxide layer.

[0038] When the magnetization of the free magnetic layer FM2 is switched by the SOT generated by the two-dimensional spin-orbit coupling layer 210, the tunneling magnetoresistance can be read through the bit line electrode (top metal) 230, and the low current density SOT magnetization switching current flowing through the word line electrode enables high-speed and low-power writing in the memory device.

[0039] The tunneling barrier can be made of an inorganic ceramic material selected from: MgO, TiO2, Al2O3, MgZnO, MgB2, Ti3N4, V3N4, BN, the like, or combinations thereof. In some embodiments, the tunneling barrier can have a multilayer structure (e.g., alternating stacks of Mg / MgO).

[0040] The fixed magnetic layer can be made of a conventional ferromagnetic material, selected from Fe, Co, Ni, CoFe, NiFe, CoFeB, NiFeB, CoFeSiB, NiFeSiB, and (Pt / Co). n The fixed magnetic layer may be an alloy, a similar material, or a combination thereof, and may be arranged as an alloy / multilayer structure. The fixed magnetic layer may have a fixed magnetization direction, which may be parallel or antiparallel to the magnetization direction of the free magnetic layer FM2.

[0041] The value of the tunneling magnetoresistance depends on the relative orientation of the magnetization directions of the two magnetic layers FM1 and FM2. When the magnetization directions of the fixed and free layers are parallel, most spin electrons (electrons with the same magnetization direction) are in low energy states on both sides, and the tunneling probability is high. In this case, the tunneling magnetoresistance has a low value (corresponding to logic "0"). When the magnetization directions of the two magnetic layers are antiparallel, the tunneling magnetoresistance has a high value (corresponding to logic "1").

[0042] The fabrication of the SOT structure involves precisely stacking a free magnetic single-crystal film and a two-dimensional spin-orbit coupled single-crystal film onto an oxide layer with patterned electrical contacts. This stacking can be performed using dry transfer technology or thin-film deposition technology.

[0043] Reference Figure 3 The device manufacturing process S100 includes the following steps:

[0044] S101: Two-dimensional spin-orbit coupled single-crystal films are prepared by dry transfer technology or thin film deposition technology.

[0045] S102: Deposit a metal layer on an insulating layer coated on a substrate by magnetron sputtering, and expose the metal layer to the surrounding environment for a predetermined period of time to form an oxide layer.

[0046] S103: Sputter conductive material onto the oxide layer to obtain an electrode layer, and perform a photolithography process to pattern the electrode layer, thereby obtaining a patterned electrode.

[0047] S104: Mechanically peel hBN into thin sheets, and select hBN sheets with a thickness in the range of about 20 nm to 50 nm.

[0048] S105: Pick up the selected hBN sheet using a polymer-based transfer stamp.

[0049] S106: In a controlled atmosphere, a selected hBN sheet carried by the transfer stamp is used to sequentially pick up a free magnetic single crystal film and a two-dimensional spin-orbit coupling film.

[0050] S107: The two-dimensional spin-orbit coupling film and the free magnetic single crystal film are sequentially transferred to the oxide layer and the electrode to form an SOT heterostructure.

[0051] In one embodiment, Fe3GaTe2(FGaT) / WTe2 / CuO is manufactured. x The heterostructure device is a SOT structure. The fabrication involves using a dry transfer technique to precisely assemble FGaT and WTe2 layers of different thicknesses onto CuO with patterned Pt electrical contacts. x / SiO2 / Si substrate.

[0052] More specifically, WTe2 single-crystal films were synthesized via chemical vapor transport (CVT). A stoichiometric mixture of W and Te powders and a transport agent were sealed in a vacuum-sealed quartz tube and placed in a dual-temperature zone furnace. The source region and the growth region were maintained at 750°C and 650°C, respectively, for 10 days, thereby obtaining millimeter-sized crystals in the growth region.

[0053] CuO was prepared by magnetron sputtering 3 nm Cu onto SiO2 (300 nm) coated on a Si substrate. x The sputtered Cu was then oxidized in air under ambient conditions for two days to obtain CuO through the natural oxidation of Cu. x layer.

[0054] Then, using ultraviolet lithography and magnetron sputtering, a Hall-shaped (approximately 8 μm × 3 μm) Pt (10 nm) electrode was fabricated on a SiO2 (300 nm) coating.

[0055] The hBN was then peeled onto the SiO2 substrate using transparent tape, and hBN of appropriate size and thickness was selected under a microscope. Subsequently, hBN was picked up sequentially using a PC / PDMS stamp. Then, in a glove box (oxygen content below 0.5 ppm), FGaT and WTe2 with appropriate shapes and thicknesses were picked up using the hBN and transferred to a Hall-shaped electrode. Preferably, a rectangular WTe2 single-crystal film was selected, with the long and short sides corresponding to the a-axis and b-axis, respectively. Then, an FGaT film smaller than the WTe2 single-crystal film was selected.

[0056] Figure 4A and Figure 4B FGaT / WTe2 / CuO is shown x A schematic diagram of a heterostructure device. The FGaT / WTe2 / CuO... x The heterostructure device has a two-dimensional spin-orbit coupling layer of WTe2 with a thickness of less than 4 unit cells (uc). The Td phase WTe2 (space group Pnm21) used in this invention exhibits obvious symmetry characteristics: it maintains mirror symmetry about the bc plane, but breaks mirror symmetry about the ac plane, where c represents the out-of-plane crystal axis (…). Figure 5 ).

[0057] The measurement of the Hall resistance involves applying a current along the a-axis of WTe2 while simultaneously detecting the transverse voltage along the b-axis. Figure 6 This allows for precise detection of magnetization switching in FGaT.

[0058] Figure 7The following diagram shows FGT / WTe2(2uc) / CuO under no magnetic field. x The current density-Hall resistance curve of the sample shows a low switching current density (approximately 1.56 × 10⁻⁶). 5 The value (A cm⁻²) is reduced by one to two orders of magnitude compared to the values ​​reported in the literature.

[0059] Figure 8 Another device was shown (hBN / FGaT (approx. 15 nm) / WTe2 (approx. 8 uc) / CuO). x (Approximately 3 nm) Anomalous Hall effect (AHE) hysteresis loop measured at room temperature with a magnetic field applied perpendicular to the plane (H∥c).

[0060] At room temperature, a 1 ms current pulse was also used to achieve field-free current switching of magnetization. Figure 9 Unless otherwise stated, all subsequent measurements were performed at room temperature (300 K).

[0061] exist Figure 10 In this paper, the current-induced field-free magnetization switching characteristics of devices with different WTe2 thicknesses are plotted as a function of current density.

[0062] Extract the critical switching current density (J) from these measurements c If the non-uniform current shunting effect between the FGaT layer and the WTe2 layer is considered, then the J of the thin WTe2 device... c It will be smaller.

[0063] like Figure 11 As shown, J was observed to decrease with decreasing WTe2 thickness. c Significantly reduced. Notably, the average J of the 2uc WTe2 device... c 3.6×10 5 A cm⁻² (minimum J) c Approximately 1.4 × 10 5 A cm⁻²).

[0064] like Figure 12 As shown, the field-free magnetization switching J c This value is one to two orders of magnitude smaller than previously reported, highlighting its significant potential for energy-efficient spintronic applications. In contrast, as the thickness of WTe2 increases, the J of the 21 uc WTe2 device decreases. c Gradually saturated to approximately 4.7 × 10⁻⁶ 6 A cm⁻², close to the previously reported value.

[0065] The reduction in critical switching current density achieved by this invention is based on two mechanisms: the (spin) Lashba-Edelstein effect (SREE) and the orbital Lashba-Edelstein effect (OREE). In both cases, additional spin current is induced in WTe2, leading to enhanced spin accumulation and increased SOT at the FGaT / WTe2 interface.

[0066] On the other hand, charge current can induce orbital angular momentum flow (orbital current J) at the metal / oxide interface. L This orbital angular momentum flow can then be converted into a spin current (J) in a metal with spin-orbit coupling. s SOC If this additional spin current is related to WTe2 / CuO x Intrinsic spin current (J) of WTe2 in heterostructure s When WTe2 is relatively thin, a significant enhancement of spin accumulation and SOT will occur at the FGaT / WTe2 interface.

[0067] To further confirm the above observations, the hBN / FGaT (approximately 15 nm) / WTe2 (2 uc) / CuO composition was analyzed. x The (approximately 3 nm) device underwent more comprehensive magnetic transport characterization. Figure 13 The current-induced fieldless magnetization switching of FGaT in the temperature range of 300 K to 350 K is shown. Deterministic magnetization reversal can be observed up to 340 K, while no identifiable switching loop is observed at 350 K.

[0068] like Figure 14 As shown, J c The temperature decreases with increasing temperature. This trend is consistent with the thermal evolution of the magnetization and coercive field of FGaT, both of which gradually weaken near their Curie temperature. The Curie temperature of the synthesized bulk FGaT single crystal is approximately 370 K, while the Tc of thin-layer FGaT may decrease. Finally, as... Figure 15 As shown, robust magnetization control is demonstrated at 300 K by applying current pulses in opposite directions along the a-axis of WTe2.

[0069] To clarify WTe2 / CuO x The interface in the manufactured hBN / FGaT / WTe2 / CuO x The role of SOT-induced magnetization switching in the study was investigated, and three other device configurations were compared: hBN / FGaT / WTe2 / SiO2, hBN / FGaT / WTe2 / Al2O3, and hBN / WTe2 / SiO2. All four device configurations have the same FGaT layer thickness (approximately 15 nm) and WTe2 layer thickness (2 μC). Figure 16Presents the current-induced R measured at room temperature and zero magnetic field. xy curve.

[0070] In the device containing FGaT, hBN / FGaT / WTe2 / CuO x hBN / FGaT / WTe2 / CuO x A distinct magnetization switching loop was observed in hBN / FGaT / WTe2 / Al2O3, and its J c Approximately 2.8 × 10⁻⁶ 5 1.2×10 6 1.1×10 6 A cm⁻². Compared to devices based on thicker WTe2, these reduced J c (Especially for FGaT / WTe2 / CuO) x The device shows enhanced charge-spin-conversion efficiency from the bottom interface of WTe2 and stronger SOT acting on FGaT.

[0071] Furthermore, for hBN / FGaT / CuO x (3 nm) control experiments on heterostructures show that, although magnetic field-assisted switching can be achieved (in a 200 Oe magnetic field along the current direction, J c Approximately 1.2 × 10 6 A cm⁻²), such as Figure 17 As shown, however, no field-free switching was observed in this device.

[0072] Although this disclosure has been described and illustrated with reference to specific embodiments thereof, such descriptions and illustrations are not limiting. The drawings are not necessarily drawn to scale. Due to manufacturing processes and tolerances, the illustrations in this disclosure may differ from actual apparatus. This disclosure may have other embodiments not specifically shown. Modifications may be made to adapt particular circumstances, materials, composition, methods, or processes to the purpose and scope of this disclosure. All such modifications are intended to fall within the scope of the appended claims. While the methods disclosed herein have been described with reference to specific operations performed in a particular order, it should be understood that these operations may be combined, subdivided, or reordered to form equivalent methods without departing from the teachings of this disclosure. Therefore, unless specifically indicated herein, the order and grouping of operations are not limiting.

Claims

1. A spin orbital moment structure, comprising: oxide layer; A two-dimensional spin-orbit coupling layer deposited on the oxide layer; as well as A free magnetic layer deposited on the two-dimensional spin-orbit coupling layer; When a switching current is applied to the spin-orbit moment structure: the two-dimensional spin-orbit coupling layer is configured to provide a master spin current, which induces an out-of-plane anti-damped spin-orbit moment perpendicular to the magnetic moment; Furthermore, an auxiliary spin current is generated at the interface between the two-dimensional spin-orbit coupling layer and the oxide layer; and The thickness of the two-dimensional spin-orbit coupling layer is less than the spin diffusion length of the two-dimensional spin-orbit coupling layer, so that the auxiliary spin current has a stacking enhancement effect on the main spin current.

2. The spin-orbit torque structure of claim 1, wherein, The free magnetic layer is made of a material with perpendicular magnetic anisotropy.

3. The spin orbit torque structure of claim 1, wherein, The two-dimensional spin-orbit coupling layer is made of a conductive material with spin-orbit coupling.

4. The spin orbit torque structure of claim 1, wherein, The oxide layer is made of a metal oxide material.

5. A memory device, comprising: The spin orbital moment structure according to claim 1; Fixed magnetic layer; A tunneling barrier is disposed between the free magnetic layer and the fixed magnetic layer; Bit line electrodes, which are electrically connected to the fixed magnetic layer; as well as A write line electrode is provided, which is electrically connected to the free magnetic layer and the oxide layer; The tunneling barrier exhibits a tunneling magnetoresistance that depends on the magnetization state of the free magnetic layer and can switch between low and high values, where the low and high values ​​represent the first logic state and the second logic state, respectively.

6. The memory device of claim 5, wherein, The free magnetic layer is made of a material with perpendicular magnetic anisotropy.

7. The memory device of claim 5, wherein, The two-dimensional spin-orbit coupling layer is made of a conductive material with spin-orbit coupling.

8. The memory device of claim 5, wherein, The oxide layer is made of a metal oxide material.

9. The memory device of claim 5, wherein, The fixed magnetic layer is made of ferromagnetic material.

10. The memory device according to claim 5, wherein, The tunneling barrier is made of inorganic ceramic material.

11. A method for manufacturing the spin orbital moment structure according to claim 1, comprising: Two-dimensional spin-orbit coupling films were prepared using dry transfer technology or thin film deposition technology. A metal layer is deposited on a substrate by magnetron sputtering, and the metal layer is exposed to the surrounding environment for a predetermined period of time to allow the formation of an oxide layer; A conductive material is sputtered onto the oxide layer to obtain an electrode layer, and a photolithography process is performed to pattern the electrode layer, thereby obtaining a patterned electrode. In a controlled atmosphere, selected hexagonal boron nitride sheets were used to sequentially pick up free magnetic single crystal films and two-dimensional spin-orbit coupled films. as well as The two-dimensional spin-orbit coupling film and the free magnetic single crystal film are sequentially transferred to the oxide layer and the electrode on the substrate to form a spin-orbit moment heterostructure.