A semiconductor fabrication method using photoresist protection
By adding a photoresist protective layer to the surface of the NixSiy alloy layer, the problems of corrosion and peeling of the alloy layer during oxide removal were solved, thereby improving the structural integrity and electrical performance stability of the alloy layer, increasing product yield and reducing costs.
Patent Information
- Application Number
- CN202611154541.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-31
- Publication Date
- 2026-11-17
AI Technical Summary
In the prior art, the NixSiy alloy layer is easily eroded and peeled off by the corrosive solution during the oxide layer removal process, which leads to ohmic contact failure, high contact resistance and poor consistency of the device, affecting production yield and cost.
After the NixSiy alloy layer is formed by high-temperature alloying, a photoresist protection step is added. The photoresist fills and covers the upper surface and all sidewalls of the alloy layer to form a sealed protective layer, which isolates the contact between the etching solution and the alloy layer. Then the oxide layer is removed.
It effectively prevents the alloy layer from corroding and falling off during the oxide layer removal process, improves the structural integrity and electrical performance stability of the alloy layer, increases product yield, reduces mass production scrap costs, has a wide range of applications, and is highly robust to the process.
Smart Images

Figure CN123124679A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor manufacturing technology, and in particular to a semiconductor fabrication method using photoresist protection. Background Technology
[0002] NixSiy nickel-silicon alloy is a commonly used ohmic contact functional layer in semiconductor devices. It has advantages such as low resistivity, excellent contact characteristics, and strong process adaptability, and is widely used in the fabrication of various semiconductor power devices and integrated circuit devices.
[0003] In related technologies, the conventional preparation process of NixSiy alloy is relatively fixed. Generally, it is as follows: a thick SiO2 oxide layer is deposited on the surface of a wafer substrate, a pattern window of a specified size is formed by photolithography and etching, then metallic nickel is deposited in the pattern window, the metal layer is stabilized by low-temperature rapid heat treatment, the excess nickel layer on the surface is cleaned and removed, and then nickel-silicon alloying is achieved by high-temperature rapid heat treatment. Finally, the surface SiO2 oxide layer is removed by wet etching to complete the preparation of the core structure of the device.
[0004] The inventors discovered that the aforementioned conventional process has unavoidable technical defects during mass production: the NixSiy alloy layer formed after high-temperature alloying has limited chemical stability and poor resistance to wet etching solutions. In the subsequent wet process for removing the SiO2 oxide layer, the exposed NixSiy alloy layer comes into direct contact with acidic or alkaline etching solutions, making it highly susceptible to erosion and peeling, resulting in defects such as alloy layer breakage, localized detachment, or even complete peeling. This defect directly leads to ohmic contact failure, high and inconsistent contact resistance, resulting in poor electrical properties, reduced production yield, and increased production costs.
[0005] Most optimization methods for this problem in related technologies are passive adjustments such as adjusting the concentration of the chemical solution, shortening the corrosion time, and lowering the corrosion temperature. These methods cannot fundamentally isolate the chemical solution from the NixSiy alloy layer, resulting in limited protective effects. At the same time, they are prone to secondary process problems such as incomplete removal of the SiO2 oxide layer, narrow process window, and poor batch consistency. They have never been able to effectively solve the core problem of NixSiy alloy layer falling off in the chemical solution.
[0006] Furthermore, if a dry method is used to remove the SiO2 oxide layer to avoid exposing the alloy layer to the etching solution, it will be limited by factors such as etching selectivity, device surface damage, and production capacity, making it difficult to directly replace the mature wet removal process. If an additional corrosion-resistant passivation film is deposited on the surface of the alloy layer for protection, new deposition and patterning equipment and processes are required, which not only increases the process complexity and cost, but the passivation film is often difficult to completely remove after the oxide layer is removed, and it is easy to remain on the surface of the alloy layer, affecting device performance. Therefore, how to isolate the contact between the etching solution and the NixSiy alloy layer from the process source without changing the existing mature process or introducing special equipment, and prevent the alloy layer from being corroded and detached during the oxide layer removal process, has become a technical problem that urgently needs to be solved in this field.
[0007] Therefore, it is necessary to propose a processing method to solve the above problems from the source of the process. Summary of the Invention
[0008] The present invention aims to provide a semiconductor fabrication method using photoresist protection to overcome the shortcomings of the prior art. The technical problem to be solved by the present invention is achieved through the following technical solution.
[0009] According to a first aspect of this application, a method for fabricating a semiconductor using photoresist protection is provided, the method comprising:
[0010] A SiO2 oxide layer is deposited on the surface of a semiconductor wafer substrate, and the SiO2 oxide layer is patterned by etching to form a pattern window;
[0011] After depositing a metallic Ni layer within the graphics window, the wafer undergoes low-temperature RTP heat treatment.
[0012] After removing the residual nickel from the surface of the SiO2 oxide layer, the wafer is subjected to high-temperature alloying RTP heat treatment, which causes the metallic Ni layer in the pattern window to react with the substrate silicon material to form a NixSiy alloy layer;
[0013] Photoresist is coated on the wafer surface and then exposed and developed to completely fill and cover the upper surface and all sidewalls of the NixSiy alloy layer, sealing off all exposed areas of the NixSiy alloy layer and forming a sealed photoresist protective layer.
[0014] While retaining the photoresist protective layer, the SiO2 oxide layer is removed using a wet process, with the photoresist protective layer preventing the wet process from contacting the NixSiy alloy layer.
[0015] The photoresist protective layer is removed to obtain the NixSiy alloy structure.
[0016] Preferably, the SiO2 oxide layer is deposited using plasma-enhanced chemical vapor deposition, and the thickness of the SiO2 oxide layer is 0.5~2μm.
[0017] Preferably, the pattern etching of the SiO2 oxide layer includes: photolithography of the SiO2 oxide layer, and dry etching process to form the pattern window of the SiO2 oxide layer, and after etching, removing residual photoresist and cleaning the wafer.
[0018] Preferably, the Ni layer is deposited in the graphics window using a magnetron sputtering process, and the thickness of the Ni layer is 100~500nm.
[0019] Preferably, the temperature of the low-temperature RTP heat treatment is 600~750℃.
[0020] Preferably, removing residual nickel from the surface of the SiO2 oxide layer includes: cleaning the wafer surface with a metal cleaning solution to remove free metal Ni adhering to the surface of the SiO2 oxide layer, while retaining the metal Ni layer within the pattern window.
[0021] Preferably, the temperature of the high-temperature alloying RTP heat treatment is 850~1000℃.
[0022] Preferably, the photoresist is a positive photoresist or a negative photoresist, and the photoresist is applied using a spin coating process, with a thickness of 1~5μm.
[0023] Preferably, the wet etching solution is a hydrofluoric acid-based buffered oxide etching solution.
[0024] Preferably, the low-temperature RTP heat treatment and the high-temperature alloying RTP heat treatment are performed in an N2 atmosphere or an Ar atmosphere; the removal of the photoresist protective layer is performed by organic solvent removal or plasma ashing removal.
[0025] The embodiments of the present invention have the following advantages:
[0026] This invention adds a photoresist protective coating step after the NixSiy alloy layer is formed by high-temperature alloying and before the SiO2 oxide layer is removed. This allows the photoresist to completely fill and coat the upper surface and all sidewalls of the NixSiy alloy layer, forming a sealed protective layer. Throughout the wet oxide layer removal process, the NixSiy alloy layer is completely physically isolated from the etching solution. This completely eliminates the problem of corrosion, damage, and detachment of the alloy layer during the oxide layer removal process from the source of the process, thereby improving the structural integrity and electrical performance stability of the NixSiy alloy layer.
[0027] This invention retains the original core process steps and parameters such as deposition, etching, and annealing, and only adds conventional photolithography and resist removal processes. It does not require new special equipment or major process adjustments, and is compatible with existing semiconductor mass production lines. The modification cost is low and the difficulty of mass production implementation is low.
[0028] The photoresist protective layer of the present invention has uniform forming and good sealing performance. There is no penetration or peeling during wet etching, and there is no residue, oxidation or impurity contamination in the subsequent photoresist removal process. It will not cause secondary damage to the substrate and alloy layer, and will not affect subsequent packaging, testing and other processes.
[0029] This invention replaces the passive protection method that relies on fine-tuning of chemical solution parameters in related technologies with physical isolation, which greatly expands the process window for oxide layer removal, improves batch production consistency, significantly increases product yield, and reduces mass production scrap costs.
[0030] The photoresist protective coating step of the present invention completely coats the upper surface and all sidewalls of the NixSiy alloy layer. In particular, it achieves reliable sealing of the weak part of the alloy layer sidewall, which is most easily penetrated by the corrosion solution in related technologies. Thus, it can obtain a stable protective effect under process conditions with different oxide layer thickness and different alloy layer thickness, and has a wide range of applications and strong process robustness. Attached Figure Description
[0031] Figure 1 This is a flowchart of the steps of a semiconductor fabrication method using photoresist protection according to the present invention;
[0032] Figure 2 This is a schematic diagram of the structure protected by photoresist in step S9 of the present invention.
[0033] Figure 3 yes Figure 2 A schematic diagram of the structure observed by a scanning electron microscope. Detailed Implementation
[0034] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. The present invention will now be described in detail with reference to the accompanying drawings and embodiments.
[0035] It should be noted that the above detailed descriptions are exemplary and intended to provide further explanation of this application. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains.
[0036] The raw materials, equipment, and testing methods used in the various embodiments and comparative examples of this invention are as follows, and are common to all embodiments and comparative examples: the semiconductor wafer substrate 1 is a single-crystal silicon wafer; the SiO2 oxide layer 2 is deposited using plasma-enhanced chemical vapor deposition (PECVD); the metallic Ni layer is deposited using magnetron sputtering, with a high-purity nickel target as the target material; both low-temperature RTP heat treatment and high-temperature alloying RTP heat treatment are performed in a rapid thermal annealing (RTP) device under a N2 protective atmosphere; the photoresist protective layer is applied using a spin coater and then exposed and patterned using a photolithography machine and a developer; the wet removal of the SiO2 oxide layer uses a hydrofluoric acid-based buffered oxide etchant (BOE); the photoresist is removed using an organic solvent or plasma ashing. The structural integrity of the alloy layer is observed using an optical microscope and a scanning electron microscope, and the contact resistance and yield are evaluated using conventional device electrical testing methods.
[0037] Example 1
[0038] This embodiment provides a semiconductor processing method that utilizes photoresist to fill an oxide layer to protect a metal layer, combined with... Figure 1 The process flow shown is as follows, with specific steps as follows.
[0039] Step S1, Substrate Pretreatment: Select a qualified single-crystal silicon semiconductor wafer substrate 1, and sequentially perform organic solvent cleaning, pure water rinsing, and drying to remove particles, oil, and impurities from the wafer surface, ensuring the cleanliness of the wafer surface, and set it aside for later use. The organic solvent cleaning is used to remove organic contaminants from the wafer surface, the pure water rinsing is used to remove cleaning residue and soluble impurities, and the drying process is used to remove moisture from the wafer surface to ensure the quality of subsequent film deposition.
[0040] Step S2, SiO2 oxide layer deposition: A SiO2 oxide layer 2 is uniformly deposited on the surface of the pretreated wafer substrate 1 using PECVD technology. The deposition thickness is 1 μm, resulting in a uniform, dense film free of pinholes. The SiO2 oxide layer 2 serves two purposes: firstly, as a dielectric layer for subsequent pattern etching to form pattern windows; and secondly, as an isolation and protection layer for areas outside the pattern windows during the alloying process, preventing metallic Ni from reacting with the substrate silicon in non-window areas.
[0041] Step S3, Pattern Etching: The SiO2 oxide layer 2 is subjected to standard photolithography. After exposure and development, the SiO2 oxide layer 2 is etched using a dry etching process to form a precise pattern window with critical dimension CD. After etching, residual photoresist is removed and the wafer is cleaned.
[0042] Step S4, Ni deposition: A high-purity Ni layer is deposited on the patterned window area of the wafer and the surface of the SiO2 oxide layer 2 using magnetron sputtering. The thickness of the Ni layer is 300 nm to ensure good adhesion and uniform thickness of the metal layer.
[0043] Step S5, Low-Temperature RTP Heat Treatment: The wafer after depositing the metallic Ni layer is fed into an RTP device and subjected to rapid heat treatment at 700°C in an N2 atmosphere to stabilize the metallic Ni layer structure, eliminate internal stress in the metal layer, and improve adhesion performance. The temperature of the low-temperature RTP heat treatment is lower than that of the high-temperature alloying RTP heat treatment. Its purpose is to first stabilize the metallic Ni layer structure and ensure its firm adhesion to the substrate, providing a good foundation for subsequent high-temperature alloying and preventing the metallic Ni layer from peeling off in subsequent processes.
[0044] Step S6, Residual Nickel Cleaning: The wafer surface is cleaned with a metal cleaning solution to remove excess free Ni metal adhering to the SiO2 oxide layer 2, retaining only the Ni metal layer within the pattern window, ensuring a clean surface free of excess metal residue. This residual nickel cleaning only removes free Ni metal from the SiO2 oxide layer 2 surface that has not participated in alloying, without affecting the Ni metal layer within the pattern window, thus ensuring that subsequent high-temperature alloying proceeds directionally within the pattern window.
[0045] Step S7, High-Temperature Alloying RTP Heat Treatment: The cleaned wafer is subjected to high-temperature rapid heat treatment at 950°C under N2 atmosphere to fully alloy the metallic Ni and the substrate silicon material within the pattern window, generating a NixSiy alloy layer 3 with stable structure and excellent resistivity. The NixSiy alloy formed by the reaction of metallic Ni and silicon at high temperature serves as the ohmic contact functional layer of the device, exhibiting low resistivity and excellent contact characteristics. Since the alloying reaction only occurs in the contact area between metallic Ni and substrate silicon within the pattern window, the NixSiy alloy layer 3 is confined within the pattern window. Its upper surface and sidewalls are surrounded by the subsequently formed photoresist protective layer and SiO2 oxide layer 2, respectively, before the SiO2 oxide layer 2 is removed.
[0046] Step S8, Photoresist Protective Coating: After the alloying process, the wafer is cleaned, and a positive photoresist is uniformly coated onto the wafer surface using a spin-coating process. The photoresist coating thickness is 3μm. Through precise exposure and development patterning, only the photoresist structure completely covering the upper surface and all sidewalls of the NixSiy alloy layer 3 is retained, ensuring that all exposed areas of the NixSiy alloy layer 3 are completely filled and coated with photoresist, forming a sealed and corrosion-resistant photoresist protective layer. In this step, the photoresist protective layer extends downwards along the upper surface of the NixSiy alloy layer 3 and completely covers all its sidewalls, forming a continuous and sealed physical isolation barrier between the NixSiy alloy layer 3 and the external etching solution, with no exposed areas or gaps where the etching solution can penetrate.
[0047] Step S9, Wet removal of SiO2 oxide layer: such as Figure 2As shown, a hydrofluoric acid-based buffered oxide etching solution is used to perform wet etching on the wafer to completely remove the SiO2 oxide layer 2 on the wafer surface. During this process, a photoresist protective layer stably isolates the etching solution, preventing it from contacting the NixSiy alloy layer 3 and thus avoiding corrosion and detachment of the NixSiy alloy layer 3. In this step, the etching solution only reacts with the SiO2 oxide layer 2 that needs to be removed, while the NixSiy alloy layer 3, covered by the photoresist protective layer, remains isolated from the etching solution. Even if the etching time is extended to ensure the complete removal of the SiO2 oxide layer 2, the NixSiy alloy layer 3 will not be damaged by over-etching, thereby broadening the process window for oxide layer removal.
[0048] Step S10, Photoresist Removal: After removing the SiO2 oxide layer 2, the photoresist protective layer is removed using an organic solvent, ultimately obtaining a complete, corrosion-free, and non-detached NixSiy alloy layer 3 structure. Figure 3 As shown, since the photoresist protective layer is an organic material, it can be completely removed by using organic solvents or plasma ashing. After removal, there is no residue, oxidation, or impurity contamination on the surface of NixSiy alloy layer 3, and it will not cause secondary damage to NixSiy alloy layer 3 and substrate 1, and will not affect subsequent packaging, testing and other processes.
[0049] Example 2
[0050] The processing method in this embodiment is basically the same as that in Embodiment 1, except that the process parameters are taken from values close to the lower end of the range. Specifically, in step S2, the deposition thickness of the SiO2 oxide layer 2 is 0.5 μm; in step S4, the thickness of the metallic Ni layer is 100 nm; in step S5, the temperature of the low-temperature RTP heat treatment is 600 °C; in step S7, the temperature of the high-temperature alloying RTP heat treatment is 850 °C; and in step S8, a negative photoresist is used, with a photoresist coating thickness of 1 μm. The remaining steps and conditions are the same as in Embodiment 1.
[0051] In this embodiment, in step S8, the photoresist completely covers the upper surface and all sidewalls of the NixSiy alloy layer 3. During the wet removal of the SiO2 oxide layer 2 in step S9, the photoresist protective layer effectively isolates the etching solution, and the NixSiy alloy layer 3 does not rust off.
[0052] Example 3
[0053] The processing method in this embodiment is basically the same as that in Embodiment 1, except that the process parameters are taken from values close to the upper end of the range. Specifically, in step S2, the deposition thickness of the SiO2 oxide layer 2 is 2 μm; in step S4, the thickness of the metallic Ni layer is 500 nm; in step S5, the temperature of the low-temperature RTP heat treatment is 750 °C; in step S7, the temperature of the high-temperature alloying RTP heat treatment is 1000 °C; in step S8, the photoresist coating thickness is 5 μm, and in step S10, the photoresist protective layer is removed by plasma ashing. The remaining steps and conditions are the same as in Embodiment 1.
[0054] In this embodiment, under the condition of a relatively thick SiO2 oxide layer 2, the photoresist coating thickness is increased in step S8 to ensure that the photoresist completely covers the upper surface and all sidewalls of the NixSiy alloy layer 3; during the wet removal process in step S9, the photoresist protective layer stably isolates the corrosive solution, and the NixSiy alloy layer 3 has a complete structure and no corrosion or peeling.
[0055] Example 4
[0056] The processing method in this embodiment is basically the same as that in Embodiment 1, except that: negative photoresist is used in step S8, and the photoresist coating thickness is 2μm; the SiO2 oxide layer 2 is removed by wet etching with hydrofluoric acid-based buffered oxide solution in step S9; the photoresist protective layer is removed by plasma ashing in step S10; both the low-temperature RTP heat treatment and the high-temperature alloying RTP heat treatment are performed in an Ar atmosphere. The remaining steps and conditions are the same as in Embodiment 1.
[0057] In this embodiment, after exposure and development, the negative photoresist completely fills and covers the upper surface and all sidewalls of the NixSiy alloy layer 3, and stabilizes and isolates the etching solution during the wet removal of the SiO2 oxide layer 2 in step S9; in step S10, plasma ashing is used to remove the photoresist, and after the photoresist is removed, there is no residue, oxidation, or impurity contamination on the surface of the alloy layer.
[0058] Comparative Example 1
[0059] This comparative example uses conventional processes from related technologies. The difference from Example 1 is that the photoresist protection coating step S8 and the photoresist removal step S10 are omitted. That is, after the NixSiy alloy layer 3 is generated by high-temperature alloying RTP heat treatment in step S7, the SiO2 oxide layer 2 is directly removed by wet etching with hydrofluoric acid-based buffered oxide solution in step S9. The remaining steps and conditions are the same as in Example 1.
[0060] In this comparative example, during the wet removal of the SiO2 oxide layer 2, the exposed NixSiy alloy layer 3 was in direct contact with the corrosive solution, and the alloy layer showed obvious erosion, damage and local detachment.
[0061] Comparative Example 2
[0062] The difference between this comparative example and Example 1 is that in step S8, the photoresist only covers the upper surface of the NixSiy alloy layer 3, but does not cover its sidewalls; that is, the sidewalls of the NixSiy alloy layer 3 remain exposed. All other steps and conditions are the same as in Example 1.
[0063] In this comparative example, during the wet removal of the SiO2 oxide layer 2 in step S9, the corrosive solution penetrates from the exposed sidewall of the NixSiy alloy layer 3, causing the alloy layer to be eroded from the sidewall and peel off.
[0064] The process parameters and performance comparisons of each embodiment and comparative example are shown in Table 1:
[0065] Table 1. Comparison of process parameters and performance between each embodiment and the comparative example.
[0066] As shown in Table 1, in Examples 1 to 4, the photoresist completely covered the upper surface and all sidewalls of the NixSiy alloy layer 3 during the oxide layer removal process, achieving complete physical isolation of the etching solution. The alloy layer shedding rate was significantly lower than that of Comparative Example 1 and Comparative Example 2, and the device yield was significantly higher than that of Comparative Example 1 and Comparative Example 2.
[0067] Explanation of the synergistic effect of protection mechanism and process
[0068] It should be noted that the core of this invention lies in the adjustment of the process sequence, namely, inserting a photoresist protective coating step S8 after the high-temperature alloying RTP heat treatment to generate the NixSiy alloy layer 3 and before the wet removal of the SiO2 oxide layer 2. In the conventional process of related technologies, the oxide layer is directly removed after high-temperature alloying, at which point the upper surface and sidewalls of the NixSiy alloy layer 3 are exposed, and the etching solution can erode the alloy layer from all directions. Due to the limited chemical stability of the NixSiy alloy layer 3 generated by high-temperature alloying and its poor resistance to acidic or alkaline etching solutions, the alloy layer will be gradually eroded from the surface and sidewalls under the continuous action of the solution, resulting in damage, local detachment, or even complete peeling.
[0069] This invention utilizes the properties of photoresist—its resistance to semiconductor wet etching solutions and its chemical stability—to completely fill and cover all exposed areas of the NixSiy alloy layer 3 with photoresist before the oxide layer removal process, forming a sealed photoresist protective layer. Throughout the wet removal of the SiO2 oxide layer 2 in step S9, the photoresist protective layer acts as a physical barrier, completely separating the etching solution from the NixSiy alloy layer 3. The etching solution only reacts with the SiO2 oxide layer 2 to be removed, without contacting the covered NixSiy alloy layer 3, thus eliminating the possibility of corrosion and detachment of the alloy layer from the process source. After the SiO2 oxide layer 2 is completely removed, the photoresist protective layer is removed in step S10, resulting in a structurally intact, corrosion-free, and detached NixSiy alloy layer 3.
[0070] Furthermore, the complete coverage of the NixSiy alloy layer 3 sidewalls by the photoresist is crucial for the protective effect. As shown in Comparative Example 2, when the photoresist only covers the upper surface of the NixSiy alloy layer 3 while the sidewalls are exposed, the etching solution will penetrate from the exposed sidewalls and gradually extend along the interface between the alloy layer and the substrate, ultimately leading to the erosion and peeling of the alloy layer. Therefore, in step S8 of this invention, by controlling the coating thickness of the photoresist and the exposure and development patterns, it is ensured that the photoresist not only covers the upper surface of the NixSiy alloy layer 3 but also extends downwards to cover all its sidewalls, thus sealing off all exposed areas of the NixSiy alloy layer 3 to achieve a reliable isolation and protection effect.
[0071] It should also be noted that the present invention retains the core process steps and process parameters of the mature deposition, etching, and annealing processes in the relevant technologies. The core processes, including the deposition thickness of the SiO2 oxide layer 2, the critical size CD of the pattern window, the deposition thickness of the metal Ni layer, and the temperatures of low-temperature RTP heat treatment and high-temperature alloying RTP heat treatment, do not need to be modified. Only the photoresist protection coating step S8 and the photoresist removal step S10 are added to the original process flow. The photoresist protection coating step S8 and the photoresist removal step S10 can be implemented using existing photolithography equipment and photoresist removal equipment in semiconductor mass production lines. There is no need to introduce special equipment or make significant adjustments to the existing process. Therefore, it has good process compatibility and low modification costs, which facilitates mass production.
[0072] Those skilled in the art should understand that the parameters given in the above embodiments, such as the deposition thickness of the SiO2 oxide layer 2, the thickness of the metallic Ni layer, the low-temperature RTP heat treatment temperature, the high-temperature alloying RTP heat treatment temperature, and the photoresist coating thickness, are all exemplary values. Adjustments within the range defined in the claims can achieve the purpose of the present invention. The photoresist can be a positive or negative photoresist, and the wet etching solution is not limited to hydrofluoric acid-based buffered oxide etching solution. Any wet etching solution capable of removing the SiO2 oxide layer 2 without damaging the photoresist protective layer is applicable. The photoresist removal method is not limited to organic solvent removal or plasma ashing removal. All the above variations do not depart from the concept of the present invention.
[0073] Furthermore, the processing method described in this invention is not only applicable to the fabrication of devices using single-crystal silicon wafers as substrates and NixSiy alloy layer 3 as the ohmic contact functional layer, but also to other semiconductor processing scenarios where the metal or alloy layer is easily eroded or detached by the etching solution during the wet oxide removal process. The photoresist protective coating step of this invention can also be used, i.e., after the metal or alloy layer is formed and before the wet oxide removal, the upper surface and all sidewalls of the metal or alloy layer are completely filled and coated with photoresist. Then, the wet oxide removal is performed while retaining the photoresist protective layer, and the photoresist is removed after the oxide layer is removed, thereby achieving reliable protection for the metal or alloy layer. The above-mentioned expansion of application scenarios should also be included within the scope of protection of this invention.
[0074] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the exemplary embodiments according to this application. As used herein, the singular form is intended to include the plural form as well, unless the context clearly indicates otherwise. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.
[0075] It should be noted that the terms "first," "second," etc., used in the specification, claims, and accompanying drawings of this application are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such terms can be used interchangeably where appropriate so that the embodiments of this application described herein can be implemented in sequences other than those illustrated or described herein.
[0076] Furthermore, the terms “comprising” and “having”, and any variations thereof, are intended to cover non-exclusive inclusion. For example, a process, method, system, product, or apparatus that includes a series of steps or units is not necessarily limited to those steps or units that are explicitly listed, but may include other steps or units that are not explicitly listed or that are inherent to such process, method, product, or apparatus.
[0077] For ease of description, spatial relative terms such as "above," "on top of," "on the upper surface of," "above," etc., are used herein to describe the spatial positional relationship of a device or feature as shown in the figures to other devices or features. It should be understood that spatial relative terms are intended to encompass different orientations in use or operation beyond the orientation of the device as described in the figures. For example, if the device in the figures were inverted, a device described as "above" or "on top of" other devices or structures would subsequently be positioned as "below" or "under" other devices or structures. Thus, the exemplary term "above" can include both "above" and "below." The device may also be positioned in other different ways, such as rotated 90 degrees or in other orientations, and the spatial relative descriptions used herein will be interpreted accordingly.
[0078] In the detailed description above, reference has been made to the accompanying drawings, which form part of this document. In the drawings, similar symbols typically identify similar parts unless the context otherwise indicates otherwise. The illustrated embodiments described in the detailed specification, drawings, and claims are not intended to be limiting. Other embodiments may be used and other changes may be made without departing from the spirit or scope of the subject matter presented herein.
[0079] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A semiconductor fabrication method utilizing photoresist protection, characterized in that, The method includes: A SiO2 oxide layer is deposited on the surface of a semiconductor wafer substrate, and the SiO2 oxide layer is patterned by etching to form a pattern window; After depositing a metallic Ni layer within the graphics window, the wafer undergoes low-temperature RTP heat treatment. After removing the residual nickel from the surface of the SiO2 oxide layer, the wafer is subjected to high-temperature alloying RTP heat treatment, which causes the metallic Ni layer in the pattern window to react with the substrate silicon material to form a NixSiy alloy layer; Photoresist is coated on the wafer surface and then exposed and developed to completely fill and cover the upper surface and all sidewalls of the NixSiy alloy layer, sealing off all exposed areas of the NixSiy alloy layer and forming a sealed photoresist protective layer. While retaining the photoresist protective layer, the SiO2 oxide layer is removed using a wet process, with the photoresist protective layer preventing the wet process from contacting the NixSiy alloy layer. The photoresist protective layer is removed to obtain the NixSiy alloy structure.
2. The semiconductor fabrication method using photoresist protection according to claim 1, characterized in that, The SiO2 oxide layer is deposited using plasma-enhanced chemical vapor deposition, and the thickness of the SiO2 oxide layer is 0.5~2μm.
3. The semiconductor fabrication method using photoresist protection according to claim 1, characterized in that, The pattern etching of the SiO2 oxide layer includes: performing photolithography on the SiO2 oxide layer, and using a dry etching process to etch the SiO2 oxide layer to form the pattern window. After etching, residual photoresist is removed and the wafer is cleaned.
4. The semiconductor fabrication method using photoresist protection according to claim 1, characterized in that, The Ni layer is deposited in a graphics window using a magnetron sputtering process, and the thickness of the Ni layer is 100~500nm.
5. The semiconductor fabrication method using photoresist protection according to claim 1, characterized in that, The temperature of the low-temperature RTP heat treatment is 600~750℃.
6. The semiconductor fabrication method using photoresist protection according to claim 1, characterized in that, The process of removing residual nickel from the surface of the SiO2 oxide layer includes: cleaning the wafer surface with a metal cleaning solution to remove the free metal Ni adhering to the surface of the SiO2 oxide layer, while retaining the metal Ni layer within the graphic window.
7. The semiconductor fabrication method using photoresist protection according to claim 1, characterized in that, The high-temperature alloying RTP heat treatment temperature is 850~1000℃.
8. The semiconductor fabrication method using photoresist protection according to claim 1, characterized in that, The photoresist is either a positive or negative photoresist, and the photoresist is applied using a spin coating process, with a thickness of 1~5μm.
9. The semiconductor fabrication method using photoresist protection according to claim 1, characterized in that, The wet etching solution is a hydrofluoric acid-based buffered oxide etching solution.
10. The semiconductor fabrication method using photoresist protection according to claim 1, characterized in that, The low-temperature RTP heat treatment and the high-temperature alloying RTP heat treatment are performed in an N2 atmosphere or an Ar atmosphere; the removal of the photoresist protective layer is performed by organic solvent removal or plasma ashing removal.