Fabrication method, etching apparatus and semiconductor equipment for high aspect ratio etched structures

By depositing metal nitride or carbonitride protective films on the sidewalls of the etching tank, the problem of vertical morphology distortion in high aspect ratio etching structures was solved, thereby improving the stability and electrical performance of the etching structure.

CN123124689APending Publication Date: 2026-11-17SHENZHEN SICARRIER IND MACHINES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611255853.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

During high aspect ratio etching, the vertical morphology of the etched structure is prone to distortion, which leads to a decrease in the electrical performance of semiconductor devices, and existing technologies are unable to effectively solve this problem.

Method used

By depositing a protective film on the sidewall of the etching tank and using alternating cycles of reactive gas and precursor gas, a metal nitride or metal carbonitride protective layer is generated. This prevents lateral etching of the sidewall and avoids charge accumulation at the bottom, allowing for precise control of the etching amount and the thickness of the protective film, thus achieving stability and accuracy in the etching morphology.

Benefits of technology

It improves the vertical topography accuracy of the etched structure, enhances the electrical performance and manufacturing yield of semiconductor devices, and reduces the probability of etch topography distortion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124689A_ABST
    Figure CN123124689A_ABST
Patent Text Reader

Abstract

This application discloses a method, etching apparatus, and semiconductor equipment for fabricating a high aspect ratio etched structure. The method includes the following steps: providing a substrate to be etched; cyclically alternating between etching and deposition processes on the substrate to form an etching trench of a predetermined depth; the deposition process includes: introducing a precursor gas and a reactive gas into an etching chamber to deposit a protective film of a target thickness on the sidewall of the etching trench; and purging out the precursor gas, reactive gas, and deposition byproducts. The protective film includes a metal nitride protective layer generated by the reaction of H radicals in the reactive gas with imino ligands in the precursor gas; and / or, the protective film includes a metal carbonitride protective layer generated by the reaction of H radicals in the reactive gas with amino ligands in the precursor gas. This reduces the probability of morphological distortion of the high aspect ratio etched structure during vertical etching.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the technical field of semiconductor etching, and in particular to a method for fabricating a high aspect ratio etched structure, an etching apparatus, and a semiconductor device. Background Technology

[0002] As semiconductor memory and logic devices evolve towards higher density and integration, the aspect ratio of etched structures continues to increase. However, during high aspect ratio etching, incident ions undergo angular deflection after being scattered by the sidewalls upon entering the etching trench. Furthermore, the charge shielding effect generated by the accumulation of positive ions at the bottom of the etching trench exacerbates the trajectory deflection of incident ions, leading to distortion of the vertical morphology of the etched structure. Simultaneously, the excessive consumption of free radicals on the sidewalls of the etching trench results in insufficient free radical concentration at the etching front, causing the etching rate to decrease with increasing aspect ratio. This can lead to problems such as conical morphology or even etching termination. The vertical morphology distortion of the etched structure affects the electrical performance of semiconductor devices. Summary of the Invention

[0003] This application discloses a method for fabricating a high aspect ratio etched structure, an etching apparatus, and a semiconductor device, which can reduce the probability of morphological distortion of the high aspect ratio etched structure during vertical etching.

[0004] In a first aspect, embodiments of this application provide a method for fabricating a high aspect ratio etched structure, comprising the following steps: providing a substrate to be etched; cyclically alternatingly performing etching and deposition processes on the substrate to be etched to form an etching trench of a predetermined depth on the substrate; wherein the deposition process includes: introducing a precursor gas and a reactive gas into an etching chamber to deposit a protective film of a target thickness on the sidewall of the etching trench, and purging out the precursor gas, the reactive gas, and deposition byproducts; wherein the protective film comprises a metal nitride protective layer generated by the reaction of H free radicals in the reactive gas and imino ligands in the precursor gas; and / or, the protective film comprises a metal carbonitride protective layer generated by the reaction of H free radicals in the reactive gas and amino ligands in the precursor gas.

[0005] The method for fabricating high aspect ratio etched structures provided in this application has several advantages. First, the protective film prevents lateral etching of the sidewalls, reducing damage to the sidewalls from free radicals and neutral species such as HF, H, and F, and improving the utilization rate of these free radicals during the etching process. Simultaneously, the metal nitride and / or metal carbonitride protective layers can prevent the accumulation of residual positive charges at the bottom of the etching trench, reducing ion scattering and avoiding distortion of the vertical etching morphology. Second, the method of alternating etching and deposition processes decouples the sidewall passivation deposition of the protective film from the etching of the substrate. This allows for precise control of the etching amount, etching time, and the thickness of the protective film formed in each deposition process, reducing the probability of morphological distortion of the high aspect ratio etched structure during vertical etching, improving the electrical performance of semiconductor devices, and ultimately increasing their manufacturing yield.

[0006] In conjunction with the first aspect, in one possible implementation, the input of precursor gas and reactant gas into the etching chamber includes: inputting the reactant gas into the etching chamber through a first input gas path, and inputting the precursor gas into the etching chamber through a second input gas path, wherein the first input gas path is independent of the second input gas path. Thus, by independently controlling the intake of the precursor gas and reactant gas, the thickness of the protective film deposited on the sidewall of the etching tank can be precisely controlled. This achieves separate delivery of precursor gas and reactant gas or other process gases, and independent regulation of the flow rate, on / off timing, and supply pressure of each gas path, avoiding premature pre-reaction of different gases in the delivery pipeline, the generation of particulate matter, or corrosion of the pipeline; simultaneously, it allows for individual matching of the precursor gas supply process window, precise control of the precursor gas concentration in the etching chamber, flexible switching of gas ratios for different process stages such as etching, passivation, and cleaning, preventing gas crosstalk between gas paths, and improving etching morphology, etching rate, and process repeatability.

[0007] In conjunction with the first aspect, in one possible implementation, before introducing the precursor gas and reactant gas into the etching chamber, the fabrication method further includes: introducing the precursor gas into a buffer chamber connected to the second input gas path; and adjusting the gas pressure in the buffer chamber to be greater than or equal to twice the gas pressure in the etching chamber. Thus, the buffer chamber can stabilize the flow rate and partial pressure of the precursor gas, avoiding interference with the precursor gas delivery caused by pressure fluctuations and airflow disturbances within the etching chamber, thereby improving the uniformity and stability of the precursor gas input. Simultaneously, utilizing the pressure difference between the buffer chamber and the etching chamber allows the precursor gas to enter the etching chamber more smoothly and controllably, reducing gas pulse impacts and instantaneous concentration fluctuations, improving the consistency of the precursor gas undergoing chemical adsorption and hydrogenation or hydrogenolysis reactions on the sidewall of the etching tank, thereby improving the uniformity of the protective film deposition thickness and the film quality, and enhancing the repeatability and structural precision of the etching process.

[0008] In conjunction with the first aspect, in one possible implementation, the step of inputting the precursor gas into the etching chamber through the second input gas path includes: inputting the precursor gas into the etching chamber through the second input gas path while maintaining the temperature of the precursor gas within the second input gas path within a target temperature range, wherein the target temperature range is 50℃-150℃. Therefore, by maintaining the temperature of the precursor gas within the second input gas path within the target temperature range, the risk of the precursor gas cooling down and condensing in the delivery pipeline is reduced, improving the stability and reliability of the precursor gas's consistently gaseous delivery, reducing material loss and pipeline blockage problems, stabilizing the delivery state of the precursor gas, improving the overall control accuracy of the precursor gas's flow rate and supply, and enhancing process stability.

[0009] In conjunction with the first aspect, in one possible implementation, the temperature of the substrate to be etched during the etching process is -100℃ to 100℃. Therefore, under the low-temperature environment of -100℃ to 100℃ during the etching process, H2O and HF from the etching byproducts generated in the etching reaction will physically adsorb onto the sidewalls of the etching tank via hydrogen bonds, forming a co-solution film. This co-solution film can chemically adsorb precursor gases to form a metal oxide protective layer, preventing HF from reacting with the sidewalls of the etching tank, reducing HF consumption, and increasing the vertical etching rate of the substrate. Simultaneously, H2O and HF can also react to generate HF2. - and H3O + , and HF2 - As a key active ion for etching, it can suppress thermal decomposition and recombination loss at low temperatures, and adsorb well on the surface of the substrate to be etched and participate in chemical reactions to achieve directional etching of the substrate.

[0010] In conjunction with the first aspect, in one possible implementation, the fabrication method further includes: increasing the temperature of the substrate to be etched after the etching process is completed. Therefore, after etching, the control system controls the temperature control system to raise the substrate temperature. On the one hand, the heated substrate can improve the adsorption activity and reaction kinetics of the precursor gas, promoting the precursor gas to fully undergo chemical reaction and uniformly deposit on the surface of the etched structure to form a dense and continuous protective film. At the same time, the protective film can quickly remove the residual positive charge accumulated at the bottom of the etching tank, suppress the charge shielding effect, reduce ion scattering of plasma, prevent distortion of vertical etching morphology, stabilize the steepness of the sidewalls and the flatness of the bottom of the high aspect ratio etching tank, and optimize the consistency of the overall etching process morphology. On the other hand, the heated substrate can increase the saturated vapor pressure of the precursor gas, promoting the full volatilization and discharge of excess precursor gas that did not participate in the formation of the protective film in the etching tank. This avoids the continuous deposition of excessive precursor gas to form an overly thick residual protective film, which could cause blockage of the etching tank opening and dimensional deviation. At the same time, it promotes the desorption of by-products inside the formed protective film, optimizes the density and uniformity of the protective film, reduces particulate contamination in the etching chamber, and facilitates subsequent processes.

[0011] In conjunction with the first aspect, in one possible implementation, the fabrication method further includes: after completing the preceding etching process, adjusting the temperature of the subsequent etching process to be lower than the temperature of the preceding etching process. Understandably, the deeper the etching depth, the greater the ion flux attenuation. This embodiment of the application improves the structural stability of the protective film formed by the deposition process by setting the etching process temperature to decrease with increasing etching depth, reducing the risk of lateral etching on the sidewalls of the etching tank, reducing ion flux attenuation, and improving vertical etching efficiency. Simultaneously, the low temperature can also suppress the desorption and diffusion loss of water molecules within the etching tank, thereby enhancing the adsorption stability of the co-solid film on the sidewalls of the etching tank, enhancing the adsorption effect of HF on the bottom wall of the etching tank, and improving the vertical etching rate.

[0012] In conjunction with the first aspect, in one possible implementation, the fabrication method further includes: after completing the preceding deposition process, increasing the saturated vapor pressure of the precursor gas in the subsequent deposition process. Thus, by increasing the saturated vapor pressure of the precursor gas in the subsequent deposition process after completing the pre-deposition step, the reaction efficiency of the precursor gas can be increased, the deposition rate of the protective film can be accelerated, the deposition thickness and density of the protective film can be increased, and the uniformity and surface smoothness of the protective film can be improved; simultaneously, the ability of the precursor gas to diffuse to the bottom of the etching tank is enhanced.

[0013] In conjunction with the first aspect, in one possible implementation, the fabrication method further includes: after completing the preceding deposition process, adjusting the thickness of the protective film formed by the subsequent deposition process to be less than the thickness of the protective film formed by the preceding deposition process. Thus, setting the thickness of the protective film formed in the subsequent deposition process to be less than the thickness of the protective film formed in the preceding deposition process allows the thicker protective film formed in the preceding deposition step to provide sufficient protection for the sidewalls of the etched structure, suppressing lateral etching of the sidewalls of the etched grooves; while using a thinner protective film in the subsequent deposition step reduces the shielding of subsequent etching ions by the protective film, improves the penetration and uniformity of longitudinal etching, improves the perpendicularity of the etching contour, and avoids defects such as sidewall tilting, local accumulation, and microburrs caused by excessively thick protective films. Therefore, while ensuring the sidewall protection effect, it improves the uniformity of etching depth and the overall structural morphology accuracy.

[0014] In conjunction with the first aspect, in one possible implementation, the protective film further includes a metal oxide protective layer, the metal nitride protective layer and / or the metal carbonitride protective layer being attached to the surface of the metal oxide protective layer, and the step of introducing the precursor gas and the reactive gas into the etching chamber includes: introducing the precursor gas into the etching chamber so that the amino ligands in the precursor gas react with the liquid film adsorbed on the tank sidewall to generate the metal oxide protective layer; purging out the precursor gas and chemisorption byproducts; and introducing the reactive gas into the etching chamber so that the H radicals in the reactive gas react with the imino ligands and / or amino ligands in the precursor gas to generate the metal nitride protective layer and / or the metal carbonitride protective layer. Therefore, forming a protective film through atomic layer deposition improves the precise control of the protective film thickness, enhances the uniformity, density, and consistency of the protective film, improves the protective ability of the protective film to protect the walls of the etching tank, and reduces the risk of etching deviation, damage, or abnormal contours caused by uneven local film thickness.

[0015] In conjunction with the first aspect, in one possible implementation, depositing a protective film of a target thickness on the wall of the etching tank includes: cyclically performing the deposition process a preset number of cycles. This ensures that a protective film of sufficient thickness is formed on the sidewall of the etching tank.

[0016] In conjunction with the first aspect, in one possible implementation, the step of introducing precursor gas and reactive gas into the etching chamber to deposit a protective film of a target thickness on the wall of the etching tank includes: simultaneously introducing precursor gas and reactive gas into the etching chamber and reacting for a target time to deposit a protective film of the target thickness on the wall of the etching tank. Thus, forming the protective film via chemical vapor deposition improves the deposition rate of the protective film and reduces the requirements for the precursor gas delivery pipeline.

[0017] In conjunction with the first aspect, in one possible implementation, the simultaneous introduction of precursor gas and reactive gas into the etching chamber includes: gradually increasing the amount of reactive gas introduced into the etching chamber while gradually decreasing the amount of precursor gas introduced into the etching chamber. Thus, by gradually increasing the amount of reactive gas introduced and simultaneously decreasing the amount of precursor gas introduced, the morphological integrity of the outermost metal nitride or metal carbonitride protective layer is improved. This allows the highly conductive metal nitride or metal carbonitride protective layer to avoid the charge shielding effect caused by residual positive charge at the bottom of the etching tank, reducing ion scattering and lowering the probability of vertical morphological distortion in the etching tank. Simultaneously, by steadily controlling the gas component ratio within the etching chamber, the protective film deposition process proceeds gradually, improving the morphological integrity and structural density of the protective film.

[0018] In conjunction with the first aspect, in one possible implementation, the protective film further includes a metal oxide protective layer, the metal nitride protective layer and / or the metal carbonitride protective layer being attached to the surface of the metal oxide protective layer. The step of introducing precursor gas and reactive gas into the etching chamber to deposit a protective film of a target thickness on the wall of the etching tank includes: introducing precursor gas into the etching chamber such that amino ligands in the precursor gas react with the liquid film adsorbed on the sidewall of the tank for a first preset time to generate the metal oxide protective layer of a first thickness; purging and discharging the precursor gas and chemisorption byproducts; and introducing the reactive gas into the etching chamber such that H radicals in the reactive gas react with imino ligands and / or amino ligands in the precursor gas for a second preset time to generate the metal nitride protective layer and / or the metal carbonitride protective layer of a second thickness, wherein the sum of the first thickness and the second thickness is equal to the target thickness. Therefore, the stepwise deposition setup enables the layered and controllable growth of the metal oxide protective layer and the metal nitride protective layer. This facilitates precise control over the thickness, composition, and interface structure of each film layer, allowing the formation of a metal nitride protective layer on the outermost side of the protective film. The high conductivity and low resistivity of the metal nitride can be used to avoid the charge shadowing effect caused by the residual positive charge at the bottom of the etching tank, reducing ion scattering, lowering the probability of vertical morphology distortion in the etching tank, and improving the density and uniformity of the protective film. At the same time, the stepwise reaction and intermediate purging steps can reduce by-product residues, avoid interference between different reactive gases, reduce defects between the layers of the protective film, improve the protective effect of the protective film on the sidewalls of the etching tank and the regularity of the morphology, and improve the stability and structural accuracy of subsequent etching processes.

[0019] In conjunction with the first aspect, in one possible implementation, the target thickness is 0.1 nm-5 nm. Thus, by setting the thickness of the protective film, a complete and continuous protective film can be formed on the sidewall of the etching tank to resist the bombardment of the etching plasma during the etching process. This allows the protective film to adhere firmly to the sidewall of the etching tank, while simultaneously improving the removal efficiency of residual positive charges at the bottom of the etching tank, suppressing charge shielding effects, improving ion scattering, and maintaining a regular vertical etching morphology. This avoids critical dimension shifts in the etching tank and clogging of openings in high aspect ratio structures caused by an excessively thick protective film, while also not hindering the interaction between the plasma and the substrate in subsequent etching processes, thus balancing charge elimination capability and pattern size processing accuracy.

[0020] In conjunction with the first aspect, in one possible implementation, the reactant gas is at least one of CxHyFz type gases, NH3, N2H4, H2, CH4, CH3I, or HF. Thus, the reactant gas can provide H radicals, which can undergo hydrogenation reduction reactions with the precursor gas to produce a metal carbonitride protective layer, or undergo hydrogenolysis reactions to generate a metal nitride protective layer or a metal carbonitride protective layer.

[0021] Secondly, embodiments of this application provide an etching apparatus including an etching chamber, a process gas supply system, a precursor gas supply system, an etching reaction system, and a control system; the etching chamber is used to contain a substrate to be etched; the process gas supply system is used to input etching gas and the reaction gas into the etching chamber; the precursor gas supply system is used to input the precursor gas into the etching chamber; the etching reaction system is used to etch the substrate to be etched; the control system is connected to the process gas supply system, the precursor gas supply system, and the etching reaction system, and the control system is used to control the etching apparatus to etch the substrate to be etched. The bottom circulation alternates between etching and deposition processes to form an etching trench of a predetermined depth on the substrate to be etched; wherein the deposition process includes: introducing a precursor gas and a reactive gas into the etching chamber to deposit a protective film of a target thickness on the sidewall of the etching trench, wherein the protective film includes a metal nitride protective layer generated by the reaction of H free radicals in the reactive gas with imine ligands in the precursor gas; and / or, the protective film includes a metal carbonitride protective layer generated by the reaction of H free radicals in the reactive gas with amino ligands in the precursor gas; and purging out the precursor gas, the reactive gas, and deposition byproducts.

[0022] In conjunction with the second aspect, in one possible implementation, the process gas supply system includes a first input gas path for supplying the reactant gas into the etching chamber; the precursor gas supply system includes a second input gas path for supplying the precursor gas into the etching chamber, wherein the first input gas path is independent of the second input gas path. Thus, by independently controlling the intake of the precursor gas and the reactant gas, the thickness of the protective film deposited on the sidewall of the etching tank can be precisely controlled. This achieves separate delivery of the precursor gas and reactant gas or other process gases, and independent regulation of the flow rate, on / off timing, and supply pressure of each gas path, avoiding premature pre-reaction of different gases in the delivery pipeline, the generation of particulate matter, or corrosion of the pipeline; simultaneously, it allows for individual matching of the precursor gas supply process window, precise control of the precursor gas concentration in the etching chamber, flexible switching of gas ratios for different process stages such as etching, passivation, and cleaning, preventing gas crosstalk between gas paths, and improving etching morphology, etching rate, and process repeatability.

[0023] In conjunction with the second aspect, in one possible implementation, the precursor gas supply system includes a second input gas path, a precursor supply source, a buffer chamber, and a precursor control valve. The precursor supply source, the buffer chamber, and the precursor control valve are disposed on the second input gas path. The precursor supply source is connected to the control system. The control system is further configured to control the precursor supply source to deliver the precursor gas to the etching chamber through the second input gas path. The buffer chamber is disposed between the precursor supply source and the precursor control valve. The precursor control valve is connected to the etching chamber. The gas pressure in the buffer chamber is greater than or equal to twice the gas pressure in the etching chamber. Therefore, the buffer chamber can stabilize the flow rate and partial pressure of the precursor gas, avoiding interference with the delivery of the precursor gas caused by pressure fluctuations and airflow disturbances inside the etching chamber, thus improving the uniformity and stability of the precursor gas input. At the same time, by utilizing the pressure difference between the buffer chamber and the etching chamber, the precursor gas can enter the etching chamber more smoothly and controllably, reducing gas pulse impacts and instantaneous concentration fluctuations, and improving the consistency of the precursor gas in chemical adsorption and hydrogenation or hydrogenolysis reactions on the sidewall of the etching tank. This, in turn, improves the uniformity of the protective film deposition thickness and the film quality, and enhances the repeatability and structural precision of the etching process.

[0024] In conjunction with the second aspect, in one possible implementation, the etching apparatus further includes a temperature control system connected to the control system, the control system being further configured to control the temperature control system to increase the temperature of the substrate to be etched after the etching process is completed. Therefore, after etching is completed, the control system controls the temperature control system to raise the temperature of the substrate to be etched. On the one hand, the heated substrate can improve the adsorption activity and reaction kinetics of the precursor gas, promote the precursor gas to fully undergo chemical reaction and uniformly deposit on the surface of the etched structure to form a dense and continuous protective film. At the same time, the protective film can quickly remove the residual positive charge accumulated at the bottom of the etching tank, suppress the charge shielding effect, reduce ion scattering of plasma, prevent distortion of vertical etching morphology, stabilize the steepness of the sidewalls and the flatness of the bottom of the high aspect ratio etching tank, and optimize the consistency of the overall etching process morphology. On the other hand, the heated substrate can increase the saturated vapor pressure of the precursor gas, promote the full volatilization and discharge of excess precursor gas that did not participate in the formation of the protective film in the etching tank, avoid the continuous deposition of excessive precursor gas to form an excessively thick residual protective film, which would cause the opening of the etching tank to be blocked and the size to be offset. At the same time, it promotes the desorption of by-products inside the formed protective film, optimizes the density and uniformity of the protective film, reduces particulate contamination in the etching chamber 1, and facilitates subsequent processes.

[0025] Thirdly, embodiments of this application provide a semiconductor device, including a unit or module for performing the fabrication method as described in any embodiment of the first aspect.

[0026] Fourthly, embodiments of this application provide a semiconductor device, including the etching apparatus described above.

[0027] Fifthly, embodiments of this application provide a control method, comprising: controlling an etching apparatus to perform alternating etching and deposition processes on a substrate to be etched, thereby forming an etching trench of a predetermined depth on the substrate; wherein the deposition process comprises: introducing a precursor gas and a reactive gas into an etching chamber to deposit a protective film of a target thickness on the sidewall of the etching trench, wherein the protective film comprises a metal nitride protective layer generated by the reaction of H radicals in the reactive gas with imino ligands in the precursor gas; and / or, the protective film comprises a metal carbonitride protective layer generated by the reaction of H radicals in the reactive gas with amino ligands in the precursor gas; and purging and discharging the precursor gas, the reactive gas, and deposition byproducts.

[0028] In one possible implementation, the above control method is executed by a control system in the etching apparatus, the control system being connected to the process gas supply system, the precursor gas supply system, and the etching reaction system.

[0029] Sixthly, embodiments of this application provide a control device. The control device includes a processor and a memory, the processor being coupled to the memory, the memory being used to store computer programs or instructions and / or data, and the processor being used to execute the computer programs or instructions stored in the memory, or to read the data stored in the memory, to execute the manufacturing methods in the above-described method embodiments.

[0030] In a seventh aspect, embodiments of this application provide a computer-readable storage medium storing instructions that, when executed on a computer, enable the computer to perform the manufacturing method as described in any embodiment of the first aspect.

[0031] Eighthly, embodiments of this application provide a computer program product containing instructions that, when executed on a processor, cause the processor to perform the manufacturing method as described in any embodiment of the first aspect. Attached Figure Description

[0032] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0033] Figure 1 This is a schematic diagram of the functional modules of the etching apparatus provided in the embodiments of this application.

[0034] Figure 2 This is a cross-sectional view of the substrate to be etched and the protective film provided in the embodiments of this application.

[0035] Figure 3 This is a schematic diagram of the functional modules of a precursor gas supply system provided in an embodiment of this application.

[0036] Figure 4 This is a schematic diagram of the functional modules of a precursor gas supply system provided in another embodiment of this application.

[0037] Figure 5 This is a molecular structure diagram of the precursor gas provided in the embodiments of this application.

[0038] Figure 6 This is a graph showing the saturated vapor pressure of TBTTEMT and TBTTDET as a function of temperature, provided in the embodiments of this application.

[0039] Figure 7 This is a process diagram of the fabrication method of the high aspect ratio etched structure provided in the embodiments of this application.

[0040] Figure 8 This is a process diagram of TBTTEMT depositing to form a protective film on the sidewall of the etching tank, as provided in the embodiments of this application.

[0041] Figure 9 This is a reaction mechanism diagram of TBTTEMT depositing to form a protective film on the sidewall of the etching tank, as provided in the embodiments of this application.

[0042] Figure 10 This is a flowchart of the steps of a method for fabricating a high aspect ratio etched structure according to an embodiment of this application.

[0043] Figure 11 This is a flowchart of the steps of a method for fabricating a high aspect ratio etched structure according to another embodiment of this application.

[0044] Figure 12 This is a flowchart of the steps of a method for fabricating a high aspect ratio etched structure according to another embodiment of this application.

[0045] Figure 13 This is a schematic diagram of the functional modules of the control device provided in the embodiments of this application.

[0046] Explanation of reference numerals in the attached figures: 100 - Etching apparatus; 1-Etching chamber; 2-Etching reaction system; 21-First electrode; 22-Second electrode; 2201-Refrigerant inlet; 2202-Refrigerant outlet; 2203-Refrigerant channel; 23-High-frequency radio frequency source; 24-Low-frequency radio frequency source; 25-High-frequency matching device; 26-Low-frequency matching device; 27-Sensor; 3-Process gas supply system; 31-First input gas path; 32-Third input gas path; 4-Precursor gas supply system; 40-First barometer; 41-Second input gas path; 42-Precursor supply source; 421-Precursor memory; 422-Ampoule; 423-First flow meter; 424-Vaporizer; 43-Buffer chamber; 44-Precursor control valve; 45-Carrier gas module; 46-Second flow meter; 47-Second barometer; 48-Insulation module; 49-Bypass pipe; 5-Manifold; 6-Host computer; 7-Control System; 8-Temperature control system; 200 - Substrate to be etched; 201 - Etching trench; 2011 - Trench sidewall; 2012 - Trench bottom wall; 210 - First film layer; 220 - Second film layer; 230 - Etching stop layer; 240 - Hard mask; 300 - Protective film; 310 - Metal oxide protective layer; 320 - Metal nitride protective layer; 330 - Metal carbonitride protective layer; 500 - Control device; 510 - Processor; 520 - Memory. Detailed Implementation

[0047] To enable those skilled in the art to better understand the present application, the technical solutions of the present application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present application, and not all embodiments. Based on the embodiments of the present application, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of the present application.

[0048] The terms “first,” “second,” etc. (if present) in the specification, claims, and accompanying drawings of this application are used to distinguish similar objects and are not necessarily used to describe a particular order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments described herein can be implemented in orders other than those illustrated or described herein. Furthermore, the terms “comprising” and “having,” and any variations thereof, are intended to cover a non-exclusive inclusion; for example, a process, method, system, unit, product, or apparatus that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to such processes, methods, products, or apparatus.

[0049] The term "gas pressure" refers to the degree of rarefaction of gas in a vacuum. If the pressure inside the measuring device is lower than atmospheric pressure, a vacuum gauge is required for pressure measurement. The value read from the vacuum gauge is called the gas pressure.

[0050] As semiconductor memory and logic devices evolve towards higher density and higher integration, the aspect ratio of etched structures continues to rise to meet the demands for increased memory capacity and device miniaturization. For example, the aspect ratio of etched structures can be 50:1, 100:1, and 200:1. The high aspect ratio of etched structures places stringent requirements on the uniformity, perpendicularity, and depth consistency of the plasma etching process.

[0051] During high aspect ratio etching, the etched structure is prone to morphological distortion due to limitations in plasma transport, ion movement trajectory, and reactant species distribution characteristics. Morphological distortion can include defects such as twisting, tilting, bowing, necking, tapering, and etch stop. Morphological distortion in the etched structure directly leads to abnormal electrical performance of semiconductor devices, thereby reducing the manufacturing rate and yield of semiconductor devices.

[0052] The morphological distortion of the etched structure is mainly caused by the following two factors. First, after the incident ions used for etching enter the etching tank, they are easily scattered by the sidewalls of the tank, causing the incident ion angle to deviate from the vertical direction. At the same time, a large number of positive ions accumulate at the bottom of the etching tank, forming a charge shadowing effect, which changes the local electric field distribution and exacerbates the incident ion angle deviation, leading to problems such as tilting, distortion, and asymmetry in the etched morphology. Second, the free radicals required for the etching reaction are largely consumed by the sidewalls of the etching tank during downward transport, resulting in insufficient supply of free radicals at the etching front. The etching rate decreases with increasing aspect ratio, thus reducing the etching rate and plasma energy, which weakens the etching verticality, ultimately forming a tapered morphology, and in extreme cases, even causing etching termination.

[0053] To address the aforementioned issues, traditional methods rely on increasing ion energy to enhance ion incident perpendicularity. However, simply increasing energy can easily lead to substrate damage, deterioration of sidewall roughness, and decreased etching selectivity. In the high aspect ratio etched structure fabrication method disclosed in this application, a passivation protective film is deposited on the sidewall of the etching trench. This protective film can prevent unnecessary consumption of free radicals on the sidewall, reducing lateral etching on the sidewall, while ensuring a sufficient supply of free radicals at the etching front, maintaining a stable and high-speed etching rate in the vertical direction. This improves defects such as taper, waist bulge, and necking, achieving vertical and uniform etching of the high aspect ratio structure.

[0054] Please refer to the following: Figure 1 and Figure 2 , Figure 1 This is a schematic diagram of the functional modules of the etching apparatus 100 provided in the embodiments of this application; Figure 2This is a cross-sectional view of the substrate 200 to be etched and the protective film 300 provided in an embodiment of this application. This application provides an etching apparatus 100. The etching apparatus 100 includes an etching chamber 1, a process gas supply system 3, a precursor gas supply system 4, an etching reaction system 2, and a control system 7. The etching chamber 1 is used to house the substrate 200 to be etched. The process gas supply system 3 is used to input etching gas and reaction gas into the etching chamber 1. The precursor gas supply system 4 is used to input precursor gas into the etching chamber 1. The etching reaction system 2 is used to etch the substrate 200 to be etched. The control system 7 is connected to the etching reaction system 2, the process gas supply system 3, and the precursor gas supply system 4. The control system 7 controls the etching apparatus 100 to perform alternating etching and deposition processes on the substrate 200 to form an etching trench 201 of a predetermined depth on the substrate 200. The deposition process includes: introducing precursor gas and reactive gas into the etching chamber 1 to deposit a protective film 300 of a target thickness on the sidewall 2011 of the etching trench 201; and purging out the precursor gas, reactive gas, and deposition byproducts. The protective film 300 includes a metal nitride protective layer 320 generated by the reaction of H radicals in the reactive gas with imino ligands in the precursor gas; and / or, the protective film 300 includes a metal carbonitride protective layer 330 generated by the reaction of H radicals in the reactive gas with amino ligands in the precursor gas. Exemplarily, the control system 7 controls the etching reaction system 2 to perform etching on the substrate 200. The control system 7 is also used to control the precursor gas supply system 4 to input precursor gas into the etching chamber 1, and to control the process gas supply system 3 to input reaction gas into the etching chamber 1, so as to perform the deposition process.

[0055] The etching apparatus 100 provided in this application embodiment controls the alternating execution of etching and deposition processes by the control system 7. The precursor gas and the reactive gas react to generate a conductive protective film 300 of metal nitride or metal carbonitride on the sidewall of the etching tank 201. This film helps to dissipate the residual positive charge accumulated at the bottom of the etching tank 201, suppress the charge shielding effect, reduce ion scattering of plasma, and avoid vertical etching morphology distortion. At the same time, the post-deposition purging can promptly remove residual gas and by-products in the chamber, ensuring that the protective film 300 is deposited uniformly and continuously without excess impurities. It can also continuously maintain the excellent etching profile of the etching tank 201 with steep sidewalls and flat bottom, improve the morphological accuracy and process yield of the high aspect ratio etching tank 201, improve the electrical performance of semiconductor devices, and thus improve their manufacturing yield.

[0056] It should be noted that, Figure 1The purpose is only to schematically describe the connection between the etching chamber 1, the process gas supply system 3, the precursor gas supply system 4, the etching reaction system 2, and the control system 7, and is not to make specific limitations on the connection position, connection relationship, and specific structure of each component. Figure 1 The etching apparatus 100 shown in this embodiment is merely a schematic diagram and does not constitute a specific limitation on the etching apparatus 100. In other embodiments of this application, the etching apparatus 100 may include... Figure 1 The etching apparatus 100 may include, but is not limited to, more components, combinations of certain components, or different components. The gas recovery device is used to recover the gases emitted by the etching apparatus 100, thereby reducing environmental pollution and improving energy efficiency.

[0057] For example, the etching apparatus 100 can be configured as a reactive ion etching apparatus. In some possible implementations, the etching apparatus 100 can also be configured as, but is not limited to, an inductively coupled plasma etching apparatus or a capacitively coupled plasma etching apparatus.

[0058] like Figure 2 As shown, the substrate 200 to be etched includes multiple first film layers 210 and multiple second film layers 220. The first film layers 210 and second film layers 220 are alternately stacked. The first film layer 210 or the second film layer 220 includes at least one of silicon oxide layer, silicon nitride layer, silicon oxynitride layer, silicon carbonitride layer, and polycrystalline silicon. The first film layer 210 and the second film layer 220 are different. Thus, the alternating stacking of the first film layer 210 and the second film layer 220 forms a periodic structure. On the one hand, it enables precise positioning between layers, which facilitates control of etching depth and etching stop position, and improves etching uniformity and process window. At the same time, the alternating deposition of silicon-based dielectric films of different compositions can buffer the film layer stress, avoiding problems such as cracking, peeling, and warping of single-component thick films due to excessive internal stress. The multi-layer structure has high overall adhesion, structural stability, and reliability. On the other hand, the periodic multilayer structure combined with the etching selectivity allows for layer-by-layer etching and layer-by-layer stopping, which is beneficial for forming fine patterns of the etched structure and improving pattern verticality and morphological quality.

[0059] Exemplarily, the first film layer 210 of the substrate 200 to be etched is configured as a silicon oxide layer. The material of the silicon oxide layer may include silicon dioxide. The second film layer 220 is configured as a silicon nitride layer. The material of the silicon nitride layer may include silicon tetranitride (Si3N4). In some possible embodiments, the substrate 200 to be etched also includes an etch stop layer 230. The material of the etch stop layer 230 may include, but is not limited to, at least one of polysilicon, Si3N4, titanium nitride, and tantalum nitride. The substrate 200 to be etched may also include a hard mask 240. The material of the hard mask 240 includes, but is not limited to, amorphous carbon or polysilicon, thereby enabling the hard mask 240 to serve as a robust pattern transfer medium, improving the sidewall perpendicularity and feature size control accuracy of high aspect ratio structures. The thickness of the hard mask 240 may be 1µm-5µm. The sum of the number of multiple first film layers 210 and multiple second film layers 220 may be 100-1000 layers. The sum of the thicknesses of the multiple first film layers 210 and the multiple second film layers 220 can be 3µm-15µm. The thicknesses of the first film layers 210 and the second film layers 220 can be the same or different.

[0060] like Figure 1 As shown, the etching reaction system 2 includes a first electrode 21 and a second electrode 22. The first electrode 21 and the second electrode 22 are disposed within the etching chamber 1. The first electrode 21 and the second electrode 22 are spaced apart and form a plasma reaction region. The substrate 200 to be etched is supported on the second electrode 22 and located in the plasma reaction region. The distance between the first electrode 21 and the second electrode 22 can be set to any value between 10 mm and 100 mm. Thus, by setting the distance between the first electrode 21 and the second electrode 22 within a suitable range, the mean free path of ions and the electric field distribution in the plasma can be flexibly controlled to uniformize the electric field between the first electrode 21 and the second electrode 22, improve the intra-wafer uniformity of the high aspect ratio etching trench 201 depth and sidewall morphology of the entire substrate 200 to be etched, and simultaneously adjust the ion bombardment energy and the ratio of ions to passivation radicals by changing the distance, adapting to the high aspect ratio etching requirements of different materials such as silicon and dielectrics, suppressing problems such as sidewall over-etching, bottom residue, and edge discharge arcing, while taking into account etching verticality and mask etching selectivity. The distance between the first electrode 21 and the second electrode 22 can be, but is not limited to, 10 mm, 50 mm, 90 mm, or 100 mm. For example, the distance between the first electrode 21 and the second electrode 22 can be 40 mm or 50 mm.

[0061] like Figure 1As shown, the first electrode 21 and the second electrode 22 work together to convert the process gas supplied by the process gas supply system 3 into charged particles (such as electrons, at least one of positive and negative ions), neutral particles (such as active free radicals), molecules, and atoms through reactions such as plasma dissociation and ionization. This provides the substrate 200 with the active groups required for etching and deposition chemical reactions. The first electrode 21 is located above the second electrode 22. The first electrode 21 can also be called the upper electrode, and the second electrode 22 can also be called the lower electrode.

[0062] The first electrode 21 may include a water-cooled plate, a heater, a gas distribution plate, and a spray nozzle. The water-cooled plate serves as the top support base for the entire first electrode 21, supporting the heater, gas distribution plate, and spray nozzle. The water-cooled plate has an internal circulating cooling channel to continuously remove heat generated by radio frequency discharge and plasma radiation, stabilizing the overall substrate temperature, preventing high-temperature deformation and seal failure of components, and blocking upward conduction of high temperature. The heater is positioned between the water-cooled plate and the gas distribution plate. The heater, in conjunction with the water-cooled plate, forms a closed-loop temperature control system, compensating for the low-temperature region caused by water cooling, eliminating the temperature gradient between the center and edge of the plate, maintaining the gas distribution plate and spray nozzle at a suitable constant temperature, inhibiting the low-temperature condensation and adhesion of etching polymer byproducts, reducing cavity particle defects, and also accelerating deposit removal during the cavity cleaning stage by raising the temperature. The gas distribution plate is positioned between the heater and the spray nozzle. The gas equalization plate has a buffer cavity and flow distribution holes inside, which can buffer the pressure fluctuations of the input functional gases, eliminate airflow turbulence, and ensure that the various functional gases are fully mixed and uniformly distributed in terms of pressure and flow rate before being delivered to the lower spray nozzle, avoiding imbalance in gas ratio and gas output area. The spray nozzle is located on the side of the gas equalization plate facing away from the heater. The spray nozzle is a core component integrating gas distribution, radio frequency electrodes, and precision temperature control. The spray nozzle has gas channels and a gas equalization structure inside. Through the micro-holes on the surface of the spray nozzle, the reactive gas is sprayed vertically and uniformly onto the surface of the substrate 200 to be etched. At the same time, the surface of the spray nozzle acts as a radio frequency carrier electrode to excite gas discharge and generate uniform plasma. The spray nozzle also integrates a multi-zone heater and a refrigerant channel 2203, which can precisely control the temperature of the surface, prevent the plasma from corroding the gas equalization plate below, and ensure a high degree of consistency in the etching rate and morphology of the entire substrate 200 to be etched.

[0063] like Figure 1As shown, the second electrode 22 is used to support the substrate 200 to be etched. Specifically, the second electrode 22 includes an electrostatic chuck and a metal base. The substrate 200 to be etched is electrostatically adsorbed onto the surface of the electrostatic chuck. A gas channel is provided inside the electrostatic chuck. The gas channel has multiple openings on the surface of the electrostatic chuck, and a high thermal conductivity gas (e.g., helium) is sealed in the gap between the substrate 200 to be etched and the electrostatic chuck. This allows for precise temperature control of the substrate through backblowing helium and a built-in temperature control circuit, ensuring a stable etching rate for the entire substrate. The material of the electrostatic chuck may include, but is not limited to, ceramic materials. Ceramic materials include, but are not limited to, at least one of alumina, aluminum nitride, zirconium oxide, or silicon carbide-doped alumina. The purity of the ceramic material is greater than or equal to 99.9%, thereby reducing the precipitation of metal impurities and lowering the risk of contamination of the substrate 200 to be etched during plasma processing.

[0064] like Figure 1 and Figure 2 As shown, the second electrode 22 is provided with a coolant inlet 2201, a coolant outlet 2202, and a coolant channel 2203 connecting the coolant inlet 2201 and the coolant outlet 2202. Thus, the coolant circulating through the coolant channel 2203 continuously removes the plasma radiation heat and etching reaction exothermic heat conducted by the electrostatic chuck, improving the temperature control accuracy of the substrate 200 to be etched and reducing the temperature gradient between the center and edge of the electrostatic chuck surface. Simultaneously, the stable temperature environment can suppress the deposition of etching byproducts on the surfaces of the substrate 200 to be etched and the electrostatic chuck, improving the etching rate and selectivity of the substrate 200 and the uniformity of the morphology of the etching trench 201, thus extending the lifespan of the second electrode 22. Specifically, the metal base is thermally connected to the electrostatic chuck. A coolant channel 2203 is provided within the metal base. The material of the coolant channel 2203 may include, but is not limited to, aluminum.

[0065] It should be noted that thermally conductive connection refers to a connection method that forms a continuous heat conduction path between multiple components. For example, multiple components are coupled through assembly methods such as direct contact, filling with intermediate thermally conductive medium, or coupling with thermally conductive connectors to achieve thermal coupling between components, thereby ensuring smooth heat transfer with low resistance.

[0066] An edge ring can be provided at the edge of the electrostatic chuck. The edge ring, arranged around the outer periphery of the electrostatic chuck, can correct the distorted plasma electric field and ion distribution at the edge of the substrate 200 to be etched, eliminating edge loading effects; simultaneously, it constrains the plasma bombardment range, preventing direct plasma erosion of the electrostatic chuck body, thus protecting the electrostatic chuck; it can also balance the RF impedance between the substrate 200 to be etched and the lower electrode region, stabilizing the etching selectivity and reducing inter-wafer process differences. The material of the edge ring may include, but is not limited to, at least one of low resistivity materials and insulating dielectric materials. Low resistivity materials may include, but are not limited to, at least one of silicon and silicon carbide, and insulating dielectric materials may include, but are not limited to, at least one of quartz and alumina.

[0067] like Figure 1 As shown, the second electrode 22 is connected to the high-frequency radio frequency source 23 and the low-frequency radio frequency source 24, thereby establishing a negative DC self-bias voltage on the surface of the substrate 200 to be etched. This allows for the directional acceleration of ions within the plasma to vertically bombard the surface of the substrate 200. Through a combination of ion physical bombardment and free radical chemical etching, high aspect ratio and anisotropic vertical etching of the substrate 200 is achieved. The ejector mechanism built into the second electrode 22, in conjunction with a robotic arm, completes the loading and unloading of the substrate 200. The high-frequency output of the high-frequency radio frequency source 23 can be any value between 20MHz and 100MHz. For example, the high-frequency output of the high-frequency radio frequency source 23 can be 20MHz, 40MHz, 60MHz, or 100MHz, etc., and the maximum power of the high-frequency radio frequency source 23 can be any value between 6kW and 20kW. For example, the maximum power of the high-frequency radio frequency source 23 can be 10kW or 18kW, etc. The low-frequency output of the low-frequency radio frequency source 24 can be any value between 100kHz and 15MHz. For example, the low-frequency output of the low-frequency radio frequency source 24 can be 100kHz, 400kHz, 600kHz, 1MHz, or 15MHz, etc. The maximum power of the low-frequency radio frequency source 24 can be any value between 10kW and 100kW; for example, the maximum power of the low-frequency radio frequency source 24 can be 50kW or 75kW, etc. The low-frequency radio frequency source 24 can be configured as a low-frequency bias source or a low-frequency voltage source. The low-frequency voltage source, for example, is a square wave source. The maximum output voltage of the low-frequency voltage source can be any value between 10kV and 30kV; for example, the maximum output voltage of the low-frequency voltage source can be 15kV or 25kV, etc.

[0068] like Figure 1As shown, in some possible embodiments, the etching reaction system 2 further includes a high-frequency matching unit 25 and a low-frequency matching unit 26. A high-frequency radio frequency (RF) source 23 can be connected to the RF matching unit 25 via an RF coaxial cable and fed to the second electrode 22 via an RF rod. A low-frequency RF source 24 is fed to the second electrode 22 via the low-frequency matching unit 26. The RF matching unit 25 can also be configured as a high-frequency filter, and the low-frequency matching unit 26 can also be configured as a low-frequency filter.

[0069] It should be noted that the terms "high frequency" and "low frequency" in this embodiment are relative. The main difference between the high-frequency radio frequency source 23 and the low-frequency radio frequency source 24 lies in their operating frequencies; the high-frequency radio frequency source 23 operates at a higher frequency than the low-frequency radio frequency source 24. For example, in this embodiment, "high frequency" refers to a frequency greater than 20MHz, and "low frequency" refers to a frequency less than 10MHz.

[0070] like Figure 1 As shown, in some possible embodiments, the etching reaction system 2 further includes a sensor 27. The etching apparatus 100 may also include a host computer 6. The sensor 27 is connected to the high-frequency radio frequency source 23, the low-frequency radio frequency source 24, and the host computer 6, and is used to collect forward data. The forward data includes, but is not limited to, at least one of radio frequency data, voltage data, current data, and power data. The host computer 6 is used to receive the forward data sent by the sensor 27, and the control system 7 is also used to control the high-frequency radio frequency source 23 and the low-frequency radio frequency source 24 to operate according to the uplink data sent by the host computer 6, thereby realizing that the host computer 6 can control the output power of the high-frequency radio frequency source 23 and the output power or output voltage of the low-frequency bias source through the closed loop control system 7. It should be noted that the uplink data includes, but is not limited to, at least one of the measured operating data of the radio frequency source, the matching unit feedback data, the hardware status data, or the alarm data. The downlink data includes, but is not limited to, at least one of the setting parameters, operating modes, start / stop commands, or protection threshold parameters associated with the radio frequency data, voltage data, current data, and power data. The control system 7 can be part of the host computer 6 or a component independent of the host computer 6, without limitation.

[0071] In another embodiment, the host computer 6 may also be a component independent of the etching apparatus 100, but with a communication connection to the etching apparatus 100, and may control multiple semiconductor process apparatuses or devices, including the etching apparatus 100.

[0072] like Figure 1As shown, in some possible embodiments, the etching apparatus 100 may further include a manifold 5. The manifold 5 is connected between the process gas supply system 3 and the precursor gas supply system 4. The manifold 5 is used to introduce the etching gas and reaction gas provided by the process gas supply system 3 and the precursor gas provided by the precursor gas supply system 4 into the etching chamber 1. Thus, the manifold 5 enables the centralized confluence and transportation of the two types of process gases, simplifies the pipeline layout, facilitates unified control of the mixed gas composition, flow rate and inlet sequence, and ensures a stable and uniform gas ratio required for the etching reaction in the etching chamber 1. Specifically, the manifold 5 is provided with multiple airflow paths. The multiple airflow paths are connected to the gas distribution plate of the first electrode 21. The number of multiple airflow paths can be two, three, four or more, and this embodiment does not specifically limit the number.

[0073] The process gas supply system 3 may include multiple process gas pipelines. For example, the number of process gas pipelines may be 10 to 30. The process gas supply system 3 is used to supply process gases. The process gases include, but are not limited to, at least one of plasma source gas, etching gas, carrier gas, purge gas, or reactant gas. The plasma source gas is capable of ionizing and / or dissociating to generate a basic plasma. The plasma source gas may be C x H y F z The etching gas can be a type of gas; or it can be at least one of gases such as NH3, N2H4, H2, CH4, CH3I, and HF. Etching gases include gases capable of generating large amounts of HF through plasma reactions. For example, the etching gas can be, but is not limited to, C. x H y F z Gases. C x H y F z The gases can be, but are not limited to, C4F6, C4F8, CH2F2, C3HF5, C3H2F6, C4H2F6, C4H4F6, and C5H2F. 10The etching gas may be at least one of CF4, etc. In some embodiments, the etching gas may further include at least one of CF3I, WF6, SiF4, NF3, PF3, H2O, NH3, N2H4, H2, CH4, CH3I, and HF. In some embodiments, the etching gas may further include halogen gases. Halogen gases may be, but are not limited to, at least one of Cl2, Br2, I2, HCl, HBr, and HI. The carrier gas may be, but is not limited to, an inert gas. An inert gas may be, but is not limited to, at least one of N2, He, Ne, Ar, Kr, or Xe. The carrier gas refers to the gas used to transport or dilute the precursor gas and / or the etching gas. The precursor gas refers to the raw material that can be chemically adsorbed onto the sidewall 2011 of the etching tank 201 in the etching environment and participate in the formation of the main material of the protective film 300. The reactive gas refers to the auxiliary gas source that reacts with the precursor gas to form the protective film 300. Purge gas is a gas used to purge etching and deposition processes. It is a process auxiliary gas that does not participate in the main reactions of thin film deposition, etching, and doping, and is used to maintain chamber cleanliness, inhibit wafer oxidation, eliminate process defects, and protect vacuum components. The purge gas can be, but is not limited to, an inert gas. It can be at least one of nitrogen or argon.

[0074] like Figure 1 As shown, the control system 7 is also used to input reactive gas into the etching chamber 1 through the first input gas path 31 and precursor gas into the etching chamber 1 through the second input gas path 41, wherein the first input gas path 31 is independent of the second input gas path 41. Thus, by independently controlling the intake of the precursor gas and reactive gas, the thickness of the protective film 300 deposited on the sidewall 2011 of the etching tank 201 can be precisely controlled. This achieves separate delivery of precursor gas and reactive gas or other process gases, independent regulation of the flow rate, on / off timing, and supply pressure of each gas path, avoiding premature pre-reaction of different gases in the delivery pipeline, the generation of particulate matter, or corrosion of the pipeline; simultaneously, it can independently match the supply process window of the precursor gas, precisely control the concentration of the precursor gas in the etching chamber 1, flexibly switch the gas ratio for different process stages such as etching, passivation, and cleaning, prevent gas crosstalk between gas paths, and improve etching morphology, etching rate, and process repeatability.

[0075] Exemplarily, the process gas supply system 3 may include a first input gas path 31. The first input gas path 31 is used to input a reactive gas into the etching chamber 1. The reactive gas is a gas used to generate H radicals. The reactive gas can be, but is not limited to, CxHyFz type gases, NH3, N2H4, H2, CH4, CH3I, or at least HF. Thus, the reactive gas can provide H radicals, which can undergo a hydrogenation reduction reaction with the imino ligands of the precursor gas to produce a metal nitride protective layer 320. Simultaneously, the H radicals can also undergo a hydrogenolysis reaction with the amino ligands in the precursor gas to generate a metal carbonitride protective layer 330. The first input gas path 31 can also be used to input etching gas, carrier gas, or other process gases.

[0076] In some embodiments, in addition to the first input gas path 31, the process gas supply system 3 also includes a third input gas path 32. The third input gas path 32 is independently configured from the first input gas path 31 and the second input gas path 41. The third input gas path 32 can be used to deliver etching gas, carrier gas, or other process gases. It is understood that the third input gas path 32 transmits different types of gases than the first input gas path 31 and the second input gas path 41. Therefore, by adding a third input gas path 32, which is independent of the first input gas path 31 and the second input gas path 41, to deliver etching gas or carrier gas, it is possible to achieve independent control of multiple types of process gases, ensuring that the flow rate and on / off timing of each gas path do not interfere with each other, avoiding premature gas reaction and cross-contamination within the pipeline, facilitating flexible adjustment of the gas ratio within the cavity, stabilizing the plasma reaction environment, and improving the uniformity and repeatability of the etching process.

[0077] Please refer to the following: Figure 1 , Figure 2 and Figure 3 , Figure 3This is a schematic diagram of the functional modules of the precursor gas supply system 4 provided in the first embodiment of this application. The precursor gas supply system 4 includes a second input gas path 41, a precursor supply source 42, a buffer chamber 43, and a precursor control valve 44. The precursor supply source 42, the buffer chamber 43, and the precursor control valve 44 are disposed on the second input gas path 41. The second input gas path 41 is connected to the precursor supply source 42 and is used to input precursor gas into the etching chamber 1. The second input gas path 41 is independent of the first input gas path 31. The precursor supply source 42 is used to provide precursor gas. Specifically, the precursor supply source 42 is connected to the control system 7. The control system 7 is used to control the precursor supply source 42 to deliver precursor gas into the etching chamber through the second input gas path 41. The buffer chamber 43 is disposed between the precursor supply source 42 and the precursor control valve 44. The precursor control valve 44 is connected to the etching chamber 1. The gas pressure in the buffer chamber 43 is greater than or equal to twice the gas pressure in the etching chamber 1. Therefore, the buffer chamber stabilizes the flow rate and partial pressure of the precursor gas, preventing interference with precursor gas delivery caused by pressure fluctuations and airflow disturbances within the etching chamber 1, thus improving the uniformity and stability of the precursor gas input. Simultaneously, the pressure difference between the buffer chamber 43 and the etching chamber 1 allows the precursor gas to enter the etching chamber 1 more smoothly and controllably, reducing gas pulse impacts and instantaneous concentration fluctuations. This enhances the consistency of the precursor gas's chemical adsorption and hydrogenation or hydrogenolysis reactions on the sidewall 2011 of the etching tank 201, thereby improving the uniformity of the protective film 300 deposition thickness and film quality, and increasing the repeatability and structural precision of the etching process.

[0078] like Figure 3As shown, the precursor supply source 42 includes a precursor storage unit 421 and a gas generator. Exemplarily, the gas generator can be configured as an ampoule 422. The precursor storage unit 421 is used to store the precursor liquid. The precursor storage unit 421 can be configured as a precursor cylinder. The ampoule 422 is used to vaporize the precursor liquid into precursor gas. Therefore, the ampoule 422 has a simple structure, small footprint, lower equipment investment and operating costs, eliminates the need for complex temperature control and vaporization regulation components, and is easy to maintain. Simultaneously, the material storage and retrieval method is simple, suitable for low-flow, intermittent gas supply conditions, with small gas output fluctuations, reducing the risk of over-vaporization and concentration imbalance. Its good sealing performance protects high-purity precursor liquids, reducing deterioration and loss. The overall structure is reliable and durable, making it more suitable for miniaturized and simplified precursor gas supply scenarios. The vaporization temperature of the ampoule 422 is any value between 30℃ and 100℃. For example, the vaporization temperature of ampoule 422 can be 30°C, 40°C, 50°C, or 100°C. Understandably, the higher the vaporization temperature of ampoule 422, the higher the saturated vapor pressure of the precursor gas. The ampoule 422 can be made of quartz, stainless steel, polytetrafluoroethylene, etc. In some embodiments, the precursor storage device 421 is used to store the precursor solid.

[0079] like Figure 3 As shown, in some possible embodiments, the precursor supply source 42 may further include a first flow meter 423. The first flow meter 423 is disposed between the precursor storage 421 and the ampoule 422, and is used to count the flow rate of the precursor liquid delivered to the ampoule 422. This allows for accurate measurement of the flow rate and total amount of liquid precursor delivered to the precursor ampoule 422, stabilizing the material delivery rate, avoiding overfilling and potential safety hazards, unifying the feeding process parameters, ensuring a balanced and stable material usage in subsequent production processes, and promptly identifying pipeline conveying abnormalities to reduce the loss of high-purity precursor materials, thus balancing the needs of material purity protection and automated feeding control.

[0080] like Figure 3 As shown, in some possible embodiments, the precursor gas supply system 4 may further include a carrier gas module 45. The carrier gas module 45 is connected to the ampoule 422 and is used to provide carrier gas so that the carrier gas can transport the precursor gas generated in the ampoule 422 to the buffer chamber 43. Thus, the carrier gas module 45 can stably supply carrier gas, which can smoothly transport the precursor gas generated in the ampoule 422 to the buffer chamber 43, improving the smoothness and continuity of precursor gas delivery, stabilizing the flow rate and supply concentration of precursor gas, ensuring stable downstream gas usage conditions, and improving the overall reliability and process consistency of the gas supply system. The carrier gas can be an inert gas. The inert gas can be, but is not limited to, at least one of Ar, He, Kr, Xe, or N2.

[0081] like Figure 3 As shown, in some possible embodiments, the precursor gas supply system 4 may further include a second flow meter 46. The second flow meter 46 is disposed between the carrier gas module 45 and the ampoule 422, and is used to count the flow rate of the carrier gas delivered to the ampoule 422. This allows for precise measurement of the carrier gas flow rate into the precursor ampoule 422, precise control of the carrier gas inflow, stable precursor gas carry-out rate and concentration, more balanced and uniform gas-liquid ratio, stable precursor gas output, and improved overall gas supply accuracy and production process consistency.

[0082] like Figure 3 As shown, in some possible embodiments, the precursor gas supply system 4 may further include a second barometer 47. The second barometer 47 is disposed between the flow meter and the ampoule 422 and is used to measure the input pressure of the carrier gas. This allows for real-time and accurate monitoring of the input pressure of the carrier gas entering the ampoule 422, facilitating timely adjustment of pressure parameters, stabilizing the pressure environment within the ampoule 422, coordinating flow control to optimize the evaporation and carry-out effect of the precursor gas, ensuring stable gas supply pressure, and improving gas supply stability and process control accuracy.

[0083] like Figure 3 As shown, the buffer chamber 43 can be configured as a storage container. The buffer chamber 43 can pressurize the precursor gas to a preset pressure. The preset pressure can be any value between 50 Torr and 500 Torr. For example, the preset pressure can be 50 Torr, 100 Torr, 250 Torr, 300 Torr, or 500 Torr, etc. Understandably, if the gas pressure in the buffer chamber 43 is too low, it will be difficult to form a sufficient pressure difference, making it impossible to stabilize the delivery state of the precursor gas, which will easily lead to fluctuations in gas flow and unstable gas supply, thereby affecting the deposition uniformity and process repeatability. If the gas pressure in the buffer chamber 43 is too high, it will easily cause excessive pressure shock of the precursor gas, which will not only aggravate the airflow disturbance, but may also lead to excessive gas supply or local high concentration, causing problems such as uneven film deposition and increased by-products. At the same time, excessively high gas pressure also poses a risk of damaging the chamber seal and affecting the safe and stable operation of the equipment. Therefore, by controlling the gas pressure in the buffer chamber 43 within a suitable range, both gas buffering and pressure stabilization effects and process safety can be balanced, ensuring smooth and controllable precursor delivery. The volume of the buffer chamber 43 can be any value between 1L and 10L. For example, the volume of the buffer chamber 43 can be, but is not limited to, 1L, 2L, 5L, 9L, or 10L.

[0084] like Figure 3As shown, in some possible embodiments, the precursor gas supply system 4 further includes a first barometer 40. The first barometer 40 is disposed between the buffer chamber 43 and the precursor control valve 44, and is used to detect the gas pressure in the second input gas path 41. The first barometer 40 is connected to the control system 7, which adjusts the precursor gas pressure in the buffer chamber 43 based on the gas pressure detected by the first barometer 40, thereby enabling the precursor control valve 44 to be in a choked flow state. It should be noted that the choked flow state refers to a state where, when gas passes through a small orifice, nozzle, or throttling device, the flow velocity reaches the local speed of sound, and the flow velocity no longer increases as the downstream pressure decreases.

[0085] like Figure 3 As shown, exemplarily, the precursor control valve 44 can connect or disconnect the second input gas path 41 from the etching chamber 1. The precursor gas can be mixed with the process gas, and the mixed gas passes through the gas distribution plate of the first electrode 21, and then is sprayed into the etching chamber 1 via a spray nozzle. A throttling orifice is provided in the precursor control valve 44. The orifice diameter can be any value between 100μm and 1000μm. Of course, in other embodiments, the precursor gas can be delivered separately from the process gas.

[0086] like Figure 3 As shown, in some possible embodiments, the precursor gas supply system 4 may further include a bypass pipe 49. The precursor control valve 44 may also connect or disconnect the second input gas path 41 from the bypass pipe 49. Understandably, when the etching chamber 1 does not require the introduction of precursor gas, the precursor gas in the second input gas path 41 can be discharged through the bypass pipe 49. The bypass pipe 49 may be connected to a negative pressure module. The precursor control valve 44 is connected to the control system 7. The control system 7 is used to control the on / off state of the precursor control valve 44 to regulate the precursor gas delivery path. In some possible embodiments, the host computer 6 may be directly connected to the precursor control valve 44. The host computer 6 controls the on / off state of the precursor control valve 44.

[0087] like Figure 3 As shown, in some possible embodiments, the precursor gas supply system 4 may further include a heat preservation module 48. The heat preservation module 48 is disposed on the second input gas passage 41 and is used to maintain the temperature of the precursor gas in the second input gas passage 41, thereby reducing the risk of the precursor gas cooling down and condensing in the delivery pipeline, improving the stability and reliability of the precursor gas in a gaseous state, reducing material loss and pipeline blockage, stabilizing the delivery state of the precursor gas, improving the overall control accuracy of the precursor gas delivery flow rate and supply, and enhancing process stability.

[0088] The temperature of the precursor gas within the second input gas path 41 can be any value between 50℃ and 150℃, thereby reducing the probability of condensation and liquefaction of the precursor gas during transportation, stabilizing the transportation state of the precursor gas, reducing material loss and pipeline blockage, accurately controlling the gas delivery volume, ensuring uniform and stable gas supply, and meeting the requirements of production process operation. The insulation temperature of the second input gas path 41 can be, but is not limited to, 50℃, 100℃, 110℃, 120℃, or 150℃. The insulation module 48 can be configured as a water bath insulation module; or, the insulation module 48 can also be configured as an insulation bushing.

[0089] Please refer to the following: Figure 2 and Figure 4 , Figure 4 This is a schematic diagram of the functional modules of a precursor gas supply system 4 provided in another embodiment of this application. The precursor gas supply system 4 in this embodiment is similar to... Figure 3 The precursor gas supply system 4 in the illustrated embodiment has a similar structure. The difference lies in that, in this embodiment, Figure 3 In the illustrated embodiment, the ampoule 422 is replaced by a vaporizer 424. Therefore, the vaporizer 424 enables efficient, uniform, and complete vaporization of the liquid precursor, resulting in higher vaporization efficiency and a more uniform and stable gas output. It is unaffected by changes in the liquid level within the ampoule 422, and can continuously and stably output precursor gas of consistent concentration. This adapts to high-flow-rate continuous gas supply conditions, facilitates precise control of the vaporization rate and gas concentration, improves gas supply continuity and process adaptability, simplifies material replenishment processes, and enhances the operational stability and production adaptability of the entire gas supply system. The vaporization temperature of the vaporizer 424 can be any value between 30°C and 100°C. For example, the vaporization temperature of the vaporizer 424 can be 30°C, 40°C, 50°C, or 100°C. Understandably, the higher the vaporization temperature of the vaporizer 424, the higher the saturated vapor pressure of the precursor gas.

[0090] like Figure 4 As shown, the precursor gas supply system 4 can omit the second barometer 47. Understandably, after replacing the ampoule 422 with the vaporizer 424, the vaporizer 424 can independently stabilize its internal outlet pressure through its built-in temperature control and vaporization adjustment structure. The gas production pressure is uniform and controllable, and there is no need to rely on an external second barometer 47 to monitor the carrier gas input pressure to adjust the operating conditions. The carrier gas inlet and vaporization gas production state have a high degree of matching, and the pressure fluctuation range is extremely small. Therefore, there is no need to set up an additional barometer between the carrier gas module and the vaporizer 424 for pressure detection and control.

[0091] It should be noted that detailed descriptions of other structures of the precursor gas supply system 4 can be found in the foregoing. Figure 3 The embodiments shown are not described in detail here.

[0092] like Figure 5As shown, exemplarily, the general formula for the precursor gas is: R 3 -N=M(NR 1 R 2 3. In some possible implementations, the general formula for the precursor gas can also be: R 3 -N=M(NR 1 R 2 )2(η 5 -C5R 4 5); or, M(NR) 1 R 2 5. Wherein, M represents a metal atom. Metal atoms include Ta, Ti, Zr, Hf, V, Nb, Cr, Mo, W, Ru, Co, Rh, Ir, Ga, In, Ge or Sn, R 1 R 2 and R 3 Each is represented as an alkyl group, R 4 The precursor gas is represented by H or alkyl, wherein the alkyl group is methyl, ethyl, or tert-butyl. Thus, the precursor gas can be chemically adsorbed onto the sidewalls 2011 and bottom wall of the etching tank 201, generating a metal oxide protective layer 310. This layer reacts with H radicals in the reaction gas to generate a metal nitride protective layer 320 or a metal carbonitride protective layer 330, thereby forming a dense, double-layered protective film 300. The protective film 300 can block the lateral erosion of the sidewalls 2011 of the etching tank 201 by active etching radicals and ions, suppress over-etching and lateral concavity defects of the sidewalls 2011, maintain the verticality of the sidewalls 2011, reduce the risk of distortion in the vertical etching morphology of the substrate 200, and simultaneously improve the etching selectivity of the mask material, ensuring high aspect ratio structural morphology accuracy.

[0093] For example, the precursor gas is configured as a metal-organic coordination complex precursor. The precursor gas can be configured as an organic framework having a metal-nitrogen double bond. Organic frameworks having a metal-nitrogen double bond include, but are not limited to, tert-butylimino-tris(ethylmethylamido)tantalum (TBTEMT, structural formula Ta[N(CH3)(C2H5)]3[=NC(CH3)3]) and tert-butylimino-tris(diethylamido)tantalum (TBTDET, structural formula Ta[N(C2H5)2]3(=N... C(CH3)3), Neopentylimino-tris(diethylamido)tantalum (NPTDET, structural formula CH2C(CH3)3][N(C2H5)2]3), Isopropylimino-tris(diethylamido)tantalum (IPTDET, structural formula Ta(=NCH(CH3)2)[N(C2H5)2]3), Tert-Butylimido-(diethylamido)cyclopentadienyl-tantalum (TBDETCp, structural formula Ta(=NC(CH3)3)[N(C2H5)2](η) 5(-C5H5), tert-amylimidotris(dimethylamido)tantalum(V) (abbreviated TAIMATA, structural formula Ta(=NC(CH3)2CH2CH3)[N(CH3)2]3), or (tert-butylimido)bis(N,N′-diisopropylacetamidinato)dimethylamido tantalum(V) (abbreviated Ta(tBuN)(iPr-amd)2(NMe2, structural formula Ta(=NCMe3)(iPrNC(CH3)NiPr)2(NMe2)), etc., at least one of the following. Therefore, the precursor gas reacts with the etching substrate 200 to generate a metal oxide protective layer 310, which can be a Ta-based film (tantalum oxide film). Thus, the Ta-based film has high selectivity for photoresist or hard mask, controllable etching rate, strong anisotropy, and low probability of vertical morphology distortion of the sidewall 2011 of the etching trench 201. It also has strong diffusion blocking ability for Cu, Si, and O, low resistance of the tantalum nitrogen compound, and reduces the probability of vertical morphology distortion of the etching trench 201. At the same time, the deposition by-products such as amines and alkanes generated during the deposition of the protective film 300 are easy to remove, easy to purge, leave no residue, and do not contaminate the etching chamber 1.

[0094] In some possible embodiments, the precursor gas may also be configured as an organic framework having a metal-nitrogen single bond. An organic framework having a metal-nitrogen single bond includes, but is not limited to, at least one of pentapenta(dimethylamido)tantalum(V) (abbreviated PDMAT, structural formula Ta(NMe2)5), pentapenta(diethylamido)tantalum(V) (abbreviated PDEAT, structural formula (Ta(NEt2)5)), or pentapenta(ethylmethylamido)tantalum(V) (abbreviated PEMAT, structural formula Ta(NMeEt)5).

[0095] Understandably, the general formula for precursor gases is: R 3 -N=M(NR 1 R 2 )3 or R 3 -N=M(NR 1 R 2 )2(η 5 -C5R 45) At this time, the H radicals in the reactant gas can undergo a hydrogenation reduction reaction with the imino ligands of the precursor gas to produce the metal nitride protective layer 320. Understandably, the precursor gas with a metal-nitrogen double bond structure has higher molecular bond energy and stronger structural stability. After plasma dissociation, the release of metal-nitrogen active groups is more uniform and complete. The reaction with the reactant gas can quickly generate a metal nitride protective layer 320 and a metal oxide protective layer 310 with higher density and more complete coverage. Compared with the metal-nitrogen single bond system, the protective film 300 does not contain excess carbon components and does not have particle defects caused by carbon accumulation. The protective film 300 has stronger resistance to ion bombardment and can more effectively suppress morphological defects such as lateral etching, side concavity, and ripples on the sidewall 2011 of the etching trench 201, improve the etching selectivity ratio of the mask and the substrate, and achieve better uniformity of passivation effect.

[0096] When the precursor gas has the general formula M(NR1R2)5, the H radicals in the reactant gas can undergo hydrogenolysis with the amino ligands in the precursor gas to generate a metal carbonitride protective layer 330. Thus, the metal carbonitride protective layer 330 can optimize the etching selectivity and chemical stability of the protective film 300 while maintaining its high density and sidewall protection capabilities, improving its resistance to plasma bombardment and etching loss under etching conditions. Furthermore, the carbonitride structure can improve the internal stress of the protective film 300, reducing the risk of cracking, peeling, and interface defects, enhancing the verticality of the etching profile and structural uniformity, and improving the forming quality of high aspect ratio structures.

[0097] like Figure 2As shown, the resistivity of both the metal nitride protective layer 320 and the metal carbonitride protective layer 330 can be any value between 200 μΩ·cm and 10000 μΩ·cm. Therefore, the highly conductive and low-resistivity metal nitride protective layer 320 or metal carbonitride protective layer 330 can be used to quickly conduct away residual positive charges accumulated at the bottom of the etching trench 201, fundamentally avoiding the charge shadowing effect; simultaneously, it reduces the probability of ion scattering, weakens the etching unevenness caused by charged ion deflection, suppresses vertical etching morphology distortion, achieves an ideal etching profile with steep sidewalls and a flat bottom, and optimizes the device patterning yield. It should be noted that resistivity, also known as volume resistivity, is an inherent physical property that measures a material's ability to resist the passage of electric current. Specifically, resistivity is defined as the ratio of the electric field strength (E) to the current density (J) within a material. For example, the resistivity of the metal nitride protective layer 320 and the metal carbonitride protective layer 330 can be 200 uΩ·cm, 500 uΩ·cm, 4000 uΩ·cm, 6000 uΩ·cm, or 10000 uΩ·cm, etc. It should be noted that although resistivity is a parameter characterizing the inherent physical properties of a material, the resistivity of the metal nitride protective layer 320 and the metal carbonitride protective layer 330 is not a constant value; this resistivity is closely related to many factors such as deposition temperature, the composition ratio of metal nitride and metal carbonitride, the density of the protective film 300, and the crystalline and / or amorphous microstructure of the protective film 300.

[0098] For example, the precursor gas is configured as TTBTEMT. TTBTEMT is structurally stable at low temperatures but undergoes thermal decomposition at high temperatures (e.g., greater than or equal to 250°C). TTBTEMT consists of a metal-organic framework (MOF) composed of amino and imino ligands. See also... Figure 5 , Figure 5 This is a molecular structure diagram of the precursor gas provided in the embodiments of this application. The molecular structure of TBTEMT is as follows: Figure 5 As shown, R 1 R 2 R 3 These are represented as alkyl ligands. The alkyl ligands are methyl, ethyl, and tert-butyl.

[0099] The precursor gas can be a material with a target saturated vapor pressure at a preset temperature. For example, the precursor gas can be a material with a high saturated vapor pressure at low temperatures, thereby preventing thermal decomposition of the precursor gas and improving the control accuracy of the thickness of the protective film 300 formed on the sidewall 2011 of the etching tank 201. It should be noted that the preset temperature (i.e., low temperature) in this application refers to a temperature below 100°C, and the target saturated vapor pressure (i.e., high saturated vapor pressure) in this application refers to a saturated vapor pressure value less than or equal to 2000 mTorr at a temperature below 100°C. Saturated vapor pressure refers to the pressure of the vapor when the precursor liquid and its own vapor reach a dynamic equilibrium in a closed, constant-temperature container; this is called the saturated vapor pressure of the substance at that temperature.

[0100] Please see Figure 6 , Figure 6 This is a graph showing the saturated vapor pressure of TBTMT and TBTDET as a function of temperature, as provided in the embodiments of this application. The vapor pressure of TBTMT at 0°C is greater than that of TBTDET at 0°C. For example, the vapor pressure of TBTMT at 0°C is approximately 16 mTorr, while the vapor pressure of TBTDET at 0°C is approximately 0.2 mTorr. Understandably, at the same temperature, a higher saturated vapor pressure indicates a higher molecular concentration of the precursor gas and a stronger gas-phase diffusion capability under the same transport conditions, making it easier for the precursor gas to pass through the narrow opening of the etching tank 201 and reach the bottom and sidewalls 2011 of the etching tank 201.

[0101] like Figure 1 and Figure 2 As shown, in some possible implementations, the control system 7 is also used to acquire the current depth of the etching tank 201 during the deposition process, and adjust the saturated vapor pressure corresponding to the precursor gas to the target saturated vapor pressure based on the current depth. Thus, by acquiring the depth of the etching tank 201 in real time during the deposition process and matching the precursor gas supply amount to this depth, the precursor gas supply amount can be dynamically adjusted according to the aspect ratio of the etching tank 201. This ensures that a protective passivation film can be uniformly formed inside etching tanks 201 at different depths, alleviating the load effect between shallow and deep etching tanks 201, continuously suppressing lateral etching on the sidewalls and bottom drilling, stably maintaining the vertically regular morphology of the etching tank 201, simultaneously widening the process adaptation range, and reducing mask loss and wafer particle defects. It is understood that the current depth of the etching tank 201 can be determined in various ways. For example, during the etching process, in-situ optical methods such as laser interferometry, broadband interferometry, and infrared back-side interferometry can be used to obtain the current depth of the etching groove 201 in real time; or, the depth can be estimated by combining the pre-calibrated etching rate with the etching time, or indirectly calculated by using an electrical test structure or process prediction model.

[0102] For example, the control system 7 is used to adjust the temperature inside the etching chamber 1; and / or to change the composition of the precursor gas until the saturated vapor pressure corresponding to the precursor gas reaches the target saturated vapor pressure. Thus, the control system 7 can flexibly adjust the precursor saturated vapor pressure to a target value matching the real-time depth of the etching trench 201, thereby dynamically adapting to the precursor transport requirements within the etching trench 201 at different depths. This ensures uniform generation of the passivation film across the entire etching trench 201, weakens the etching load effect, suppresses sidewall etching and bottom drilling, stably obtains a vertically regular high aspect ratio etching trench 201 morphology, broadens the process control window, and reduces the process limitations caused by a single control method.

[0103] like Figure 1 and Figure 2 As shown, in one possible implementation, the precursor gas can be a single gas. The control system 7 is also used to use the target precursor gas as the updated precursor gas, wherein the composition of the target precursor gas is different from that of the original precursor gas, and the saturated vapor pressure of the target precursor gas is greater than that of the original precursor gas. Thus, by replacing it with a target precursor gas with a different composition and a higher saturated vapor pressure, the molecular concentration of the precursor gas in the etching chamber 1 can be increased, enhancing the diffusion and delivery capacity of the precursor to the depth of the high aspect ratio etching groove 201, compensating for the deficiency of insufficient precursor gas supply at the bottom of the deep groove, so that a protective film 300 is uniformly formed on the sidewall 2011 and bottom wall of the etching groove 201, suppressing lateral etching of the sidewall 2011 and drilling of the bottom wall of the etching groove 201, weakening the load effect between the deep and shallow etching grooves 201, and improving the vertical and flat etching morphology of the etching groove 201.

[0104] In one possible implementation, the precursor gas can be a mixture of gases. The control system 7 is also used to update the proportions of various gases in the precursor gas composition. Updating the proportions of various gases in the precursor gas composition includes: reducing the proportion of at least one of one or more gases with higher saturated vapor pressure ranking in the precursor gas; and / or increasing the proportion of at least one of one or more gases with lower saturated vapor pressure ranking in the precursor gas. The multiple precursor gases can be ordered by saturated vapor pressure.

[0105] For example, the temperature of the substrate 200 to be etched during the etching process is any value between -100℃ and 100℃. Therefore, in a low-temperature environment where the temperature of the substrate to be etched is controlled within -100℃ to 100℃ during the etching process, H2O and HF in the etching byproducts generated during the etching reaction of the substrate 200 will be physically adsorbed onto the sidewall 2011 of the etching tank 201 through hydrogen bonds, forming a co-solution film. This co-solution film can chemically adsorb the precursor gas to form a metal oxide protective layer 310, thereby preventing HF from reacting with the sidewall 2011 of the etching tank 201, reducing HF consumption, and increasing the vertical etching rate of the substrate 200. Simultaneously, H2O and HF can also react to generate HF2. - and H3O + , and HF2 - As key active ions for etching, these ions can suppress thermal decomposition and recombination losses at low temperatures, and are well adsorbed on the surface of the substrate 200 to be etched, participating in chemical reactions to achieve directional etching of the substrate 200. The temperature of the substrate 200 during the etching process can be -100℃, -50℃, 0℃, 50℃, or 100℃, etc. The gas pressure for the etching process can be 10mTorr-30mTorr.

[0106] Understandably, under low-temperature etching conditions (e.g., less than or equal to 100°C), the proportion of HF molecules and HF radicals in the plasma formed by the dissociation and / or ionization of etching gases is relatively high, typically reaching 10%-95%. Under room-temperature or high-temperature (greater than 100°C) etching conditions, the main etching reactant C... x F y Free radicals are typically present in low concentrations, such as 1%-10%. HF molecules, HF atoms, H free radicals, and F free radicals in the plasma can be transported to the sidewalls 2011 and bottomwalls 2012 of the etching tank 201 via Knudsen diffusion. For example, the first film layer 210 of the substrate 200 to be etched is configured as SiO2, and the second film layer 220 is configured as Si3N4, and both undergo etching chemical reactions with HF gas. The etching reaction equation for the first film layer 210 is denoted as Equation (1), and the etching reaction equation for the second film layer 220 is denoted as Equation (2), where s represents a solid, g represents a gas, and l represents a liquid.

[0107]

[0108] Understandably, under low-temperature etching process conditions, C x F yThe low content of free radicals prevents the deposition of a protective film 300 on the sidewall 2011 of the etching trench 201, resulting in the gradual lateral etching of the SiO2 film sidewalls. Ammonium fluorosilicate (AFS), formed by the spontaneous chemical etching reaction of SiN and HF, is unstable and easily decomposes under ion bombardment or heating, leading to the gradual lateral etching of the Si3N4 film sidewalls. In this embodiment, a protective film 300 is formed on the sidewall 2011 of the etching trench 201 via atomic layer deposition (ALD) and / or chemical vapor deposition (CVD), thereby reducing the risk of distortion in the vertical etching morphology of the substrate 200.

[0109] The first film layer 210 generates byproducts during the etching reaction, such as H2O and HF. H2O and HF are physically adsorbed onto the sidewalls 2011 and bottom wall 2012 of the etching tank 201 via hydrogen bonds, forming a co-solution film. H2O and HF can further react to generate HF. - 2 and H3O + The specific reaction equation is denoted as equation (3).

[0110]

[0111] Please refer to the following: Figure 2 , Figure 7 , Figure 8 and Figure 9 , Figure 7 This is a process diagram of the fabrication method of the high aspect ratio etched structure provided in the embodiments of this application; Figure 8 This is a process diagram of the deposition of a protective film 300 on the sidewall 2011 of the etching tank 201 by TBTEMT, as provided in the embodiments of this application. Figure 9 This is a reaction mechanism diagram showing the deposition of a protective film 300 by TBTENT on the sidewall 2011 of the etching tank 201, as provided in this embodiment. The formation of the protective film 300 includes the following steps: step1-step2: Step 1: Precursor gas is introduced into etching chamber 1. The precursor gas diffuses into etching tank 201 and is chemically adsorbed on the side wall 2011 and bottom wall 2012 of etching tank 201, forming a metal oxide protective layer 310.

[0112] Specifically, the sidewall surfaces of SiO2 and SiN are exposed to a plasma environment, resulting in the formation of numerous OH and H free radicals. TBTMT reacts with the liquid water adsorbed on the sidewalls of the etching tank 201 via chemisorption. The amino ligands in TBTMT undergo oxidation with the OH free radicals in the liquid water, generating a Ta2O5 film (i.e., the metal oxide protective layer 310). Consequently, some amino ligands detach from the metal-organic framework (MOF) and form deposition byproducts, including HR. 1 HR 2 and HNR 1 R 2 , where R 1 and R 2 These are alkyl groups, such as methyl and ethyl, linked to amino ligands in the molecular structure of the precursor gas. These deposition byproducts can be removed using a molecular pump. A metal oxide protective layer 310 can be formed on the sidewall 2011 of the etching tank 201, thereby preventing further reaction between HF and the sidewall 2011 of the etching tank 201, reducing HF loss, and improving the vertical etching rate. The molecular structure of the precursor gas adsorbed on the sidewall 2011 of the etching tank 201 can also further undergo oxidation reactions with liquid water (e.g., ... Figure 9 Path 1 shown: The remaining amino ligands (amido) and imino ligands (imido) detach from the metal-organic framework (MOF) to generate metal oxides Ta2O5 and H2NR3, wherein R 3 It is an alkyl group, such as tert-butyl, attached to an imino ligand in the precursor molecule.

[0113] In the second step, a reaction gas is introduced into the etching chamber 1. The precursor gas adsorbed on the sidewall 2011 of the etching tank 201 undergoes a reduction reaction with the H radicals in the reaction gas to generate metal nitride TaN. x and / or TaC y N z and HR 3 (like Figure 9 Path 2 in the equation, where 0.5≤x≤1, 0.5≤y≤1, 0.5≤z≤1, R 3 It is an alkyl group, such as tert-butyl, attached to an imide ligand in the precursor molecule.

[0114] Specifically, H radicals in the reactant gas react with imino ligands and / or amino ligands in the precursor gas to generate a metal nitride protective layer 320 and / or a metal carbonitride protective layer 330. Of course, in some embodiments, the molecular structure of the precursor gas adsorbed on the sidewall 2011 of the etching tank 201 can further undergo a reduction reaction with the H active radicals in the plasma component to generate the metal nitride protective layer 320 and / or the metal carbonitride protective layer 330. Understandably, because the metal nitride protective layer 320 and the metal carbonitride protective layer 330 have high conductivity (typically greater than or equal to 200 μΩ·cm), the accumulation of residual positive charge at the bottom of the etching tank 201 is reduced, ion scattering is reduced, and distortion of the vertical etching morphology is avoided.

[0115] It should be noted that the protective film 300 can be generated by CVD reaction, that is, the first and second steps can be performed simultaneously; or, the protective film 300 can be generated by ALD reaction, that is, the first and second steps are performed alternately and cyclically, for example, the number of cycles for the first and second steps can be 5 to 50 times. The thickness of the protective film 300 can be any value in the range of 0.1 nm to 5 nm. Understandably, if the thickness of the protective film 300 is less than 0.1 nm, the protective film 300 cannot completely and continuously cover the sidewall 2011 of the etching trench 201. For example, the protective film 300 may have missing, porous, or broken areas, which will prevent the sidewall 2011 of the etching trench 201 from forming a continuous conductive path for balancing surface potential, suppressing charge accumulation, or regulating the electric field of the plasma sheath. The protective film 300 has poor structural stability and is prone to peeling off from the sidewall 2011 of the etching trench 201 after continuous plasma bombardment during the etching process. At the same time, it reduces the conduction efficiency of residual positive charge at the bottom of the trench, the charge shielding effect cannot be suppressed, and the intensified ion scattering causes distortion of the etching morphology. When the thickness of the protective film 300 exceeds 5 nm, the excessively thick protective film 300 will reduce the opening size of the etching trench 201, causing the opening of the high aspect ratio etching trench 201 to be blocked, blocking the plasma action area, interfering with the subsequent etching process, and reducing the pattern processing accuracy and structural forming quality. This embodiment of the application sets the thickness of the protective film 300 to any value between 0.1 nm and 5 nm, thereby enabling the formation of a complete and continuous protective film 300 on the sidewall 2011 of the etching trench 201. This allows the protective film 300 to adhere firmly to the sidewall 2011 of the etching trench 201, while improving the efficiency of removing residual positive charges from the bottom of the etching trench 201, suppressing charge shielding effects, improving ion scattering, and maintaining a regular vertical etching morphology. It also avoids critical dimension shifts in the etching trench 201 and blockage of openings in high aspect ratio structures caused by an excessively thick protective film 300, and does not hinder the interaction between plasma and the substrate in subsequent etching processes, thus balancing charge elimination capability and pattern dimensional processing accuracy. The thickness of the protective film 300 can be 0.1 nm, 2 nm, or 5 nm, etc.

[0116] like Figure 1 and Figure 2As shown, in some possible embodiments, the etching apparatus 100 further includes a temperature control system 8 connected to the control system 7. The control system 7 is also used to control the temperature control system 8 to raise the temperature of the substrate 200 to be etched after the etching process is completed, providing a suitable temperature for subsequent deposition processes. On the one hand, the heated substrate 200 can improve the adsorption activity and reaction kinetics rate of the precursor gas, promoting a full chemical reaction of the precursor gas and uniformly depositing a dense and continuous protective film 300 on the sidewall 2011 of the etching tank 201. Simultaneously, the protective film 300 can quickly remove residual positive charges accumulated at the bottom of the etching tank 201, suppressing charge shielding effects, reducing ion scattering of plasma, preventing distortion of the vertical etching morphology, and stabilizing the steepness and flatness of the sidewall 2011 of the high aspect ratio etching tank 201. This optimizes the overall etching process morphology consistency. On the other hand, the heated substrate 200 increases the saturated vapor pressure of the precursor gas, causing excess precursor gas that did not participate in the formation of the protective film 300 within the etching tank 201 to evaporate and dissipate. This prevents excessive precursor gas from continuously depositing and forming an overly thick residual protective film 300, which could cause blockage of the etching tank 201 opening and dimensional deviation. Simultaneously, it promotes the desorption of byproducts within the already formed protective film 300, optimizing the density and uniformity of the protective film 300, reducing particulate contamination within the etching chamber 1, and facilitating subsequent processes. The temperature control system 8 can be mounted on the first electrode 21 and / or the second electrode 22.

[0117] During the deposition process, the temperature of the substrate 200 to be etched can be any value within the range of 50℃-100℃. This increases the saturated vapor pressure of the precursor gas in the etching chamber 1, allowing the precursor gas to uniformly adhere to the sidewalls 2011 of the etching tank 201. This improves the density and bonding strength of the protective film 300, while avoiding deformation, damage, and excessive thermal stress of the substrate 200 caused by excessively high temperatures. It also allows for control of the deposition rate, optimization of film quality, reduction of processing difficulty in subsequent etching processes, and improvement of overall process stability and product yield. The temperature of the substrate 200 to be etched during the deposition process can be 50℃, 60℃, 70℃, 80℃, 90℃, or 100℃, etc.

[0118] The application embodiment provides a method for fabricating a high aspect ratio etched structure, which is performed by the aforementioned etching apparatus 100. The following is in conjunction with... Figure 1 and Figure 10 The fabrication method of the high aspect ratio etched structure in the embodiments of this application is described in detail.

[0119] Step S101: Provide a substrate to be etched.

[0120] The substrate to be etched has a surface to be processed. A patterned mask structure is arranged on the surface to be processed. The patterned mask structure is used to define at least one area to be etched, so as to selectively remove the material of the area to be etched in a subsequent etching process to form an etching trench.

[0121] Step S102: The substrate to be etched is subjected to alternating etching and deposition processes to form an etching trench of a predetermined depth on the substrate. The deposition process includes: introducing a precursor gas and a reactive gas into the etching chamber to deposit a protective film of a target thickness on the sidewall of the etching trench; and purging out the precursor gas, the reactive gas, and deposition byproducts. The protective film includes a metal nitride protective layer generated by the reaction of H radicals in the reactive gas and imino ligands in the precursor gas; and / or, the protective film includes a metal carbonitride protective layer generated by the reaction of H radicals in the reactive gas and amino ligands in the precursor gas.

[0122] The method for fabricating high aspect ratio etched structures provided in this application has several advantages. First, the protective film prevents lateral etching of the sidewalls, reducing damage to the sidewalls from free radicals and neutral species such as HF, H, and F, and improving the utilization rate of these free radicals during the etching process. Simultaneously, the metal nitride and / or metal carbonitride protective layers can prevent the accumulation of residual positive charges at the bottom of the etching tank, reducing ion scattering and avoiding distortion of the vertical etching morphology. Second, the method of alternating etching and deposition processes decouples the sidewall passivation deposition of the protective film from the etching of the substrate. This allows for precise control of the etching amount, etching time, and the thickness of the protective film formed in each deposition process, reducing the probability of morphological distortion of the high aspect ratio etched structure during vertical etching.

[0123] For example, the number of etching and deposition cycles can be set to any value between 10 and 100. Understandably, when the number of cycles is less than 10, excessive etching in a single cycle can easily cause sidewall tilting and profile deterioration. When the number of cycles exceeds 100, it significantly prolongs the process time, reduces production capacity, and the accumulation of excess film layers from multiple depositions can cause deviations in the critical dimensions of the etching tank. This range balances the uniformity of the high aspect ratio etching tank morphology, dimensional accuracy, and equipment production efficiency. In this embodiment, by setting the number of etching and deposition cycles to within the range of 10 to 100, the etching tank depth is processed step-by-step, layer by layer. Each cycle only removes a small amount of etching material and simultaneously deposits a protective film. This allows the metal nitride and / or metal carbonitride protective layers deposited in each round to continuously guide residual charge at the bottom of the etching tank, suppress charge shielding effects, and reduce ion scattering and morphological distortion caused by single-stage deep etching. Simultaneously, multiple cycles precisely control the overall depth of the etching tank to a preset standard. The number of etching and deposition cycles can be set according to factors such as the aspect ratio of the etching trench and the etching parameters of the substrate to be etched; this application embodiment does not impose specific limitations. The number of etching and deposition cycles can be set to 10, 30, 50, 80, or 100 times, etc.

[0124] In some possible implementations, the input of precursor gas and reactant gas into the etching chamber includes: inputting precursor gas into the etching chamber through a second input gas path, and inputting reactant gas into the etching chamber through a first input gas path. The first input gas path is independent of the second input gas path. In some possible implementations, the input of precursor gas and reactant gas into the etching chamber includes steps S206-S208. Therefore, by independently controlling the intake of the precursor gas and reactant gas, the thickness of the protective film deposited on the sidewall of the etching tank can be precisely controlled. It enables separate delivery of precursor gas and reactant gas, and independent control of the flow rate, on / off timing, and supply pressure of each gas path, avoiding premature pre-reaction of different gases in the delivery pipeline, the generation of particulate matter, or corrosion of the pipeline; at the same time, it can independently match the gas supply process window of the precursor gas, precisely control the concentration of the precursor gas in the etching chamber, flexibly switch the gas ratio of different process stages such as etching, passivation, and cleaning, prevent gas crosstalk between gas paths, and improve etching morphology, etching rate, and process repeatability.

[0125] In some possible implementations, before introducing the precursor gas and reactant gas into the etching chamber, the fabrication method further includes: introducing the precursor gas into a buffer chamber connected to the second input gas path; and adjusting the gas pressure in the buffer chamber to be greater than or equal to twice the gas pressure in the etching chamber. Thus, the buffer chamber can stabilize the flow rate and partial pressure of the precursor gas, avoiding interference with precursor gas delivery caused by pressure fluctuations and airflow disturbances within the etching chamber, thereby improving the uniformity and stability of the precursor gas input. Simultaneously, utilizing the pressure difference between the buffer chamber and the etching chamber allows the precursor gas to enter the etching chamber more smoothly and controllably, reducing gas pulse impacts and instantaneous concentration fluctuations, improving the consistency of the precursor gas undergoing chemical adsorption and hydrogenation or hydrogenolysis reactions on the sidewall of the etching tank, thereby improving the uniformity of the protective film deposition thickness and film quality, and enhancing the repeatability and structural precision of the etching process.

[0126] In some possible implementations, the step of inputting the precursor gas into the etching chamber through the second input gas path includes: inputting the precursor gas into the etching chamber through the second input gas path while maintaining the temperature of the precursor gas within the second input gas path within a target temperature range, wherein the target temperature range is 50℃-150℃. Therefore, by maintaining the temperature of the precursor gas within the second input gas path within the target temperature range, the risk of the precursor gas cooling down and condensing in the delivery pipeline is reduced, improving the stability and reliability of the precursor gas's consistently gaseous delivery, reducing material loss and pipeline blockage problems, stabilizing the delivery state of the precursor gas, improving the overall control accuracy of the precursor gas's flow rate and supply, and enhancing process stability.

[0127] In some possible implementations, the fabrication method further includes controlling the heat preservation module to maintain a constant temperature for the precursor gas in the second input gas path. The target temperature can be, but is not limited to, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, or 150°C. It is understood that the fabrication method of this application is executed by the aforementioned etching apparatus, specifically by the heat preservation module performing the heat preservation step, thereby achieving a heat preservation effect on the precursor gas and achieving the same technical effect as the etching apparatus.

[0128] In some possible implementations, the fabrication method further includes: after completing the preceding deposition process, adjusting the thickness of the protective film formed in the subsequent deposition process to be less than the thickness of the protective film formed in the preceding deposition process. Therefore, setting the thickness of the protective film formed in the subsequent deposition process to be less than the thickness of the protective film formed in the preceding deposition process allows the thicker protective film formed in the preceding deposition step to provide sufficient protection for the sidewalls of the etched structure, suppressing lateral etching of the sidewalls of the etched grooves; while using a thinner protective film in the subsequent deposition step reduces the shielding of subsequent etching ions by the protective film, improves the penetration and uniformity of longitudinal etching, improves the perpendicularity of the etching contour, and avoids defects such as sidewall tilting, local accumulation, and microburrs caused by excessively thick protective films. This ensures the sidewall protection effect while improving the uniformity of etching depth and the overall structural morphology accuracy. Understandably, when the protective film is formed by atomic layer deposition, the thickness of the protective film can be determined by controlling the number of deposition cycles. When the protective film is formed by chemical vapor deposition, the thickness of the protective film can be determined by controlling the reaction time of the deposition process.

[0129] In some possible implementations, the fabrication method further includes: acquiring the current depth of the etched trench, and adjusting the saturated vapor pressure of the precursor gas to a target saturated vapor pressure based on the current depth. Thus, by acquiring the real-time depth of the etched trench during the deposition process and matching the precursor gas to the corresponding target saturated vapor pressure based on this depth, the precursor gas supply can be dynamically adjusted according to the aspect ratio of the etched trench. This allows for the uniform formation of a protective passivation film within etched trenches of different depths, mitigating the load effect between shallow and deep etched trenches, continuously suppressing lateral etching on the sidewalls and bottom drilling, maintaining a stable and regular vertical etched trench morphology, simultaneously widening the process adaptability range, and reducing mask loss and wafer particle defects.

[0130] For example, adjusting the saturated vapor pressure of the precursor gas to the target saturated vapor pressure includes: adjusting the temperature within the etching chamber; and / or, changing the composition of the precursor gas until the saturated vapor pressure of the precursor gas reaches the target saturated vapor pressure. Thus, the control system can flexibly adjust the precursor saturated vapor pressure to a target value matching the real-time depth of the etching tank by adjusting the etching chamber temperature and changing the precursor gas composition. This dynamically adapts to the precursor transport requirements within etching tanks of different depths, ensuring uniform passivation film formation across the entire etching tank, reducing etching load effects, suppressing sidewall etching and bottom drilling, stably obtaining a vertically regular high aspect ratio etching tank morphology, broadening the process control window, and reducing the process limitations caused by a single control method.

[0131] Exemplarily, the fabrication method further includes: after completing the preceding deposition treatment, increasing the saturated vapor pressure of the precursor gas in the subsequent deposition treatment. It is understood that the fabrication method of this application is executed using the aforementioned etching apparatus. Specifically, the vaporization temperature of the precursor gas can be adjusted using the ampoule 422, thereby adjusting the saturated vapor pressure of the precursor gas to a saturated vapor pressure corresponding to the target temperature, achieving the same technical effect as the etching apparatus. In some embodiments, at the same vaporization temperature, the saturated vapor pressure of the precursor gas can also be adjusted by changing to a different type of precursor. The method of adjusting the saturated vapor pressure of the precursor gas can be described based on the etching apparatus; this application embodiment does not specifically limit this method.

[0132] Combination Figure 10 The embodiments shown below Figures 11-12 The illustrated embodiment is a detailed description of the method for fabricating the high aspect ratio etched structure of this application.

[0133] like Figure 11 As shown, the method includes the following steps S201-S212.

[0134] Step S201: Provide a substrate to be etched.

[0135] Step S201 can be found in Figure 10 The details of step S101 are omitted here.

[0136] Step S202: Etching gas is introduced into the etching chamber, and an initial etching trench is formed on the substrate to be etched, wherein the depth of the initial etching trench is less than a preset depth.

[0137] Step S203: Purge the etching reaction byproducts and the etching gas.

[0138] Specifically, when the depth of the initial etching trench is less than the preset depth, at least one etching process is performed on the substrate exposed by the initial etching trench until an etching trench with a preset depth is formed within the etchable layer. Subsequent etching processes etch the substrate along the initial etching trench formed in the previous etching process, and after multiple etching processes, the multiple initial etching trenches constitute the etchable trench. Specifically, the sum of the depths of the multiple initial etching trenches is equal to the depth of the etchable trench (i.e., the preset depth).

[0139] It should be noted that the etching process includes steps S202 and S203. Step S202 specifically includes: providing plasma source gas into the etching chamber and ionizing and / or dissociating the plasma source gas to generate basic plasma; providing etching gas into the etching chamber and preparing etching plasma; accelerating ions in the plasma to form high-energy bombarding ions and etching the substrate.

[0140] Specifically, plasma source gas is supplied to the etching chamber, and the high-frequency radio frequency source is turned on and set to a low-power setting to ionize and / or dissociate the etching gas, initially generating basic plasma (such as H radicals). Then, etching gas is supplied to the etching chamber, and the high-frequency radio frequency source is switched to a high-power setting to improve the ionization efficiency of the etching gas and prepare high-density etching plasma. Next, the low-frequency radio frequency source is turned on, and its power or bias voltage is adjusted to a high level to accelerate ions within the plasma, forming high-energy bombardment ions (such as Ar). + Kr + Xe + HF + (at least one of the following), to enhance the anisotropic etching effect on the substrate to be etched. Finally, the etching reaction products are purged with an inert gas. The purging gas in the purging step can be an inert gas. Exemplarily, the plasma source gas may include NH3 and H2, and the etching gas may include HF, PF... 3、 Cl2, HBr, NF 3、 CH2F2 and Kr. The purging gas in the purging step can be N2.

[0141] Step S203 employs gas purging. The gas can be, but is not limited to, an inert gas. For example, the inert gas is at least one of N2, Ar, Kr, or Xe. Understandably, inert gases are chemically stable and will not undergo side reactions with the protective film on the surface of the etching tank, residual precursors in the etching chamber, or reaction byproducts during the purging process. They can quickly replace and remove residual precursor gases, reaction gases, and deposition byproducts from inside the chamber.

[0142] In some possible implementations, the substrate to be etched is at a temperature of -100°C to 100°C during the etching process. It is understood that the fabrication method of this application is performed using the aforementioned etching apparatus, specifically by using a temperature control unit to perform a temperature control step on the substrate to be etched, thereby enabling the etching process of the substrate to be etched at a low temperature, achieving the same technical effect as the etching apparatus, namely, increasing the vertical etching rate of the substrate to be etched and achieving directional etching of the substrate to be etched.

[0143] Step S204: Increase the temperature of the substrate to be etched. In some possible embodiments, after each etching process, the fabrication method further includes increasing the temperature of the substrate to be etched. It is understood that the fabrication method of this application is executed by the aforementioned etching apparatus, specifically by a temperature control unit to perform the temperature control step on the substrate to be etched. This achieves the same technical effect as the etching apparatus by increasing the temperature of the substrate during the deposition process, ensuring sufficient chemical reaction of the precursor gas and uniform deposition on the surface of the etched structure to form a dense and continuous protective film. This optimizes the density and uniformity of the protective film, reduces particulate contamination in the etching chamber, and facilitates subsequent processes. Of course, in some embodiments, step S205 can be executed directly after step S203.

[0144] Step S205: A precursor gas is introduced into the etching chamber so that the amino ligands in the precursor gas react with the liquid film adsorbed on the sidewall of the groove to generate the metal oxide protective layer.

[0145] For the selection of precursor gases, please refer to [reference needed]. Figure 1 The etching device 100 will not be described in detail here.

[0146] Step S206: Purge and discharge the precursor gas and chemical adsorption byproducts.

[0147] The gas used in the purging step in step S203 is the same as that used in step S206, and will not be described again here.

[0148] Step S207: The reaction gas is introduced into the etching chamber, so that the H radicals in the reaction gas react with the imine ligands and / or amino ligands in the precursor gas to generate the metal nitride protective layer and / or the metal carbonitride protective layer. The metal nitride protective layer and / or the metal carbonitride protective layer adhere to the metal oxide protective layer to form a protective film.

[0149] Step S208: Purge and remove the reaction gas and deposited byproducts.

[0150] The gas used in the purging step in step S203 is the same as that used in step S208, and will not be described again here.

[0151] It should be noted that the deposition process includes steps S205 to S208. The deposition process employs atomic layer deposition (ALD). Therefore, by forming a protective film through ALD, the thickness of the protective film is more precisely controlled, its uniformity, density, and consistency are improved, its ability to protect the etching tank walls is enhanced, and the risks of etching deviations, damage, or abnormal contours due to localized uneven film thickness are reduced.

[0152] Step S209: Determine whether the thickness of the protective film is less than the target thickness. If the thickness of the protective film is less than the target thickness, return to step S206; if the thickness of the protective film is greater than or equal to the target thickness, proceed to step S210.

[0153] Step S209 specifically includes: obtaining the thickness of the initial protective film formed on the sidewall of the etching tank. If the thickness of the initial protective film is less than the target thickness, at least one deposition process is performed on the initial protective film until the thickness of the protective film is greater than or equal to the target thickness. Subsequent deposition processes deposit along the initial protective film formed in the previous deposition process, and after multiple deposition processes, a plurality of the initial protective films constitute the protective film. Specifically, the sum of the thicknesses of the plurality of initial protective films is equal to the thickness of the protective film (i.e., the target thickness).

[0154] In some possible implementations, depositing a protective film of a target thickness on the wall of the etching tank includes: repeatedly performing the deposition process a preset number of cycles. This ensures that a sufficiently thick protective film is formed on the sidewalls of the etching tank. The target thickness is any value between 0.1 nm and 5 nm. This sufficiently thick protective film can better resist the bombardment of the etching plasma during the etching process and ensures that there is sufficient space in the etching tank for the etching plasma to enter the bottom of the etching tank.

[0155] Understandably, if the thickness of the protective film is less than 0.1 nm, it cannot completely and continuously cover the surface of the etching trench, resulting in a break in the conductive path. The protective film has poor structural stability and is prone to peeling off from the sidewall of the etching trench after continuous plasma bombardment during the etching process. At the same time, it reduces the conduction efficiency of residual positive charge at the bottom of the trench, and the charge shielding effect cannot be suppressed. The increased ion scattering leads to distortion of the etching morphology. When the thickness of the protective film exceeds 5 nm, the excessively thick protective film will reduce the opening size of the etching trench, causing blockage of the opening of the high aspect ratio etching trench, blocking the plasma interaction area, interfering with the subsequent etching process, and reducing the pattern processing accuracy and structural forming quality. This application embodiment is based on setting the thickness of the protective film within the range of 0.1nm-5nm, thereby enabling the formation of a complete and continuous protective film on the sidewall of the etching tank. This allows the protective film to adhere firmly to the sidewall of the etching tank, resisting the bombardment force of the etching plasma during the etching process. Simultaneously, it improves the removal efficiency of residual positive charges at the bottom of the etching tank, suppresses charge shielding effects, improves ion scattering, and maintains a regular vertical etching morphology. It avoids critical dimension shifts in the etching tank and clogging of openings in high aspect ratio structures caused by excessively thick protective films, while not hindering the interaction between the plasma and the substrate in subsequent etching processes, thus balancing charge elimination capability and pattern dimensional processing accuracy. The target thickness of the protective film can be 0.1nm, 2nm, 4nm, or 5nm, etc. The target thickness can be user-defined or set by the factory default of the etching apparatus, and this application embodiment does not impose specific limitations.

[0156] It should be noted that when the protective film is formed by atomic layer deposition, the amount of precursor gas and reactant gas introduced is maintained within the saturation supply range, so that the thickness of the protective film mainly increases with the increase of the number of deposition cycles. The fluctuation of the amount of precursor gas and reactant gas introduced has a negligible effect on the thickness of the protective film, thereby achieving a protective film of the target thickness after performing the deposition process for a preset number of cycles.

[0157] The preset number of cycles can be set, but is not limited to, 5-50 times. Understandably, too few cycles result in insufficient protective film thickness and incomplete coverage, leading to weak protective performance and potential failure. Too many cycles result in an excessively thick protective layer and redundant accumulation, increasing process time and production costs, and potentially causing film cracking and peeling. This also affects the opening size of the etching tank, prolonging the processing time of subsequent etching and deposition processes. This embodiment uses atomic layer deposition to form a protective film at a preset number of cycles, thereby precisely forming a protective film of a set thickness on the sidewall of the etching tank. This results in good film uniformity and high adhesion, improving the protective effect of the film, controlling the overall process rhythm, and reducing unnecessary energy consumption and time. Simultaneously, it improves the dimensional accuracy of the etching tank, ensuring stable and smooth operation of subsequent processes. The preset number of cycles can be, but is not limited to, 5, 10, 20, 30, 40, or 50 times. For example, the preset number of cycles can be 12 times.

[0158] Step S210: Determine whether the depth of the etching groove is less than the preset depth. If the depth of the etching groove is less than the preset depth, return to step S202; if the depth of the etching groove is equal to the preset depth, proceed to step S212.

[0159] Step S211: Adjust the temperature of the subsequent etching process to be lower than the temperature of the preceding etching process.

[0160] Understandably, in some possible implementations, when the depth of the etching tank is less than the preset depth, step S211 can be executed first, followed by step S202. The deeper the etching depth, the greater the ion flux attenuation. This embodiment of the application improves the structural stability of the protective film formed by the deposition process by setting the etching temperature to decrease with increasing etching depth, reducing the risk of lateral etching on the sidewalls of the etching tank, decreasing ion flux attenuation, and improving vertical etching efficiency. Simultaneously, the low temperature can also suppress the desorption and diffusion loss of water molecules within the etching tank, thereby enhancing the adsorption stability of the co-solid film on the sidewalls of the etching tank, enhancing the adsorption effect of HF on the bottom wall of the etching tank, and improving the vertical etching rate.

[0161] Step S212: Remove the protective film.

[0162] When the etching tank reaches a preset depth, the protective film formed on the sidewalls of the etching tank is removed. This prevents precursor deposits from affecting subsequent processes and the performance of the chip device. The protective film can be removed using dry etching and / or wet etching processes at high or room temperature. Dry etching processes can use gases such as CxFy, Cl2, BCl3, and SF6 to remove TaN and Ta2O deposited on the sidewalls of the etching tank. 5。Wet etching processes can employ either hot alkaline solutions or hot acidic solutions. Hot alkaline solutions can be, but are not limited to, at least one of KOH and NaOH solutions, while hot acidic solutions can be, but are not limited to, at least one of HF, HCl, and HNO3 solutions.

[0163] like Figure 12 As shown, another embodiment of this application provides a method for fabricating a high aspect ratio etched structure, the method including the following steps S301-S309.

[0164] Step S301: Provide a substrate to be etched.

[0165] Step S302: Etching gas is introduced into the etching chamber and an initial etching trench is formed on the substrate to be etched, wherein the depth of the initial etching trench is less than a preset depth.

[0166] Step S303: Purge the etching reaction byproducts and the etching gas.

[0167] Step S304: Increase the temperature of the substrate to be etched.

[0168] Steps S301-S304 can be found in [reference]. Figure 11 The steps S201-S204 are described in detail, and will not be repeated here.

[0169] Step S305: Precursor gas and reactant gas are simultaneously introduced into the etching chamber and reacted for a target time to deposit a protective film of target thickness on the wall of the etching tank.

[0170] The target time can be any value between 5s and 50s. Understandably, if the reaction time of chemical vapor deposition (CVD) is too short, the precursor gas reaction will be insufficient, resulting in a thin, unevenly deposited protective film that fails to meet usage requirements. Conversely, if the reaction time is too long, the protective film may become excessively thickened, extending the process cycle, increasing production costs, and potentially causing the protective film to become loose, peel, or detach. Furthermore, it can alter the original dimensions of the etching tank, interfering with the accuracy and effectiveness of subsequent processing steps. This application achieves precise deposition of a tank wall protective film of a specified thickness by simultaneously introducing precursor and reactive gases into the etching chamber and maintaining a reaction time between 5s and 50s. This results in a stable film formation rate, a dense and uniform film layer, improved protective film effectiveness, better control of the overall process rhythm, and reduced unnecessary energy consumption and time. Simultaneously, it improves the dimensional accuracy of the etching tank, ensuring stable and smooth operation of subsequent processes. The target time can be, but is not limited to, 5s, 10s, 20s, 30s, 40s, or 50s. For example, the preset number of loops can be 8 seconds.

[0171] In some possible implementations, simultaneously introducing precursor gas and reactive gas into the etching chamber includes: gradually increasing the amount of reactive gas introduced into the etching chamber while gradually decreasing the amount of precursor gas introduced. Thus, by gradually increasing the reactive gas flow rate and simultaneously decreasing the precursor gas flow rate, the morphological integrity of the outermost metal nitride or metal carbonitride protective layer is improved. This allows the highly conductive metal nitride or metal carbonitride protective layer to avoid the charge shielding effect caused by residual positive charge at the bottom of the etching tank, reducing ion scattering and lowering the probability of vertical morphological distortion in the etching tank. Simultaneously, by steadily controlling the gas component ratio within the etching chamber, the protective film deposition process proceeds gradually, improving the morphological integrity and structural density of the protective film.

[0172] In some possible implementations, the step of introducing precursor gas and reactive gas into the etching chamber to deposit a protective film of a target thickness on the wall of the etching tank includes: introducing precursor gas into the etching chamber such that amino ligands in the precursor gas react with the liquid film adsorbed on the sidewall of the tank for a first preset time to generate the metal oxide protective layer of a first thickness; purging out the precursor gas and chemisorption byproducts; and introducing reactive gas into the etching chamber such that H radicals in the reactive gas react with imino ligands and / or amino ligands in the precursor gas for a second preset time to generate the metal nitride protective layer and / or the metal carbonitride protective layer of a second thickness, wherein the sum of the first thickness and the second thickness is equal to the target thickness. It should be noted that when the protective film is formed by chemical vapor deposition, the amount of precursor gas and reactant gas introduced is maintained within the saturation supply range, so that the thickness of the protective film mainly increases with the extension of the deposition time. The fluctuation of the amount of precursor gas and reactant gas introduced has a negligible effect on the thickness of the protective film. This achieves the deposition of a metal oxide protective layer of a first thickness within a first preset time, and the deposition of a metal nitride protective layer and / or a metal carbonitride protective layer of a second thickness within a second preset time.

[0173] Therefore, by using a stepwise deposition setup, the layered and controllable growth of the metal oxide protective layer and the metal nitride protective layer can be achieved. This facilitates precise control over the thickness, composition, and interface structure of each film layer, enabling the formation of a metal nitride protective layer on the outermost side of the protective film. The high conductivity and low resistivity of the metal nitride can be used to avoid the charge shadowing effect caused by the residual positive charge at the bottom of the etching tank, reducing ion scattering, lowering the probability of vertical morphology distortion in the etching tank, and improving the density and uniformity of the protective film. At the same time, the stepwise reaction and intermediate purging steps can reduce by-product residues, avoid mutual interference between different reactive gases, reduce defects between the layers of the protective film, improve the protective effect of the protective film on the sidewalls of the etching tank and the morphological regularity, and improve the stability and structural accuracy of subsequent etching processes.

[0174] Step S306: Purge and discharge the precursor gas, the reactant gas, and the deposition byproducts.

[0175] The gas used in the purging step in step S203 is the same as that used in step S306, and will not be described again here.

[0176] It should be noted that the deposition process includes steps S305 and S306. The deposition process employs chemical vapor deposition (CVD) to form a protective film, thereby increasing the deposition rate of the protective film and reducing the requirements for the precursor gas delivery pipeline.

[0177] Step S307: Determine whether the depth of the etching groove is less than the preset depth. If the depth of the etching groove is less than the preset depth, return to step S308; if the depth of the etching groove is equal to the preset depth, proceed to step S309.

[0178] Step S308: Adjust the temperature of the subsequent etching process to be lower than the temperature of the preceding etching process.

[0179] Step S308 can be referred to Figure 11 The description of step S211 is omitted here.

[0180] Step S309: Remove the protective film.

[0181] Step S309 can be referred to Figure 11 The description of step S212 is omitted here.

[0182] In another embodiment, this application provides a control method that can be executed by the control system described in any of the foregoing embodiments. The method includes the operations / steps performed by the foregoing control system, which can be referred to the relevant descriptions in the foregoing embodiments without further elaboration.

[0183] In another embodiment, this application provides a semiconductor device including a unit or module for performing any of the above-described methods for fabricating high aspect ratio etched structures.

[0184] In one implementation, such as Figure 1 As shown, the semiconductor device includes the etching apparatus 100 described above.

[0185] remove Figure 1 In addition to the etching apparatus 100 shown, the semiconductor device may include, but is not limited to, a transport system, a monitoring and diagnostic system, a transition cavity system, or a vacuum system. The transport system is used to transport the substrate 200 to be etched. The monitoring and diagnostic system acquires process status parameters of the substrate 200 during the etching and deposition processes. The transition cavity system may include, but is not limited to, a cleaning system or an exhaust system. The vacuum system provides a vacuum environment for the etching chamber and the transition cavity system to maintain the pressure in each chamber.

[0186] For example, the semiconductor device is a reactive ion etching device, an inductively coupled plasma etching device, or a capacitively coupled plasma etching device, etc.

[0187] Please see Figure 13 In another embodiment, this application provides a control device 500. The control device 500 includes a processor 510 and a memory 520. The processor 510 is coupled to the memory 520. The memory 520 is used to store computer programs or instructions and / or data. The processor 510 is used to execute the computer programs or instructions stored in the memory 520, or to read the data stored in the memory 520, to perform the manufacturing methods in the above-described method embodiments.

[0188] Optionally, there may be one or more processors 510.

[0189] Optionally, the memory 520 may be one or more.

[0190] Alternatively, the memory 520 can be integrated with the processor 510, or it can be set separately.

[0191] In another embodiment, this application provides a computer-readable storage medium storing instructions that, when executed on a computer, cause the computer to perform the operations / steps performed by the control system described in any of the above embodiments.

[0192] In another embodiment, this application provides a computer program product containing instructions that, when executed by a processor, cause the processor to perform the operations / steps performed by the control system described in any of the above embodiments.

[0193] In one exemplary embodiment, the aforementioned computer-readable storage medium may include, but is not limited to, various media capable of storing computer programs, such as a USB flash drive, read-only memory (ROM), random access memory (RAM), portable hard disk, magnetic disk, or optical disk.

[0194] Furthermore, this application also provides a chip including a processor. A memory for storing a computer program is provided independently of the chip, and the processor is used to execute the computer program stored in the memory so that the manufacturing methods in the various method embodiments of this application are executed.

[0195] Furthermore, the chip may also include a communication interface. The communication interface may be an input / output interface or an interface circuit, etc. Furthermore, the chip may also include a memory.

[0196] It should be understood that the processor in the embodiments of this application can be an integrated circuit chip with the ability to process signals. In implementation, each step of the above method embodiments can be completed by the integrated logic circuits in the processor's hardware or by instructions in software form. The processor can be a central processing unit (CPU), or other general-purpose processors, digital signal processors (DSPs), application-specific integrated circuits (ASICs), field-programmable gate arrays (FPGAs), or other programmable logic devices, discrete gate or transistor logic devices, or discrete hardware components. A general-purpose processor can be a microprocessor or any conventional processor. The steps of the method disclosed in the embodiments of this application can be directly implemented by a hardware encoding processor, or implemented by a combination of hardware and software modules in the encoding processor. The software modules can be located in random access memory, flash memory, read-only memory, programmable read-only memory, electrically erasable programmable memory, registers, or other mature storage media in the art. The storage medium is located in memory, and the processor reads the information in the memory and, in conjunction with its hardware, completes the steps of the above method.

[0197] The memory in the embodiments of this application can be volatile memory or non-volatile memory, or may include both volatile and non-volatile memory. The non-volatile memory can be read-only memory (ROM), programmable read-only memory (PROM), erasable programmable read-only memory (EPROM), electrically erasable programmable read-only memory (EEPROM), or flash memory. The volatile memory can be random access memory (RAM), which serves as an external cache. By way of example, but not limitation, many forms of RAM are available, such as static random access memory (SRAM), dynamic random access memory (DRAM), synchronous dynamic random access memory (SDRAM), double data rate synchronous dynamic random access memory (DDRSDRAM), enhanced synchronous dynamic random access memory (ESDRAM), and synchronous link dynamic memory (SLDRAM).

[0198] It should be noted that when the processor is a general-purpose processor, DSP, ASIC, FPGA, or other programmable logic device, discrete gate or transistor logic device, or discrete hardware component, the memory can be integrated into the processor.

[0199] It should also be noted that the memory described herein is intended to include, but is not limited to, these and any other suitable types of memory.

Claims

1. A method for fabricating a high aspect ratio etched structure, characterized in that, Includes the following steps: Provide the substrate to be etched; The substrate to be etched is subjected to alternating etching and deposition processes to form etching trenches of a predetermined depth on the substrate; wherein the deposition process includes: A precursor gas and a reactant gas are introduced into the etching chamber to deposit a protective film of a target thickness on the sidewall of the etching tank, wherein the protective film includes a metal nitride protective layer generated by the reaction of H radicals in the reactant gas with imine ligands in the precursor gas; and / or, the protective film includes a metal carbonitride protective layer generated by the reaction of H radicals in the reactant gas with amino ligands in the precursor gas. The precursor gas, the reactant gas, and the deposition byproducts are purged out.

2. The manufacturing method according to claim 1, characterized in that, The process of introducing precursor gas and reactant gas into the etching chamber includes: The reactant gas is introduced into the etching chamber through a first input gas path, and the precursor gas is introduced into the etching chamber through a second input gas path, wherein the first input gas path is independent of the second input gas path.

3. The manufacturing method according to claim 2, characterized in that, Before introducing the precursor gas and reactant gas into the etching chamber, the fabrication method further includes: The precursor gas is introduced into the buffer chamber connected to the second input gas path; and The air pressure in the buffer chamber is adjusted to be greater than or equal to twice the air pressure in the etching chamber.

4. The manufacturing method according to any one of claims 2-3, characterized in that, The step of introducing the precursor gas into the etching chamber through the second input gas path includes: The precursor gas is introduced into the etching chamber through the second input gas path, while maintaining the temperature of the precursor gas in the second input gas path within the target temperature range of 50°C-150°C.

5. The manufacturing method according to any one of claims 1-4, characterized in that, The temperature of the substrate to be etched during the etching process is -100℃ to 100℃.

6. The manufacturing method according to claim 5, characterized in that, The fabrication method further includes: increasing the temperature of the substrate to be etched after the etching process is completed.

7. The manufacturing method according to any one of claims 1-6, characterized in that, The manufacturing method further includes: After the preceding etching process is completed, the temperature of the subsequent etching process is adjusted to be lower than the temperature of the preceding etching process.

8. The manufacturing method according to any one of claims 1-7, characterized in that, The manufacturing method further includes: After completing the aforementioned deposition process, the saturated vapor pressure of the precursor gas in the subsequent deposition process is increased.

9. The manufacturing method according to any one of claims 1-8, characterized in that, The manufacturing method further includes: After the preceding deposition process is completed, the thickness of the protective film formed by the subsequent deposition process is adjusted to be less than the thickness of the protective film formed by the preceding deposition process.

10. The manufacturing method according to any one of claims 1-9, characterized in that, The protective film further includes a metal oxide protective layer, wherein the metal nitride protective layer and / or the metal carbonitride protective layer are attached to the surface of the metal oxide protective layer, and the introduction of precursor gas and reactive gas into the etching chamber includes: A precursor gas is introduced into the etching chamber so that the amino ligands in the precursor gas react with the liquid film adsorbed on the sidewall of the tank and generate the metal oxide protective layer. The precursor gas and chemically adsorbed byproducts are purged out. The reaction gas is introduced into the etching chamber so that the H radicals in the reaction gas react with the imine ligands and / or amino ligands in the precursor gas to generate the metal nitride protective layer and / or the metal carbonitride protective layer.

11. The manufacturing method according to claim 10, characterized in that, The deposition of a protective film of target thickness on the wall of the etching tank includes: The deposition process is repeated cyclically a preset number of times.

12. The manufacturing method according to any one of claims 1-9, characterized in that, The process of introducing precursor gas and reactive gas into the etching chamber to deposit a protective film of a target thickness on the wall of the etching tank includes: Precursor gas and reactant gas are simultaneously introduced into the etching chamber, and the reaction is carried out for a target time to deposit a protective film of a target thickness on the wall of the etching tank.

13. The manufacturing method according to claim 12, characterized in that, The simultaneous introduction of precursor gas and reactant gas into the etching chamber includes: Gradually increase the amount of the reactant gas introduced into the etching chamber, while gradually decreasing the amount of the precursor gas introduced into the etching chamber.

14. The manufacturing method according to any one of claims 1-9, characterized in that, The protective film further includes a metal oxide protective layer, the metal nitride protective layer and / or the metal carbonitride protective layer being attached to the surface of the metal oxide protective layer; the step of introducing precursor gas and reactive gas into the etching chamber to deposit a protective film of target thickness on the wall of the etching tank includes: A precursor gas is introduced into the etching chamber so that the amino ligands in the precursor gas react with the liquid film adsorbed on the sidewall of the tank for a first preset time, and generate the metal oxide protective layer of a first thickness. The precursor gas and chemically adsorbed byproducts are purged out. The reaction gas is introduced into the etching chamber so that the H radicals in the reaction gas react with the imine ligands and / or amino ligands in the precursor gas for a second preset time, and generate the metal nitride protective layer and / or the metal carbonitride protective layer of a second thickness, wherein the sum of the first thickness and the second thickness is equal to the target thickness.

15. The manufacturing method according to any one of claims 1-14, characterized in that, The reactant gas is C. x H y F z Gas 、 NH 3、 N2H 4、 H 2、 CH 4、 CH3I or at least one of HF.

16. An etching apparatus, characterized in that, include: Etching chamber, used to hold the substrate to be etched; A process gas supply system is used to input etching gas and reaction gas into the etching chamber; A precursor gas supply system is used to input the precursor gas into the etching chamber; An etching reaction system for etching the substrate to be etched; The control system is connected to the process gas supply system, the precursor gas supply system, and the etching reaction system. The control system is used for: The etching apparatus is controlled to perform alternating etching and deposition processes on the substrate to be etched, thereby forming an etching trench of a predetermined depth on the substrate; wherein the deposition process includes: A precursor gas and a reactant gas are introduced into the etching chamber to deposit a protective film of a target thickness on the sidewall of the etching tank. The protective film includes a metal nitride protective layer generated by the reaction of H radicals in the reactant gas with imino ligands in the precursor gas; and / or, the protective film includes a metal carbonitride protective layer generated by the reaction of H radicals in the reactant gas with amino ligands in the precursor gas. The precursor gas, the reactant gas, and the deposition byproducts are purged out.

17. The etching apparatus as claimed in claim 16, characterized in that, The process gas supply system includes a first input gas path for inputting the reaction gas into the etching chamber; the precursor gas supply system includes a second input gas path for inputting the precursor gas into the etching chamber, wherein the first input gas path is independent of the second input gas path.

18. The etching apparatus as claimed in claim 16, characterized in that, The precursor gas supply system includes a second input gas path, a precursor supply source, a buffer chamber, and a precursor control valve. The precursor supply source, the buffer chamber, and the precursor control valve are disposed on the second input gas path. The precursor supply source is connected to the control system. The control system is also used to control the precursor supply source to deliver the precursor gas to the etching chamber through the second input gas path. The buffer chamber is disposed between the precursor supply source and the precursor control valve. The precursor control valve is connected to the etching chamber. The gas pressure in the buffer chamber is greater than or equal to twice the gas pressure in the etching chamber.

19. The etching apparatus according to any one of claims 16-18, characterized in that, The etching apparatus also includes a temperature control system connected to the control system. The control system is further configured to control the temperature control system to increase the temperature of the substrate to be etched after the etching process is completed.

20. A semiconductor device, characterized in that, It includes units or modules for performing the fabrication method of the high aspect ratio etched structure as described in any one of claims 1-15.