A method and system for exposing the back side of a wafer TSV

By using a dual-threshold witness unit and partitioned liquid treatment technology, the silicon removal rate is monitored in real time, solving the problem of etching endpoint control during TSV backside exposure and achieving a more precise and uniform silicon removal effect.

CN123124691APending Publication Date: 2026-11-17SOUTHEAST UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611267133.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies make it difficult to accurately control the etching endpoint during the exposure of the back side of through silicon vias (TSVs), resulting in localized thickness unevenness, warping, and copper contamination. Furthermore, the propagation path of the etching front is affected by various factors, making it difficult to control precisely.

Method used

By employing a dual-threshold witness unit to detect the time difference of events on the conductive end face, combined with a partitioned control method for multiple liquid processing units, and through a dielectric isolation structure between the conductive detection end face and the sidewall, the silicon removal rate is monitored and adjusted in real time to achieve partitioned etching and liquid switching.

Benefits of technology

It reduces the estimation error of the pre-processing thickness map or preset etching rate, improves the accuracy and uniformity of the etching endpoint, reduces the risk of local over-etching and copper contamination, and is suitable for etching control in different crystal orientations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124691A_ABST
    Figure CN123124691A_ABST
Patent Text Reader

Abstract

This invention relates to the fields of semiconductor manufacturing and advanced packaging technology, and discloses a method and system for revealing the back side of a wafer TSV. A wafer containing TSVs, after temporary bonding and back-side thinning, is divided into multiple monitored areas. A dual-threshold witness unit, electrically isolated from the product TSV, is pre-formed within the dicing channel of each area. The witness unit has first and second conductive detection end faces with a known depth difference along the wafer thickness direction and insulated sidewalls. Multiple liquid processing heads form mutually isolated local liquid films in each area. When the silicon etching solution sequentially contacts two detection end faces, the event time is recorded, and the silicon removal rate for that area is calculated from the height difference. A controller, combining the equivalent remaining silicon removal amount from the second event to the target TSV exposure state of the product and the equivalent residual silicon removal amount during liquid switching, determines the etching stop time for each area, allowing the area that reaches the target first to switch to the cleaning solution while other areas continue etching.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method and system for exposing the back side of a wafer TSV, belonging to the field of semiconductor manufacturing and advanced packaging technology. Background Technology

[0002] Through-Silicon Vias (TSVs) backside exposure typically occurs after device face bonding. Most of the silicon is removed through mechanical thinning and chemical mechanical polishing, followed by the removal of residual silicon above the TSV ends using dry or wet etching. The thinned wafer may exhibit variations in total thickness, localized thickness inhomogeneities, and warpage. The silicon wet etching rate is also affected by crystal orientation, doping, temperature, silicon etchant concentration, dissolved silicon amount, and local flow field. If a uniform etching time is used across the entire wafer, under-etching and over-etching often occur simultaneously in the center, edges, or localized areas. Conversely, using dry etching alone can cause copper contamination of device layer 120 (see [link to documentation]). Figure 2 To mitigate the risks associated with wet etching, which requires gentle and precise control over the etching endpoint, a wet etching process is necessary.

[0003] In wet etching, the pre-processing thickness map and preset etching rate only reflect the initial state and cannot fully reflect the aging of the etching solution, temperature drift, and changes in the flow field of the etching head during wafer processing. If the signal generated by the first contact of the conductive filler TSV of the product with the silicon etching solution is used as the endpoint, it usually only reflects the first exposed position, and the product structure involved in the detection may bring corrosion, contamination, or electrical performance risks. For the back mask opening and etching from the window towards the TSV, the propagation path of the etching front is simultaneously affected by crystal orientation, window distance, window width, aperture ratio, and local flow field. Simply calculating the endpoint using a single lateral or longitudinal rate may not accurately describe the actual time it takes for the etching front to reach the back end of the TSV.

[0004] Therefore, there is a need for a partitioned control method that can obtain the actual silicon removal rate of different regions during the formal wafer processing and combine the measured rate with the product TSV target exposure state, control response delay, and liquid displacement residual etching. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a wafer TSV backside exposure method and system. The silicon removal rate of each monitored area is obtained by the time difference of corresponding events between two conductive detection terminals, thereby reducing the estimation error caused by relying solely on the pre-processing thickness map or preset etching rate.

[0006] To achieve the above objectives, the present invention is implemented using the following technical solution:

[0007] In a first aspect, the present invention provides a method for exposing the back side of a wafer TSV, comprising:

[0008] The wafer containing TSV is divided into at least two monitored regions; a dual threshold witness unit electrically isolated from TSV is formed in the dicing track corresponding to each region; the witness unit has a first conductive detection end face and a second conductive detection end face facing the back of the wafer, with a known height difference along the wafer thickness direction and sidewall insulation.

[0009] The device side of the wafer is bonded to the carrier substrate and thinned from the back side;

[0010] Multiple liquid processing units are used to form mutually isolated local liquid films in each monitored area;

[0011] For each region, when the silicon etching solution contacts the first conductive detection end face and the corresponding electrical response meets the preset event criteria, the first event is determined to be completed and the time of completion of the first event is recorded; when the silicon etching solution contacts the second conductive detection end face and the corresponding electrical response meets the same preset event criteria, the second event is determined to be completed and the time of completion of the second event is recorded, and the silicon removal rate of each region is calculated in combination with the height difference.

[0012] Obtain the equivalent remaining silicon removal amount required for each region from the time the second event determination is completed until the product TSV reaches the target back-side exposure state, and the equivalent residual silicon removal amount generated from the time the silicon etching solution is stopped to the time the cleaning solution replacement is completed;

[0013] Based on the silicon removal rate of each region, the equivalent residual silicon removal amount required for each region from the completion of the second event determination to the product TSV reaching the target back-side exposure state, and the equivalent residual silicon removal amount generated in each region from the cessation of silicon etching solution supply to the completion of cleaning solution replacement, the etching stop time for each region is determined respectively, so that the region that reaches the target first is switched to cleaning solution, and other regions continue etching until the etchant concentration in the local liquid film of each region is reduced to the preset replacement concentration threshold.

[0014] Furthermore, each of the dual threshold witness units includes a first detection conductor and a second detection conductor, the first detection conductor and the second detection conductor having a first conductive detection end face and a second conductive detection end face facing the back of the wafer, and respectively connected to the test contact terminal through independent and insulated leads;

[0015] Except for the first conductive detection end face, the second conductive detection end face, and the test contact end, the sidewalls, connecting parts, and leads of the first detection conductor and the second detection conductor are all covered by a dielectric isolation layer;

[0016] The dielectric isolation layer terminates at the periphery of the corresponding conductive detection end face without covering the conductive detection end face, so that the conductive detection end face can directly contact the processing liquid after the silicon above it is removed.

[0017] The first conductive detection end face is closer to the back side of the wafer than the second conductive detection end face, and the distance between the two along the wafer thickness direction is a known height difference ΔH.

[0018] Furthermore, the first detection conductor and the second detection conductor have the same detection end face material, area, sidewall isolation structure and corresponding mask opening, except that the depth of the detection end face along the wafer thickness direction is different.

[0019] Furthermore, both the first detection conductor and the second detection conductor include a conductive body, an adhesion / blocking layer located around the conductive body, and a sidewall dielectric isolation layer located around it.

[0020] The first conductive detection end face, the second conductive detection end face, and the test contact end are not covered by the sidewall dielectric isolation layer.

[0021] Furthermore, bonding the device side of the wafer to the carrier substrate and thinning it from the back side includes:

[0022] The device face of the wafer is instantaneously bonded to the carrier, and the wafer is thinned from the back side so that a residual silicon layer is retained above the back face of the product TSV, the first conductive detection face, and the second conductive detection face.

[0023] Furthermore, multiple liquid processing units are used to form mutually isolated local liquid films in each monitored area, including:

[0024] Multiple liquid processing units, each corresponding to a monitored area, are used to form a local liquid film that is separated from each other in each monitored area, and silicon etching solution supply, cleaning solution supply and liquid recovery are performed independently for each monitored area.

[0025] At least one of liquid recovery and gas isolation is implemented at the boundary of adjacent monitored areas, so that the concentration of etchant entering the adjacent monitored area from one monitored area is lower than the preset cross-contamination concentration threshold, thereby enabling different monitored areas to be in etching state, liquid switching state or cleaning state respectively.

[0026] The liquid processing unit includes a liquid supply and recovery processing head corresponding to the monitored area. The processing head has a liquid supply port, an annular liquid recovery port, and an annular gas isolation port located outside the recovery port, so that different areas can be in etching, switching, or cleaning states respectively.

[0027] A transition zone is provided between adjacent monitored areas; at any given time, only one of the adjacent liquid processing units is allowed to supply silicon etching solution to the transition zone, while the other liquid processing unit performs liquid recovery and / or gas isolation on one side of the transition zone.

[0028] Furthermore, the silicon etching solution is a tetramethylammonium hydroxide solution with a mass fraction of 5% to 25% or a potassium hydroxide solution with a mass fraction of 15% to 35%, and the etching temperature is 50°C to 85°C.

[0029] The cleaning solution is deionized water or an aqueous solution that has a diluting, displacement or neutralizing effect on the silicon etching solution and is compatible with the TSV material.

[0030] Furthermore, for each region, when the silicon etching solution contacts the first conductive detection end face and the corresponding electrical response meets the preset event criterion, the first event is determined to be completed and the completion time of the first event is recorded; when the silicon etching solution contacts the second conductive detection end face and the corresponding electrical response meets the same preset event criterion, the second event is determined to be completed and the completion time of the second event is recorded, and the silicon removal rate of each region is calculated in combination with the height difference, including:

[0031] By using a counter electrode immersed in a corresponding local liquid film and an AC detection source, a detection circuit is formed between the detection conductor and the counter electrode, thereby obtaining the corresponding electrical response; the electrical response includes impedance amplitude, impedance phase and / or AC current;

[0032] In the i-th monitored area, when the silicon etching solution establishes direct liquid-phase electrical contact with the first conductive detection end face, and the corresponding electrical response satisfies the preset event criterion, the completion time t of the first event determination is recorded. 1,i ;

[0033] When the silicon etching solution establishes direct liquid-phase electrical contact with the second conductive detection end face and the corresponding electrical response satisfies the same preset event criterion, the completion time t of the second event determination is recorded. 2,i ;

[0034] The silicon removal rate v of the i-th monitored region is calculated using the following formula. i :

[0035] v i =ΔH / (t) 2,i -t 1,i ).

[0036] Furthermore, the preset event criterion is:

[0037] Using the electrical response collected within a predetermined time window before the event occurs as a dynamic baseline, when the changes of at least two electrical characteristic quantities among impedance amplitude, impedance phase and alternating current relative to the dynamic baseline reach the corresponding preset change thresholds and continue for a duration not less than a preset duration threshold, it is determined to be a valid event.

[0038] Furthermore, at least two dual-threshold witness units are set up in the same monitored area, and the method further includes:

[0039] When multiple dual-threshold witness units are set up in the same monitored area, the silicon removal rate calculated by each witness unit is fused together:

[0040] After removing outliers that exceed the predetermined statistical range, the median, weighted average, or predetermined quantile is used as the silicon removal rate for that region.

[0041] Furthermore, the equivalent residual silicon removal amount required for each region from the completion of the second event determination to the product TSV reaching the target back-side exposure state, and the equivalent residual silicon removal amount generated from the cessation of silicon etching solution supply to the completion of cleaning solution replacement, including:

[0042] Under conditions of crystal orientation, doping conditions, silicon etching solution composition, temperature, liquid processing unit gap, liquid supply flow rate, recovery flow rate, local liquid film conditions, and back-side processing opening structure above the TSV and dual-threshold witness unit, which are the same as or pre-calibrated as the wafer to be processed, the preset event criteria are used to pre-establish a calibration mapping relationship between the process state corresponding to the completion time of the second event judgment and the product TSV reaching the target back-side end exposure state, so as to obtain the equivalent remaining silicon removal amount L corresponding to the regional equivalent silicon removal rate. i The exposure state of the target back end is characterized by at least one of the exposure height of the product TSV back end relative to the adjacent silicon surface and the circumferential exposure integrity.

[0043] By conducting liquid switching tests using the same liquid treatment unit gap, temperature, supply flow rate, recovery flow rate, cleaning fluid flow rate, and valve sequence, the equivalent response and the amount of silicon removed by displacement ΔS were determined from the time the silicon etching solution supply stopped until the etchant concentration in the corresponding local liquid film decreased to a preset displacement concentration threshold. i The equivalent response and the amount of silicon removed by substitution ΔS i This includes the amount of silicon removed during command output, valve response, liquid transport, and cleaning fluid replacement.

[0044] Furthermore, the position of the conductive detection end face of the second detection conductor is set such that when the second event occurs, the equivalent remaining silicon removal amount L i It is greater than the sum of the maximum equivalent residual silicon removal amount, the silicon removal amount during the detection confirmation time, the silicon removal amount during the controller operation and valve response time, the silicon removal amount during the liquid transport delay, and the preset safety margin.

[0045] Furthermore, based on the silicon removal rate of each region, the equivalent residual silicon removal amount required for each region from the completion of the second event determination to the product TSV reaching the target backside exposure state, and the equivalent residual silicon removal amount generated in each region from the cessation of silicon etching solution supply to the completion of cleaning solution replacement, the etching stop time for each region is determined respectively, so that the region that reaches the target first switches to cleaning solution, while other regions continue etching, until the etchant concentration in the local liquid film of each region is reduced to the preset replacement concentration threshold, including:

[0046] From the time t when the second event is determined to be completed 2,i Timing begins, and the switching waiting time T for each monitored area is calculated using the following formula. i :

[0047] T i =max{0, (L i -ΔS i ) / v i};

[0048] Among them, T i Let i be the switching waiting time for the i-th monitored area;

[0049] After the switching waiting time T i At the same time, a command to stop the supply of silicon etching solution is output to the corresponding liquid processing unit and cleaning solution is supplied. Meanwhile, the supply of silicon etching solution continues to other monitored areas that have not yet reached their respective switching waiting time, until the etchant concentration in the local liquid film of each monitored area is reduced to the preset replacement concentration threshold.

[0050] If the calculated T i If the value is zero, it is immediately determined that the area needs to enter the erosion stop and switchover process.

[0051] In a second aspect, the present invention provides a wafer TSV backside exposure system, comprising:

[0052] A processing station is used to hold a TSV-containing wafer; the wafer is pre-divided into at least two monitored areas, and a dual threshold witness unit is provided in the dicing track of each monitored area. The witness unit has a first conductive detection end face and a second conductive detection end face facing the back of the wafer, with a known height difference along the wafer thickness direction and sidewall insulation.

[0053] Multiple liquid processing units, each corresponding to a monitored area, are configured to form a local liquid film isolated from other areas in the corresponding monitored area and to independently supply silicon etching solution or cleaning solution.

[0054] The detection circuit is electrically connected to each of the dual threshold witness units and is used to collect the electrical response signal when the silicon etching solution contacts each conductive detection end face;

[0055] The controller, which is communicatively connected to each of the liquid processing units and the detection circuit, is configured to determine the completion time of the first event and the second event based on the electrical response signal, calculate the silicon removal rate of each region, and determine the etching stop time of each region based on the silicon removal rate, the pre-calibrated equivalent remaining silicon removal amount, and the equivalent residual silicon removal amount. When the corresponding region reaches the etching stop time, the controller controls the liquid processing unit of that region to stop supplying silicon etching solution and switch to cleaning solution, while maintaining the etching of other regions.

[0056] Furthermore, a transition zone is provided between adjacent monitored areas; for two adjacent liquid processing units, at any given time, the controller only allows one of them to supply silicon etching solution to the transition zone, and controls the other to maintain liquid recovery and / or gas isolation on the side near the transition zone.

[0057] Furthermore, the controller includes:

[0058] The parameter storage module is configured to store configuration parameters and calibration data for each monitored area. The configuration parameters include the known height difference ΔH between the first and second conductive detection end faces in the dual-threshold witness unit corresponding to each area. The calibration data includes the equivalent residual silicon removal amount L required for each area from the completion time of the second event determination until the product TSV reaches the target back-side exposure state. i And the equivalent residual silicon removal amount ΔS generated in each region from the cessation of silicon etching solution supply to the completion of cleaning solution replacement. i ;

[0059] The event determination and rate calculation module is configured to record the first event time t when the silicon etching solution in the i-th monitored area establishes direct liquid phase electrical contact with the first conductive detection end face and the second conductive detection end face, respectively, and the electrical response of the corresponding detection end face meets the preset event criteria. 1,i Second event time t 2,i And according to v i =ΔH / (t) 2,i -t 1,i Calculate the equivalent silicon removal rate v of the i-th monitored region. i ;

[0060] The residual and excess amount compensation module is configured to compensate for the excess amount of silicon removed based on a pre-calibrated equivalent excess silicon removal amount L. i and equivalent residual silicon removal amount ΔS i According to T i =max{0, (L i -ΔS i ) / v iThe i-th monitored area is determined from the second event time t. 2,i Switching wait time T i ;

[0061] The zone valve control module is configured to, after the switching waiting time T, i At that time, the corresponding liquid processing unit stops supplying silicon etching solution and supplies cleaning solution, while other monitored areas that have not yet reached their respective switching waiting time continue to be etched, so that different monitored areas are in etching state, liquid switching state or cleaning state respectively at the same time.

[0062] Furthermore, the controller is used to perform the following steps:

[0063] Step S1: Obtain the configuration parameters and calibration data for each monitored area. The configuration parameters include the known height difference ΔH between the first conductive detection end face and the second conductive detection end face in the dual threshold witness unit corresponding to each area. The calibration data includes the equivalent remaining silicon removal amount L required for each area from the time of completion of the second event determination until the product TSV reaches the target backside exposure state. i And the equivalent residual silicon removal amount ΔS generated in each region from the cessation of silicon etching solution supply to the completion of cleaning solution replacement. i ;

[0064] Step S2: Real-time acquisition of electrical response signals from the detection end face of each monitored area. When silicon etching solution is detected to be in contact with the first conductive detection end face and the corresponding electrical response meets the preset event criteria, the first event is determined to be completed and the time t of the first event completion is recorded. 1,i When silicon etching solution is detected to contact the second conductive detection end face and the corresponding electrical response satisfies the same preset event criterion, the second event is determined to be completed and the completion time t of the second event is recorded. 2,i ;

[0065] Step S3: Based on the known height difference ΔH and the completion time t of the first event determination 1,i and the completion time t of the second event determination 2,i The silicon removal rate v of each monitored region is calculated using the following formula. i :

[0066] v i =ΔH / (t 2,i -t 1,i );

[0067] Step S4: From the time t when the second event is determined to be complete 2,i Starting from this point, the handover waiting time T for each monitored area is calculated using the following formula. i :

[0068] T i =max{0,(L i -ΔS i ) / v i};

[0069] Among them, L i ΔS represents the equivalent residual silicon removal amount in the i-th monitored region. i The equivalent residual silicon removal amount for the i-th monitored area;

[0070] Step S5: Determine the completion time t based on the second event. 2,i Timing begins from the starting point of the timeout. When the cumulative time of the i-th monitored area reaches the switching waiting time T... i When the time comes, a command to stop supplying silicon etching solution is sent to the liquid processing unit corresponding to the area, and a command to supply cleaning solution is sent. At the same time, the supply of silicon etching solution continues to other monitored areas that have not yet reached their respective switching waiting time.

[0071] Step S6: After all monitored areas have completed switching and output a command to stop supplying silicon etching solution, output a processing end signal.

[0072] Compared with the prior art, the beneficial effects achieved by the present invention are as follows:

[0073] In the same wafer and the same wet processing process, this invention obtains the silicon removal rate of each monitored area by the time difference of corresponding events between two conductive detection terminals, thereby reducing the estimation error caused by relying solely on the pre-processing thickness map or preset etching rate.

[0074] This invention employs multiple supply / recovery heads corresponding to different regions, allowing different regions to be in etching, switching, or cleaning states respectively. Regions that reach the target exposure state first can be switched to cleaning solution in a timely manner, while other regions continue etching, reducing localized over-etching caused by using the slowest region as the uniform endpoint for the entire sheet.

[0075] This invention clearly distinguishes the conductive detection end face from the sidewall dielectric isolation structure. A velocity measurement event is only formed when the silicon etching solution comes into direct contact with the exposed conductive detection end face and meets the event criteria. This can reduce misjudgments caused by sidewall wetting, changes in liquid film thickness, and temperature changes.

[0076] This invention uses the equivalent amount of remaining silicon removed to represent the complex etching path between the second event and the target exposure state of the product TSV, and is compatible with processes that are mainly vertically removed and processes that use segmented annular windows to generate lateral under-etching.

[0077] In the implementation using a monitoring chip to optimize the segmented annular window, the arrival time difference of the etching front at different crystal orientations of the same TSV can be reduced. Dual-threshold velocimetry and zoned liquid switching are used to reduce the endpoint differences between different monitored areas, thereby forming a two-level control of intra-regional homogenization and inter-regional homogenization. Attached Figure Description

[0078] Figure 1 This is a flowchart of the wafer TSV backside exposure method of the present invention;

[0079] Figure 2 This is a schematic diagram of a cross-section of a wafer after temporary bonding and back-side thinning.

[0080] Figure 3 A top-view diagram showing the segmented annular window surrounding a single TSV;

[0081] Figure 4 A schematic diagram showing the compensation relationship between window distance and window width under different crystal orientations (𝜽) f For rapid etching angle; 𝜽 s (For slow etching angle)

[0082] Figure 5 A schematic cross-sectional view of a dual-threshold witness unit with an exposed conductive detection end face and a sidewall dielectric isolation structure;

[0083] Figure 6 A schematic diagram showing the distribution of multiple monitored areas and dual-threshold witness units;

[0084] Figure 7 A schematic diagram illustrating the process of the etching front merging towards the back end of the TSV through a segmented annular window;

[0085] Figure 8 This is a timeline diagram of the first and second events;

[0086] Figure 9 A schematic diagram of the liquid treatment unit structure in an adjacent monitored area;

[0087] Figure 10 This diagram illustrates the dual-threshold velocity measurement, equivalent residual quantity compensation, and zoned liquid switching closed-loop control for multiple monitored areas.

[0088] The reference numerals in the figure represent the following: 100, wafer; 110, TSV; 111, TSV conductive filler; 112, adhesive / barrier layer; 113, sidewall insulating layer; 120, device layer; 130, temporary bonding adhesive; 140, carrier; 150, residual silicon layer; 160, hard mask layer; 161, segmented annular window; 162, hard mask bridge; 170, dual threshold witness cell; 171, first detection conductor; 171a, first conductive detection end face; 172, second detection conductor; 172a, second conductive detection end face. ; 173. Detect conductor adhesion / barrier layer; 174. Detect conductor sidewall dielectric isolation layer; 175. Test pad / carrier test port; 180. Liquid supply / recovery head; 181. Liquid supply port; 182. Annular liquid recovery port; 183. Annular gas isolation port; 184. Counter electrode; 190. Controller; 191. Event determination and rate calculation module; 192. Equivalent residual quantity and equivalent remaining quantity compensation module; 193. Regional valve control; Z1. Wafer center region; Z2. Wafer middle region; Z3. Wafer edge region. Detailed Implementation

[0089] The present invention will be further described below with reference to the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and should not be used to limit the scope of protection of the present invention.

[0090] Example 1:

[0091] This embodiment provides a method for exposing the back side of a wafer TSV, wherein the TSV includes a conductive filler, an adhesion layer and / or a barrier layer disposed around the conductive filler, and a sidewall insulating layer 113 located between the TSV and a silicon substrate, comprising:

[0092] (1) A wafer 100 pre-formed with the TSV110 and the dual threshold witness unit 170 is provided. The wafer 100 is pre-divided into at least two monitored areas. At least one dual threshold witness unit 170 electrically isolated from the product TSV110 is provided in the dicing track corresponding to each monitored area. Each dual threshold witness unit 170 includes a first detection conductor 171 and a second detection conductor 172. The first detection conductor 171 and the second detection conductor 172 have a first conductive detection end face 171a and a second conductive detection end face 172a facing the back side of the wafer 100, and are respectively connected by independent and insulated leads. The wire is connected to the test contact terminal; except for the first conductive detection end face 171a, the second conductive detection end face 172a and the test contact terminal, the sidewalls, connecting portions and leads of the first detection conductor 171 and the second detection conductor 172 are all covered by a dielectric isolation layer. The dielectric isolation layer terminates at the periphery of the corresponding conductive detection end face without covering the conductive detection end face, so that the conductive detection end face can directly contact the processing liquid after the silicon above it is removed; the first conductive detection end face 171a is closer to the back side of the wafer 100 than the second conductive detection end face 172a, and the distance between the two along the thickness direction of the wafer 100 is a known height difference ΔH.

[0093] The first detection conductor 171 and the second detection conductor 172 have the same detection end face material, area, sidewall isolation structure and corresponding mask opening, except that the depth of the detection end face along the thickness direction of the wafer 100 is different.

[0094] The detection conductor includes a conductive body (at least one of copper, copper alloy, tungsten, doped polycrystalline silicon, TiN, Pt, Au, or Ru), an adhesion / barrier layer 112 (Ti, TiN, Ta, TaN, or a combination thereof) located around the conductive body, and a sidewall dielectric isolation layer (silicon oxide, silicon nitride, silicon carbide, polymer, or a composite dielectric layer thereof) located around it; the conductive detection end face is not covered by the sidewall dielectric isolation layer.

[0095] (2) The device side of the wafer 100 is bonded to the carrier 140 with temporary bonding adhesive 130, and thinned from the back side of the wafer 100 so that a residual silicon layer 150 is retained above the back side of the product TSV110, the first conductive detection end face 171a and the second conductive detection end face 172a.

[0096] (3) Using multiple liquid processing units corresponding to each monitored area, a local liquid film is formed in each monitored area, and silicon etching solution supply, cleaning solution supply and liquid recovery are implemented independently for each monitored area; at least one of liquid recovery and gas isolation is implemented at the boundary of adjacent monitored areas, so that the concentration of etchant entering the adjacent monitored area from one monitored area is lower than the preset cross-contamination concentration threshold, so that different monitored areas can be in etching state, liquid switching state or cleaning state respectively;

[0097] Each liquid processing unit includes a liquid supply / recovery processing head 180 corresponding to the corresponding monitored area. The processing head has a liquid supply port, an annular liquid recovery port 182, and an annular gas isolation port 183 located outside the recovery port, so that different areas can be in etching, switching, or cleaning states respectively. A region transition zone is provided between adjacent monitored areas. At any given time, only one of the adjacent liquid processing units is allowed to supply silicon etching solution to the region transition zone, and the other liquid processing unit performs liquid recovery and / or gas isolation on one side of the region transition zone.

[0098] The silicon etching solution is a tetramethylammonium hydroxide solution with a mass fraction of 5% to 25% or a potassium hydroxide solution with a mass fraction of 15% to 35%, and the etching temperature is 50°C to 85°C; the cleaning solution is deionized water or an aqueous solution that has a dilution, displacement or neutralization effect on the silicon etching solution and is compatible with TSV materials.

[0099] (4) In the i-th monitored area, when the silicon etching solution establishes direct liquid phase electrical contact with the first conductive detection end face and the electrical response of the corresponding detection end face meets the preset event criteria including the response threshold and the duration threshold, the first event determination completion time t is recorded. 1,i When the silicon etching solution establishes direct liquid-phase electrical contact with the second conductive detection end face and meets the same preset event criteria, the completion time t of the second event determination is recorded. 2,i According to v i =ΔH / (t) 2,i -t 1,i Calculate the silicon removal rate v of the i-th monitored region. i Among them, the interface capacitance change, parasitic impedance change or detection baseline drift caused solely by the silicon etching solution wetting the dielectric isolation layer are not determined as the first event or the second event.

[0100] A detection circuit is formed between the detection conductor and the counter electrode by using a counter electrode immersed in a corresponding local liquid film and an AC detection source; the detection circuit collects the impedance amplitude, impedance phase and / or AC current, and determines the first event and the second event based on the detection electrical response.

[0101] At least two dual-threshold witness units are set up in the same monitored area, and the control rate of the area is determined based on the median, weighted average, predetermined quantile, or statistical value after outlier removal obtained from multiple witness units.

[0102] (5) Under the same or pre-calibrated crystal orientation, doping conditions, silicon etching solution composition, temperature, liquid processing unit gap, liquid supply flow rate, recovery flow rate, local liquid film conditions, and back-side processing opening structure above the product TSV and dual threshold witness unit as the wafer to be processed, the same event determination method as in step (4) is used to pre-establish the calibration mapping relationship between the process state corresponding to the completion time of the second event determination and the product TSV reaching the target back-side end exposure state, and obtain the equivalent remaining silicon removal amount L corresponding to the equivalent silicon removal rate of the region. i The exposure state of the target back end is characterized by at least one of the exposure height of the product TSV back end relative to the adjacent silicon surface and the circumferential exposure integrity.

[0103] By conducting liquid switching experiments using the same liquid treatment unit gap, temperature, supply flow rate, recovery flow rate, cleaning fluid flow rate, and valve sequence as in actual processing, the equivalent response and silicon removal amount ΔS during the period from the output of the command to stop silicon etchant supply until the etchant concentration in the corresponding local liquid film decreases to a preset replacement concentration threshold were determined. i The equivalent response and the amount of silicon removed by substitution ΔS i This includes command output, valve response, liquid transport, and the amount of silicon removed during cleaning fluid replacement;

[0104] The position of the conductive detection end face of the second detection conductor is set such that when the second event occurs, the equivalent residual silicon removal amount L i The silicon removal amount is greater than the sum of the maximum equivalent residual silicon removal amount, the silicon removal amount during the detection and confirmation time, the silicon removal amount during the controller operation and valve response time, the silicon removal amount during the liquid transport delay, and the preset safety margin, satisfying the following:

[0105] L i >ΔS maxi +v maxi ·Δt+M i ,

[0106] Where, ΔS maxi For the maximum residual removal amount, v maxi The maximum silicon removal rate is measured using a monitoring chip; Δt is the sum of event confirmation, control calculation, valve response, and liquid transport time; M i This provides a safety margin so that the second event occurs before the product TSV reaches the target state.

[0107] (6) From the time t when the second event is determined to be completed 2,i Start timing from T i =max{0, (L i -ΔS i ) / v i Determine the handover waiting time T for the i-th monitored area. i After the switching waiting time T i At that time, a command to stop the supply of silicon etching solution is output to the corresponding liquid processing unit and cleaning solution is supplied. At the same time, the supply of silicon etching solution continues to other monitored areas that have not yet reached their respective switching waiting time, until the etchant concentration in the local liquid film of each monitored area is reduced to the preset replacement concentration threshold.

[0108] Specifically, such as Figure 1 As shown, a method for exposing the back side of a wafer TSV is provided, which mainly includes the following steps.

[0109] S101: The device face of the wafer is instant-bonded to the carrier substrate, and thinned from the back side of the wafer, leaving a residual silicon layer between the back face of the TSV and the back side of the wafer. The thickness of the residual silicon layer can vary at different locations on the wafer surface.

[0110] S102: Divide the back side of the wafer into at least two monitored regions, and form at least one dual-threshold witness cell within the scribe line corresponding to each monitored region. The dual-threshold witness cell is electrically isolated from the product TSV and includes a first detection conductor and a second detection conductor. Each detection conductor has a conductive detection end face facing the back side of the wafer, and its sidewalls, connections, and individual leads, except for the conductive detection end face, are covered by a dielectric isolation layer. The conductive detection end face of the first detection conductor is closer to the back side of the wafer than the conductive detection end face of the second detection conductor, and the two conductive detection end faces are spaced apart along the wafer thickness direction by a known height difference ΔH, and both are covered by a residual silicon layer before etching.

[0111] S103: Utilizing multiple liquid processing units corresponding to each monitored area, local liquid films are formed in each area to isolate them from each other, and etching solution supply, liquid recovery, and cleaning solution supply are implemented independently. Multiple liquid processing units can operate simultaneously, so that the area that reaches the target state first is in the liquid switching or cleaning state, while other areas continue to be etched.

[0112] S104: When the etching solution establishes direct liquid phase electrical contact with the conductive detection end face of the first detection conductor, and the electrical response of the corresponding detection channel satisfies the preset event criterion, the first event time t is determined. 1,i When the etching solution establishes direct liquid-phase electrical contact with the conductive detection end face of the second detection conductor and satisfies the aforementioned criterion, the second event time t is determined. 2,iCalculate the silicon removal rate v of the i-th monitored region based on the known height difference ΔH and the two event times. i .

[0113] v i =ΔH / (t) 2,i -t 1,i )

[0114] The sidewalls, connections, and leads of the detection conductor are covered by a dielectric layer, while the detection end face remains electrically exposed. When the etching solution comes into contact with the dielectric layer on the sidewalls, a slow parasitic response may occur, but direct conductive contact cannot be formed. An event is only determined when the end face makes direct contact and the preset amplitude, phase, current, and duration criteria are met.

[0115] S105: Equivalent residual silicon removal amount L required from the state corresponding to the second event, measured in advance via a monitoring wafer or process verification wafer, until the product TSV reaches the target back end exposure state. i And the equivalent residual silicon removal amount ΔS generated during the period from the cessation of etching solution supply to the completion of cleaning solution replacement. i L i It is not necessarily equivalent to the simple physical straight-line distance from the second detection surface to the target surface, but rather an equivalent thickness parameter used to characterize the processing time required for complex longitudinal, lateral, or oblique etching paths of the product's TSV.

[0116] S106: Determine the switching waiting time T for the i-th monitored area according to the following formula. i :

[0117] T i =max{0, (L i -ΔS i ) / v i}

[0118] At the second event time t 2,i After T i When the switching time is reached, the supply of etching solution to the i-th monitored area is stopped, and cleaning solution and recovery liquid are supplied to that area; the other monitored areas that have not yet reached their respective switching times continue to receive etching solution. The second detection end face should be located before the target endpoint, and allowances should be made for event confirmation, control calculation, valve response, liquid transport, residual etching, and safety margin.

[0119] S107: After the cleaning solution has been replaced in each monitored area, stop the wet process, rinse with deionized water and dry the wafer, and then perform hard mask removal, back passivation layer formation, redistribution, bonding pad formation or other back interconnect structure formation.

[0120] Example 2:

[0121] This embodiment provides a method for exposing the back side of a wafer TSV, which differs from Embodiment 1 in the structure and fabrication of the dual threshold witness unit:

[0122] like Figure 2 As shown, wafer 100 includes a plurality of TSVs 110. Each TSV 110 includes a conductive filler 111, an adhesion / barrier layer 112 disposed therearound it, and a sidewall insulating layer 113 located between the TSV sidewall and the silicon substrate. The conductive filler 111 may be copper, copper alloy, tungsten, or other conductive materials suitable for TSV interconnection; the adhesion / barrier layer 112 may include Ti, TiN, Ta, TaN, or combinations thereof; the sidewall insulating layer 113 may include silicon oxide, silicon nitride, silicon carbide, polymer, or a composite dielectric layer thereof.

[0123] In one fabrication method, first and second witness blind vias of different depths are formed within the scribe line using a step-by-step etching method. The depth difference corresponds to the height difference ΔH between the two conductive detection end faces. Subsequently, a dielectric isolation layer 174 and an optional adhesion / barrier layer 173 are formed within the witness blind vias. The bottom adhesion / barrier layer 173 and dielectric isolation layer 174 are then directionally removed using plasma etching technology, followed by filling and planarization of the conductive substrate. The first detection conductor 171 and the second detection conductor 172 are respectively connected to the device surface test pad or the carrier board test port 175 via independent leads.

[0124] like Figure 5 As shown, the first detection conductor 171 and the second detection conductor 172 preferably have a hierarchical structure similar to that of TSV, including a conductive body, an optional adhesion / blocking layer 173, and a sidewall dielectric isolation layer 174. For a copper or copper alloy conductive body, a Ta, TaN, Ti, or TiN blocking layer can be provided; for Pt, Au, TiN, Ru, or doped polycrystalline silicon, whether or not a blocking layer is provided can be selected according to material compatibility. The conductive detection end face can be formed by the conductive body, so that when the etching solution contacts the sidewall, it cannot directly conduct with the conductive body, but a significant electrical response is generated after the silicon etching front reaches the conductive detection end face.

[0125] Except for the difference in depth, the first detection conductor 171 and the second detection conductor 172 preferably have the same end face material, area, surface treatment, sidewall isolation structure, lead structure, and mask opening, so that the time difference t 2,i -t 1,i It primarily reflects the silicon removal time corresponding to the height difference ΔH, reducing judgment bias caused by differences in material, area, and parasitic impedance. ΔH can range from 0.1 μm to 1 μm; too small a ΔH is detrimental to event resolution, while too large a ΔH reduces the timeliness of response to changes in local etching rates.

[0126] Example 3:

[0127] This embodiment provides a method for exposing the back side of a wafer TSV, which differs from Embodiment 1 in the determination of electrical events and the suppression of sidewall wetting:

[0128] During wet etching, an AC detection voltage is applied between each detection conductor and the counter electrode 184, and impedance amplitude, impedance phase, AC current, and / or equivalent charge transfer resistance are acquired. When the etching solution only wets the dielectric isolation layer 174, although it may cause interface capacitance, parasitic capacitance, or baseline drift, the response is usually smaller than the abrupt change when the conductive substrate is exposed because the conductive substrate is still isolated by the dielectric layer.

[0129] like Figure 8 As shown, the impedance characteristics within a predetermined time window before the etching reaches the first detection conductor are used as the baseline. When at least two characteristics reach their respective thresholds and remain so for a predetermined time, the controller determines that a detection event has occurred, thereby reducing false detections caused by bubbles, flow fluctuations, and electrical noise.

[0130] Example 4:

[0131] This embodiment provides a method for exposing the back side of a wafer TSV, which differs from Embodiment 1 in that it uses multiple liquid treatment heads and partitioned etch stop:

[0132] like Figure 6 As shown, the back side of the wafer is divided into at least two monitored regions, such as the wafer center region Z1, the wafer middle region Z2, and the wafer edge region Z3. The regions can be concentric ring regions, sectors, grid regions, or other regions determined according to the residual thickness map, and each region is equipped with one or more dual-threshold witness units 170.

[0133] like Figure 9 and Figure 10 As shown, each region is equipped with an independently operating liquid supply / recovery processing head 180. The processing head 180 includes a liquid supply port 181, an annular liquid recovery port 182, and an optional annular inert gas isolation port 183 to form a confined local liquid film on the back side of the wafer and reduce inter-region liquid cross-contamination. A region transition zone of predetermined width is provided between adjacent monitored regions. The effective processing range of the local liquid film formed by each processing head extends to the corresponding region boundary, but at any given time, only one of the two adjacent processing heads is allowed to supply silicon etchant to the region transition zone. The other processing head maintains liquid recovery and / or gas isolation on the side near the region transition zone to prevent the etchant and cleaning fluid from mixing at the region boundary.

[0134] Unlike a single movable processing head that processes multiple regions sequentially, the multiple processing heads in this embodiment can work in parallel over time and control the etching solution, cleaning solution, and liquid recovery separately through independent valve groups, so that different regions are in etching, switching, or cleaning states respectively, thereby reducing the over-etching differences between regions.

[0135] For the i-th region, controller 190 determines the time of the first event t. 1,i Second event time t 2,i And ΔH is calculated when the silicon removal rate v is... i When there are multiple witness units in the same area, the control rate can be determined by the mean, median, weighted value, quantile value, or statistical value after removing outliers.

[0136] Example 5:

[0137] This embodiment provides a method for exposing the back side of a wafer TSV, which differs from Embodiment 1 in the equivalent amount of residual silicon removed and the residual etching compensation:

[0138] When the exposure path of the product TSV adopts a segmented annular window, the etching front can propagate longitudinally, laterally, and obliquely. Therefore, with the equivalent remaining silicon removal amount L i This indicates the remaining processing capacity required for the product TSV to reach the target exposure state from the second event.

[0139] In one calibration method, a simulated TSV, a dual-threshold witness unit, and a mask window, identical or equivalent to those on the actual wafer, are formed on the monitoring chip. The time difference Δt between the second event and the simulated TSV reaching the target exposure state is recorded. refi and reference rate v refi And determine L according to the following formula: i =v refi ×Δt refi .

[0140] Even after the etching solution supply is stopped, residual etching solution in the local liquid film and pipelines may still continue to remove silicon. Equivalent residual silicon removal amount ΔS i The test calibration can be switched, using the same head gap, flow rate, temperature, and valve timing as the actual process, and measuring the silicon removal thickness from the time the stop command is issued until the etchant concentration falls below the threshold. ΔS i It can establish parameter tables corresponding to temperature, flow rate, gap, and pipeline status, and can also correct online based on the conductivity, pH, or etchant concentration of the recovered liquid.

[0141] The preferred position of the second detection end face 172a satisfies: L i >ΔS maxi +v maxi ·Δt+M i , where ΔS maxi For the maximum residual removal amount, v maxi M represents the maximum silicon removal rate, Δt is the sum of event confirmation, control calculation, valve response, and liquid transport time, and M is the maximum silicon removal rate. i This provides a safety margin so that the second event occurs before the product TSV reaches the target state.

[0142] Example 6:

[0143] This embodiment provides a method for exposing the back side of a wafer TSV, which differs from Embodiment 1 in that it uses an optimized segmented annular window for monitoring the wafer:

[0144] This implementation is an optional optimization for TSV circumferential etching consistency and is not a necessary technical condition for implementing dual-threshold on-chip speed measurement, equivalent remaining quantity and equivalent residual quantity compensation, and multi-processor head partition switching. Without setting a segmented ring window, the aforementioned dual-threshold speed measurement and partition switching can still be implemented independently.

[0145] like Figure 3 As shown, a hard mask 160 resistant to alkaline etching solution is formed on the back side of the wafer, and segmented annular windows 161 surrounding the TSV 110 are formed within it. The windows avoid the orthogonal projection area of ​​the conductive filler, and hard mask bridges 162 are retained between adjacent window segments to reduce the risk of the etching solution directly contacting the conductive filler and to maintain mask continuity. Witness openings corresponding to the first and second detection conductors are also formed in the hard mask. The two witness openings have the same shape and size, and the witness openings have a pre-calibrated equivalent etching time correspondence with the segmented annular windows around the product TSV.

[0146] To reduce the arrival time difference of the etching front at different crystal orientations along the circumference of a single TSV within the same monitored area, a parameter matrix containing multiple candidate window cells is formed on a monitoring wafer with the same crystal orientation, doping type, and doping concentration range as the wafer to be processed. This matrix includes window distance d(θ), window width w(θ), angular duty cycle η(θ), and the number of window segments. Figure 4 As shown, mask windows of different widths and distances can be optimally designed based on different etching rates. Etching is performed using the same etching solution composition, temperature, head gap, supply flow rate, recovery flow rate, and local liquid film conditions as the actual wafer. The arrival time t of the etching front at each direction to the simulated TSV target exposure interface is measured. arr Select a time range such that the difference between the maximum and minimum arrival times at different azimuths does not exceed a preset tolerance ε. t Window parameter: maxθ[t arr (θ)]-minθ[t arr (θ)]≤ε t The window parameters include at least two of the following: distance from the window to the TSV, window width, angular duty cycle, and number of window segments.

[0147] like Figure 7 As shown, at the initial time t0, the etching solution enters the residual silicon layer 150 through the segmented annular window 161. cThe etching fronts converge at the TSV end from multiple directions at all times. The monitoring chip can evaluate the first exposure time, the time to full exposure, the central residual silicon, the circumferential exposure height difference, and damage to the TSV end face and insulation layer.

[0148] Example 7:

[0149] This embodiment provides a method for exposing the back side of a wafer TSV, which differs from Embodiment 1 in the system and control process:

[0150] The system for implementing the above method includes a wafer processing stage, multiple liquid processing units, a detection circuit, and a controller 190. Each liquid processing unit corresponds to at least one monitored area and includes an etching solution supply branch, a cleaning solution supply branch, a recovery branch, and an optional gas isolation branch. The detection circuit includes an AC detection source, an impedance and / or current acquisition unit, and a counter electrode 184.

[0151] like Figure 10 As shown, the controller 190 includes an event determination and rate calculation module 191, an equivalent residual quantity and equivalent residual quantity compensation module 192, and a zone valve control module 193. The event determination and rate calculation module 191 calculates based on ΔH, t... 1,i and t 2,i Calculate v i The equivalent residual quantity and equivalent residual quantity compensation module 192 are based on v i L i and ΔS i Determine the handover wait time T i The regional valve control module 193 controls the etching solution, cleaning solution, recovery and gas isolation branches of each region respectively.

[0152] In one example, the silicon removal rate in the wafer center region Z1 is higher than that in the wafer edge region Z3. After reaching its switching moment, the wafer center region Z1 stops etchant supply and immediately undergoes cleaning fluid replacement, while the wafer center region Z2 and wafer edge region Z3 continue etching. Subsequently, the wafer center region Z2 and wafer edge region Z3 enter the cleaning state at their respective switching moments. Only after all regions have completed cleaning fluid replacement does the system perform a unified rinsing and drying of the entire wafer. This forms a closed-loop control relationship of "direct contact event—regional wafer rate—equivalent remaining amount / residual amount compensation—multi-processor head zone switching".

[0153] Example 8:

[0154] This embodiment provides a wafer TSV backside exposure system for processing wafers containing TSVs whose backside is divided into at least two monitoring areas. Each monitoring area has a scribe line containing a dual-threshold witness unit electrically isolated from the product TSV. The dual-threshold witness unit includes a first conductive detection end face and a second conductive detection end face facing the backside of the wafer. The first conductive detection end face is located on the back side of the second conductive detection end face, and the two are spaced apart along the wafer thickness direction by a known height difference ΔH. The conductive detection end face is exposed, and the sidewalls of the corresponding detection conductors are covered by a dielectric isolation layer. The system includes:

[0155] (a) A processing stage for holding the wafer that has undergone temporary bonding and back-side thinning;

[0156] (b) Multiple liquid processing units corresponding to each monitored area, each liquid processing unit including a silicon etching solution supply branch, a cleaning solution supply branch and a liquid recovery branch, and configured to form a local liquid film in the corresponding monitored area that is separated from other monitored areas, so as to independently implement silicon etching solution supply, cleaning solution supply and liquid recovery for each monitored area.

[0157] (c) A detection circuit connected to each dual-threshold witness unit, the detection circuit including an AC detection source and a counter electrode immersed in the corresponding local liquid film, and used to acquire at least one of impedance amplitude, impedance phase and AC current;

[0158] (d) A controller, comprising an event determination and rate calculation module, a residual quantity and residual quantity compensation module, and a region valve control module; the event determination and rate calculation module is configured to record the first event time t when the silicon etching solution in the i-th monitored region establishes direct liquid phase electrical contact with the first conductive detection end face and the second conductive detection end face respectively, and the electrical response of the corresponding detection end face satisfies the preset event criterion. 1,i Second event time t 2,i And according to v i =ΔH / (t) 2,i -t 1,i Calculate the equivalent silicon removal rate v of the i-th monitored region. i The remaining amount and residual amount compensation module is configured to compensate for the amount of equivalent residual silicon removed in advance based on a pre-calibrated amount L. i and equivalent residual silicon removal amount ΔS i According to T i =max{0, (L i -ΔS i ) / v i The i-th monitored area is determined from the second event time t. 2,i Switching wait time T iThe area valve control module is configured to, after the switching waiting time T, i At that time, the corresponding liquid processing unit stops supplying silicon etching solution and supplies cleaning solution, while other monitored areas that have not yet reached their respective switching waiting time continue to be etched, so that different monitored areas are in etching state, liquid switching state or cleaning state respectively at the same time.

[0159] The preset event criteria include an electrical response change threshold and a duration threshold. The event determination and rate calculation module is configured to use the electrical response collected within a predetermined time window before the detection event occurs as a baseline. When the changes of at least two electrical characteristic quantities among impedance amplitude, impedance phase, and alternating current relative to the baseline reach the corresponding preset change thresholds and remain at least as long as the duration threshold, it is determined that the silicon etching solution establishes direct liquid phase electrical contact with the corresponding conductive detection end face.

[0160] A transition zone is provided between adjacent monitored areas; for two adjacent liquid processing units, at any given time, the controller only allows one of them to supply silicon etching solution to the transition zone, and controls the other to maintain liquid recovery and / or gas isolation on the side near the transition zone.

[0161] Specifically, the controller includes:

[0162] The parameter storage module is configured to store configuration parameters and calibration data for each monitored area. The configuration parameters include the known height difference ΔH between the first and second conductive detection end faces in the dual-threshold witness unit corresponding to each area. The calibration data includes the equivalent residual silicon removal amount L required for each area from the completion time of the second event determination until the product TSV reaches the target back-side exposure state. i And the equivalent residual silicon removal amount ΔS generated in each region from the cessation of silicon etching solution supply to the completion of cleaning solution replacement. i ;

[0163] The event determination and rate calculation module 191 is configured to record the first event time t when the silicon etching solution in the i-th monitored area establishes direct liquid phase electrical contact with the first conductive detection end face and the second conductive detection end face respectively, and the electrical response of the corresponding detection end face meets the preset event criteria. 1,i Second event time t 2,i And according to v i =ΔH / (t) 2,i -t 1,i Calculate the equivalent silicon removal rate v of the i-th monitored region. i ;

[0164] The residual amount and residual amount compensation module 192 is configured to compensate for the amount of residual silicon removed according to a pre-calibrated equivalent residual silicon removal amount L. i and equivalent residual silicon removal amount ΔS i According to T i =max{0, (L i -ΔS i ) / v i The i-th monitored area is determined from the second event time t. 2,i Switching wait time T i ;

[0165] The zone valve control module 193 is configured to, after the switching waiting time T, i At that time, the corresponding liquid processing unit stops supplying silicon etching solution and supplies cleaning solution, while other monitored areas that have not yet reached their respective switching waiting time continue to be etched, so that different monitored areas are in etching state, liquid switching state or cleaning state respectively at the same time.

[0166] Specifically, the controller is used to perform the following steps:

[0167] Step S1: Obtain the configuration parameters and calibration data for each monitored area. The configuration parameters include the known height difference ΔH between the first conductive detection end face and the second conductive detection end face in the dual threshold witness unit corresponding to each area. The calibration data includes the equivalent remaining silicon removal amount L required for each area from the time of completion of the second event determination until the product TSV reaches the target backside exposure state. i And the equivalent residual silicon removal amount ΔS generated in each region from the cessation of silicon etching solution supply to the completion of cleaning solution replacement. i ;

[0168] Step S2: Real-time acquisition of electrical response signals from the detection end face of each monitored area. When silicon etching solution is detected to be in contact with the first conductive detection end face and the corresponding electrical response meets the preset event criteria, the first event is determined to be completed and the time t of the first event completion is recorded. 1,i When silicon etching solution is detected to contact the second conductive detection end face and the corresponding electrical response satisfies the same preset event criterion, the second event is determined to be completed and the completion time t of the second event is recorded. 2,i ;

[0169] Step S3: Based on the known height difference ΔH and the completion time t of the first event determination 1,i and the completion time t of the second event determination 2,i The silicon removal rate v of each monitored region is calculated using the following formula. i :

[0170] v i =ΔH / (t2,i -t 1,i )

[0171] Step S4: From the time t when the second event is determined to be complete 2,i Starting from this point, the handover waiting time T for each monitored area is calculated using the following formula. i :

[0172] T i =max{0,(L i -ΔS i ) / v i}

[0173] Among them, L i ΔS represents the equivalent residual silicon removal amount in the i-th monitored region. i The equivalent residual silicon removal amount for the i-th monitored area;

[0174] Step S5: Determine the completion time t based on the second event. 2,i Timing begins from the starting point of the timeout. When the cumulative time of the i-th monitored area reaches the switching waiting time T... i When the time comes, a command to stop supplying silicon etching solution is sent to the liquid processing unit corresponding to the area, and a command to supply cleaning solution is sent. At the same time, the supply of silicon etching solution continues to other monitored areas that have not yet reached their respective switching waiting time.

[0175] Step S6: After all monitored areas have completed switching and output a command to stop supplying silicon etching solution, output a processing end signal.

[0176] Those skilled in the art will understand that embodiments of this application can be provided as methods, systems, or computer program products. Therefore, this application can take the form of a completely hardware embodiment, a completely software embodiment, or an embodiment combining software and hardware aspects. Furthermore, this application can take the form of a computer program product embodied on one or more computer-usable storage media (including but not limited to disk storage, CD-ROM, optical storage, etc.) containing computer-usable program code.

[0177] This application is described with reference to flowchart illustrations and / or block diagrams of methods, apparatus (systems), and computer program products according to embodiments of this application. It will be understood that each block of the flowchart illustrations and / or block diagrams, and combinations of blocks in the flowchart illustrations and / or block diagrams, can be implemented by computer program instructions. These computer program instructions can be provided to a processor of a general-purpose computer, special-purpose computer, embedded processor, or other programmable data processing apparatus to produce a machine, such that the instructions, which execute via the processor of the computer or other programmable data processing apparatus, generate instructions for implementing the flowchart... Figure 1One or more processes and / or boxes Figure 1 A device that provides the functions specified in one or more boxes.

[0178] These computer program instructions may also be stored in a computer-readable storage medium that can direct a computer or other programmable data processing device to function in a particular manner, such that the instructions stored in the computer-readable storage medium produce an article of manufacture including instruction means, which are implemented in a process Figure 1 One or more processes and / or boxes Figure 1 The function specified in one or more boxes.

[0179] These computer program instructions may also be loaded onto a computer or other programmable data processing equipment to cause a series of operational steps to be performed on the computer or other programmable equipment to produce a computer-implemented process, thereby providing instructions that execute on the computer or other programmable equipment for implementing the process. Figure 1 One or more processes and / or boxes Figure 1 The steps of the function specified in one or more boxes.

[0180] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method for exposing the back side of a wafer TSV, characterized in that, include: The wafer containing TSVs, whose device layers have been fabricated, is divided into at least two monitored regions; a dual threshold witnessing unit electrically isolated from TSVs is formed in the dicing track corresponding to each region; the witnessing unit has a first conductive detection end face and a second conductive detection end face facing the back of the wafer, with a known height difference along the wafer thickness direction and sidewall insulation. The device side of the wafer is bonded to the carrier substrate and thinned from the back side; Multiple liquid processing units are used to form mutually isolated local liquid films in each monitored area; For each region, when the silicon etching solution contacts the first conductive detection end face and the corresponding electrical response meets the preset event criteria, the first event is determined to be completed and the time of completion of the first event is recorded; when the silicon etching solution contacts the second conductive detection end face and the corresponding electrical response meets the same preset event criteria, the second event is determined to be completed and the time of completion of the second event is recorded, and the silicon removal rate of each region is calculated in combination with the height difference. Obtain the equivalent remaining silicon removal amount required for each region from the time the second event determination is completed until the product TSV reaches the target back-side exposure state, and the equivalent residual silicon removal amount generated from the time the silicon etching solution is stopped to the time the cleaning solution replacement is completed; Based on the silicon removal rate of each region, the equivalent residual silicon removal amount required for each region from the completion of the second event determination to the product TSV reaching the target back-side exposure state, and the equivalent residual silicon removal amount generated in each region from the cessation of silicon etching solution supply to the completion of cleaning solution replacement, the etching stop time for each region is determined respectively, so that the region that reaches the target first is switched to cleaning solution, and other regions continue etching until the etchant concentration in the local liquid film of each region is reduced to the preset replacement concentration threshold.

2. The wafer TSV backside exposure method according to claim 1, characterized in that, Each of the dual threshold witness units includes a first detection conductor and a second detection conductor, the first detection conductor and the second detection conductor having a first conductive detection end face and a second conductive detection end face facing the back of the wafer, respectively, and are respectively connected to the test contact terminal through independent and insulated leads; Except for the first conductive detection end face, the second conductive detection end face, and the test contact end, the sidewalls, connecting parts, and leads of the first detection conductor and the second detection conductor are all covered by a dielectric isolation layer; The dielectric isolation layer terminates at the periphery of the corresponding conductive detection end face without covering the conductive detection end face, so that the conductive detection end face can directly contact the processing liquid after the silicon above it is removed. The first conductive detection end face is closer to the back side of the wafer than the second conductive detection end face, and the distance between the two along the wafer thickness direction is a known height difference ΔH.

3. The wafer TSV backside exposure method according to claim 2, characterized in that, The first detection conductor and the second detection conductor have the same detection end face material, area, sidewall isolation structure and corresponding mask opening, except that the depth of the detection end face along the wafer thickness direction is different. Both the first detection conductor and the second detection conductor include a conductive body, an adhesion / blocking layer located around the conductive body, and a sidewall dielectric isolation layer located around it. The first conductive detection end face, the second conductive detection end face, and the test contact end are not covered by the sidewall dielectric isolation layer.

4. The wafer TSV back-side exposure method according to claim 1, characterized in that, Bonding the device side of the wafer to a carrier substrate and thinning it from the back side includes: The device face of the wafer is instantaneously bonded to the carrier, and the wafer is thinned from the back side so that a residual silicon layer is retained above the back face of the product TSV, the first conductive detection face, and the second conductive detection face.

5. The wafer TSV backside exposure method according to claim 1, characterized in that, Multiple liquid processing units are used to form mutually isolated local liquid films in each monitored area, including: Multiple liquid processing units, each corresponding to a monitored area, are used to form a local liquid film that is separated from each other in each monitored area, and silicon etching solution supply, cleaning solution supply and liquid recovery are performed independently for each monitored area. At least one of liquid recovery and gas isolation is implemented at the boundary of adjacent monitored areas, so that the concentration of etchant entering the adjacent monitored area from one monitored area is lower than the preset cross-contamination concentration threshold, thereby enabling different monitored areas to be in etching state, liquid switching state or cleaning state respectively. The liquid processing unit includes a liquid supply and recovery processing head corresponding to the monitored area. The processing head has a liquid supply port, an annular liquid recovery port, and an annular gas isolation port located outside the recovery port, so that different areas can be in etching, switching, or cleaning states respectively. A transition zone is provided between adjacent monitored areas; at any given time, only one of the adjacent liquid processing units is allowed to supply silicon etching solution to the transition zone, while the other liquid processing unit performs liquid recovery and / or gas isolation on one side of the transition zone.

6. The wafer TSV backside exposure method according to claim 5, characterized in that, The silicon etching solution is a tetramethylammonium hydroxide solution with a mass fraction of 5% to 25% or a potassium hydroxide solution with a mass fraction of 15% to 35%, and the etching temperature is 50°C to 85°C. The cleaning solution is deionized water or an aqueous solution that has a diluting, displacement or neutralizing effect on the silicon etching solution and is compatible with the TSV material.

7. The wafer TSV back-side exposure method according to claim 1, characterized in that, For each region, when the silicon etching solution contacts the first conductive detection end face and the corresponding electrical response meets the preset event criterion, the first event is determined to be completed and the completion time of the first event is recorded; when the silicon etching solution contacts the second conductive detection end face and the corresponding electrical response meets the same preset event criterion, the second event is determined to be completed and the completion time of the second event is recorded, and the silicon removal rate of each region is calculated in combination with the height difference, including: By using a counter electrode immersed in a corresponding local liquid film and an AC detection source, a detection circuit is formed between the detection conductor and the counter electrode, thereby obtaining the corresponding electrical response; the electrical response includes impedance amplitude, impedance phase and / or AC current; In the i-th monitored area, when the silicon etching solution establishes direct liquid-phase electrical contact with the first conductive detection end face, and the corresponding electrical response satisfies the preset event criterion, the completion time t of the first event determination is recorded. 1,i ; When the silicon etching solution establishes direct liquid-phase electrical contact with the second conductive detection end face and the corresponding electrical response satisfies the same preset event criterion, the completion time t of the second event determination is recorded. 2,i ; The silicon removal rate v of the i-th monitored region is calculated using the following formula. i : v i =ΔH / (t 2,i -t 1,i ); The preset event criterion is: Using the electrical response collected within a predetermined time window before the event occurs as a dynamic baseline, when the changes of at least two electrical characteristic quantities among impedance amplitude, impedance phase and alternating current relative to the dynamic baseline reach the corresponding preset change thresholds and continue for a duration not less than a preset duration threshold, it is determined to be a valid event.

8. The wafer TSV backside exposure method according to claim 1, characterized in that, Obtain the equivalent remaining silicon removal amount required for each region from the completion of the second event determination to the product TSV reaching the target backside exposure state, and the equivalent residual silicon removal amount generated from the cessation of silicon etching solution supply to the completion of cleaning solution replacement, including: Under conditions of crystal orientation, doping conditions, silicon etching solution composition, temperature, liquid processing unit gap, liquid supply flow rate, recovery flow rate, local liquid film conditions, and back-side processing opening structure above the TSV and dual-threshold witness unit, which are the same as or pre-calibrated as the wafer to be processed, the preset event criteria are used to pre-establish a calibration mapping relationship between the process state corresponding to the completion time of the second event judgment and the product TSV reaching the target back-side end exposure state, so as to obtain the equivalent remaining silicon removal amount L corresponding to the regional equivalent silicon removal rate. i The exposure state of the target back end is characterized by at least one of the exposure height of the product TSV back end relative to the adjacent silicon surface and the circumferential exposure integrity. By conducting liquid switching tests using the same liquid treatment unit gap, temperature, supply flow rate, recovery flow rate, cleaning fluid flow rate, and valve sequence, the equivalent response and the amount of silicon removed by displacement ΔS were determined from the time the silicon etching solution supply stopped until the etchant concentration in the corresponding local liquid film decreased to a preset displacement concentration threshold. i The equivalent response and the amount of silicon removed by substitution ΔS i This includes the amount of silicon removed during command output, valve response, liquid transport, and cleaning fluid replacement.

9. The wafer TSV back-side exposure method according to claim 8, characterized in that, Based on the silicon removal rate of each region, the equivalent residual silicon removal amount required for each region from the completion of the second event determination to the product TSV reaching the target backside exposure state, and the equivalent residual silicon removal amount generated in each region from the cessation of silicon etching solution supply to the completion of cleaning solution replacement, the etching stop time for each region is determined respectively. This allows regions that reach the target first to switch to cleaning solution, while other regions continue etching, until the etchant concentration in the local liquid film of each region is reduced to the preset replacement concentration threshold, including: From the time t when the second event is determined to be completed 2,i Timing begins, and the switching waiting time T for each monitored area is calculated using the following formula. i : T i =max{0,(L i -ΔS i ) / v i }; Among them, T i Let i be the switching waiting time for the i-th monitored area; After the switching waiting time T i At the same time, a command to stop the supply of silicon etching solution is output to the corresponding liquid processing unit and cleaning solution is supplied. Meanwhile, the supply of silicon etching solution continues to other monitored areas that have not yet reached their respective switching waiting time, until the etchant concentration in the local liquid film of each monitored area is reduced to the preset replacement concentration threshold. If the calculated T i If the value is zero, it is immediately determined that the area needs to enter the erosion stop and switchover process.

10. A wafer TSV backside exposure system, characterized in that, include: A processing station is used to hold a TSV-containing wafer; the wafer is pre-divided into at least two monitored areas, and a dual threshold witness unit is provided in the dicing track of each monitored area. The witness unit has a first conductive detection end face and a second conductive detection end face facing the back of the wafer, with a known height difference along the wafer thickness direction and sidewall insulation. Multiple liquid processing units, each corresponding to a monitored area, are configured to form a local liquid film isolated from other areas in the corresponding monitored area and to independently supply silicon etching solution or cleaning solution. The detection circuit is electrically connected to each of the dual threshold witness units and is used to collect the electrical response signal when the silicon etching solution contacts each conductive detection end face. The controller, which is communicatively connected to each of the liquid processing units and the detection circuit, is configured to determine the completion time of the first event and the second event based on the electrical response signal, calculate the silicon removal rate of each region, and determine the etching stop time of each region based on the silicon removal rate, the pre-calibrated equivalent remaining silicon removal amount, and the equivalent residual silicon removal amount. When the corresponding region reaches the etching stop time, the controller controls the liquid processing unit of that region to stop supplying silicon etching solution and switch to cleaning solution, while maintaining the etching of other regions.