A combined cleaning method for nanoscale particles and metal ion residues on wafer surfaces

By employing multi-stage cleaning methods and synergistic technologies, the challenge of cleaning nanoscale particles and metal ion residues on wafer surfaces has been solved, achieving efficient and environmentally friendly wafer cleaning results that meet the ultra-cleanliness requirements of advanced processes.

CN123124700APending Publication Date: 2026-11-17ANHUI FULLERDE CHANGJIANG SEMICON MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611212153.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies are insufficient to efficiently remove nanoscale particles and metal ion residues from wafer surfaces, especially in advanced processes where there are problems of low cleaning efficiency and secondary contamination.

Method used

A multi-stage cleaning method is employed, including surface pre-assessment, nano-sized particle dispersion treatment, alkaline cleaning, chelation cleaning, megasonic-assisted cleaning, and multi-stage purification and drying. The synergistic effect of dispersants, chelating agents, and nano-sized silica particles is combined to ensure cleaning effectiveness and prevent re-adhesion.

Benefits of technology

It achieves efficient removal of nanoscale particles and metal ions, significantly improves cleaning efficiency, meets the ultra-cleanliness requirements of advanced processes, and reduces cleaning fluid consumption and production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124700A_ABST
    Figure CN123124700A_ABST
Patent Text Reader

Abstract

This invention discloses a combined cleaning method for nanoscale particles and metal ion residues on wafer surfaces. The method utilizes a super-depth-of-field microscope and a surface particle counter to pre-assess and determine the particle size and metal ion type. The method then sequentially performs nanoscale particle dispersion treatment, alkaline cleaning, chelation cleaning, and megasonic-assisted enhanced cleaning. This method achieves efficient combined removal of nanoscale particles and metal ions, overcoming cleaning bottlenecks, significantly reducing metal residues, meeting the requirements of advanced processes for ultra-clean surfaces, and simultaneously reducing cleaning solution and water consumption, thus offering both economic and environmental benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of semiconductor manufacturing, and specifically relates to a combined cleaning method for nanoscale particles and metal ion residues on wafer surfaces. Background Technology

[0002] Semiconductor manufacturing processes are the core support of the modern information technology industry, and wafer surface cleaning technology, as a key link in integrated circuit manufacturing, directly affects the performance, reliability, and yield of semiconductor devices. With advanced process nodes continuously moving towards extreme miniaturization, the requirements for wafer surface contamination control are becoming increasingly stringent. Even trace amounts of surface contaminants can lead to device performance degradation or even failure, resulting in significant economic losses. Wafer surface contaminants are diverse, with nanoscale particles and residual metal ions being the two most harmful sources. Nanoscale particles mainly originate from processing steps such as mechanical grinding and chemical mechanical planarization, while metal ions are mostly introduced through etching and deposition processes. These two types of contaminants pose a particularly prominent threat to device yield in advanced processes.

[0003] Among these, the combined cleaning technology for nanoscale particles and metal ion residues on wafer surfaces has become a core research topic in the semiconductor cleaning field. This technology aims to achieve the synergistic removal of different types of contaminants by optimizing the cleaning process and cleaning solution formulation. It effectively removes metal ions while removing particulate matter, avoiding secondary pollution during the cleaning process, thereby meeting the stringent requirements of advanced processes for ultra-clean wafer surfaces.

[0004] Existing technologies have explored various methods for cleaning wafer surfaces, but significant shortcomings remain. The patented technology with publication number CN116631848A employs SC1 cleaning solution, SC2 cleaning solution, and SC1 cleaning solution with added chelating agents for stepwise cleaning of silicon wafers. However, this method primarily targets particles of conventional sizes, with limited effectiveness in removing nanoscale particles. Furthermore, the use of traditional RCA cleaning processes results in relatively low cleaning efficiency, failing to meet the ultra-clean surface requirements of advanced processes. Additionally, it does not effectively control particle re-adhesion during the cleaning process, potentially leading to secondary contamination of the surface after cleaning. The patent technology published in CN111211042B uses a combination of alkaline and acidic cleaning to remove particulate impurities and metal ions from the silicon wafer surface. However, this process is mainly for post-polishing cleaning of large-diameter silicon wafers, limiting its application. The combination of alkaline and acid cleaning is not effective in removing nanoscale particles, especially those smaller than 100 nm. Furthermore, it may introduce new particles during the cleaning process, making true combined cleaning difficult. It also lacks targeted removal solutions for different types of metal ions, and the cleaning effect is limited by the cleaning solution formulation and process parameters. These technical solutions indicate that existing wafer cleaning technologies still face significant technical bottlenecks in the combined cleaning of nanoscale particles and metal ion residues. There is an urgent need to develop a combined cleaning method that can efficiently and synergistically remove nanoscale particles and metal ions, achieving ultra-clean wafer surface cleaning to meet the high cleanliness requirements of advanced processes. Summary of the Invention

[0005] The purpose of this invention is to provide a combined cleaning method for nanoscale particles and metal ion residues on wafer surfaces, which can effectively solve the problems mentioned in the background art.

[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0007] A combined cleaning method for nanoscale particles and metal ion residues on wafer surfaces includes the following specific steps: Step 1, surface pre-assessment and contaminant analysis: Macroscopic morphology of the wafer surface is observed using a super-depth-of-field microscope; nanoscale particles are detected using a surface particle counter based on light scattering principle, with a detection limit of 50 nm; metal ion type is quantitatively detected using inductively coupled plasma mass spectrometry, with a detection limit of 0.01 μg / L to 0.1 μg / L for metal ion concentration in solution, and a corresponding detection limit of 0.1 ng / cm³ for the calculated surface density of metal ions on the wafer surface. 2 ~0.5ng / cm 2 This reduces the van der Waals forces between nanoscale particles, making the particles loosely dispersed and easier to remove in subsequent cleaning steps, while also reducing the risk of particle re-adhesion during the cleaning process.

[0008] Step 2, nanoscale particle dispersion treatment: The wafer is placed in a pretreatment solution containing a dispersant and subjected to ultrasonic dispersion treatment. The dispersant is sodium polyacrylate or polyethylene glycol with a molecular weight of 5000 to 50000 and a mass concentration of 0.01% to 0.5%. The ultrasonic power density is 0.8 W / cm² to 2 W / cm² and the treatment time is 8 min to 30 min.

[0009] Step 3, the first step is alkaline cleaning. The first stage of cleaning is carried out using an alkaline cleaning solution containing surfactants and silica sol. The alkaline cleaning solution is a mixture of ammonium hydroxide and hydrogen peroxide, with the volume ratio of ammonia water to hydrogen peroxide being 1:1 to 1:10. The cleaning solution temperature is 60℃ to 85℃, the pH value is 10 to 11.5, the silica sol mass fraction is 0.01% to 0.5%, the particle size is 5nm to 50nm, the surfactant mass fraction is 0.001% to 0.01%, and the cleaning time is 8min to 20min. This is to remove most of the organic contaminants and large particles from the wafer surface, and at the same time form a temporary protective layer on the wafer surface that can be removed by subsequent cleaning steps to prevent the re-adhesion of particles during the cleaning process.

[0010] Step 4, the second step of chelation cleaning, uses an acidic chelation cleaning solution containing a chelating agent for the second stage of cleaning. The chelating agent is one or more combinations of ethylenediaminetetraacetic acid, nitric acid triacetic acid, or diethylenetriaminepentaacetic acid, with a total concentration of 0.01 mol / L to 0.1 mol / L. The pH value of the cleaning solution is 4.0 to 6.0, the temperature is 40℃ to 60℃, and the treatment time is 5 min to 15 min. This selectively chelates and removes residual metal ions from the wafer surface while avoiding corrosion of the wafer surface.

[0011] Step 5, enhanced removal of nanoparticles: a third-stage cleaning is performed using a megasonic-assisted chemical cleaning solution with a megasonic frequency of 0.8MHz to 1.0MHz. The cleaning solution contains nano-sized silica particles with a particle size of 10nm to 100nm and a mass concentration of 0.1g / L to 1g / L. The pH value of the cleaning solution is 8.5 to 9.5, and a borate-sodium borate buffer system is used with a buffer concentration of 0.01mol / L to 0.05mol / L.

[0012] Step 6, Surface purification and drying: High-purity deionized water is used for multi-stage overflow cleaning. The resistivity of the deionized water in the initial cleaning stage is 15 MΩ·cm to 18 MΩ·cm, and the resistivity in the final cleaning stage is 17.5 MΩ·cm to 18.2 MΩ·cm. The cleaning time for each stage is 30 s to 120 s, the number of cleaning stages is 3 to 5, and the water flow rate is 0.5 L / min to 2 L / min. Then, isopropanol with a purity of 99.9% or higher is used for vapor-phase drying. During the drying process, the temperature gradient on the wafer surface is 1℃ / cm to 5℃ / cm. This temperature gradient is achieved by arranging 3 infrared temperature sensors along the radial direction of the wafer in the spin-drying chamber and adjusting the power of the heating lamps in different zones. The heating power of the edge area is 60% to 90% of that of the center area. The spin-drying speed is 500 rpm to 3000 rpm, and the drying time is 2 min to 10 min to prevent water marks and re-adhesion of particles.

[0013] Step 7: Verification of cleaning effect. A laser particle counter and atomic absorption spectrometer were used to sample and test the surface of the cleaned wafer. The detection limit for particulate matter was 50 nm, and the detection limit for metal ions was 0.1 ng / cm³. 2 ~0.5ng / cm 2 Only wafers that meet the cleanliness standards can proceed to the next process.

[0014] Preferably, in step 1, the magnification of the ultra-depth-of-field microscope is 100x to 500x, the field of view is 2.5mm×1.9mm to 10mm×7.5mm, the surface particle counter adopts the principle of light scattering, the laser wavelength is 488nm or 635nm, the detection sensitivity can identify particles with a lower limit of 50nm, and the metal ion type analysis adopts inductively coupled plasma mass spectrometry, the detection range covers sodium, magnesium, aluminum, potassium, calcium, iron, copper and zinc elements.

[0015] Preferably, the pretreatment solution in step 2 further contains a nonionic surfactant with a concentration of 0.001% to 0.01%, an ultrasonic frequency of 40kHz to 80kHz, and the wafer reciprocates in the pretreatment solution during the treatment process with a reciprocating oscillation frequency of 0.1Hz to 0.5Hz and an oscillation amplitude of 20mm to 50mm to enhance the dispersion effect and avoid excessive local temperature.

[0016] Preferably, in step 3, the cleaning solution also contains 0.01%–0.5% silica sol with a mass fraction of 5 nm–50 nm. During the cleaning process, the cleaning solution is circulated and renewed at a flow rate of 0.5 L / min–2 L / min to ensure that the particulate matter concentration in the cleaning solution is maintained at 10. 6 Below 1 / L.

[0017] Preferably, the chelating cleaning solution in step 4 also contains a corrosion inhibitor with a concentration of 0.01% to 0.1%. The corrosion inhibitor is a silane coupling agent or a molybdate substance. During the cleaning process, nitrogen gas is used for stirring at a stirring rate of 50 mL / min to 200 mL / min to accelerate the chelation reaction and prevent carbon dioxide in the air from dissolving into the cleaning solution and causing local pH fluctuations.

[0018] Preferably, in step 5, the megasonic-assisted cleaning solution contains silica particles with a particle size of 10nm to 100nm, a mass concentration of 0.1g / L to 1g / L, a pH value of 8.5 to 9.5, uses a borate-sodium borate buffer system with a buffer concentration of 0.01mol / L to 0.05mol / L, has a megasonic transducer array power of 100W to 500W, a distance of 10mm to 30mm between the wafer and the megasonic transducer, and the wafer moves in the megasonic field at a linear velocity of 0.1mm / s to 5mm / s to ensure cleaning uniformity.

[0019] Preferably, in step 6, the high-purity deionized water adopts a multi-stage ion exchange and ultraviolet sterilization process. The resistivity of the deionized water in the initial cleaning stage is 15 MΩ·cm to 18 MΩ·cm, and the resistivity in the final cleaning stage is 17.5 MΩ·cm to 18.2 MΩ·cm. The cleaning time for each stage is 30s to 120s. The overflow cleaning adopts a top-in-bottom-out or bottom-in-top-out method with a water flow rate of 0.5L / min to 2L / min. The gas phase drying adopts a combination of rotary spin drying and gas phase drying with a spin drying speed of 500rpm to 3000rpm.

[0020] Preferably, the process also includes an intermediate rinsing step between step 3 and step 4: the wafer is rapidly rinsed with deionized water for 30 to 120 seconds, the resistivity of the deionized water is 10 MΩ·cm to 15 MΩ·cm, and the water film on the wafer surface remains intact during the rinsing process to ensure that no chemical reaction occurs between the alkaline cleaning solution and the chelating cleaning solution, which would affect the cleaning effect and the wafer surface quality.

[0021] Preferably, the method further includes a metal ion reduction step between step 4 and step 5: the wafer is treated with a reducing agent solution with a concentration of 0.01 mol / L to 0.1 mol / L, the reducing agent being ascorbic acid or sodium bisulfite, the treatment time being 2 min to 10 min, and the pH value of the reducing agent solution being 5.0 to 7.0, so as to reduce the oxidized metal ions that may exist on the wafer surface to their elemental state, so that they can be removed by megasonic cleaning in subsequent steps.

[0022] Preferably, the dispersion processing time in step 2 is determined as follows: based on the surface density D of particles with a diameter ≥ 50 nm measured by the surface particle counter in step 1, when D ≤ 1000 particles / cm²2 When the processing time is 8 minutes; when 1000 < D ≤ 5000 pieces / cm 2 When the processing time is 15 minutes; when D > 5000 pieces / cm 2 The processing time is 25 minutes; intermediate values ​​are calculated using linear interpolation.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. Highly efficient removal capability of nanoscale particles

[0025] Breakthrough in cleaning nanoscale particles: Through the multi-stage synergistic effect of dispersion treatment, alkaline cleaning, and megasonic-assisted cleaning, highly efficient removal of particles within a preset particle size range is achieved, with a significantly improved removal rate that is significantly superior to the removal efficiency of existing RCA cleaning processes for nanoscale particles. The cavitation effect of megasonic waves and the synergistic effect of chemical cleaning solutions containing nanoscale silica particles effectively solve the problem of particle re-adhesion in traditional cleaning methods, and the re-adhesion rate of surface particles after cleaning is effectively controlled.

[0026] 2. Precise metal ion removal effect

[0027] Multi-chelating agent synergistic system: The chelating agent formula achieves selective removal of metal ions by chelating various common metal ions such as iron, copper, aluminum, and zinc within a preset chelating capacity range. Combined with an acidic cleaning environment with precise pH control, the system achieves selective removal of metal ions. The reduction step reduces oxidized metal ions to their elemental state, further enhancing the removal effect. The residual amount of metal ions after cleaning is within a preset residual amount range, meeting the requirements of advanced processes for ultra-clean surfaces.

[0028] 3. Optimized cleaning process

[0029] Multi-stage cleaning combined with intermediate treatment: Through a complete process flow including surface pre-assessment, dispersion treatment, two-stage alkaline-chelation cleaning, megasonic enhanced removal, and multi-stage purification and drying, the combined and efficient removal of nanoscale particles and metal ions is achieved; the setting of intermediate rinsing and reduction steps effectively prevents mutual interference and side reactions between cleaning solutions, ensuring the independence of each cleaning step and the stability of the overall process.

[0030] 4. Significant resource conservation and environmental benefits

[0031] Cleaning solution recycling: The alkaline cleaning solution is recycled and renewed. Precise control of the cleaning solution flow rate and renewal frequency ensures the cleaning effect while minimizing cleaning solution consumption. Water and chemical consumption are reduced: Compared with the prior art, the cleaning solution consumption of the present invention is effectively reduced. The water consumption for cleaning a single wafer is controlled within the preset water consumption range, which effectively reduces production costs and environmental impact, and meets the requirements of green development in the semiconductor manufacturing industry. Attached Figure Description

[0032] Figure 1 This is a schematic diagram of the overall technical solution architecture of the combined cleaning method for nanoscale particles and metal ion residues on wafer surfaces provided by the present invention, showing the complete process flow from pre-evaluation to effect verification.

[0033] Figure 2 This is a schematic diagram illustrating the core principle framework of the synergistic effect of various stages in the present invention, including nanoscale particle dispersion treatment, alkaline cleaning, chelation cleaning, and megasonic wave enhanced removal.

[0034] Figure 3 This is a schematic diagram illustrating the technical principle of the cavitation effect and the synergistic removal of nanoscale particles by nanoscale silica particles in the megasonic-assisted chemical cleaning stage of this invention. Detailed Implementation

[0035] Example 1

[0036] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments.

[0037] This invention provides a combined cleaning method for nanoscale particles and metal ion residues on wafer surfaces. The method comprises seven core steps: Step 1, surface pre-assessment and contaminant analysis; Step 2, nanoscale particle dispersion treatment; Step 3, first-step alkaline cleaning; Step 4, second-step chelation cleaning; Step 5, enhanced nanoscale particle removal; Step 6, surface purification and drying; and Step 7, cleaning effect verification. The technical implementation of each step is described in detail below.

[0038] In Step 1, surface pre-assessment and contaminant analysis, a super depth-of-field microscope is first used to observe the macroscopic morphology of the wafer surface. The magnification of the super depth-of-field microscope is set within the range of 100x to 500x, and can be dynamically adjusted according to the degree of contamination on the wafer surface. The field of view is set from 2.5mm × 1.9mm to 10mm × 7.5mm, and full coverage observation of the wafer surface is achieved through a stitched scanning method. The super depth-of-field microscope employs an advanced depth-of-field extension algorithm, which can maintain image clarity over a large vertical range, making it suitable for rapid assessment of the three-dimensional morphology of the wafer surface. This device is equipped with a high-resolution CCD image sensor with over 5 million pixels. Combined with dedicated image analysis software, it can automatically identify and mark macroscopic defect areas on the wafer surface, including scratches, chipping, and uneven etching. In this embodiment, the ultra-depth-of-field microscope specifically adopts the Keyence VHX-7000 series digital microscope, equipped with a VH-Z20T high-magnification zoom lens (20x to 2000x magnification range) and a VH-Z100T wide-field zoom lens (100x to 1000x magnification range). The image sensor is a 4K CMOS type with 12 million pixels, and it works with a VHX-7100 control unit to realize automatic depth-of-field synthesis and three-dimensional measurement functions.

[0039] The surface particle counter uses the principle of light scattering to detect nanoscale particles. The laser source employs an argon-ion laser with a wavelength of 488 nm or a semiconductor laser with a wavelength of 635 nm, achieving power stability better than ±2%. The optical collection system uses a dark-field scattered light collection configuration, with the collection angle set within the range of 30° to 60°, achieving a signal-to-noise ratio better than 60 dB. The detection sensitivity can identify particles with a lower diameter limit of 50 nm, and it has a detection probability of over 95% for particles with diameters ranging from 50 nm to 10 μm. The surface particle counter is equipped with an automated scanning platform with a scanning step accuracy better than 1 μm, and the scanning area can cover wafers of different sizes, such as 6-inch, 8-inch, and 12-inch wafers. Detection data is transmitted to the process control server in real time for particle size distribution statistics and areal density calculation. The particle size distribution is fitted using a Weibull distribution model, and the areal density is calculated using a direct counting method. The detection results are characterized by the number of particles per square centimeter (particles / cm²). In this embodiment, the surface particle counter specifically adopts the KLA-Tencor Surfscan SP5 wafer surface particle detection system, equipped with a 488nm wavelength argon ion laser, a detection lower limit of 50nm (on the silicon wafer surface), a scanning rate covering the full surface detection of 200mm and 300mm wafers, and equipped with automatic focusing and automatic leveling functions.

[0040] Metal ion type analysis was performed using inductively coupled plasma mass spectrometry (ICP-MS) for quantitative detection. The ICP-MS system is equipped with a highly sensitive quadrupole mass analyzer with a mass resolution better than 0.7 amu, accurately distinguishing the mass numbers of different metal elements. The detection range covers common metal elements such as sodium (Na, atomic weight 22.99), magnesium (Mg, atomic weight 24.31), aluminum (Al, atomic weight 26.98), potassium (K, atomic weight 39.10), calcium (Ca, atomic weight 40.08), iron (Fe, atomic weight 55.85), copper (Cu, atomic weight 63.55), and zinc (Zn, atomic weight 65.38). The detection limit for metal ion concentration in solution ranges from 0.01 μg / L to 0.1 μg / L, and the corresponding detection limit for the surface density of metal ions on the wafer surface is 0.1 ng / cm³. 2 Up to 0.5 ng / cm 2 This method meets the stringent requirements of advanced manufacturing processes for the detection of residual metal ions. Sample pretreatment employs microwave digestion to transfer contaminants from the wafer surface to an acidic solution, followed by ICP-MS analysis. The concentration of residual metal ions is expressed as the mass of metal per square centimeter of wafer surface (ng / cm³). 2 Characterization was performed. In this embodiment, the ICP-MS specifically used an Agilent 8900 tandem quadrupole inductively coupled plasma mass spectrometer, equipped with standard nickel and platinum cone interfaces, an RF power of 1200W–1600W, a carrier gas flow rate of 0.8L / min–1.2L / min, a sampling depth of 8mm–12mm, and a pulse counting / analog dual-mode detector with a dynamic linear range of up to 10. 9 Magnitude.

[0041] Based on the preliminary assessment results, the subsequent cleaning process parameters are dynamically adjusted. When the particle surface density is greater than 1000 particles / cm², the processing time and ultrasonic power density of step 2 dispersion treatment are increased; when the total metal ion concentration is greater than 100 ng / cm², the parameters are adjusted accordingly. 2 If the aluminum ion concentration is found to be significantly high, the processing time of step 4 (chelation cleaning) is increased and the concentration of the chelating agent is increased; if the aluminum ion concentration is detected to be significantly high, the proportion of aluminum ion selective chelating agent in step 4 is increased. This dynamic adjustment mechanism is achieved through a preset parameter mapping table, which automatically matches the optimal cleaning process formula based on pre-evaluation data.

[0042] In step 2, the nanoscale particulate dispersion process, the wafer is placed in a pretreatment solution containing a dispersant and subjected to ultrasonic dispersion. The dispersant is sodium polyacrylate or polyethylene glycol, with a molecular weight controlled within the range of 5000 to 50000. The mass concentration of the dispersant is set within the range of 0.01% to 0.5%. The pretreatment solution also contains a nonionic surfactant at a concentration of 0.001% to 0.01%. The operating frequency of the ultrasonic generator is set within the range of 40kHz to 80kHz. The ultrasonic power density is set at 0.5W / cm². 2 Up to 2W / cm 2 Within the specified range. During processing, the wafer is oscillated back and forth in the pretreatment solution, with the oscillation frequency set between 0.1Hz and 0.5Hz, and the oscillation amplitude set between 20mm and 50mm. The processing time is set between 8 minutes and 30 minutes, with the specific time determined according to the pre-assessed particulate contamination level according to the following segmentation rules: based on the surface density D (unit: particles / cm³) of particles with a diameter ≥50nm measured by the surface particle counter in step 1. 2 When D≤1000 pieces / cm 2 When the processing time is 8 minutes; when 1000 < D ≤ 5000 pieces / cm 2 When the processing time is 15 minutes; when D > 5000 pieces / cm 2 The processing time was 25 minutes; intermediate values ​​were calculated using linear interpolation. This segmentation rule also applies to other embodiments. The purpose of this dispersion treatment step is to reduce the van der Waals forces between nanoscale particles, making the particles loosely dispersed, facilitating their effective removal in subsequent cleaning steps, and reducing the risk of particle re-adhesion during cleaning. After the dispersion treatment is completed, the wafer is removed from the dispersion solution using vacuum adsorption and transferred to the next cleaning process.

[0043] In step 3, the first step of alkaline cleaning, an alkaline cleaning solution containing surfactants and silica sol is used for the first stage of cleaning. The alkaline cleaning solution is a mixture of ammonium hydroxide (NH4OH) and hydrogen peroxide (H2O2), i.e., the classic SC-1 cleaning solution formula. The volume ratio of ammonia to hydrogen peroxide is controlled within the range of 1:1 to 1:10, with a typical ratio of 1:5 to 1:6. The cleaning solution temperature is set within the range of 60℃ to 85℃, with a typical value of 70℃ to 80℃. Within this temperature range, ammonia can effectively volatilize and remove organic pollutants, and hydrogen peroxide can decompose into water and oxygen, releasing active oxygen, thus having both oxidation and cleaning effects. The pH value of the cleaning solution is controlled within the range of 10 to 11.5, and is monitored in real time using an online pH sensor, with pH fluctuations controlled within ±0.2.

[0044] The cleaning solution contains 0.01% to 0.5% silica sol by mass, with a particle size ranging from 5 nm to 50 nm. The main component of the silica sol is nano-sized silica particles, which are stable in an alkaline environment and can form a uniform temporary protective layer on the wafer surface. The thickness of this temporary protective layer is controlled within the range of 1 nm to 10 nm, effectively isolating contaminants in the cleaning solution from the wafer surface and preventing the re-adhesion of particles generated during the cleaning process. This temporary protective layer can be effectively removed in the subsequent chelation cleaning step. Anionic or nonionic surfactants are used, with a mass fraction ranging from 0.001% to 0.01%. The surfactants can reduce the surface tension of the cleaning solution to within the range of 30 mN / m to 40 mN / m, enhancing the wettability of the cleaning solution on the wafer surface, while also having an emulsifying and dispersing effect.

[0045] During the cleaning process, the cleaning solution is circulated and replenished at a preset flow rate. The circulation pump is a magnetically driven centrifugal pump with a flow control accuracy better than ±5%. The cleaning solution flow rate is set within the range of 0.5 L / min to 2 L / min, with the specific value determined based on the cleaning tank volume and the number of wafers. The cleaning solution is continuously filtered through a filter with a filtration accuracy of 0.2 μm to 0.5 μm to ensure that the particulate matter concentration in the cleaning solution is always maintained at the critical value of 10. 6 The filter element density is below 1 / L. When the filtration differential pressure exceeds the set threshold, the filter element is automatically replaced. The cleaning time is set between 5 and 20 minutes, with the specific time determined based on the pre-assessed organic contaminant content. During the cleaning process, the cleaning solution temperature is precisely controlled using a PID temperature control system, with a temperature control accuracy better than ±2℃.

[0046] An intermediate rinsing step is set between steps 3 and 4, using deionized water for rapid rinsing of the wafer. The resistivity of the deionized water used for rinsing is set within the range of 10 MΩ·cm to 15 MΩ·cm, and the water temperature is set within the range of 20°C to 30°C. The rinsing time is set within the range of 30 to 120 seconds, using an overflow rinsing method with the water flow direction parallel to the wafer surface to avoid direct rinsing and re-adhesion of particles. During rinsing, the wafer is rotated at a low speed of 5 to 20 revolutions per minute to maintain the integrity of the water film on the wafer surface. After rinsing, most of the moisture on the wafer surface is removed by nitrogen purging, creating conditions for the next step of chelation cleaning. The design of the intermediate rinsing step ensures that no chemical reaction occurs between the alkaline cleaning solution and the chelation cleaning solution, preventing residual ammonia from affecting the pH stability of the chelation cleaning solution.

[0047] In step 4, the second step of chelation cleaning, an acidic chelation cleaning solution containing a chelating agent is used for the second stage of cleaning. The chelating agent is one or a combination of ethylenediaminetetraacetic acid (EDTA), nitric acid triacetic acid (NTA), or diethylenetriaminepentaacetic acid (DTPA). EDTA has the highest chelation capacity and a stability constant for iron ions reaching 10. 25 The stability constant for copper ions reaches 10. 18 In summary, NTA exhibits a faster chelation rate, making it suitable for removing weakly adsorbed metal ions; DTPA, with its larger molecular weight and lower steric hindrance, is suitable for removing large-sized metal oxide particles. The total concentration of the chelating agent is set within the range of 0.01 mol / L to 0.1 mol / L, and the specific ratio is optimized and adjusted based on the pre-assessed type and concentration of metal ions.

[0048] The pH of the chelation cleaning solution is controlled within the range of 4.0 to 6.0, and is stabilized using an acetate-sodium acetate buffer system or a citric acid-sodium citrate buffer system. The cleaning solution temperature is set within the range of 40℃ to 60℃, with a typical value of 50℃ to 55℃. Within this temperature range, the chelation reaction rate is moderate, ensuring effective removal of metal ions without causing wafer surface oxidation due to excessive temperature. The processing time is set within the range of 5 minutes to 15 minutes.

[0049] The chelating cleaning solution also contains a preset concentration of corrosion inhibitor. The corrosion inhibitor is a silane coupling agent or a molybdate, with a concentration set between 0.01% and 0.1%. Silane coupling agents (such as γ-aminopropyltriethoxysilane) can form a hydrophobic protective film on the wafer surface, preventing the acidic cleaning solution from corroding the silicon surface; molybdates (such as sodium molybdate) can form a passivation film on the metal surface, inhibiting the dissolution of metal ions. The corrosion inhibition efficiency is required to be better than 95%, effectively protecting the wafer surface from corrosion in acidic environments.

[0050] Nitrogen gas is used for stirring during the cleaning process, with the stirring rate set between 50 mL / min and 200 mL / min. Nitrogen gas is evenly released from the bottom of the cleaning tank through a porous distribution plate, forming fine bubbles that gently stir the cleaning solution. Nitrogen stirring accelerates mass transfer during the chelation reaction, promoting the diffusion of metal ions into the solution; simultaneously, the nitrogen covering layer prevents carbon dioxide from dissolving into the cleaning solution, avoiding localized pH fluctuations. After cleaning, the wafers are removed from the chelation cleaning solution using vacuum adsorption and transferred to subsequent processing steps.

[0051] A metal ion reduction step is set between steps 4 and 5, where the wafer is treated with a reducing agent solution of a preset concentration. The reducing agent is ascorbic acid (C5H8O5) or sodium bisulfite (NaHSO3), with a concentration set between 0.01 mol / L and 0.1 mol / L. The pH of the reducing agent solution is controlled between 5.0 and 7.0, and a phosphate buffer system is used for stabilization. The treatment time is set between 2 and 10 minutes, and the temperature is room temperature (20°C to 25°C).

[0052] The working principle of the metal ion reduction step is to reduce the oxidized metal ions that may exist on the wafer surface to their elemental state. For example, ferric ions (Fe3+) 3+ ) is reduced to ferrous ions (Fe) 2+ ), divalent copper ions (Cu 2+ It is reduced to elemental copper (Cu) 0 Elemental metals are more easily removed physically during subsequent megasonic cleaning. This reduction step significantly improves the overall removal efficiency of metal ions, especially for metal residues present in oxide form.

[0053] In step 5, enhanced removal of nanoparticles, a third-stage cleaning process using megasonic-assisted chemical cleaning solution is employed. The megasonic frequency is set within the range of 0.8 MHz to 1.0 MHz, with typical values ​​of 0.92 MHz or 1.0 MHz. Compared to ultrasound, megasonic waves have a shorter wavelength and a more uniform energy distribution, resulting in a more uniform cavitation effect on the wafer surface. The megasonic transducer array, made of piezoelectric ceramic, is positioned at the bottom or sidewall of the cleaning tank, with the total power of the transducer array set between 100 W and 500 W. The distance between the wafer and the megasonic transducer is set between 10 mm and 30 mm; too close a distance may result in excessive energy and damage to the wafer surface, while too large a distance leads to energy attenuation and reduced cleaning efficiency.

[0054] The megasonic-assisted cleaning solution contains nanoscale silica particles with a particle size ranging from 10 nm to 100 nm and a particle concentration ranging from 0.1 g / L to 1 g / L. These nanoscale silica particles act as cavitation nuclei in the megasonic field, significantly enhancing the intensity and density of the cavitation effect. When the cavitation bubbles collapse on the wafer surface, they generate high-speed microjets and a localized high-temperature, high-pressure microenvironment, physically stripping the nanoscale particles adsorbed on the wafer surface. Simultaneously, the rolling friction of the nanoscale silica particles themselves also contributes to particle removal.

[0055] The synergistic mechanism between the megasonic cavitation effect and the nanoscale silica particles in this step is as follows: When the megasonic frequency is 0.8MHz to 1.0MHz, the sound wave propagates in the liquid, generating periodic compression and rarefaction phases. During the rarefaction phase half-cycle, dissolved gases in the liquid precipitate to form cavitation bubble nuclei. It should be noted that the nanoscale silica particles (10nm to 100nm) added in this invention do not directly act as cavitation bubble nuclei (their resonant frequency is much higher than 1MHz), but rather as a cavitation enhancement medium—their high specific surface area provides a large number of preferential nucleation sites, reducing the threshold sound pressure for cavitation and significantly increasing the cavitation event density by approximately 3 to 5 times under the same megasonic power. During the positive pressure half-cycle, the bubble nuclei undergo a violent collapse process, generating shock waves and microjets. When this high-energy shock wave acts on the particle-wafer interface, the combined effect of the weakly alkaline chemical solution (pH=8.5~9.5) hydrolyzes and weakens the silicon-oxygen bonds or metal-oxygen bonds at the interface, reducing the adhesion between the particles and the wafer surface. At this point, the shear stress generated by the cavitation microjets is sufficient to overcome the adhesion force, effectively peeling off particles with a diameter of 10nm~100nm. The peeled particles are then encapsulated by surfactants and dispersants in the cleaning solution, forming a stable dispersion state and preventing re-adhesion.

[0056] To verify this synergistic effect, the present invention provides the following comparative verification method: Under the same megasonic power (300W) and the same cleaning solution (pH=9.0, boric acid-sodium borate buffer), the following tests were conducted: (1) a cleaning solution without nano-silica particles; (2) a cleaning solution containing 0.5 g / L of 50 nm silica particles. After cleaning wafers with the same degree of contamination for 5 minutes, the particle removal rate was detected using the method in step 7. The experimental results show that after adding nano-silica particles, the removal rate of 50 nm particles increased from about 60% to over 95%. Those skilled in the art can reproduce this effect using the above method. The buffer system is used to maintain the pH value of the cleaning solution and ensure the continuous effectiveness of the chemical action. The megasonic cleaning time is set in the range of 3 to 10 minutes, and the specific time is determined according to the pre-assessed degree of nano-sized particle contamination.

[0057] The wafer moves at a preset linear velocity within a megaacoustic field. The wafer carrier platform is driven by a stepper motor, allowing for linear velocity adjustment within the range of 0.1 mm / s to 5 mm / s. The wafer passes through the megaacoustic cleaning area at a constant linear velocity, ensuring uniform cleaning energy across the wafer surface at different locations. During the cleaning process, the cleaning solution is continuously circulated and replenished, with a circulation flow rate set within the range of 0.2 L / min to 1 L / min. After cleaning, the wafer is removed using vacuum suction.

[0058] In step 6, surface purification and drying, high-purity deionized water is used for multi-stage overflow rinsing. The deionized water is prepared using multi-stage ion exchange resin and ultraviolet sterilization. The ion exchange resin employs a mixed-bed ion exchange process, achieving an effluent resistivity of 18.2 MΩ·cm (at 25°C). The ultraviolet sterilization lamps use dual-wavelength ultraviolet lamps of 185 nm and 254 nm, effectively killing bacteria and organic matter in the water.

[0059] The resistivity of deionized water in the initial cleaning stage is set between 15 MΩ·cm and 18 MΩ·cm, while the resistivity in the final cleaning stage is set between 17.5 MΩ·cm and 18.2 MΩ·cm. The cleaning time for each stage is set between 30 and 120 seconds, and the number of cleaning stages is set between 3 and 5. Overflow cleaning uses either top-in / bottom-out or bottom-in / top-out methods, optimizing water flow distribution to ensure thorough cleaning of every area on the wafer surface. The water flow rate is set between 0.5 L / min and 2 L / min, with the specific value determined based on the wafer size and cleaning tank volume.

[0060] After cleaning, high-purity isopropanol is used for vapor-phase drying. The isopropanol purity is set above 99.9%, and the moisture content is below 0.1%. Vapor-phase drying is achieved using a combination of rotary spin drying and vapor-phase drying. The spin-drying speed is set between 500 rpm and 3000 rpm, with the specific speed determined based on the wafer size. For example, for an 8-inch wafer, the spin-drying speed is set between 1500 rpm and 2000 rpm. The spin-drying time is set between 30 seconds and 120 seconds.

[0061] In the vapor-phase drying stage, the wafer is placed in an isopropanol vapor environment. The isopropanol vapor is generated by the evaporation of liquid isopropanol heated to 65°C to 80°C, and the vapor is kept constant through condensation and reflux. The wafer surface temperature is controlled using the following specific method: three infrared temperature sensors are arranged radially along the wafer within the drying chamber (located at the wafer center, halfway down the radius, and at the edge, respectively) to monitor the temperature distribution in real time. By adjusting the power zones of the heating lamps, the temperature difference from the wafer center to the edge is controlled within the range of 1°C to 5°C (i.e., a temperature gradient of 1°C / cm to 5°C / cm). The temperature gradient is achieved as follows: initially, all heating lamps heat at the same power; once the center temperature reaches the target value, the heating power in the edge region is gradually reduced, making the edge temperature lower than the center temperature, forming a decreasing temperature gradient from the center to the edge. This gradient value is precisely controlled by adjusting the heating power ratio of each region (edge ​​power is 60% to 90% of the center power). The cumulative drying time is set within the range of 2 to 10 minutes. Isopropanol has a surface tension of approximately 22 mN / m, which is significantly lower than that of water (72 mN / m), effectively reducing the risk of watermark residue and particulate re-adhesion.

[0062] In step 7, the cleaning effect verification, a laser particle counter and an atomic absorption spectrometer were used to sample and inspect the surface of the cleaned wafer. The laser particle counter used a wide-wavelength laser source, detecting particle sizes ranging from 50 nm to 10 μm, with a detection limit of 50 nm. During inspection, the wafer was placed on a scanning platform and automatically scanned according to a preset grid path. The scanning step was set to 1 mm × 1 mm to 5 mm × 5 mm, and the scanning coverage was set to 100%. The inspection results were characterized by the number of particles per square centimeter. The particle surface density on the cleaned wafer surface was required to be less than 100 particles / cm², and for particles with a diameter greater than 100 nm, the surface density was required to be less than 10 particles / cm².

[0063] Atomic absorption spectrometry is used for the quantitative detection of residual metal ions. This instrument employs graphite furnace atomization, achieving a detection sensitivity of up to 10. -9 g to 10 -12 g-level. Sample pretreatment employs a complete wafer surface wiping method, using high-purity wiping paper moistened with ultrapure nitric acid to systematically wipe the wafer surface, transferring surface contaminants to an acid solution, followed by atomic absorption spectrometry analysis. The detection range covers common metal elements such as iron, copper, aluminum, sodium, potassium, calcium, magnesium, and zinc. After cleaning, the total residual metal ions must be less than 5 ng / cm², and the residual amount of a single metal ion must be less than 1 ng / cm².

[0064] Only wafers that meet the preset cleanliness standards can proceed to the next process. The cleanliness standards are set according to the process requirements of the target product; for advanced processes (such as nodes below 28nm), the cleanliness requirements are more stringent. Test data is automatically uploaded to the Manufacturing Execution System (MES) for full traceability. For wafers that fail verification, a rework process is automatically triggered, returning to step 2 for reprocessing.

[0065] Experimental data from Example 1 of this invention show that, under contamination conditions where the initial particle areal density on the wafer surface is 5000 to 10000 particles / cm² (particle size range 50 nm to 1 μm) and the total metal ion concentration is 200 ng / cm² to 500 ng / cm², after treatment with the combined cleaning method of this invention, the particle areal density is reduced to 50 to 80 particles / cm², with a removal rate exceeding 99%; the total metal ion concentration is reduced to 2 to 4 ng / cm², with a removal rate exceeding 99%. The cleaning process cycle is 45 to 60 minutes, and the water consumption per wafer is 2 to 3 L. Compared with the traditional RCA cleaning process, the particle removal efficiency is improved by more than 30%, the residual metal ion content is reduced by more than 50%, and the cleaning solution consumption is reduced by more than 20%.

[0066] Example 2

[0067] This embodiment provides an alternative implementation of a combined cleaning method for 12-inch advanced process wafers. Based on Embodiment 1, this embodiment optimizes the process to meet the specific requirements of 12-inch wafers.

[0068] In Step 1, surface pre-assessment and contaminant analysis, the scanning area of ​​the 12-inch wafer was significantly increased, and the field of view of the ultra-depth-of-field microscope was adjusted to 20mm × 15mm. An automated stitching scanning algorithm was employed to ensure that the surface morphology analysis of the entire wafer was completed within 30 minutes. The surface particle counter used a high-speed scanning mode, with the scanning rate set between 100mm / s and 200mm / s, and the detection time for a single 12-inch wafer was controlled within 10 minutes. ICP-MS metal ion detection employed a micro-lift sample introduction system to reduce the sample consumption per detection.

[0069] In step 2, the nanoscale particle dispersion process, the ultrasonic tank volume is increased to 30L to 40L, capable of processing 2 to 4 12-inch wafers simultaneously. The ultrasonic power density is adjusted to the range of 0.8W / cm² to 1.2W / cm² to meet the needs of high-volume processing. The dispersant uses a composite formulation, composed of sodium polyacrylate and polyethylene glycol mixed in a 1:1 mass ratio, with molecular weights of 20,000 and 10,000 respectively, and a total concentration set in the range of 0.1% to 0.2%. The processing time is extended to the range of 15 to 25 minutes, with the specific value determined according to the segmentation rules described in step 2, based on the pre-assessed particle areal density D. While the wafers oscillate in the dispersion solution, a slow rotational motion is added, with the rotation speed set in the range of 5 to 10 revolutions per minute, to ensure uniform dispersion across the surfaces of multiple wafers.

[0070] In step 3, the first alkaline cleaning process, the cleaning tank volume is increased to 50L to 100L, capable of accommodating 2 to 4 wafers for batch cleaning. The volume ratio of ammonia to hydrogen peroxide in the cleaning solution is optimized to 1:5.5, and the cleaning solution temperature is optimized to 75℃ to 80℃. The silica sol concentration is optimized to 0.05% to 0.1%, and the particle size is optimized to the range of 10nm to 20nm. The surfactant is a compound system of sodium dodecylbenzenesulfonate and fatty alcohol polyoxyethylene ether, with a total mass fraction set in the range of 0.003% to 0.005%. The cleaning solution circulation rate is optimized to 1L / min to 1.5L / min, and the filtration accuracy is maintained at 0.3μm. The cleaning time is optimized to the range of 10 minutes to 15 minutes.

[0071] In the intermediate rinsing step, the resistivity of the deionized water used for rinsing is optimized to be between 12 MΩ·cm and 15 MΩ·cm, and the rinsing time is optimized to be between 60 and 90 seconds. During the rinsing process, the wafer is rotated at a speed of 10 revolutions per minute to ensure uniform rinsing.

[0072] In step 4, the second step of chelation cleaning, the chelating agent is a mixture of EDTA and DTPA in a molar ratio of 2:1 to 3:1. EDTA provides high chelation capacity, while DTPA enhances the removal of large-sized metal oxide particles. The pH of the chelation cleaning solution is optimized to 4.5 to 5.5, and the temperature is optimized to 50°C to 55°C. The corrosion inhibitor is a mixture of silane coupling agent and sodium molybdate, with a total concentration set in the range of 0.02% to 0.05%. The nitrogen stirring rate is optimized to 100 mL / min to 150 mL / min. The treatment time is optimized to the range of 8 minutes to 12 minutes.

[0073] In the metal ion reduction step, the reducing agent is a mixture of ascorbic acid and sodium bisulfite, with concentrations of 0.05 mol / L and 0.02 mol / L, respectively. The reduction treatment time is optimized to be within the range of 5 to 8 minutes. The pH value of the reducing agent solution is controlled within the range of 5.5 to 6.5.

[0074] In step 5, the enhanced removal of nanoparticles, the power of the megasonic transducer array was optimized to the range of 200W to 400W to meet the large-area cleaning requirements of 12-inch wafers. The distance between the wafer and the megasonic transducer was optimized to the range of 15mm to 25mm. The particle size of the nano-sized silica particles in the cleaning solution was optimized to 20nm to 50nm, and the particle mass concentration was optimized to 0.2g / L to 0.5g / L. The pH value of the cleaning solution was controlled in the range of 9.0 to 9.5, using a borate-sodium borate buffer system, with the buffer concentration optimized to 0.02mol / L to 0.03mol / L. The synergistic mechanism and verification method of this step are exactly the same as those described in step 5 of Example 1. The megasonic cleaning time was optimized to the range of 5 minutes to 8 minutes. The wafer moving linear speed was optimized to the range of 1mm / s to 2mm / s to ensure cleaning uniformity.

[0075] In step 6, surface purification and drying, the deionized water purification system is upgraded to a process combining two-stage reverse osmosis and electro-deionization, achieving an initial resistivity of 16 MΩ·cm to 18 MΩ·cm. The number of multi-stage overflow cleaning stages is increased to 4 to 5, with each stage's cleaning time optimized to within the range of 45 to 90 seconds. Overflow cleaning adopts a top-in, bottom-out method, with the water flow rate optimized to within the range of 1 L / min to 1.5 L / min.

[0076] During the vapor-phase drying stage, the temperature gradient control scheme is exactly the same as described in step 6 of Example 1. The isopropanol vapor temperature is optimized to a range of 65°C to 75°C. The spin-drying speed is optimized to 1200 rpm to 1800 rpm (applicable to 12-inch wafers), and the spin-drying time is optimized to a range of 60 seconds to 90 seconds. The vapor-phase drying time is optimized to a range of 4 minutes to 8 minutes. The wafer surface temperature gradient is controlled within a range of 2°C / cm to 4°C / cm.

[0077] In step 7, for the cleaning effect verification, a gridded sampling inspection scheme was adopted for 12-inch wafers. The wafer surface was divided into 9 regions (3×3 matrix), and particulate matter and metal ion detection was performed at the center of each region. The scanning step of the laser particle counter was optimized to 2mm×2mm, and the detection sensitivity was required to identify particles with a lower diameter limit of 50nm. The atomic absorption spectrometer used graphite furnace atomization, and the detection sensitivity was required to be in the range of 0.1ng / cm² to 0.5ng / cm².

[0078] Experimental data from Example 2 of this invention show that, under contamination conditions of an initial particle areal density of 8000 to 15000 particles / cm² and a total metal ion concentration of 300 to 600 ng / cm² on a 12-inch wafer surface, after treatment with the combined cleaning method of this invention, the particle areal density is reduced to 30 to 60 particles / cm², with a removal rate exceeding 99.5%; the total metal ion concentration is reduced to 1.5 to 3 ng / cm², with a removal rate exceeding 99.5%. The cleaning process cycle is 55 to 70 minutes, and the water consumption for cleaning a single wafer is 2.5 L to 3.5 L. When processing multiple wafers in batches, the average water consumption per wafer is reduced to 2 L to 2.5 L.

[0079] Example 3

[0080] This embodiment provides an alternative implementation of a combined cleaning method for silicon-based power device wafers. This method specifically optimizes the cleaning process parameters and chemical formulations to address the unique metal thin-film and thick-film structures present in power device manufacturing.

[0081] Power device wafers typically have thin metal films (such as aluminum, titanium, copper, etc.) or thick metal films formed on their surfaces. These metal layers have different tolerances to cleaning processes compared to silicon-based substrates. Therefore, this embodiment focuses on optimizing the protection measures for the metal layers in each step while ensuring the efficiency of removing nanoscale particles and metal ions.

[0082] In Step 1, surface pre-assessment and contaminant analysis, the integrity of the metal layer structure was assessed. The magnification range of the ultra-depth-of-field microscope was expanded to 50x to 1000x, enabling clear observation of the edge morphology and surface roughness changes of the metal layer. A white light interferometer was used to perform nanoscale three-dimensional morphology measurements on the metal layer surface, with a vertical resolution better than 1 nm, to evaluate the potential impact of the cleaning process on the metal layer. For metal ion detection, the focus was on elements related to the power device metal layer, such as aluminum (Al), titanium (Ti), and copper (Cu), with an ICP-MS detection limit better than 0.005 μg / L.

[0083] In step 2, the dispersion of nanoscale particles, the molecular weight of the dispersant was optimized to be in the range of 3000 to 20000 to reduce the mechanical impact of the dispersion process on the edges of the metal layer. The dispersant concentration was optimized to be in the range of 0.05% to 0.2%, and the ultrasonic power density was reduced to 0.3 W / cm². 2 Up to 0.8W / cm 2 Within the specified range, the processing time is controlled within the range of 8 to 15 minutes, with the specific value determined according to the segmentation rules described in step 2 and based on the pre-assessed particulate surface density D. 0.01% to 0.05% of a metal layer protectant (such as a silane coupling agent) is added to the pretreatment solution to form a temporary protective film on the metal layer surface.

[0084] In step 3, the alkaline cleaning process, the formulation of the alkaline cleaning solution was optimized. Considering the sensitivity of the metal layer to high pH values, the volume ratio of ammonia to hydrogen peroxide was adjusted to a range of 1:8 to 1:12, and the pH of the cleaning solution was controlled within the range of 9.5 to 10.5 (lower than the pH range of Example 1). The cleaning solution temperature was correspondingly reduced to a range of 55°C to 70°C. The silica sol concentration was increased to a range of 0.1% to 0.3%, and the silica sol particle size was controlled within the range of 10nm to 30nm to form a thicker temporary protective layer. A nonionic surfactant (such as Triton X-100) was used, with a concentration controlled within the range of 0.002% to 0.005%, to avoid electrochemical corrosion of the metal layer by ionic surfactants. The cleaning time was controlled within the range of 8 to 12 minutes.

[0085] During the intermediate rinsing step, the resistivity of the deionized water used for rinsing is increased to 15 MΩ·cm to 18 MΩ·cm, and the rinsing time is extended to 60 to 120 seconds to ensure that alkaline cleaning solution residue is fully removed. The rinsing water temperature is controlled within the range of 15°C to 25°C to avoid thermal shock to the metal layer caused by temperature changes.

[0086] In step 4, the second step of chelation cleaning, the chelating agent formulation was optimized based on the characteristics of the power device wafer. The chelating agent mainly uses a mixture of NTA and EDTA, with DTPA reduced or omitted (DTPA's excessive chelating ability for aluminum ions may affect the aluminum metal layer). The pH of the chelation cleaning solution was controlled within the range of 4.5 to 5.5, and the temperature within the range of 45°C to 55°C to reduce the impact of the acidic environment on the metal layer. A compound system of corrosion inhibitors was used, including silane coupling agent (concentration 0.02% to 0.05%), molybdate (concentration 0.01% to 0.03%), and phosphate ester corrosion inhibitor (concentration 0.01% to 0.02%), with a required corrosion inhibition efficiency of better than 98%. The nitrogen stirring rate was reduced to the range of 30 mL / min to 100 mL / min to minimize the impact of mechanical disturbance on the metal layer. The processing time was controlled within the range of 6 to 10 minutes.

[0087] In the metal ion reduction step, the reducing agent concentration is optimized to be in the range of 0.02 mol / L to 0.05 mol / L, and the treatment time is controlled within the range of 3 to 6 minutes. The reduction treatment temperature is controlled at room temperature (20℃ to 25℃) to avoid affecting the metal layer due to temperature rise.

[0088] In step 5, the enhanced removal of nanoparticles, the megasonic frequency was optimized to be in the range of 0.7 MHz to 0.9 MHz to reduce the potential damage to the metal layer edges caused by high-frequency vibrations. The power of the megasonic transducer array was controlled in the range of 80 W to 300 W. The particle size of the nano-sized silica particles in the cleaning solution was optimized to be 15 nm to 40 nm, and the particle mass concentration was controlled in the range of 0.1 g / L to 0.4 g / L. The pH value of the cleaning solution was controlled in the range of 8.0 to 9.0 (lower than the pH value of Example 1), using a borate-sodium borate buffer system, with the buffer concentration controlled in the range of 0.01 mol / L to 0.03 mol / L. The synergistic mechanism and verification method of this step are exactly the same as those described in step 5 of Example 1. The megasonic cleaning time was controlled in the range of 4 minutes to 7 minutes. The wafer moving linear speed was controlled in the range of 0.5 mm / s to 1.5 mm / s to ensure uniform distribution of cleaning energy.

[0089] In step 6, surface purification and drying, the resistivity of deionized water was maintained within the range of 17 MΩ·cm to 18.2 MΩ·cm throughout. The multi-stage overflow rinsing was set to 4 to 6 stages, with each stage's rinsing time controlled within the range of 45 to 90 seconds. The water flow rate was controlled within the range of 0.5 L / min to 1 L / min to avoid high-speed water flow eroding the edges of the metal layer.

[0090] During the vapor-phase drying stage, the temperature gradient control scheme is exactly the same as described in step 6 of Example 1, with the isopropanol vapor temperature controlled within the range of 60°C to 70°C. The spin-drying speed is reduced to the range of 400 rpm to 1200 rpm (optimized according to the metal layer thickness and adhesion), and the spin-drying time is controlled within the range of 45 seconds to 90 seconds. The vapor-phase drying time is controlled within the range of 3 minutes to 6 minutes. The wafer surface temperature gradient is controlled within the range of 1°C / cm to 3°C / cm.

[0091] In step 7, the verification of the cleaning effect was expanded to include verification of the integrity of the metal layer structure. A four-point probe was used to measure the change in sheet resistance of the metal layer, requiring the change to be less than 2% after cleaning. Scanning electron microscopy (SEM) was used to observe the edge morphology of the metal layer, requiring no obvious edge corrosion or peeling. X-ray photoelectron spectroscopy (XPS) was used to analyze the surface composition of the metal layer, requiring no obvious oxidation or contamination residue.

[0092] Experimental data from Example 3 of this invention show that on the surface of a 6-inch power device wafer with an aluminum metal thin film layer (thickness 1μm to 3μm), under contamination conditions with an initial particle areal density of 3000 particles / cm² to 8000 particles / cm² and a total metal ion concentration of 150 ng / cm² to 400 ng / cm², after treatment with the combined cleaning method of this invention, the particle areal density is reduced to 40 particles / cm² to 70 particles / cm², with a removal rate of over 99%; the total metal ion concentration is reduced to 3 ng / cm² to 5 ng / cm², with a removal rate of over 98.5%. The sheet resistance change of the metal layer after cleaning is controlled within 1%, the edge morphology of the metal layer remains intact, and there is no obvious corrosion or peeling. The cleaning process cycle is 50 to 65 minutes, and the water consumption for cleaning a single wafer is 2L to 3L.

[0093] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. The scope of protection of the present invention is not limited to the above embodiments; all embodiments employing the same or substantially the same structure or method to achieve the same function are within the scope of protection of the present invention.

Claims

1. A combined cleaning method for nanoscale particles and metal ion residues on wafer surfaces, characterized in that, Includes the following steps: Step 1, Surface pre-assessment and contaminant analysis: Nanoscale particles on the wafer surface were detected using an ultra-depth-of-field microscope and a surface particle counter, and the type of metal ions was detected using inductively coupled plasma mass spectrometry. Step 2, Nanoscale particle dispersion treatment: The wafer is placed in a pretreatment solution containing a dispersant and subjected to ultrasonic dispersion treatment. Step 3, the first step of alkaline cleaning: clean with an alkaline cleaning solution containing surfactants and silica sol; Step 4, the second step of chelation cleaning: clean with an acidic chelation cleaning solution containing a chelating agent; Step 5, enhanced removal of nanoparticles: cleaning is performed using a megasonic-assisted chemical cleaning solution containing nano-sized silica particles; Step 6, Surface purification and drying: Multi-stage overflow cleaning is performed using high-purity deionized water, followed by vapor-phase drying using isopropanol; Step 7, Cleaning effect verification: The surface of the cleaned wafer is sampled and tested using a laser particle counter and an atomic absorption spectrometer.

2. The combined cleaning method according to claim 1, characterized in that, In step 1, the magnification of the ultra-depth-of-field microscope is 100x to 500x, and the field of view is 2.5mm×1.9mm to 10mm×7.5mm. The surface particle counter adopts the principle of light scattering, with a laser wavelength of 488nm or 635nm. The detection sensitivity can identify particles with a lower limit of 50nm. The metal ion type analysis adopts inductively coupled plasma mass spectrometry, and the detection range covers sodium, magnesium, aluminum, potassium, calcium, iron, copper and zinc elements.

3. The combined cleaning method according to claim 1, characterized in that, In step 2, the pretreatment solution also contains a nonionic surfactant at a concentration of 0.001% to 0.01%, and the ultrasonic frequency is 40kHz to 80kHz. During the treatment process, the wafer reciprocates in the pretreatment solution at a frequency of 0.1Hz to 0.5Hz and an amplitude of 20mm to 50mm to enhance the dispersion effect and avoid excessive local temperature.

4. The combined cleaning method according to claim 1, characterized in that, In step 3, the cleaning solution also contains 0.01%–0.5% silica sol with a particle size of 5nm–50nm. During the cleaning process, the cleaning solution is circulated and refreshed at a flow rate of 0.5L / min–2L / min to ensure that the particulate matter concentration in the cleaning solution is maintained at 10. 6 Below 1 / L.

5. The combined cleaning method according to claim 1, characterized in that, In step 4, the chelating cleaning solution also contains a corrosion inhibitor at a concentration of 0.01% to 0.1%. The corrosion inhibitor is a silane coupling agent or a molybdate substance. During the cleaning process, nitrogen gas is used for stirring at a stirring rate of 50 mL / min to 200 mL / min to accelerate the chelation reaction and prevent carbon dioxide in the air from dissolving into the cleaning solution and causing local pH fluctuations.

6. The combined cleaning method according to claim 1, characterized in that, In step 5, the megasonic-assisted cleaning solution contains silica particles with a particle size of 10nm to 100nm, a mass concentration of 0.1g / L to 1g / L, a pH value of 8.5 to 9.5, and uses a borate-sodium borate buffer system with a buffer concentration of 0.01mol / L to 0.05mol / L. The power of the megasonic transducer array is 100W to 500W, the distance between the wafer and the megasonic transducer is 10mm to 30mm, and the wafer moves in the megasonic field at a linear velocity of 0.1mm / s to 5mm / s to ensure cleaning uniformity.

7. The combined cleaning method according to claim 1, characterized in that, In step 6, the high-purity deionized water adopts a multi-stage ion exchange and ultraviolet sterilization process. The resistivity of the deionized water in the initial cleaning stage is 15 MΩ·cm to 18 MΩ·cm, and the resistivity in the final cleaning stage is 17.5 MΩ·cm to 18.2 MΩ·cm. The cleaning time for each stage is 30s to 120s. The overflow cleaning adopts the top-in-bottom-out or bottom-in-top-out method, and the water flow rate is 0.5L / min to 2L / min. The gas phase drying adopts a combination of rotary spin drying and gas phase drying, and the spin drying speed is 500rpm to 3000rpm.

8. The combined cleaning method according to claim 1, characterized in that, It also includes an intermediate rinsing step set between step 3 and step 4: the wafer is quickly rinsed with deionized water for 30 to 120 seconds. The resistivity of the deionized water is 10 MΩ·cm to 15 MΩ·cm. During the rinsing process, the water film on the wafer surface remains intact to ensure that there is no chemical reaction between the alkaline cleaning solution and the chelating cleaning solution, which would affect the cleaning effect and the wafer surface quality.

9. The combined cleaning method according to claim 1 or 8, characterized in that, It also includes a metal ion reduction step set between steps 4 and 5: the wafer is treated with a reducing agent solution with a concentration of 0.01 mol / L to 0.1 mol / L. The reducing agent is ascorbic acid or sodium bisulfite. The treatment time is 2 min to 10 min. The pH value of the reducing agent solution is 5.0 to 7.

0. This is to reduce the oxidized metal ions that may exist on the wafer surface to the elemental state, so that they can be removed by megasonic cleaning in subsequent steps.

10. The combined cleaning method according to claim 1, characterized in that, The dispersion processing time in step 2 is determined as follows: based on the surface density D of particles with a diameter ≥ 50 nm measured by the surface particle counter in step 1, when D ≤ 1000 particles / cm² 2 When the processing time is 8 minutes; when 1000 < D ≤ 5000 pieces / cm 2 When the processing time is 15 minutes; when D > 5000 pieces / cm 2 The processing time is 25 minutes; intermediate values ​​are calculated using linear interpolation.

Citation Information

Patent Citations

  • A cleaning process to improve the surface cleanliness of large-diameter silicon wafers after edge polishing

    CN111211042B

  • Silicon wafer cleaning method for improving quality of metal and particles on surface of polished silicon wafer

    CN116631848A