A method for etching power devices using small linewidth photolithography
By using an I-line lithography machine and an anti-reflective layer to form a sidewall structure on the photoresist sidewall, the problem of stringent warpage requirements of DUV equipment is solved, enabling low-cost, highly compatible small-linewidth lithography processing.
Patent Information
- Application Number
- CN202611431530.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, DUV equipment has stringent requirements on wafer warpage, resulting in low wafer compatibility for power devices with large warpage, high equipment costs, and difficulty in achieving small linewidth lithography processing.
By using an I-line lithography machine and I-line photoresist, combined with an anti-reflective layer, and forming a sidewall structure on the sidewall of the photoresist, small linewidth photolithography can be achieved, avoiding the use of DUV equipment.
It reduces equipment and chemical costs, improves wafer warpage compatibility, enables small linewidth lithography on wafers with greater warpage, avoids wafer scrap, and simplifies the process flow.
Smart Images

Figure CN123124764A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of semiconductor device processing technology, and specifically relates to a method for small linewidth photolithography etching of power devices. Background Technology
[0002] Power devices have undergone continuous iterations to improve power density, and the unit cell size of devices has been continuously reduced. The iterative iteration of device structures has also further increased the requirements for wafer manufacturing processes and equipment capabilities. Small linewidth photolithography in mainstream power device structures and processing technologies is mainly used for key layers of devices, such as the trench layer and contact hole layer of trench gate IGBTs (Insulated Gate Bipolar Transistors).
[0003] Existing processing methods typically employ more advanced lithography equipment and photoresists, such as DUV (Deep Ultraviolet) lithography machines and DUV photoresists. However, DUV equipment is not only expensive to acquire, but also has extremely stringent requirements regarding wafer warp. For power device wafers, especially IGBT wafers with significant warp, conventional DUV equipment cannot process them properly when the warp exceeds 150μm, easily leading to wafer scrap. Because DUV equipment has stricter requirements regarding wafer warp, it has lower compatibility with power device wafers, especially those with large warps.
[0004] In addition, although there are existing technologies that use BARC for photolithography, they are usually used in conjunction with DUV photolithography coating to serve as an anti-reflective coating to improve the stability of the linewidth during DUV exposure. Summary of the Invention
[0005] To address the aforementioned problems in the prior art, this invention provides a method for small-linewidth photolithography etching of power devices. This invention provides a method for small-linewidth photolithography etching of power devices, comprising: Select a substrate wafer to be processed, and deposit a hard mask layer or a dielectric layer on the substrate wafer to be processed; I-line photoresist is coated onto the hard mask layer or dielectric layer to obtain the coated device; The coated device is exposed and developed using an I-line lithography machine to form an initial photoresist pattern; An anti-reflective layer is coated on the top, sidewalls, and exposed hard mask layer or dielectric layer surface of the initial photoresist pattern to obtain the coated device. Dry etching is performed on the coated device to remove the anti-reflective layer covering the top of the initial photoresist pattern and the surface of the hard mask layer or dielectric layer. The anti-reflective layer attached to the sidewalls of the photoresist forms sidewalls. Dry etching is then performed on the hard mask layer or dielectric layer to form a power device with a small linewidth structure by removing the photoresist.
[0006] In one embodiment of the present invention, the thickness of the hard mask layer or dielectric layer is 0.10 μm-1.50 μm.
[0007] In one embodiment of the present invention, the thickness of the I-line photoresist is 5000Å-30000Å.
[0008] In one embodiment of the present invention, when using an I-line lithography machine for exposure, the target CD is 0.30μm-0.50μm and the wavelength of the exposure light source is 340nm-400nm.
[0009] In one embodiment of the present invention, the thickness of the anti-reflective layer is 400Å-2000Å, and the thickness of the anti-reflective layer is adjusted according to the linewidth requirements after etching.
[0010] In one embodiment of the present invention, the antireflective layer comprises BARC or TARC or a photoresist material with similar viscosity.
[0011] In one embodiment of the present invention, the width of the sidewall is positively correlated with the coating thickness when coating the antireflective layer; the height of the sidewall is positively correlated with the coating thickness when coating the I-line photoresist.
[0012] In one embodiment of the present invention, the upper limit of the absolute value of the warp of the substrate wafer to be processed is between 150 μm and 200 μm.
[0013] In one embodiment of the present invention, the linewidth of the power device having a small linewidth structure is less than or equal to 0.30 μm.
[0014] The beneficial effects of this invention are: Significantly reduced processing costs: The processing technology provided by this invention can meet the manufacturing requirements of small linewidth lithography without using DUV equipment or DUV-specific photoresist; Significantly improved wafer warpage compatibility: Under the same linewidth requirements, this invention has greater compatibility with wafer warpage, and the wafer warpage tolerance is relaxed from 150μm in DUV equipment to more than 200μm, effectively avoiding wafer scrap due to excessive warpage. The process is simple and reliable: This invention adds a BARC coating process, which does not require hardware modification of existing I-line lithography equipment, making it highly adaptable. Attached Figure Description
[0015] Figure 1 This is a schematic diagram illustrating the steps of a small-linewidth photolithography etching method for power devices provided in an embodiment of the present invention; Figures 2-4 This is a schematic diagram comparing a method for small-linewidth photolithography etching of power devices provided in an embodiment of the present invention with a conventional processing method; Figure 5 This is a schematic diagram comparing the device structure after processing using a small-linewidth photolithography etching method for power devices provided in an embodiment of the present invention with that of a conventional method. Detailed Implementation
[0016] The present invention will be further described in detail below with reference to specific embodiments, but the implementation of the present invention is not limited thereto.
[0017] The purpose of this invention is to provide a photolithography etching method based on I-line photolithography equipment to achieve small linewidth processing capabilities, without the need for DUV photolithography machines to achieve linewidth photolithography capabilities such as 0.25µm or even less than 0.2µm, thereby reducing production line equipment investment costs and wafer manufacturing costs.
[0018] like Figure 1 As shown in the embodiment of the present invention, a method for small-linewidth photolithography etching of power devices may include the following steps: S1, Select the substrate wafer to be processed, and deposit a hard mask layer or dielectric layer on the substrate wafer to be processed.
[0019] After the processing corresponding to step S1, a comparative schematic diagram of the processing procedures of the embodiment of the present invention and the conventional solution is shown below. Figure 2 As shown, the two processes are similar.
[0020] The hard mask layer or dielectric layer is a small linewidth layer that requires photolithography and etching, and its thickness can be 0.10 μm-1.50 μm. This embodiment of the invention uses 0.2 μm as an example.
[0021] S2, Coating I-line photoresist onto a hard mask layer or dielectric layer to obtain the coated device; The thickness of the I-line photoresist can range from 5000 Å to 30000 Å.
[0022] S3, using an I-line lithography machine to expose and develop the coated device to form the initial photoresist pattern.
[0023] When using an I-line lithography machine for exposure, the target depth (CD) is 0.30μm-0.50μm, and the wavelength of the exposure light source is 340nm-400nm. In this embodiment of the invention, the target CD can be set to 0.3μm, resulting in a linewidth of approximately 0.3µm after development.
[0024] The height of the subsequently formed sidewalls is adjusted by regulating the thickness of the I-line photoresist to ensure subsequent etching resistance. The sidewall structure must guarantee that the underlying material will not be etched. After the processing corresponding to steps S2 and S3, a comparative schematic diagram of the processing procedures of the embodiment of the present invention and the conventional solution is shown below. Figure 3 As shown, the embodiments of the present invention only require coating the dielectric layer with I-line photoresist and then exposing and developing it using an I-line lithography machine. In contrast, conventional methods require coating the dielectric layer with BARC and DUV photoresist sequentially and must use a DUV lithography machine for exposure.
[0025] Understandably, the embodiments of the present invention can be processed using an I-line lithography machine, which offers better cost-effectiveness compared to DUV lithography machines and has better compatibility with wafers with large warpage. The upper limit of the absolute value of the wafer warpage (Warp) of the substrate wafer to be processed can be between 150μm and 200μm. In contrast, the upper limit of the absolute value of the wafer warpage (Warp) of DUV equipment is typically between 100-150μm. It can be seen that the embodiments of the present invention are more compatible and adaptable to wafers with large warpage, such as IGBTs.
[0026] Compared to conventional solutions, this invention utilizes an I-line lithography machine and photoresist, resulting in lower equipment and chemical costs. Conventional solutions, requiring a linewidth of around 0.2µm, cannot process wafers with warpage exceeding 150µm on DUV. However, this invention allows wafers with warpages of 150µm-200µm or even up to 250µm to be processed on I-line lithography equipment, preventing wafer scrap due to excessive warpage.
[0027] S4. An anti-reflective layer is coated on the top and sidewalls of the initial photoresist pattern and on the surface of the exposed hard mask layer or dielectric layer to obtain the coated device.
[0028] The thickness of the anti-reflective layer can be 400Å-2000Å, and the thickness can be adjusted according to the linewidth requirements after etching.
[0029] The photoresist for the anti-reflective layer can include BARC, TARC, or photoresists with similar viscosities. Selection primarily considers requirements such as suitable sidewall etching resistance and coating thickness. The size of the CD (Cut-off Disc) is adjusted by regulating the thickness of the anti-reflective layer; the coating thickness needs to be between 400 Å and 2000 Å. The thickness of the I-line photoresist and the anti-reflective layer ensure the etching depth of the hard mask layer or dielectric layer and the CD size.
[0030] The embodiments of the present invention only add a BARC coating process and a conventional dry etching process, which enables the fabrication of structures with small linewidths on an I-line lithography platform.
[0031] S5. Dry etching is performed on the coated device to remove the anti-reflective layer covering the top of the initial photoresist pattern and the surface of the hard mask layer or dielectric layer. The anti-reflective layer attached to the sidewalls of the photoresist forms sidewalls. Dry etching is performed on the hard mask layer or dielectric layer to form a power device with a small linewidth structure by removing the photoresist.
[0032] Dry etching is performed on the coated device to remove the anti-reflective layer covering the top of the initial photoresist pattern and the surface of the hard mask layer or dielectric layer. The anti-reflective layer attached to the sidewalls of the photoresist forms sidewalls. Dry etching continues to complete the etching of the hard mask layer or dielectric layer. Then, the power device with a small linewidth structure is obtained by removing the photoresist.
[0033] The width of the sidewalls is positively correlated with the coating thickness of the anti-reflective layer; the height of the sidewalls is positively correlated with the coating thickness of the I-line photoresist. In this embodiment of the invention, by adding an anti-reflective layer, a sidewall structure is formed on the photoresist sidewalls after exposure and development on the I-line lithography platform. The sidewall dimensions are adjusted by changing the thickness of the anti-reflective layer, ultimately ensuring that the bottom linewidth meets processing requirements after etching.
[0034] A comparative schematic diagram of the processing procedures of this embodiment and a conventional method after etching away the anti-reflective layer covering the initial photoresist pattern is shown below. Figure 4 As shown in the diagram, a comparison of the device structures after processing is presented. Figure 5 As shown, the embodiments of the present invention can achieve the same technical effect as conventional solutions using DUV lithography machines by simply coating an anti-reflective BARC layer and etching it with an I-line lithography machine.
[0035] Power devices with small linewidth structures have a linewidth of less than or equal to 0.30 μm.
[0036] The core principle of this invention lies in the following: After exposure and development on the photoresist sidewalls of an I-line lithography platform, an anti-reflective layer is coated to form a sidewall structure. The width of the sidewalls is used to reduce the final etched linewidth. By adjusting the thickness of the anti-reflective layer, the sidewall dimensions can be precisely controlled, ensuring that the bottom linewidth after etching meets processing requirements. This invention primarily improves the lithography and etching processes. By using an I-line lithography machine, I-line photoresist, and an anti-reflective layer in conjunction with the etching process, the requirement for small linewidth etching is achieved. The final etched CD achieves the capabilities of conventional DUV lithography without requiring additional, more advanced and expensive DUV equipment.
[0037] This invention enables the fabrication of small-linewidth lithography without using DUV technology, and offers greater compatibility with wafer warpage while maintaining the same linewidth requirements. This invention primarily addresses the need to fabricate small-linewidth power devices without DUV equipment, requiring only the introduction of sidewall structures composed of BARC or TARC to achieve the fabrication of power devices with small-linewidth structures.
[0038] According to the solution provided in the embodiments of the present invention, it is possible to process hard mask layers and hole layers of Trench MOS on an I-line lithography platform without the need for a DUV lithography machine. For example, the processing of low-voltage Trench MOS devices generally requires lithography and etching of a 0.2µm hard mask layer and contact hole layer.
[0039] According to the solution provided in the embodiments of the present invention, the hole layer processing of micro-trench IGBTs can be realized on an I-line lithography platform without the need for a DUV lithography machine. A 0.2µm contact hole structure can be achieved, offering higher cost-effectiveness. Furthermore, due to the relatively large wafer warpage of micro-trench IGBTs, the embodiments of the present invention have better compatibility compared to the DUV solution.
[0040] It should be noted that, in the description of this invention, the terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," and "counterclockwise," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.
[0041] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this invention, "a plurality of" means two or more, unless otherwise explicitly specified.
[0042] The above description is merely a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention are included within the scope of protection of the present invention.
Claims
1. A method for small-linewidth photolithography etching of power devices, characterized in that, include: Select a substrate wafer to be processed, and deposit a hard mask layer or a dielectric layer on the substrate wafer to be processed; I-line photoresist is coated onto the hard mask layer or dielectric layer to obtain the coated device; The coated device is exposed and developed using an I-line lithography machine to form an initial photoresist pattern; An anti-reflective layer is coated on the top, sidewalls, and exposed hard mask layer or dielectric layer surface of the initial photoresist pattern to obtain the coated device. Dry etching is performed on the coated device to remove the anti-reflective layer covering the top of the initial photoresist pattern and the surface of the hard mask layer or dielectric layer. The anti-reflective layer attached to the sidewalls of the photoresist forms sidewalls. Dry etching is then performed on the hard mask layer or dielectric layer to form a power device with a small linewidth structure by removing the photoresist.
2. The method for small-linewidth photolithography etching of power devices according to claim 1, characterized in that, The thickness of the hard mask layer or dielectric layer is 0.10μm-1.50μm.
3. The method for small-linewidth photolithography etching of power devices according to claim 1, characterized in that, The thickness of the I-line photoresist is 5000Å-30000Å.
4. The method for small-linewidth photolithography etching of power devices according to claim 1, characterized in that, When using an I-line lithography machine for exposure, the target CD is 0.30μm-0.50μm, and the wavelength of the exposure light source is 340nm-400nm.
5. The method for small-linewidth photolithography etching of power devices according to claim 1, characterized in that, The thickness of the anti-reflective layer is 400Å-2000Å, and the thickness of the anti-reflective layer is adjusted according to the linewidth requirements after etching.
6. The method for small-linewidth photolithography etching of power devices according to claim 1, characterized in that, The anti-reflective layer comprises BARC or TARC or a photoresist material with similar viscosity.
7. The method for small-linewidth photolithography etching of power devices according to claim 1, characterized in that, The width of the sidewall is positively correlated with the coating thickness when applying the anti-reflective layer; the height of the sidewall is positively correlated with the coating thickness when applying the I-line photoresist.
8. The method for small-linewidth photolithography etching of power devices according to claim 1, characterized in that, The upper limit of the absolute value of the warp of the substrate wafer to be processed is between 150μm and 200μm.
9. The method for small-linewidth photolithography etching of power devices according to claim 1, characterized in that, The power device with a small linewidth structure has a linewidth of less than or equal to 0.30 μm.